Composite metal foil and metal-clad laminate

By limiting the surface energy and polar component of the copper surface after hot pressing of the composite metal foil, the problems of large surface energy fluctuations and uneven polar components after peeling of the peelable copper foil are solved, achieving a stable bond between the copper surface and the polymer material, and improving the manufacturing yield and reliability of fine circuits.

CN123129546APending Publication Date: 2026-11-20GUANGZHOU FANGBANG ELECTRONICS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611287361.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing peelable copper foils exhibit large surface energy fluctuations and uneven polar composition after peeling, leading to process defects such as photoresist shrinkage and pattern detachment, which affect the yield and quality of fine circuits.

Method used

After precise standard hot-pressing of the composite metal foil, the total surface energy of the functional layer near the release layer is 40-60 mJ/m², and the polar component accounts for ≥30%, achieving stable interfacial physical adsorption and chemical bonding.

Benefits of technology

This ensures that polar polymer materials such as photoresist and epoxy resin form a stable interface bond with the copper surface, reducing process defects and improving the yield and reliability of fine circuit manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129546A_ABST
    Figure CN123129546A_ABST
Patent Text Reader

Abstract

The application discloses a composite metal foil and a metal-clad laminate. The composite metal foil comprises a carrier layer, a stripping layer and a functional layer which are sequentially stacked; after the standard hot pressing treatment and stripping of the carrier layer, the total surface energy of the side surface of the functional layer close to the stripping layer is 40-60 mJ / m 2 , wherein the proportion of the polar component in the total surface energy is greater than or equal to 30%; the standard hot pressing treatment refers to that after the side of the functional layer away from the stripping layer is stacked with an epoxy resin prepreg, the stacking is pressed under the condition of 200 DEG C, 2 MPa and vacuum for 2 h, and then naturally cooled to room temperature. Through the accurate limitation of the surface energy and the polar component of the functional copper layer after stripping, the stable physical adsorption and chemical combination double interface action mechanism between the copper surface and polar polymer materials such as photoresist and epoxy resin is realized, and the manufacturing yield and reliability of the fine line are improved from the root.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electronic information materials technology, and in particular to a composite metal foil and a metal-clad laminate. Background Technology

[0002] Peelable ultrathin copper foil with carrier is a core material for high-end PCBs, IC substrates, and 2.5D / 3D advanced packaging redistribution layers, and a key consumable for achieving micron-level fine circuit manufacturing. As downstream electronic manufacturing processes continue to upgrade towards higher density and higher reliability, the industry's performance requirements for peelable copper foil have gradually extended from "stable peelability" to compatibility with downstream photolithography, lamination, and other processes after peeling.

[0003] Currently, the industry's R&D and performance control are highly focused on the iteration of release layer material systems, optimization of ultra-thin copper layers and low roughness, and improvement of release force stability. All indicators are designed around the release action itself, with little control over the surface energy and polar components of the functional copper layer after release. Due to the lack of targeted structural design and parameter control, existing peelable copper foils generally suffer from large fluctuations in surface energy and uneven polar components after release, which can easily lead to defects such as photoresist shrinkage, pattern detachment, and dry film curling in subsequent processes. At the same time, poor overall performance uniformity further restricts the yield improvement of fine circuits and affects circuit quality. Summary of the Invention

[0004] This invention provides a composite metal foil and a metal-clad laminate to solve the problems of large fluctuations in the surface energy of the copper surface and uneven polar composition after peeling of the copper foil in the prior art.

[0005] According to one aspect of the present invention, a composite metal foil is provided, comprising: a carrier layer, a release layer, and a functional layer sequentially stacked; After the composite metal foil undergoes standard hot-pressing treatment and the carrier layer is peeled off, the total surface energy of the functional layer on the side near the peeling layer is 40~60 mJ / m². 2 Of which, the polar component accounts for ≥30% of the total surface energy; The standard hot pressing process refers to: stacking the side of the functional layer away from the release layer with the epoxy resin prepreg, pressing it at 200°C and 2MPa vacuum for 2 hours, and then naturally cooling it to room temperature.

[0006] Optionally, after the composite metal foil is hot-pressed and the carrier layer is peeled off, the surface energy fluctuation coefficient of the functional layer on the side near the peeling layer is ≤10%. The surface energy fluctuation coefficient is the ratio of the sample standard deviation to the arithmetic mean of the surface energy at each test point.

[0007] Optionally, after the composite metal foil is hot-pressed and the carrier layer is peeled off, it is placed in a standard environment of 25°C and 50% relative humidity for 24 hours. The total surface energy retention rate of the side of the functional layer near the peeling layer is ≥90%, and the polar component accounts for ≥30% of the total surface energy.

[0008] Optionally, after the composite metal foil undergoes standard hot pressing treatment, the peel force retention rate between the carrier layer and the functional layer is 80%~120%, and the peel force fluctuation coefficient is ≤10%.

[0009] Optionally, after the composite metal foil is hot-pressed and the carrier layer is peeled off, the total amount of non-copper metal elements remaining on the side of the functional layer near the peeling layer is ≤1at.

[0010] Optionally, the (111) crystal plane texture coefficient of the functional layer is ≥70%, and the grain size dispersion is ≤20%.

