A basalt fiber composite reinforced polypropylene material and a method for producing the same
By mixing and hot-pressing basalt fibers without organosilane coupling treatment with low-melting-point copolyester fibers in multiple layers, combined with low-temperature pre-bonding and high-pressure hot-pressing processes, the problems of insufficient interfacial bonding strength and warping deformation in basalt fiber reinforced polypropylene composites were solved, thereby improving the mechanical properties and dimensional stability of the material.
Patent Information
- Application Number
- CN202611579995.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-13
- Publication Date
- 2026-11-20
AI Technical Summary
Existing basalt fiber reinforced polypropylene composites require complex organosilane coupling surface modification treatment during preparation, resulting in complicated production processes. The interfacial coupling agent is prone to volatilization and degradation during high-temperature processing, leading to uneven resin wetting, insufficient interlayer bonding strength, and the material is prone to warping and deformation during hot pressing.
Basalt short fibers without organosilane coupling treatment are mixed with single-component low-melting-point copolyester short fibers and polypropylene short fibers in a specific ratio. Through multi-layer stacking and hot pressing, a spatially interwoven support network is formed. The low-melting-point copolyester short fibers soften or melt during hot pressing to establish a solid skeleton support. Combined with low-temperature pre-bonding, low-pressure preheating and high-pressure hot pressing consolidation processes, uniform resin penetration and material densification are achieved.
It improves the mechanical stability and flexural tensile properties of composite materials, solves the problems of fiber slippage and agglomeration, ensures the flatness and dimensional stability of materials, and achieves a combination of high surface adhesion and internal rigidity.
Smart Images

Figure CN123129547A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polypropylene composite materials, specifically to a basalt fiber reinforced polypropylene material and its preparation method. Background Technology
[0002] In practical applications, basalt fibers are often incorporated into polypropylene composites to enhance their mechanical properties. In existing manufacturing processes, to improve the interfacial compatibility between inorganic basalt fibers and the organic polypropylene matrix, surface chemical modification of the basalt fibers is typically achieved using organosilane coupling agents. This method is not only complex in its production process, but the coupling agent is also prone to volatilization and degradation during subsequent high-temperature hot pressing. Furthermore, because conventional short-fiber felts lack internal solid-state support during heating and pressing, basalt fibers are prone to slippage and agglomeration with the resin melt flow, making it difficult to maintain a uniformly distributed support network and thus reducing the mechanical stability of the final molded product.
[0003] Existing composite reinforced skeleton felts often employ a uniform structural design in the thickness direction. During hot pressing and consolidation, due to the lack of sufficient resin enrichment on the surface, the material surface often has numerous pores and insufficient flatness, resulting in low heat-fusion bonding strength with the outer backing layer and decorative surface layer. If the overall polypropylene resin content is increased to improve surface adhesion, the proportion of inorganic basalt fiber in the core layer will be correspondingly reduced, causing the composite material to lose its overall rigidity and making it difficult to simultaneously meet the requirements of high surface adhesion and high internal support in terms of structure.
[0004] Furthermore, conventional hot pressing typically employs a single molding method involving direct heating and pressurization. This method can easily lead to premature liquefaction of the outer resin layer, which can seal venting channels, resulting in uneven wetting of the matrix resin within the fiber gaps and residual air. During the cooling and demolding stage after molding, conventional processes often lack effective physical constraints on the shrinkage of polymer crystallization. The volume shrinkage generated during polypropylene chain rearrangement can trigger the release of internal stress, causing warping and deformation of the final product and making it difficult to guarantee the dimensional stability of the material. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a basalt fiber reinforced polypropylene material and its preparation method. This invention solves the problems that existing basalt fiber reinforced polypropylene composite materials typically require complex organosilane coupling surface modification treatment of basalt fibers during preparation, resulting in complicated production processes, easy volatilization and degradation of interfacial coupling agents during high-temperature processing, and uneven resin impregnation and insufficient interlayer bonding strength in conventional short fiber composite felts.
[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a basalt fiber composite reinforced polypropylene material, comprising a backing material, a composite skeleton felt, an adhesive backing layer, and a decorative surface layer, which are stacked from bottom to top and formed by hot pressing. The composite skeleton felt comprises a core fiber felt; based on the total mass of the fibers in the core fiber felt, the core fiber felt comprises the following components by mass percentage: 50%–70% core basalt short fibers without organosilane coupling treatment, 5%–10% single-component low-melting-point copolyester short fibers, and 20%–45% core polypropylene short fibers, and the sum of the mass percentages of each component is 100%.
[0007] By adopting the above technical solution, since basalt short fibers without organosilane coupling treatment are directly mixed with single-component low-melting-point copolyester short fibers and polypropylene short fibers in a specific ratio, and the structure is designed as a multi-layer composite that is then hot-pressed and solidified, the following effects are achieved: Basalt short fibers, single-component low-melting-point copolyester short fibers, and polypropylene short fibers are mixed, laid, and needle-punched to construct a spatially interwoven support network within the core fiber mat. The basalt short fibers, untreated with organosilane coupling, retain their original surface morphology and mechanically entangle with the polypropylene short fibers through positional movement caused by needle punching, forming a preliminary structural connection. The single-component low-melting-point copolyester short fibers soften or melt first upon heating and flow along the fiber junctions. After cooling and solidification, a solid skeletal support network is established at the fiber intersections, preventing fiber slippage and agglomeration during subsequent high-temperature processing.
[0008] During the hot-pressing consolidation process, the short polypropylene fibers in the core layer melt and transform into a fluid resin matrix. Under external pressure, the matrix penetrates into the basalt fiber network, displacing residual air and completing the overall coating of the reinforcing fibers. This results in a composite structure with polypropylene as the continuous phase and basalt fibers as the dispersed reinforcing skeleton, which improves the overall bending and tensile mechanical properties of the composite material.
[0009] Preferably, the composite skeleton felt is a single-layer composite skeleton felt or a three-layer gradient composite skeleton felt; When the composite skeleton felt is a single-layer composite skeleton felt, the composite skeleton felt is composed of the core fiber felt; When the composite skeleton felt is a three-layer gradient composite skeleton felt, the three-layer gradient composite skeleton felt includes, from bottom to top, a bottom surface fiber felt, a core fiber felt, and a top surface fiber felt; based on the total mass of fibers in the bottom surface fiber felt or the top surface fiber felt, the bottom surface fiber felt or the top surface fiber felt contains the following components by mass percentage: 20% to 40% of surface basalt short fibers without organosilane coupling treatment, 5% to 10% of the single-component low-melting-point copolyester short fibers, and 50% to 75% of surface polypropylene short fibers, and the sum of the mass percentages of each component is 100%.
[0010] By adopting the above technical solution, a gradient distribution of resin content is established in the thickness direction of the three-layer gradient composite skeleton felt. The high content of short polypropylene fibers in the surface fiber felt allows for the formation of a continuous resin layer between the upper and lower surfaces during hot-pressing and melting. The polypropylene melt in the surface layer not only seals surface pores to improve smoothness but also cross-links with the core layer interface downwards and forms a hot-melt bond with the backing layer and backing material upwards. The core layer maintains a high content of basalt fibers, providing the main rigid support. This structure achieves a combination of high resin adhesion on the surface and a high-rigidity skeleton inside.