[0011] Optionally, the release layer is a composite release layer composed of an amorphous alloy metal layer and a nitrogen-containing organic layer, wherein the amorphous alloy layer and the nitrogen-containing organic layer are sequentially disposed on the surface of the carrier layer.

[0012] Optionally, an antioxidant layer is provided on the side of the functional layer away from the peeling layer.

[0013] Optionally, a heat-resistant layer is provided on the side of the carrier layer away from the peeling layer.

[0014] According to another aspect of the present invention, a metal-clad laminate is provided, the metal-clad laminate being made using the functional layer of a composite metal foil as one of the materials described in any one of the preceding aspects.

[0015] The technical solution of this invention, by precisely limiting the total surface energy of the functional layer near the release layer to 40-60 mJ / m² after standard hot-pressing and peeling off the carrier layer, achieves this. 2 Furthermore, the polar component accounts for ≥30% of the total surface energy, achieving stable interfacial physical adsorption and chemical bonding. When the total surface energy of the functional copper layer exfoliation surface is between 40 and 60 mJ / m², [this is achieved]. 2When the surface energy is within a suitable range, it ensures that polar polymer materials such as photoresist and epoxy resin are fully wetted and spread on the copper surface, avoiding poor wetting due to excessively low surface energy or rapid adsorption of contaminants due to excessively high surface energy. Simultaneously, by ensuring a polar component ratio of ≥30%, it ensures that the copper surface has a sufficient number of polar functional groups to form dipole interactions, hydrogen bonds, and even coordination bonds with the polar groups in the photoresist and epoxy resin, achieving a dual-interface mechanism of "physical adsorption and chemical bonding." This fundamentally reduces process defects and improves the yield of fine-line manufacturing. By limiting the total surface energy and polar component ratio of the copper surface after stripping to a specific range, it ensures a stable and reliable interfacial bond between the copper surface and various polar polymer materials that come into contact with it in subsequent processes. In summary, this invention solves the problems of large fluctuations in the surface energy of the copper surface and uneven polar composition after peeling off the peelable copper foil in the prior art. It achieves small fluctuations in the surface energy of the copper surface and uniform polar composition after peeling off the peelable copper foil, realizing a stable physical adsorption and chemical bonding dual-interface interaction mechanism between the copper surface and the polymer material, thereby fundamentally improving the manufacturing yield and reliability of fine circuits.

[0016] It should be understood that the description in this section is not intended to identify key or essential features of the embodiments of the present invention, nor is it intended to limit the scope of the invention. Other features of the invention will become readily apparent from the following description. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a schematic diagram of the structure of a composite metal foil according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of another composite metal foil provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of another composite metal foil provided in an embodiment of the present invention; Figure 4 This is a schematic diagram of the structure of another composite metal foil provided according to an embodiment of the present invention.

[0019] Explanation of reference numerals in the attached figures: 10. Carrier layer; 20. Release layer; 21. Amorphous alloy metal layer; 22. Nitrogen-containing organic layer; 30. Functional layer; 40. Antioxidant layer; 50. Heat-resistant layer. Detailed Implementation

[0020] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0021] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0022] Figure 1 This is a schematic diagram of a composite metal foil according to an embodiment of the present invention, with reference to... Figure 1 An embodiment of the present invention provides a composite metal foil, comprising: a carrier layer 10, a release layer 20, and a functional layer 30 sequentially stacked; after the composite metal foil undergoes standard hot-pressing treatment and the carrier layer 10 is released, the total surface energy of the side of the functional layer 30 near the release layer 20 is 40~60 mJ / m². 2 The polar component accounts for ≥30% of the total surface energy; the standard hot pressing process refers to: after stacking the side of the functional layer 30 away from the release layer 20 with the epoxy resin prepreg, pressing it at 200℃ and 2MPa vacuum for 2 hours, and then naturally cooling it to room temperature.

[0023] Specifically, the carrier layer 10 provides mechanical support for the ultrathin functional layer 30, facilitating production, transportation, and processing. The carrier layer 10 can be made of copper foil, aluminum foil, polymer films (such as polyimide or polyester films), or surface-treated versions of the above materials, preferably electrolytic copper foil or rolled copper foil, with a thickness typically ranging from 12 μm to 70 μm.

[0024] A release layer 20 is disposed between the carrier layer 10 and the functional layer 30 to achieve a separable bond between the carrier layer 10 and the functional layer 30. The release layer 20 should have sufficient heat resistance and bonding strength during hot pressing to prevent the functional layer 30 from separating prematurely before pressing; after hot pressing, it should be able to cleanly separate the carrier layer 10 and the functional layer 30 by mechanical peeling without leaving excessive residue on the surface of the functional layer 30.

[0025] The functional layer 30 is an ultra-thin metal layer, preferably a copper layer or a copper alloy layer, with a thickness of 0.5μm to 10μm, more preferably 1.5μm to 5μm. The side of the functional layer 30 away from the release layer 20 (i.e., the rough or processed surface of the functional layer 30) is used for lamination with the circuit substrate, and the side of the functional layer 30 close to the release layer 20 (i.e., the glossy surface of the functional layer 30) is exposed after the release carrier is removed, serving as the processing surface for subsequent circuit fabrication processes such as photolithography and electroplating.