[0011] Preferably, the core layer basalt short fibers without organosilane coupling treatment have a single fiber diameter of 13μm to 18.7μm and a cut length of 64mm; the core layer polypropylene short fibers have a linear density of 8D to 11D and a cut length of 64mm; and the single-component low-melting-point copolyester short fibers have a fiber length of 45.9mm to 70.4mm. When the composite skeleton felt is a three-layer gradient composite skeleton felt, the diameter of a single basalt short fiber in the surface layer that has not undergone organosilane coupling treatment is 8.1μm to 13μm, and the cutting length is 81mm to 121mm; the linear density of the surface polypropylene short fiber is 5.4D to 8D, and the cutting length is 64mm.
[0012] By adopting the above technical solution, the core layer basalt short fibers use a diameter of 13μm to 18.7μm and a cutting length of 64mm, which ensures the stiffness of individual fibers while facilitating the formation of dense stress transfer nodes in the core layer. The surface layer basalt short fibers use a smaller diameter of 8.1μm to 13μm and a larger length of 81mm to 121mm, which improves the flexibility and winding efficiency of the surface fiber web and reduces the risk of coarse fibers piercing the surface. The matching of the fiber length ranges of each component ensures the consistency of the movement trajectory of fibers of different materials during the carding and web laying process, prevents component separation caused by excessive differences in length, and improves the uniformity of the overall material distribution.
[0013] Preferably, the backing material has an areal density of 100 g / m³. 2Polyethylene terephthalate needle-punched nonwoven fabric; The adhesive layer is applied at a rate of 45g / m² per unit area. 2 ~110g / m 2 It is composed of low-density polyethylene powder; The decorative surface layer has a surface density of 450 g / m³. 2 Polyethylene terephthalate needle-punched fabric or fabric with a surface density of 750 g / m 2 Polyamide tufted fabric.
[0014] By adopting the above technical solution, polyethylene terephthalate needle-punched nonwoven fabric is used as the backing material. Its temperature resistance prevents direct contact between the mold and the substrate during hot pressing and provides scratch protection during assembly. The low-density polyethylene powder has a lower melting temperature than the polypropylene in the skeleton. During hot pressing, it first transforms into a highly viscous melt, partially penetrating the pores of the top layer of the composite skeleton felt and the back of the decorative surface layer. After cooling and solidification, it forms a continuous anti-peel bonding layer, maintaining the adhesion stability of the decorative surface layer.
[0015] Preferably, the single-component low-melting-point copolyester staple fiber is formed from a single low-melting-point modified copolyester, and the heat bonding temperature is 110℃~130℃. The base resin for the core layer polypropylene short fibers is fiber-grade isotactic polypropylene homopolymer, with a melt flow rate of 13.5 g / 10 min to 38.5 g / 10 min and a density of 0.90 g / cm³ under conditions of 230°C and 2.16 kg load. 3 ~0.91g / cm 3 ; The core basalt short fibers that have not undergone organosilane coupling treatment are obtained by completely melting natural basalt ore at 1450℃~1500℃, flowing it out through a platinum-rhodium alloy spinneret and drawing it into continuous fiber filaments. During the drawing process, pure water atomization spray is used for cooling and no organosilane coupling treatment is performed. After drying to remove moisture, the fibers are cut.
[0016] By adopting the above technical solution, the thermal bonding temperature of the single-component low-melting-point copolyester is limited to 110℃ to 130℃, which is lower than the conventional melting temperature of polypropylene short fibers. This difference in physical properties allows the copolyester's bonding function to be activated in the preheating stage of the composite material, while the polypropylene fibers remain solid and supportive, preventing overall softening and collapse. The melt flow rate of the polypropylene short fibers is limited to 13.5 g / 10 min to 38.5 g / 10 min, giving it a suitable dynamic viscosity that can overcome the flow resistance of the basalt fiber network to achieve deep penetration, while preventing resin overflow and loss under high pressure due to excessively low viscosity. The basalt short fibers are cooled only by pure water atomization during the stretching and forming stage, eliminating the volatilization and thermal degradation side reactions of the organic coupling agent under subsequent high-temperature hot pressing. The composite material directly relies on mechanical embedding and physical van der Waals forces at high temperature to complete the bonding of the two-phase interface.
[0017] Secondly, the present invention provides a method for preparing a basalt fiber composite reinforced polypropylene material, comprising the following steps: The composite skeleton felt is prepared by mixing, web-laying and needle-punching the short fibers of each component that constitute the composite skeleton felt according to the formula. The composite skeleton felt was individually subjected to low-temperature pre-bonding treatment and then cooled to room temperature; The backing material, the composite skeleton felt that has undergone the low-temperature pre-bonding treatment, the low-density polyethylene powder used to form the adhesive layer, and the decorative surface layer are laid out sequentially from bottom to top to obtain the composite blank to be molded. The composite blank to be molded is placed into a mold for preheating and hot pressing. After the hot pressing is completed, the cooling cycle of the mold is started under pressure to cool it. The pressure is released and the mold is demolded to obtain the basalt fiber reinforced polypropylene material.
[0018] By adopting the above technical solution, the following effects were achieved: The hybrid web-laying and needle-punching processes use mechanical force to displace two-dimensionally distributed short fibers along their thickness. The interweaving of polypropylene fibers, basalt fibers, and low-melting-point copolyester fibers in physical space constructs a porous framework structure with initial strength. In the low-temperature pre-bonding stage, applied heat only triggers the phase change of the low-melting-point component. After softening or melting, the low-melting-point copolyester short fibers converge at the junctions of adjacent fibers. Upon cooling and solidification, the spatial relative positions of each component are locked, preventing deformation during subsequent processing. In the hot-pressing consolidation stage, the system temperature exceeds the melting point of the polypropylene short fibers, transforming them into a mobile phase. External mechanical pressure overcomes the permeation resistance of the porous network, driving the polypropylene melt to permeate through the voids in the basalt fiber framework and expel air from the pores, achieving densification of the composite material. The cooling stage is conducted under maintained external pressure, limiting the free shrinkage of the polypropylene macromolecular chains during the cooling crystallization process. This prevents product warping caused by internal stress release, ensuring the flatness and stability of the material's macroscopic dimensions.
[0019] Preferably, the specific process for obtaining the composite skeleton felt is as follows: When preparing a single-layer composite skeleton felt, the corresponding mass percentages of the untreated basalt short fibers in the core layer, the single-component low-melting-point copolyester short fibers, and the core layer polypropylene short fibers are weighed out and mixed. The mixture is then carded to form a continuous fiber web, which is then cross-laid to form a mixed fiber web. This mixed fiber web is then directly needle-punched to obtain a total areal density of 900 g / m². 2 ~2200g / m 2 The single-layer composite skeleton felt; the overall needle-punching density is 45 needles / cm. 2 ~110 stitches / cm 2 The needle insertion depth is 8mm to 11mm; When preparing a three-layer gradient composite skeleton felt, the corresponding mass percentages of the untreated basalt short fibers, single-component low-melting-point copolyester short fibers, and surface polypropylene short fibers are weighed out and mixed, and then formed into a continuous fiber web by a carding machine and cross-laid to form two surface mixed fiber webs; the corresponding mass percentages of the untreated basalt short fibers, single-component low-melting-point copolyester short fibers, and core polypropylene short fibers are weighed out and mixed, and then formed into a continuous fiber web by a carding machine and cross-laid to form a core mixed fiber web; The two surface layer hybrid fiber webs and the core layer hybrid fiber web are pre-needled, with a pre-needling density of 27 needles / cm. 2 ~66 stitches / cm 2 The needle penetration depth ranged from 5.4 mm to 8 mm, yielding surface densities of 225 g / m³. 2 ~550g / m 2The surface fiber felt has a surface density of 450 g / m². 2 ~1100g / m 2 The core fiber felt; two surface fiber felts are respectively used as the bottom surface fiber felt and the top surface fiber felt, and are stacked in the order of the bottom surface fiber felt, the core fiber felt, and the top surface fiber felt, and then subjected to overall secondary needle punching, with a needle punching density of 45 needles / cm. 2 ~110 stitches / cm 2 The needle penetration depth is 8mm to 11mm, and the total surface density is 900g / m³. 2 ~2200g / m 2 The three-layer gradient composite skeleton felt.
[0020] By employing the above technical solutions, the carding process opens up fiber clumps, allowing the short fibers of each component to separate and align in the direction of mechanical movement. Multi-layer folding and cross-laying transform the unidirectional fiber web into a multi-directional interwoven mixed fiber web, providing mechanical uniformity in all in-plane directions. For three-layer gradient composite felts, the pre-needling process imparts initial bonding force to the single-layer fiber web, facilitating subsequent transfer and layering. Secondary needle punching after overall stacking uses needles to guide the surface fibers into the core layer, establishing interlayer physical interweaving channels in the thickness direction. A needle depth of 8mm to 11mm ensures that the fibers penetrate the entire material cross-section, relying on mechanical friction to lock the relative positions of different layers, preventing interlayer slippage under heat and pressure.
[0021] Preferably, the specific process of the low-temperature pre-bonding treatment is as follows: the composite skeleton felt is placed in the upper and lower mesh belt heating equipment, the low-temperature pre-bonding temperature of the heating mesh belt is set to 120℃~135℃, and a pre-bonding pressure of 0.09MPa~0.33MPa is applied for heating; after the central area of the composite skeleton felt is heated to 120℃~135℃, it is held for 27s~132s.
[0022] By employing the above technical solution, the heating mesh belt is set at a temperature of 120°C to 135°C, which falls between the thermal bonding temperature of the single-component low-melting-point copolyester and the melting point of polypropylene. At this temperature, the short polypropylene fibers remain solid, providing thermal compression support in the thickness direction. The applied pre-bonding pressure initially compresses the loose porous felt, reducing the fiber spacing. The isothermal process softens or melts the copolyester, completing its spreading and wetting at the fiber junctions. After cooling and removal of the heat source, uniform polymer bonding points are formed within the system, endowing the porous skeleton with internal structural support capabilities to resist subsequent high-pressure molding deformation.
[0023] Preferably, during the preheating process, the mold temperature is set to 170℃~180℃, a low-pressure preheating pressure of 0.09MPa~0.55MPa is applied, and the time is 54s~198s; During the hot pressing and consolidation, the molding pressure is increased to 0.9 MPa to 3.3 MPa, and the pressure is held at 170°C to 180°C for 27 to 132 seconds. During the cooling process, the pressure is released when the temperature of the basalt fiber reinforced polypropylene material drops to 60°C to 80°C.
[0024] By employing the above technical solution, a low-pressure preheating environment at 170℃ to 180℃ ensures unobstructed airflow channels within the material. This temperature is higher than the melting point of polypropylene resin, and the low-pressure maintenance process guarantees uniform heat transfer from the material's surface to the central region, preventing heat transfer defects such as the outer resin liquefying and sealing channels before the inner layer melts. The instantaneous increase in molding pressure after preheating forces the polypropylene melt, which is in a viscous state, to undergo extrusion flow, forcibly penetrating into the gaps between the basalt fibers to achieve a dense bond between the resin matrix phase and the reinforcing inorganic fiber phase. When heating is stopped and circulating cooling is initiated, the continuously applied pressure suppresses the volume shrinkage caused by polymer crystal rearrangement. When the overall material temperature drops to 60℃ to 80℃, the polypropylene structure is essentially frozen. At this point, the pressure is released for demolding, ensuring the dimensional accuracy of the product.
[0025] This invention provides a basalt fiber reinforced polypropylene material and its preparation method. It has the following beneficial effects: 1. This invention prepares a composite skeleton felt by mixing basalt short fibers without organosilane coupling treatment with single-component low-melting-point copolyester short fibers and polypropylene short fibers. This avoids the complex processes associated with chemical modification of the fiber surface and the problem of volatilization and degradation of coupling agents during high-temperature hot pressing. The mechanical entanglement generated by the mixed web-laying and needle punching, combined with the solid anchoring points established at the fiber junctions after the low-melting-point copolyester softens or melts upon heating and cools, stabilizes the internal fiber support network of the material. This prevents the slippage and agglomeration of basalt fibers during subsequent high-temperature and high-pressure processing, ensuring the mechanical stability of the final molded product.
[0026] 2. This invention designs the composite skeleton felt with a gradient structure of higher polypropylene fiber content in the surface layer and higher basalt fiber content in the core layer, enabling resin-rich zones to form on both the upper and lower surfaces during hot-pressing. The surface-rich polypropylene melt effectively seals pores to improve the smoothness of the material's surface and forms a stable hot-melt bond with the outer adhesive layer and decorative surface layer. Simultaneously, the high content of inorganic basalt fiber retained in the core layer maintains the overall rigidity of the composite material, achieving a combination of high surface adhesion and high internal support.
[0027] 3. This invention achieves phased physical shaping and resin impregnation of the composite material by sequentially performing low-temperature pre-bonding, low-pressure preheating, high-pressure hot-pressing consolidation, and pressure-holding cooling on the composite preform, utilizing the differences in the melting points of each component. The low-temperature pre-bonding and low-pressure preheating processes lock in the porous skeleton morphology and ensure uniform heat conduction. High-pressure hot-pressing consolidation forces the polypropylene melt to deeply penetrate within the fiber gaps and expel residual air. The final pressure-holding cooling effectively limits the volume shrinkage during polymer chain segment crystallization rearrangement, solving the problems of uneven resin impregnation and warping deformation of products caused by internal stress release in conventional processing. Attached Figure Description
[0028] Figure 1 This is a tensile load-displacement curve diagram of the present invention; Figure 2 The tensile stress-strain curves of the specimens in Example 2, Comparative Example 2, and Comparative Example 3 are shown. Figure 3 The graphs show the peel load as a function of displacement for the samples of Example 2 and Comparative Example 4. Figure 4 Here are the gas chromatograms of the samples from Example 2 and Comparative Example 3; Figure 5 Infrared spectra of basalt short fibers prepared in Example 2 and Comparative Example 3. Detailed Implementation
[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0030] It should be noted that the composite skeleton felt of the present invention is divided into single-layer composite skeleton felt and three-layer gradient composite skeleton felt according to different structures. When it is a single-layer composite skeleton felt, its whole is composed of core fiber felt; when it is a three-layer gradient composite skeleton felt, it has a gradient layer structure of bottom surface fiber felt, core fiber felt and top surface fiber felt.