[0026] Surface energy definition: Solid surface energy is the excess free energy per unit area of ​​a solid surface, with units of mJ / m². 2 (or mN / m), essentially refers to the interfacial force generated by uneven forces on the molecules of a solid surface, directly determining the spreading ability of a liquid on a solid surface and the interfacial bonding strength between two materials. In the context of peelable copper foil (composite metal foil), this parameter specifically refers to the surface energy of the bright surface of the ultra-thin functional copper layer (the side originally in contact with the peeling layer) after the carrier is peeled off, reflecting the cleanliness, chemical state, and interfacial bonding ability of the copper surface after peeling.

[0027] Surface energy is measured using the standard testing method (Owens-Wendt two-liquid contact angle method). According to the Owens-Wendt interfacial interaction theory, the total surface energy of a solid can be decomposed into two independent components: the dispersive component, which is contributed by intermolecular van der Waals forces (dispersion forces), belongs to nonpolar interactions, and exists on the surface of all materials; and the polar component, which is contributed by polar forces such as dipole interactions, hydrogen bonds, and coordination bonds, and is directly related to the polar functional groups and charged points of the surface.

[0028] Total surface energy = dispersion component + polar component. The proportion of the polar component reflects the strength of the surface polarity and directly determines the chemical bonding ability between the copper surface and polar polymers (photoresist, epoxy resin).

[0029] The determination of the surface energy range is based on the interfacial bonding quality of downstream processes such as photoresist coating, dry film lamination, and resin curing, which is essentially determined by the interfacial forces between the copper surface and the polymer material. The total surface energy determines the liquid spreading ability and physical adsorption strength, while the polar component determines the strength of chemical bonds such as hydrogen bonds and coordination bonds. Both together determine the photoresist adhesion, pattern fidelity, and resin bonding reliability. This invention controls the residual level and chemical state of the copper surface after stripping, locking the surface energy range within the optimal range for downstream processes.

[0030] When the total surface energy is below 40 mJ / m 2 This indicates that the copper surface has a lot of low surface energy organic stripping agents and hydrocarbon oil stains. In the downstream process, the photoresist coating will have pinholes, shrinkage, and other defects. After the dry film is laminated, defects such as edge lifting and plating leakage are likely to occur, which can easily lead to open circuits / short circuits. At the same time, the physical adsorption force between the resin and the copper surface is insufficient, and the bonding force after lamination is not up to standard.

[0031] When the total surface energy exceeds the upper limit of 60 mJ / m 2 This usually indicates that the copper surface has undergone excessive oxidation or has adsorbed a large amount of polar contaminants such as acid radicals and metal ions, which will lead to uneven etching rates and excessive side etching of the circuit lines in subsequent processes. At the same time, if the photoresist adhesion is too strong, it will be difficult to remove the photoresist after development, and it is easy to leave residues, which will affect subsequent electroplating processes.

[0032] If and only if the total surface energy is 40–60 mJ / m 2 Within a certain range, the copper surface has suitable wettability and interfacial reactivity, which can ensure the full spread of polar polymer materials and form appropriate amounts of hydrogen bonds, coordination bonds and other chemical bonds with the polar groups therein, so as to achieve the optimal "physical adsorption + chemical bonding" synergistic interfacial effect.

[0033] Furthermore, the photoresists and epoxy resins used downstream are both polar polymer materials, and their reliable bonding with the copper surface relies heavily on polar chemical bonds (hydrogen bonds, coordination bonds). If the polar component accounts for less than 30% of the total surface energy, even if the total surface energy meets the standard, it indicates that the surface is mainly composed of non-polar hydrocarbon residues, with insufficient polar binding sites. The photoresist and copper surface are only bonded by weak van der Waals forces, making it prone to pattern detachment and plating peeling under the washing of developing and electroplating solutions. A polar component accounting for ≥30% of the total surface energy ensures that the copper surface has sufficient hydroxyl and oxidation sites to form a stable chemical bond with the polymer, significantly improving process tolerance. The requirement of a polar component accounting for ≥30% of the total surface energy ensures that the copper surface has a sufficient number of polar interaction sites (such as surface oxides and hydroxyl groups) to form chemical bonds with the polar functional groups in the photoresist and epoxy resin, ensuring interfacial bonding strength.

[0034] The standard hot-pressing process is defined as follows: the side of the functional layer 30 furthest from the release layer 20 is laminated with an epoxy resin prepreg, and then pressed at 200°C and 2MPa vacuum for 2 hours, followed by natural cooling to room temperature. This standard hot-pressing condition simulates the typical pressing process conditions of peelable copper foil in actual circuit board manufacturing.

[0035] This invention provides a peelable metal foil. By precisely defining the total surface energy range and polar component ratio of the ultra-thin functional copper layer after standard hot-pressing peeling, the surface of this foil can form a stable physical adsorption and chemical bond with polar polymer materials such as photoresist and epoxy resin. This reduces process defects such as photoresist pinholes, dry film edge lifting and plating, and insufficient resin adhesion from the root, significantly improving the manufacturing yield of fine circuits. It fills the performance control gap in the interface compatibility dimension of the peelable copper foil industry, improves the success rate of etched circuits, and meets the fine circuit manufacturing needs of high-end electronics.

[0036] During circuit fabrication, the side of the functional layer in the metal foil furthest from the release layer is pressed onto the circuit substrate. Then, the carrier layer is peeled off using the release layer, leaving the functional layer on the circuit substrate. At this point, the side of the functional layer closest to the release layer is exposed as the outer surface of the circuit. This invention limits the copper surface area after peeling to 40-60 mJ / m. 2 With a total surface energy and a polar component ratio of ≥30%, the copper surface ensures a stable "physical adsorption and chemical bonding" dual-interface interaction between the copper surface and polar polymer materials such as photoresist and epoxy resin. This fundamentally avoids defects such as photoresist pinholes, pattern detachment, dry film curling, and insufficient resin adhesion. Actual measurements show that this can improve the process yield of lines with linewidths below 10μm by 8%~12%, effectively improving the quality of line etching.

[0037] The technical solution of this invention, by precisely limiting the total surface energy of the functional layer near the release layer to 40-60 mJ / m² after standard hot-pressing and peeling off the carrier layer, achieves this. 2 Furthermore, the polar component accounts for ≥30% of the total surface energy, achieving stable interfacial physical adsorption and chemical bonding. When the total surface energy of the functional copper layer exfoliation surface is between 40 and 60 mJ / m², [this is achieved]. 2When the surface energy is within a suitable range, it ensures that polar polymer materials such as photoresist and epoxy resin are fully wetted and spread on the copper surface, avoiding poor wetting due to excessively low surface energy or rapid adsorption of contaminants due to excessively high surface energy. Simultaneously, by ensuring a polar component ratio of ≥30%, it ensures that the copper surface has a sufficient number of polar functional groups to form dipole interactions, hydrogen bonds, and even coordination bonds with the polar groups in the photoresist and epoxy resin, achieving a dual-interface mechanism of "physical adsorption and chemical bonding." This fundamentally reduces process defects and improves the yield of fine-line manufacturing. By limiting the total surface energy and polar component ratio of the copper surface after stripping to a specific range, it ensures a stable and reliable interfacial bond between the copper surface and various polar polymer materials that come into contact with it in subsequent processes. In summary, this invention solves the problems of large fluctuations in the surface energy of the copper surface and uneven polar composition after peeling off the peelable copper foil in the prior art. It achieves small fluctuations in the surface energy of the copper surface and uniform polar composition after peeling off the peelable copper foil, realizing a stable physical adsorption and chemical bonding dual-interface interaction mechanism between the copper surface and the polymer material, thereby fundamentally improving the manufacturing yield and reliability of fine circuits.

[0038] Optionally, after the composite metal foil is hot-pressed and the carrier layer is peeled off, the surface energy fluctuation coefficient of the functional layer on the side closest to the peeling layer is ≤10%; the surface energy fluctuation coefficient is the ratio of the sample standard deviation to the arithmetic mean of the surface energy at each test point.

[0039] Specifically, peelable copper foil is a large-roll, wide-width product. If the thickness, residue, and degree of oxidation of the peeling layer are uneven at different locations along the entire roll, it will lead to a discrete distribution of surface energy. The surface energy fluctuation coefficient directly reflects the performance uniformity of the entire product and is a core guarantee for the yield of mass production.

[0040] A surface energy fluctuation coefficient of ≤10% ensures that the surface energy of all areas of the entire copper surface meets the process requirements. If the fluctuation coefficient >10%, significant performance differentiation will occur across the entire surface; edge areas may have a surface energy below 40mJ / m² due to excessive residue. 2 The central region may have a surface energy exceeding 60 mJ / m due to heavier oxidation. 2 Large-size substrates often suffer from localized yield failures, forcing customers to cut and reuse them, resulting in a significant decrease in material utilization. This invention limits the fluctuation to within 10%, reducing the risk of localized failures, improving the uniformity of surface energy across the entire surface, and enhancing both material yield and utilization.

[0041] By quantitatively limiting the uniformity of the surface energy across the entire copper surface, the consistency of the copper interface characteristics in different areas during the processing of large-area circuit boards is ensured, avoiding selective process defects caused by unevenness across the entire surface. Limiting the surface energy fluctuation coefficient to ≤10% guarantees the uniformity of the copper surface performance, avoids process defects caused by localized surface energy anomalies, improves the yield and reliability of large-area circuit board processing, and provides a guarantee for the large-scale stable production of large-format, high-density circuit boards.

[0042] Optionally, after the composite metal foil is hot-pressed and the peeling carrier layer is removed, it is placed in a standard environment of 25°C and 50% relative humidity for 24 hours. The total surface energy retention rate of the side of the functional layer near the peeling layer is ≥90%, and the polar component accounts for ≥30% of the total surface energy.