[0031] The main raw materials and reagents used in the following preparation examples, embodiments and comparative examples are as follows. Unless otherwise specified, all chemical reagents are commercially available analytical grade or higher grade products.
[0032] Fiber-grade isotactic polypropylene homopolymer, CAS number 9003-07-0, with repeating structural unit (-CH2-CH(CH3)-). nThis homopolymer is a high-performance polypropylene, with a melt flow rate of 13.5–38.5 g / 10 min and a density of 0.90–0.91 g / cm³ under conditions of 230°C and 2.16 kg load. 3 It is used as a base resin for preparing thermoplastic matrix polypropylene short fibers.
[0033] The single-component low-melting-point copolyester staple fiber is a commercially available industrial-grade product. The fiber is composed of a single low-melting-point modified copolyester with a length of 45.9–70.4 mm and a heat bonding temperature of 110–130 °C. It is used as an auxiliary heat bonding fiber in the skeleton felt.
[0034] Natural basalt ore is a multi-component inorganic mineral composed of SiO2, Al2O3, Fe2O3 / FeO, CaO, MgO, and alkali metal oxides, with a preferred SiO2 mass fraction of 45%–52% and an Al2O3 mass fraction of 12%–18%. Basalt ore is melted at high temperatures and drawn into basalt fibers using a stencil. The resulting basalt fibers are not subjected to organosilane coupling treatment and are used as reinforcing fibers in polypropylene composites.
[0035] Low-density polyethylene (LDPE) powder, CAS number 9002-88-4, with repeating structural unit (-CH2-CH2-). n A density of 0.910–0.925 g / cm³ was selected. 3 Low-density polyethylene powder with a melting temperature of 105-115℃ and a particle size of 112.5-198μm is used to form a backing layer between the decorative surface layer and the composite skeleton felt by heating and melting.
[0036] Polyethylene terephthalate (PET) needle-punched fabric, polyamide (PA) tufted fabric, and polyethylene terephthalate (PET) needle-punched nonwoven fabric all use commercially available industrial-grade automotive interior materials. The areal density of the PET needle-punched fabric is 450 g / m². 2 The areal density of PA tufted fabric is 750 g / m². 2 The areal density of PET needle-punched nonwoven fabric is 100 g / m². 2 PET needle-punched fabric or PA tufted fabric is used as the decorative surface layer, and PET needle-punched nonwoven fabric is used as the backing material.
[0037] Preparation Example 1: This preparation example provides a basalt short fiber, a polypropylene short fiber, and a single-component low-melting-point copolyester short fiber, including the following steps: (1) Preparation of basalt short fibers: Natural basalt ore is washed, crushed, and fed into an industrial furnace, where it is completely melted at 1450℃. The resulting melt flows out through a platinum-rhodium alloy spinneret at the bottom of the furnace and is drawn into continuous fiber filaments by a drawing machine. During the drawing process, only pure water atomization spray is used for cooling, and no organosilane coupling treatment is performed. After cooling, the continuous fiber filaments are bundled and dried in an oven to remove moisture before being sent to a cutting machine for length cutting.
[0038] By adjusting the drawing and cutting parameters respectively, surface basalt short fibers (i.e., basalt short fibers used for surface fiber felt) with a single fiber diameter of 8.1 μm and a cutting length of 81 mm were obtained; and core basalt short fibers (i.e. basalt short fibers used for core fiber felt) with a single fiber diameter of 13 μm and a cutting length of 64 mm were obtained.
[0039] (2) Preparation of polypropylene short fibers: Fiber-grade isotactic polypropylene homopolymer is melt-extruded at 230°C in a twin-screw extrusion spinning machine. The resulting melt is extruded through a spinneret and cooled and solidified in a side-blowing airflow to form nascent fibers. The nascent fibers are bundled by traction rollers and conveyed to a drawing unit, where they undergo hot drawing and heat setting treatment before being sent to a cutting machine for cutting.
[0040] By adjusting the spinning, drawing, and cutting parameters respectively, surface polypropylene short fibers (i.e. polypropylene short fibers used for surface fiber mats) with a linear density of 5.4D and a cutting length of 64mm were obtained; and core polypropylene short fibers (i.e. polypropylene short fibers used for core fiber mats) with a linear density of 8D and a cutting length of 64mm were obtained.
[0041] (3) Selection of single-component low-melting-point copolyester staple fiber: Commercially available industrial-grade single-component low-melting-point copolyester staple fiber is selected. The single-component low-melting-point copolyester staple fiber is formed from a single low-melting-point modified copolyester and does not adopt core-sheath, core-shell or other multi-layer composite fiber structures; its heat bonding temperature is 130℃ and the fiber length is 45.9mm.
[0042] Preparation Example 2: This preparation example provides a basalt short fiber, a polypropylene short fiber, and a single-component low-melting-point copolyester short fiber, including the following steps: (1) Preparation of basalt short fibers: Natural basalt ore is washed, crushed, and fed into an industrial furnace, where it is completely melted at 1475°C. The resulting melt flows out through a platinum-rhodium alloy spinneret at the bottom of the furnace and is drawn into continuous fiber filaments by a drawing machine. During the drawing process, only pure water atomization spray is used for cooling, and no organosilane coupling treatment is performed. After cooling, the continuous fiber filaments are bundled and dried in an oven to remove moisture before being sent to a cutting machine for length cutting.
[0043] By adjusting the drawing and cutting parameters respectively, surface basalt short fibers (i.e. basalt short fibers used for surface fiber felt) with a single fiber diameter of 11μm and a cutting length of 100mm were obtained; and core basalt short fibers (i.e. basalt short fibers used for core fiber felt) with a single fiber diameter of 15μm and a cutting length of 64mm were obtained.
[0044] (2) Preparation of polypropylene short fibers: Fiber-grade isotactic polypropylene homopolymer is melt-extruded at 245°C in a twin-screw extrusion spinning machine. The resulting melt is extruded through a spinneret and cooled and solidified in a side-blowing airflow to form nascent fibers. The nascent fibers are bundled by traction rollers and conveyed to a drawing unit, where they undergo hot drawing and heat setting treatment before being sent to a cutting machine for cutting.
[0045] By adjusting the spinning, drawing, and cutting parameters respectively, surface polypropylene short fibers (i.e. polypropylene short fibers used for surface fiber mats) with a linear density of 7D and a cutting length of 64mm were obtained; and core polypropylene short fibers (i.e. polypropylene short fibers used for core fiber mats) with a linear density of 9D and a cutting length of 64mm were obtained.
[0046] (3) Selection of single-component low-melting-point copolyester staple fiber: Commercially available industrial-grade single-component low-melting-point copolyester staple fiber is selected. The single-component low-melting-point copolyester staple fiber is formed from a single low-melting-point modified copolyester and does not adopt core-sheath, core-shell or other multi-layer composite fiber structures; its heat bonding temperature is 120℃ and the fiber length is 58mm.
[0047] Preparation Example 3: This preparation example provides a basalt short fiber, a polypropylene short fiber, and a single-component low-melting-point copolyester short fiber, including the following steps: (1) Preparation of basalt short fibers: Natural basalt ore is washed, crushed, and fed into an industrial furnace, where it is completely melted at 1500℃. The resulting melt flows out through a platinum-rhodium alloy spinneret at the bottom of the furnace and is drawn into continuous fiber filaments by a drawing machine. During the drawing process, only pure water atomization spray is used for cooling, and no organosilane coupling treatment is performed. After cooling, the continuous fiber filaments are bundled and dried in an oven to remove moisture before being sent to a cutting machine for length cutting.
[0048] By adjusting the drawing and cutting parameters respectively, surface basalt short fibers (i.e. basalt short fibers used for surface fiber felt) with a single fiber diameter of 13μm and a cutting length of 121mm were obtained; and core basalt short fibers (i.e. basalt short fibers used for core fiber felt) with a single fiber diameter of 18.7μm and a cutting length of 64mm were obtained.
[0049] (2) Preparation of polypropylene short fibers: Fiber-grade isotactic polypropylene homopolymer is melt-extruded at 260°C in a twin-screw extrusion spinning machine. The resulting melt is extruded through a spinneret and cooled and solidified in a side-blowing airflow to form nascent fibers. The nascent fibers are bundled by traction rollers and conveyed to a drawing unit, where they undergo hot drawing and heat setting treatment before being sent to a cutting machine for cutting.
[0050] By adjusting the spinning, drawing, and cutting parameters respectively, surface polypropylene short fibers (i.e. polypropylene short fibers used for surface fiber mats) with a linear density of 8D and a cutting length of 64mm were obtained; and core polypropylene short fibers (i.e. polypropylene short fibers used for core fiber mats) with a linear density of 11D and a cutting length of 64mm were obtained.
[0051] (3) Selection of single-component low-melting-point copolyester staple fiber: Commercially available industrial-grade single-component low-melting-point copolyester staple fiber is selected. The single-component low-melting-point copolyester staple fiber is formed from a single low-melting-point modified copolyester and does not adopt core-sheath, core-shell or other multi-layer composite fiber structures; its heat bonding temperature is 110℃ and the fiber length is 70.4mm.
[0052] Example 1: This embodiment provides a method for preparing a basalt fiber reinforced polypropylene material, including the following steps: (1) Layered fiber blending, web laying and pre-needling: Based on the total fiber mass of the surface mixed fiber web, 20% of the surface basalt short fibers obtained in Preparation Example 1, 5% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 1, and 75% of the surface polypropylene short fibers obtained in Preparation Example 1 were weighed out, opened and mixed using an opening device, formed into a continuous fiber web by a carding machine, and then formed into a surface mixed fiber web by cross-laying. Two surface mixed fiber webs were prepared in total.
[0053] Based on the total fiber mass of the core layer mixed fiber web, 50% of the core layer basalt short fibers prepared in Preparation Example 1, 5% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 1, and 45% of the core layer polypropylene short fibers prepared in Preparation Example 1 were weighed out, opened and mixed by an opening device, formed into a continuous fiber web by a carding machine, and then formed into a core layer mixed fiber web by cross-laying.
[0054] The formed surface mixed fiber web and core mixed fiber web were pre-needled, with a pre-needling density of 27 needles / cm. 2 The needle-punching depth is 5.4 mm, forming two surface fiber mats and one core fiber mat.
[0055] (2) Three-layer gradient composite, secondary needle punching and low-temperature pre-bonding: Both surface fiber mats have an areal density of 225 g / m². 2 These were used as the bottom and top layer fiber felts, respectively; the areal density of the core fiber felt was 450 g / m². 2 The fibers are layered in the following order: bottom layer, core layer, and top layer, forming a three-layer composite fiber felt. The three-layer composite fiber felt is then subjected to a second needle-punching process with a needle density of 45 needles / cm². 2 The needle penetration depth was 8 mm, and the total surface density was 900 g / m³. 2 The three-layer gradient composite skeleton felt.
[0056] The three-layer gradient composite skeleton felt was placed in an upper and lower mesh belt heating device for separate low-temperature pre-bonding treatment. The low-temperature pre-bonding temperature of the heating mesh belt was set to 135℃, and a pre-bonding pressure of 0.33MPa was applied to the three-layer gradient composite skeleton felt for heating. After the central area of the three-layer gradient composite skeleton felt reached 135℃, it was held for 132s, and then cooled to room temperature.
[0057] (3) Composite hierarchical assembly: On the workbench, layers with a surface density of 100g / m³ are laid from bottom to top. 2 The PET needle-punched nonwoven fabric, the three-layer gradient composite skeleton felt obtained and pre-bonded at low temperature in step (2), the adhesive layer, and the surface density of 450 g / m 2 The PET needle-punched fabric. The adhesive backing layer is specifically composed of a unit area spreading rate of 45g / m². 2 Low-density polyethylene powder is evenly sprinkled onto the side of the PET needle-punched fabric facing the three-layer gradient composite skeleton felt. This yields the composite blank to be molded.
[0058] (4) Hot pressing, consolidation, and pressure holding cooling: The composite blank to be molded is placed into the mold of the hydraulic molding equipment for hot pressing. The mold is controlled to close. In the initial stage of mold closure, the mold temperature is set to 170℃, and a low preheating pressure of 0.55MPa is applied for preheating for 54 seconds.
[0059] The molding pressure was then increased to 0.9 MPa, and hot pressing was completed by holding the pressure at 170°C for 27 seconds.
[0060] After hot pressing and consolidation, the mold cooling cycle is activated while maintaining the mold closed and a molding pressure of 0.9 MPa for cooling. When the temperature of the composite material drops to 60°C, the pressure is released and the material is demolded to obtain basalt fiber reinforced polypropylene.
[0061] Example 2: This embodiment provides a method for preparing a basalt fiber reinforced polypropylene material, including the following steps: (1) Layered fiber blending, web laying and pre-needling: Based on the total fiber mass of the surface mixed fiber web, 30% of the surface basalt short fibers obtained in Preparation Example 2, 7.5% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 2, and 62.5% of the surface polypropylene short fibers obtained in Preparation Example 2 were weighed out, opened and mixed using an opening device, formed into a continuous fiber web by a carding machine, and then formed into a surface mixed fiber web by cross-laying. Two surface mixed fiber webs were prepared in total.
[0062] Based on the total fiber mass of the core layer mixed fiber web, 60% of the core layer basalt short fibers obtained in Preparation Example 2, 7.5% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 2, and 32.5% of the core layer polypropylene short fibers obtained in Preparation Example 2 were weighed out, opened and mixed by an opening device, formed into a continuous fiber web by a carding machine, and then formed into a core layer mixed fiber web by cross-laying.
[0063] The formed surface mixed fiber web and core mixed fiber web were pre-needled, with a pre-needling density of 45 needles / cm. 2 The needle-punching depth is 7mm, forming two surface fiber mats and one core fiber mat.
[0064] (2) Three-layer gradient composite, secondary needle punching and low-temperature pre-bonding: The areal density of both surface fiber mats is 400 g / m². 2 These were used as the bottom and top surface fiber felts, respectively; the areal density of the core fiber felt was 700 g / m². 2 The fibers are layered in the following order: bottom layer, core layer, and top layer, forming a three-layer composite fiber felt. The three-layer composite fiber felt is then subjected to a second needle-punching process with a needle density of 75 needles / cm². 2 With a needle penetration depth of 9 mm, a total surface density of 1500 g / m³ was obtained. 2 The three-layer gradient composite skeleton felt.