[0043] Specifically, freshly peeled copper surfaces have high surface activity and spontaneously absorb moisture and hydrocarbon impurities from the air over time, while undergoing slow natural oxidation, leading to continuous decay of surface energy and a gradual decrease in polar components. Conventional products require subsequent processes to be completed within 1-2 hours after peeling, resulting in extremely poor production scheduling flexibility. Any temporary adjustments to the production line can lead to material scrap. The product of this invention can slow down the rate of surface energy decay after peeling, extend the effective operating window, and reduce the risk of material scrap. By limiting the temporal stability of the copper surface energy, it ensures that the peeled copper surface maintains good interfacial activity during storage and transportation in downstream processes, providing ample operating time for production organization.

[0044] Total surface energy retention is the ratio of surface energy after placement to surface energy before placement. By ensuring that the total surface energy retention is ≥90% and the polar component accounts for ≥30% after 24 hours of placement in a standard environment, the copper surface after stripping has excellent chemical stability and environmental adaptability. The surface energy does not decay rapidly over time, providing ample operating time for downstream processes and facilitating continuous and large-scale operation of the production line.

[0045] Optionally, after standard hot pressing treatment, the composite metal foil retains 80% to 120% of the peel force between the carrier layer and the functional layer, and the peel force fluctuation coefficient is ≤10%.

[0046] Specifically, the peel force retention rate is the ratio of the tested peel force after hot pressing to the baseline peel force before hot pressing. The peel force fluctuation coefficient is the ratio of the sample standard deviation to the arithmetic mean of the peel force at each test point. Peel stability is a prerequisite for surface energy stability: if the peel force drifts significantly after pressing, it will inevitably be accompanied by increased diffusion of interfacial elements and uneven degradation of the organic layer, ultimately resulting in uneven distribution of surface residues and drastic fluctuations in surface energy. Limiting peel force stability fundamentally supports the uniformity and controllability of surface energy at the peel interface.

[0047] When the peel force retention rate is less than 80%, the peel force decays excessively, indicating severe high-temperature degradation of the peel layer. During lamination, the copper layer is prone to displacement and detachment, and the degradation products remain unevenly, leading to significant fluctuations in surface energy. When the peel force retention rate is greater than 120%, the peel force is abnormally high, indicating severe interdiffusion of interfacial elements, forming strongly bonded intermetallic compounds. After peeling, the metal residue exceeds the standard, and the polar component of the surface energy is abnormally high.

[0048] When the peel force fluctuation coefficient is limited to less than 10%, it indicates good peel force stability and avoids local anomalies caused by heat pressing. The uniformity of peel force directly corresponds to the uniformity of interface state. Excessive fluctuation will inevitably be accompanied by spatial dispersion of surface energy. The two are positively correlated. Therefore, this application limits the peel force fluctuation to a small value, which can effectively improve the stability of the copper surface energy after peeling.

[0049] By limiting the peel force retention rate after hot pressing to 80%–120% and the peel force fluctuation coefficient to ≤10%, the stability and controllability of peel performance before and after the hot pressing process are ensured, avoiding drastic drift of peel force due to thermal history, and ensuring the consistency of peel behavior during large-area processing.

[0050] Optionally, after the composite metal foil is hot-pressed and the carrier layer is peeled off, the total amount of non-copper metal elements remaining on the side of the functional layer near the peeling layer is ≤1at.

[0051] Specifically, residual non-copper metal elements (such as Ni, Cr, and Mo from the release layer) correspond to polar impurities, which can cause abnormal fluctuations in local surface energy. If the total amount of residual non-copper metal elements is greater than 1, it indicates severe interdiffusion of elements during high-temperature bonding, which not only leads to local surface energy fluctuations and abnormal polar components, but also affects the uniformity of subsequent etching, causing linewidth deviations. Simultaneously, there is a long-term reliability risk due to metal migration. Therefore, when the total amount of residual non-copper metal elements on the side of the functional layer closest to the release layer is ≤1 at%, surface energy stability can be ensured, which is beneficial for improving release stability and avoiding interface adhesion and incomplete release problems caused by residues.

[0052] The total amount of non-copper metal elements remaining, i.e. the percentage of metal atoms remaining, is the proportion of the number of atoms of non-copper metal elements (such as Ni, Cr, Mo, Zn, Ti, etc.) from the peeling layer to the total number of atoms on the bright surface of the functional copper layer after standard hot pressing and stripping carrier. The unit is at% (atomic percentage); the lower the value, the cleaner the peeling interface.

[0053] Test method: X-ray photoelectron spectroscopy (XPS) was used for scanning.

[0054] Operating procedures: Take a sample of the stripped functional copper layer and test it at a depth of 3-5 nm from the surface; collect the full spectrum and fine spectra of each characteristic element; quantitatively calculate the atomic percentage of each element using the sensitivity factor method; sum up the atomic percentages of all non-copper metal elements to obtain the percentage of non-copper metal residue atoms. Furthermore, test at least three different locations on the same sample and take the arithmetic mean of the results.

[0055] By limiting the total amount of non-copper metal elements to ≤1at%, the high cleanliness of the stripping interface is ensured, avoiding interference from residual elements in the stripping layer on the intrinsic surface energy properties of the copper surface, and ensuring the high cleanliness of the stripping interface and the repeatability of the intrinsic surface energy properties of the copper surface.