[0065] The three-layer gradient composite skeleton felt was placed in an upper and lower mesh belt heating device for separate low-temperature pre-bonding treatment. The low-temperature pre-bonding temperature of the heating mesh belt was set to 128℃, and a pre-bonding pressure of 0.2MPa was applied to the three-layer gradient composite skeleton felt for heating. After the central area of the three-layer gradient composite skeleton felt reached 128℃, it was held for 75 seconds, and then cooled to room temperature.
[0066] (3) Composite hierarchical assembly: On the workbench, layers with a surface density of 100g / m³ are laid from bottom to top. 2The PET needle-punched nonwoven fabric, the three-layer gradient composite skeleton felt obtained and pre-bonded in step (2) and the adhesive backing layer, and the surface density of 750g / m 2 PA tufted fabric. The adhesive backing layer is specifically composed of a unit area coverage of 75g / m². 2 Low-density polyethylene powder is evenly sprinkled onto the side of the PA tufted fabric facing the three-layer gradient composite skeleton felt. This yields the composite blank to be molded.
[0067] (4) Hot pressing, consolidation, and pressure holding cooling: The composite blank to be molded is placed into the mold of the hydraulic molding equipment for hot pressing. The mold is controlled to close. In the initial stage of mold closure, the mold temperature is set to 175℃, and a low-pressure preheating pressure of 0.3MPa is applied for preheating for 120s.
[0068] The molding pressure was then increased to 2.0 MPa, and hot pressing was completed by holding the pressure at 175°C for 75 seconds.
[0069] After hot pressing and consolidation, the mold cooling cycle is activated while maintaining the mold closed and a molding pressure of 2.0 MPa for cooling. When the temperature of the composite material drops to 70°C, the pressure is released and the material is demolded to obtain basalt fiber reinforced polypropylene.
[0070] Example 3: This embodiment provides a method for preparing a basalt fiber reinforced polypropylene material, including the following steps: (1) Layered fiber blending, web laying and pre-needling: Based on the total fiber mass of the surface mixed fiber web, 40% of the surface basalt short fibers obtained in Preparation Example 3, 10% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 3, and 50% of the surface polypropylene short fibers obtained in Preparation Example 3 were weighed out, opened and mixed using an opening device, formed into a continuous fiber web by a carding machine, and then formed into a surface mixed fiber web by cross-laying. Two surface mixed fiber webs were prepared in total.
[0071] Based on the total fiber mass of the core layer mixed fiber web, 70% of the core layer basalt short fibers obtained in Preparation Example 3, 10% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 3, and 20% of the core layer polypropylene short fibers obtained in Preparation Example 3 were weighed out, opened and mixed by an opening device, formed into a continuous fiber web by a carding machine, and then formed into a core layer mixed fiber web by cross-laying.
[0072] The formed surface mixed fiber web and core mixed fiber web were pre-needled, with a pre-needling density of 66 needles / cm. 2 The needle-punching depth is 8mm, forming two surface fiber mats and one core fiber mat.
[0073] (2) Three-layer gradient composite, secondary needle punching and low-temperature pre-bonding: Both surface fiber mats have an areal density of 550 g / m². 2 These were used as the bottom and top layer fiber mats, respectively; the areal density of the core fiber mat was 1100 g / m². 2 The fibers are layered in the following order: bottom layer, core layer, and top layer, forming a three-layer composite fiber felt. The three-layer composite fiber felt is then subjected to a second needle-punching process with a needle density of 110 needles / cm². 2 The needle penetration depth was 11 mm, and the total surface density was 2200 g / m³. 2 The three-layer gradient composite skeleton felt.
[0074] The three-layer gradient composite skeleton felt was placed in an upper and lower mesh belt heating device for separate low-temperature pre-bonding treatment. The low-temperature pre-bonding temperature of the heating mesh belt was set to 120℃, and a pre-bonding pressure of 0.09MPa was applied to the three-layer gradient composite skeleton felt for heating. After the central area of the three-layer gradient composite skeleton felt reached 120℃, it was held for 27 seconds, and then cooled to room temperature.
[0075] (3) Composite hierarchical assembly: On the workbench, layers with a surface density of 100g / m³ are laid from bottom to top. 2 The PET needle-punched nonwoven fabric, the three-layer gradient composite skeleton felt obtained and pre-bonded at low temperature in step (2), the adhesive layer, and the surface density of 450 g / m 2 The PET needle-punched fabric. The adhesive backing layer is specifically composed of a unit area spreading rate of 110g / m². 2 Low-density polyethylene powder is evenly sprinkled onto the side of the PET needle-punched fabric facing the three-layer gradient composite skeleton felt. This yields the composite blank to be molded.
[0076] (4) Hot pressing, consolidation, and pressure holding cooling: The composite blank to be molded is placed into the mold of the hydraulic molding equipment for hot pressing. The mold is controlled to close. In the initial stage of mold closure, the mold temperature is set to 180℃, and a low preheating pressure of 0.09MPa is applied for preheating for 198s.
[0077] The molding pressure was then increased to 3.3 MPa, and hot pressing was completed by holding the pressure at 180°C for 132 seconds.
[0078] After hot pressing and consolidation, the mold cooling cycle is activated while maintaining the mold closed and a molding pressure of 3.3 MPa. When the temperature of the composite material drops to 80°C, the pressure is released and the material is demolded to obtain basalt fiber reinforced polypropylene.
[0079] Example 4: This embodiment provides a method for preparing a basalt fiber reinforced polypropylene material, including the following steps: (1) Fiber blending, web laying and needle punching: Based on the total fiber mass of the single-layer mixed fiber web (i.e., core layer fiber felt), 50% of the core layer basalt short fibers obtained in Preparation Example 2, 7.5% of the single-component low-melting-point copolyester short fibers selected in Preparation Example 2, and 42.5% of the core layer polypropylene short fibers obtained in Preparation Example 2 were weighed out, mixed, and opened using an opening device. The web was then formed into a continuous fiber web by a carding machine and further formed into a mixed fiber web by cross-laying.
[0080] The resulting hybrid fiber web is directly needle-punched as a whole, with a needle-punching density of 75 needles / cm. 2 With a needle penetration depth of 9 mm, a total surface density of 1500 g / m³ was obtained. 2 The single-layer composite skeleton felt (i.e., the single-layer composite skeleton felt is composed of a core layer fiber felt).
[0081] (2) Low-temperature pre-bonding: The single-layer composite skeleton felt was placed in an upper and lower mesh belt heating device for separate low-temperature pre-bonding treatment. The low-temperature pre-bonding temperature of the heating mesh belt was set to 128℃, and a pre-bonding pressure of 0.2MPa was applied to the single-layer composite skeleton felt for heating. After the central area of the single-layer composite skeleton felt reached 128℃, it was held for 75 seconds, and then cooled to room temperature.
[0082] (3) Composite hierarchical assembly: On the workbench, layers with a surface density of 100g / m³ are laid from bottom to top. 2 The PET needle-punched nonwoven fabric, the single-layer composite skeleton felt obtained and pre-bonded in step (2) and completed with low temperature, the adhesive layer, and the surface density of 750 g / m 2 PA tufted fabric. The adhesive backing layer is specifically composed of a unit area coverage of 75g / m². 2 Low-density polyethylene powder is evenly sprinkled onto the side of the PA tufted fabric facing the single-layer composite skeleton felt. This yields the composite blank to be molded.
[0083] (4) Hot pressing, consolidation, and pressure holding cooling: The composite blank to be molded is placed into the mold of the hydraulic molding equipment for hot pressing. The mold is controlled to close. In the initial stage of mold closure, the mold temperature is set to 175℃, and a low-pressure preheating pressure of 0.3MPa is applied for preheating for 120s.
[0084] The molding pressure was then increased to 2.0 MPa, and hot pressing was completed by holding the pressure at 175°C for 75 seconds.
[0085] After hot pressing and consolidation, the mold cooling cycle is activated while maintaining the mold closed and a molding pressure of 2.0 MPa for cooling. When the temperature of the composite material drops to 70°C, the pressure is released and the material is demolded to obtain basalt fiber reinforced polypropylene.
[0086] Comparative Example 1: Compared with Example 2, the difference is that no single-component low-melting-point copolyester staple fiber is added in the layered fiber blending, web laying and pre-needling steps, and it is replaced by an equal mass of polypropylene staple fiber, while the rest are the same.
[0087] Comparative Example 2: Compared with Example 2, the difference is that the low-temperature pre-bonding treatment in step (2) is cancelled, and the obtained three-layer gradient composite skeleton felt is directly applied to the composite layer assembly in step (3) and directly hot-pressed. All other aspects are the same.
[0088] Comparative Example 3: Compared with Example 2, the difference is that the basalt short fibers used are commercially available basalt short fibers that have been surface-treated with γ-aminopropyltriethoxysilane coupling agent and polyurethane film-forming agent, with a total content of 0.8 wt% for the surface treatment agent; the length and single fiber diameter of the basalt short fibers are consistent with those of the basalt short fibers corresponding to Example 2, and all other aspects are the same.
[0089] Comparative Example 4: Compared to Example 2, the difference lies in that the surface layer mixed fiber web and the core layer mixed fiber web use completely identical fiber specifications. In both the surface layer mixed fiber web and the core layer mixed fiber web, the basalt short fibers are uniformly designed with a single fiber diameter of 15μm and a cut length of 64mm, and the polypropylene short fibers are uniformly designed with a linear density of 9D and a cut length of 64mm; all other specifications are the same.
[0090] Comparative Example 5: Compared with Example 2, the difference is that all basalt short fibers are replaced with alkali-free glass short fibers with the same mass fraction, monofilament diameter and cutting length as the replaced basalt short fibers, while the rest are the same.
[0091] Test Example 1: This test is used to evaluate the physical structural stability at each stage of molding.
[0092] (1) Room temperature tensile and thickness rebound test: The three-layer gradient composite skeleton felt that has undergone low temperature pre-bonding treatment in Examples 1 to 3, the single-layer composite skeleton felt that has undergone low temperature pre-bonding treatment in Example 4, and the three-layer gradient composite skeleton felt that has not undergone low temperature pre-bonding treatment in Comparative Example 2 were used as test materials. Each test material was cut into strips with a length of 250 mm and a width of 50 mm.
[0093] The strip-shaped specimen was clamped in the upper and lower fixtures of the universal testing machine. The tensile speed was set to 100 mm / min. The displacement and corresponding tensile load during the tensile process were recorded. Taking the specimens of Example 2 and Comparative Example 2 as examples, the records were recorded as the skeleton felt specimen after low-temperature pre-bonding in Example 2 and the skeleton felt specimen without low-temperature pre-bonding in Comparative Example 2, respectively. The maximum load measured during the tensile process was taken as the maximum tensile load. Another square specimen with a side length of 100 mm was taken. The initial thickness t0 was measured using a thickness gauge. A uniformly distributed load of 2 kPa was applied for compression for 60 s. After unloading and resting for 120 s, the recovered thickness t1 was measured. The thickness resilience R was calculated according to R = t1 / t0 × 100%.
[0094] (2) Finished product thickness uniformity and roller test mass loss rate test: The basalt fiber reinforced polypropylene materials after demolding in Examples 1 to 4 and Comparative Example 2 were used as the test materials. Sixteen measurement points were uniformly selected on the surface of the finished product, the thickness of each point was measured, and the range value was calculated. The square finished product sample with a size of 100mm×100mm after the edges were cut was weighed and placed in the roller drop tester. The speed was set to 30r / min. After running for 500 revolutions, the sample was taken out, the loose material was cleaned, and the sample was weighed again. The percentage of mass loss of the sample before and after the test was calculated as the roller test mass loss rate.
[0095] The test results are shown in Table 1.
[0096] Table 1. Test data on the physical structural stability at each stage of molding:
[0097] in conclusion: According to the data in Table 1, the samples of Examples 1 to 4 exhibited maximum tensile loads ranging from 36.4 N to 58.7 N in room temperature tensile tests, with thickness resilience rates ranging from 84.1% to 90.5%. The sample of Comparative Example 2 without low-temperature pre-bonding treatment had a maximum tensile load of 14.2 N and a thickness resilience rate of 62.8%.
[0098] Combination Figure 1 It can be seen that the tensile load-displacement curve of the skeleton felt sample after low-temperature pre-bonding in Example 2 is generally at a higher load level, while the tensile load-displacement curve of the skeleton felt sample without low-temperature pre-bonding in Comparative Example 2 is generally at a lower load level. The comparison results between Example 2 and Comparative Example 2 show that the single-component low-melting-point copolyester staple fiber softens or melts at least partially during the low-temperature pre-bonding process, which is beneficial to the generation of thermal bonding. The synergistic effect of thermal bonding and the thickness-direction mechanical entanglement formed by secondary needle punching helps to improve the overall structural stability and thickness recovery ability of the skeleton felt, thereby reducing the degree of relative movement and local loosening of the fiber layer during subsequent handling and molding processes to a certain extent.
[0099] The final product thickness range and roller test mass loss rate data show that the final product thickness range of Examples 1 to 4 is controlled within the range of 0.09 mm to 0.21 mm, and the roller test mass loss rate is less than 0.7%. Compared with Example 2, Comparative Example 2, due to the lack of low-temperature pre-bonding treatment, exhibits weaker structural stability of its skeleton felt before molding, resulting in a larger thickness range and a higher roller test mass loss rate after molding. Its final product thickness range is 0.41 mm, and its roller test mass loss rate is 2.37%.
[0100] Test Example 2: This test compares the basic mechanical properties.
[0101] (1) Tensile properties test at room temperature: The basalt fiber reinforced polypropylene materials after molding and demolding in Examples 1 to 4 and Comparative Examples 1 to 5 were used as the test materials. Each test material was cut into dumbbell-shaped specimens of type 1B as specified in GB / T1040.2-2022 using a mechanical sample cutting device. The total length of the specimen was 150 mm, the width of the narrow part was 10 mm, and the gauge length was 50 mm. Before the test, the actual average thickness of the narrow part was measured, and the initial cross-sectional area was determined according to the width of the narrow part and the average thickness.