[0056] Optionally, the (111) crystal plane texture coefficient of the functional layer is ≥70%, and the grain size dispersion is ≤20%.

[0057] Specifically, the texture factor of the (111) crystal plane in the functional layer characterizes the degree of preferred orientation of the (111) crystal plane in the functional copper layer, expressed as a percentage. The higher the value, the larger the proportion of the (111) crystal plane, the denser the atomic arrangement of the copper layer, and the stronger the resistance to thermal diffusion and electromigration. Test method: X-ray diffraction (XRD) is used to scan the bright surface of the functional copper layer. After removing the surface anti-rust layer, the test is performed. The diffraction peak intensity of each crystal plane is fitted, and the texture factor of the (111) crystal plane is calculated by the Harris texture factor method. The grain size dispersion is the ratio of the sample standard deviation to the arithmetic mean of the grain size in each test area.

[0058] Copper's (111) crystal plane has the densest atomic arrangement, resulting in the lowest surface energy, the most uniform etching rate, and the strongest anti-diffusion capability. A copper layer with a high (111) crystal plane texture not only inhibits the diffusion of copper atoms into the release layer at high temperatures, reducing metal residue, but more importantly, the etching rate difference between different crystal orientations is small during micro-etching, leading to a uniform surface morphology after etching, stable surface energy dispersion components, and small grain size dispersion, further ensuring the uniformity of the entire etching process. This effectively stabilizes the surface energy after release. When the (111) crystal plane texture coefficient is <70%, the proportion of (200), (220), and other crystal planes in the copper layer increases, and the difference in micro-etching rate between different crystal planes can reach over 30%. After micro-etching, the surface roughness increases significantly, the surface energy dispersion components change abruptly, and the total surface energy exceeds the acceptable range. Simultaneously, the copper atom diffusion activation energy decreases, making interfacial interdiffusion more likely to occur at high temperatures, resulting in excessive metal residue. (111) When the crystal texture coefficient is ≥70%, the surface roughness decreases significantly after micro-etching, the surface energy dispersion component decreases abruptly, and the total surface energy does not exceed the qualified range; interfacial interdiffusion is not likely to occur at high temperature, and the metal residue does not exceed the standard.

[0059] Furthermore, when the grain size dispersion is >20%, the etching rate difference between large and small grains is significant, resulting in an uneven surface after micro-etching and abnormal local surface energy, which may lead to excessive overall fluctuation coefficient. When the grain size dispersion is ≤20%, the etching rate difference between large and small grains is not significant, the surface after micro-etching is relatively smooth, and no abnormalities are observed in local surface energy.

[0060] By limiting the (111) crystal plane texture coefficient of the functional layer to ≥70% and the grain size dispersion to ≤20%, the resistance to thermal diffusion and electromigration of the copper layer is enhanced, improving the uniformity and precision of the etched lines. This provides support for the uniformity and stability of interface performance at the microstructural level. Optimizing the microtexture and grain uniformity of the functional copper layer enhances its resistance to thermal diffusion and electromigration, while simultaneously supporting the uniformity and stability of interface performance at the microstructural level.

[0061] Figure 2 This is a schematic diagram of another composite metal foil provided according to an embodiment of the present invention, with reference to... Figure 2 Optionally, the release layer 20 is a composite release layer composed of an amorphous alloy metal layer 21 and a nitrogen-containing organic layer 22, with the amorphous alloy layer 21 and the nitrogen-containing organic layer 22 sequentially disposed on the surface of the carrier layer.

[0062] Specifically, the amorphous alloy metal layer 21 can form a stable interfacial metallurgical bond with the carrier layer 10 and a weaker physical bond with the organic layer 22, thus avoiding affecting the peeling stability. Among them, the amorphous alloy metal layer 21 has high density and large diffusion activation energy, which physically blocks the high-temperature diffusion of copper atoms and reduces metal residue during peeling. Meanwhile, the nitrogen-containing organic layer 22 is easy to peel off and remove, reducing the adhesion between the functional layer 30 and the carrier layer 10 during peeling, improving the cleanliness of the surface of the functional layer 30 after peeling, and improving the surface energy stability.

[0063] The amorphous alloy metal layer 21 can be composed of Ni-P alloy, Ni-W alloy, Co-W alloy, etc., and the nitrogen-containing organic layer 22 can be composed of a nitrogen-containing silane coupling agent (such as aminopropyltrimethoxysilane) or a nitrogen-containing heterocyclic compound (such as benzotriazole and its derivatives). This composite structure achieves precise control of peel strength and good performance of clean peeling even after high-temperature hot pressing through the synergistic effect of the inorganic and organic layers.

[0064] By defining the release layer as a composite release layer consisting of an amorphous alloy metal layer and a nitrogen-containing organic layer, the differential and precise control of the release strength is achieved through the synergistic effect of the inorganic and organic layers, while ensuring that it can still be cleanly released after high-temperature hot pressing.

[0065] Figure 3 This is a schematic diagram of another composite metal foil provided according to an embodiment of the present invention, with reference to... Figure 3Optionally, an antioxidant layer 40 is provided on the side of the functional layer 30 away from the peeling layer 20.

[0066] Specifically, an anti-oxidation layer 40 is provided on the side of the functional layer 30 away from the release layer 20 to enhance the anti-oxidation effect of the composite metal foil before application, effectively protect the metal activity of the pressing surface of the functional layer 30, and ensure a strong chemical bond with the epoxy resin during hot pressing.

[0067] Figure 4 This is a schematic diagram of another composite metal foil provided according to an embodiment of the present invention, with reference to... Figure 4 Optionally, a heat-resistant layer 50 is provided on the side of the carrier layer 10 away from the peeling layer 20.

[0068] Specifically, the heat-resistant layer 50 enhances the high-temperature resistance of the metal foil during hot pressing. Its function is to provide insulation, reducing the temperature of the release layer 20 and ensuring its thermal stability. The heat-resistant layer 50 can be made of materials such as tetrafluoroethylene (PTFE) film, polyimide (PI) film, or heat-resistant adhesives. All of these materials possess certain heat resistance properties and can effectively protect the copper foil from heat damage during the pressing process.

[0069] By setting a heat-resistant layer on the side of the carrier layer away from the release layer, the heat resistance, oxidation resistance and anti-adhesion of the outer surface of the carrier layer are improved, ensuring the smooth progress of the hot pressing process and avoiding the impact of high-temperature deformation of the carrier layer on the structural integrity of the release layer.

[0070] Standard hot-pressing conditions for composite metal foil: The laminate structure is FR-4 substrate + epoxy resin prepreg + peelable copper foil to be tested (functional copper layer facing the prepreg), vacuum degree ≤1kPa, temperature is increased to 200℃ at 3℃ / min, pressure is applied at 2MPa and held for 2h, and then cooled to room temperature at 2℃ / min before being removed.

[0071] Test methods for composite metal foils: Surface energy and polar component: Owens-Wendt two-liquid contact angle method, the probe solution is ultrapure water and diiodomethane, the droplet volume is 2μL, and the test is performed after standing for 30s; Peel strength and retention rate: 180° peel test, peel speed 50 mm / min, sample width 25 mm; Surface elemental residues: X-ray photoelectron spectroscopy (XPS), with a testing depth of 3~5 nm; Copper layer texture coefficient: X-ray diffraction (XRD), Harris method to calculate (111) crystal plane texture coefficient.

[0072] The composite metal foil is verified through specific embodiments below.

[0073] Standard hot pressing conditions: After stacking the side of each composite metal foil away from the release layer with the epoxy resin prepreg (FR-4 substrate + epoxy resin prepreg), press it at 200℃ and 2MPa vacuum for 2 hours, and then let it cool naturally to room temperature.

[0074] Fine circuit fabrication conditions: After stripping the carrier layer, photoresist (5μm thick) is applied to the exposed surface of the functional copper layer (the bright surface that was originally in contact with the stripping layer). After exposure and development, a circuit pattern with a line width / line spacing of 8μm / 8μm is formed, and then etching is performed.

[0075] Example 1 A composite metal foil employs a stacked structure comprising a carrier layer (35μm electrolytic copper foil), a release layer (30nm amorphous Ni-P alloy layer + 5nm nitrogen-containing silane coupling agent layer), and a functional layer (3μm electrodeposited copper layer).

[0076] Performance test results after standard hot pressing and peeling of the carrier layer: Total surface energy 52 mJ / m 2 The polar component accounts for 36%, the total surface energy retention rate is 95%, the surface energy fluctuation coefficient is 7%, and the circuit process yield is 92%.

[0077] Example 2 The method is basically the same as in Example 1, except that the surface energy properties of the copper surface after peeling are controlled by adjusting the thickness of the nitrogen-containing organic layer of the peeling layer (from 5nm to 2nm).

[0078] Performance test results after standard hot pressing and peeling of the carrier layer: Total surface energy 45 mJ / m 2 The polar component accounts for 31%, the total surface energy retention rate is 98%, the surface energy fluctuation coefficient is 9%, and the circuit process yield is 88%.

[0079] Example 3 The process is basically the same as in Example 1, except that the material of the nitrogen-containing organic layer of the release layer is adjusted (from nitrogen-containing silane coupling agent to benzotriazole organic layer) so that the copper surface after release has higher surface energy properties.

[0080] Performance test results after standard hot pressing and peeling of the carrier layer: Total surface energy 58 mJ / m 2 The polar component accounts for 42%, the total surface energy retention rate is 85%, the surface energy fluctuation coefficient is 8%, and the circuit process yield is 90%.

[0081] Comparative Example 1 Commercially available peelable copper foil products are used, with a single metal layer as the release layer (excluding nitrogen-containing organic layers) and an electrodeposited copper layer as the functional layer. No directional control of surface energy is performed.

[0082] Performance test results after standard hot pressing and peeling of the carrier layer: Total surface energy 32 mJ / m 2 The polar component accounts for 18%, the total surface energy retention rate is 88%, the surface energy fluctuation coefficient is 22%, and the circuit process yield is 68%.

[0083] Comparative Example 2 The same layered structure as in Example 1 was used, but the coating thickness of the nitrogen-containing organic layer was too large (about 50 nm), resulting in excessively high surface energy of the copper surface after peeling.

[0084] Performance test results after standard hot pressing and peeling of the carrier layer: Total surface energy 68 mJ / m 2 The polar component accounts for 45%, the total surface energy retention rate is 76%, the surface energy fluctuation coefficient is 7%, and the circuit process yield is 80%.

[0085] The composite metal foils prepared using the above embodiments and comparative examples were tested, and the test results are shown in Table 1 below: Table 1 The above three embodiments and two comparative examples fully demonstrate that when the total surface energy is 40–60 mJ / m 2 When the polar component accounts for ≥30% (Examples 1-3), the copper surface has suitable wettability and sufficient chemical bonding sites, which can form a stable "physical adsorption and chemical bonding" dual interface with the photoresist. The process yield can reach more than 88%, which is significantly better than the comparative example.

[0086] When the total surface energy is below 40 mJ / m 2 When the polar component ratio is less than 30% (Comparative Example 1), the copper surface wettability is insufficient and the chemical bonding force is weak, resulting in a significant increase in the photoresist shrinkage rate and pattern detachment rate, with a process yield of only 68%, which verifies the necessity of limiting the lower limit of total surface energy and polar component ratio.

[0087] When the total surface energy exceeds 60 mJ / m 2 In Comparative Example 2, although the copper surface has high initial activity, it is thermodynamically unstable and its surface energy decays rapidly in the air. The effective operating window in actual production is extremely short, which cannot meet the actual needs of large-scale production, thus verifying the necessity of limiting the upper limit of total surface energy.

[0088] In summary, only by strictly controlling the total surface energy within 40–60 mJ / m² can this be achieved. 2Furthermore, only when the polar component accounts for ≥30% can the copper surface be ensured to have good wettability, sufficient chemical bonding force, and sufficiently stable interface characteristics in the actual production environment. This reduces process defects such as photoresist shrinkage, pattern detachment, and dry film warping from the source, and significantly improves the manufacturing yield of fine lines.

[0089] Furthermore, embodiments of the present invention also provide a metal-clad laminate, which is made using a functional layer in the composite metal foil of any embodiment of the present invention as one of the materials.

[0090] The metal-clad laminate provided by this invention inherits all the interface compatibility advantages of the aforementioned composite metal foil, and is suitable for fine circuit fabrication in advanced processes such as mSAP, improving the reliability and integration of end products, and strongly supporting the continuous upgrading of electronic products towards higher density and higher reliability.

[0091] Since the metal-clad laminate is made using the functional layer of the composite metal foil provided in any embodiment of the present invention, the above-mentioned metal-clad laminate has the same beneficial effects as the composite metal foil, and will not be repeated here.

[0092] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can be made according to design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A composite metal foil, characterized in that, include: The carrier layer, the stripping layer, and the functional layer are stacked in sequence. After the composite metal foil undergoes standard hot-pressing treatment and the carrier layer is peeled off, the total surface energy of the functional layer on the side near the peeling layer is 40~60 mJ / m². 2 Of which, the polar component accounts for ≥30% of the total surface energy; The standard hot pressing process refers to: stacking the side of the functional layer away from the release layer with the epoxy resin prepreg, pressing it at 200°C and 2MPa vacuum for 2 hours, and then naturally cooling it to room temperature.

2. The composite metal foil according to claim 1, characterized in that, After the composite metal foil is hot-pressed and the carrier layer is peeled off, the surface energy fluctuation coefficient of the functional layer on the side near the peeling layer is ≤10%. The surface energy fluctuation coefficient is the ratio of the sample standard deviation to the arithmetic mean of the surface energy at each test point.

3. The composite metal foil according to claim 1, characterized in that, After the composite metal foil is hot-pressed and the carrier layer is peeled off, it is placed in a standard environment of 25°C and 50% relative humidity for 24 hours. The total surface energy retention rate of the side of the functional layer near the peeling layer is ≥90%, and the polar component accounts for ≥30% of the total surface energy.

4. The composite metal foil according to claim 1, characterized in that, After the composite metal foil undergoes standard hot pressing treatment, the peel force retention rate between the carrier layer and the functional layer is 80%~120%, and the peel force fluctuation coefficient is ≤10%.

5. The composite metal foil according to claim 1, characterized in that, After the composite metal foil is hot-pressed and the carrier layer is peeled off, the total amount of non-copper metal elements remaining on the side of the functional layer near the peeling layer is ≤1at.

6. The composite metal foil according to claim 1, characterized in that, The (111) crystal plane texture coefficient of the functional layer is ≥70%, and the grain size dispersion is ≤20%.

7. The composite metal foil according to claim 1, characterized in that, The release layer is a composite release layer composed of an amorphous alloy metal layer and a nitrogen-containing organic layer, wherein the amorphous alloy layer and the nitrogen-containing organic layer are sequentially disposed on the surface of the carrier layer.

8. The composite metal foil according to claim 1, characterized in that, An antioxidant layer is provided on the side of the functional layer away from the peeling layer.

9. The composite metal foil according to claim 1, characterized in that, A heat-resistant layer is provided on the side of the carrier layer away from the peeling layer.