[0102] The specimen was placed in the upper and lower clamps of the universal testing machine, and the tensile rate was set to 50 mm / min. The test was started, and the maximum tensile load of the specimen during the tensile process until fracture was recorded. The tensile strength was calculated based on the initial cross-sectional area of the specimen. Simultaneously, the tensile stress and corresponding strain of the universal testing machine during the tensile process were recorded. Taking the specimens of Example 2, Comparative Example 2, and Comparative Example 3 as examples, the corresponding tensile stress-strain curves were obtained. Five parallel specimens were prepared for each group of test objects, and the arithmetic mean was taken as the tensile strength test result for that group.
[0103] (2) Room temperature bending performance test: The finished material after demolding from the same batch as the tensile performance test was used as the test object. It was cut into strip-shaped bending specimens with a length of 120 mm and a width of 50 mm. Before the test, the thickness of the specimen was measured within the span and the average value was taken. This average thickness was used to calculate the bending strength and bending modulus. A three-point bending test assembly was installed on the universal testing machine, the span was set to 80 mm, and the loading head descent rate was 10 mm / min. The test was started, and the load and deflection changes of the specimen during the bending process were recorded. The bending strength and bending modulus were calculated. Five parallel specimens were prepared for each group of test objects, and the arithmetic mean was taken as the bending test result of the group.
[0104] The test results are shown in Table 2.
[0105] Table 2. Basic Mechanical Performance Test Data:
[0106] in conclusion: As can be seen from the data in Table 2, Examples 1 to 4 all exhibit certain tensile and bending load-bearing capacity. Among them, Example 2 has the highest comprehensive mechanical properties, with a tensile strength of 75.6 MPa and a bending strength of 115.1 MPa.
[0107] Compared to Example 2, the tensile strength, flexural strength, and flexural modulus of Comparative Examples 1 and 2 were all reduced. The data indicate that in the absence of single-component low-melting-point copolyester staple fibers or the omission of low-temperature pre-bonding treatment, the structural stability and load-bearing capacity of the skeleton felt during subsequent molding processes are reduced to some extent, resulting in a corresponding decrease in tensile and flexural properties. Combined with... Figure 2 It can be seen that the specimen of Comparative Example 2 fractured under relatively low tensile stress, and its fracture stress was significantly lower than that of the specimen of Example 2. This result suggests that omitting the low-temperature pre-bonding treatment is often detrimental to the tensile load-bearing capacity of the final material.
[0108] By comparing the data from Example 2 and Comparative Example 4, the impact of using different fiber specifications in the surface and core layers can be evaluated. The surface and core mixed fiber webs of Comparative Example 4 use completely identical fiber specifications, resulting in lower flexural modulus and flexural strength compared to Example 2. Example 2 forms a gradient structure by using different basalt fiber contents, basalt fiber specifications, and polypropylene short fiber specifications in the surface and core layers; under the test conditions, this gradient hierarchical structure corresponds to higher tensile strength, flexural strength, and flexural modulus. Example 4 uses a single-layer composite skeleton felt, and its mechanical properties are also lower than those of Example 2, indicating that under the composition and process conditions corresponding to Example 4, the overall mechanical properties of the single-layer skeleton structure are weaker than the three-layer gradient structure of Example 2.
[0109] Comparative Example 3 used basalt short fibers surface-treated with γ-aminopropyltriethoxysilane coupling agent and polyurethane film-forming agent, and its mechanical properties were similar to those of Example 2. Figure 2 It can be seen that the slopes of the initial linear segments of the tensile stress-strain curves of the specimens in Example 2 and Comparative Example 3 are quite similar, indicating that they have similar stiffness responses in the initial tensile stage. The data shows that, under the test conditions, Example 2, without additional organosilane coupling treatment of the basalt short fibers, still achieved tensile and flexural properties similar to Comparative Example 3; this result indicates that the needle-punched mechanical entanglement and polypropylene melt consolidation in this scheme contribute to the formation of an effective load-transfer structure. Comparative Example 5, which uses alkali-free chopped glass fibers instead of basalt short fibers, exhibits lower flexural strength and flexural modulus than Example 2, indicating that under the test conditions, the basalt short fiber system is advantageous for obtaining higher flexural performance.
[0110] Test Example 3: This test compares the interlayer peel strength.
[0111] Room temperature peel performance test: The basalt fiber reinforced polypropylene materials after demolding in Examples 1 to 4 and Comparative Example 4 were used as the test materials. Each test material was cut into strips 200 mm long and 25 mm wide using a sample cutting device. A 50 mm peel was pre-peeled from one end of the sample along the interface between the decorative surface layer and the three-layer gradient composite skeleton felt or the single-layer composite skeleton felt. The pre-peeled ends were fixed in the upper and lower clamps of a universal testing machine, and the clamp movement speed was set to 100 mm / min.
[0112] Initiate the test and record the displacement and corresponding peel load during the peeling process. Taking the samples from Example 2 and Comparative Example 4 as examples, obtain the corresponding peel load-displacement curves. Discard the initial peak stress and take the average peel load of the effective peeling range. Divide the average value by the sample width to calculate the interlayer peel strength, in N / mm. Prepare 5 parallel samples for each test object and take the arithmetic mean as the peel strength test result for that group.
[0113] The test results are shown in Table 3.
[0114] Table 3. Data on interlayer peel strength test:
[0115] in conclusion: Combining the data in Table 3 and Figure 3 The peel load-displacement curves show that the interlaminar peel strength of Examples 1 to 3 reached 1.58 N / mm to 2.58 N / mm. The interlaminar peel strength of Example 4 and Comparative Example 4 was lower than that of Examples 1 to 3. From... Figure 3 It can be seen that the peel load-displacement curve of the sample in Example 2 is generally higher than that of the sample in Comparative Example 4.
[0116] Compared to Comparative Example 4, Example 2 used basalt short fibers and polypropylene short fibers of different specifications for its surface and core layers, resulting in an increase in interlayer peel strength from 1.55 N / mm to 2.58 N / mm. The results suggest that under these test conditions, the difference in fiber specifications between the surface and core layers helps improve interlayer bonding performance. In Example 2, the mass percentage of polypropylene short fibers in the surface mixed fiber web was higher than that in the core mixed fiber web. During hot pressing, the higher polypropylene content in the surface layer facilitates the formation of more polypropylene melt, which in turn increases the contact and melt bonding between the surface layer of the reinforcing felt and the backing layer. The different fiber specifications in the surface and core layers also contribute to improving the interfacial bonding strength between the backing layer and the reinforcing layer. Example 4 used a single-layer composite reinforcing felt, and under its corresponding composition and process conditions, its interlayer peel strength was generally lower than that of Example 2.
[0117] Test Example 4: This test evaluates the emission performance of materials inside the vehicle and characterizes the surface organic components.
[0118] (1) Total Volatile Organic Compound Emission Test: The basalt fiber reinforced polypropylene materials after demolding in Examples 1 to 4 and Comparative Example 3 were used as the test materials. Each test material was cut into 100mm × 100mm samples. Before the test, the mass m of each sample was weighed and recorded, and placed in a sampling bag with a polytetrafluoroethylene liner. 2L of high-purity nitrogen was filled into the sampling bag, and after sealing, it was placed in a constant temperature oven at 65°C for 2 hours. The sampling bag was then removed, and the gas inside the bag was extracted by connecting the sampling bag gas valve with a thermal desorption tube.
[0119] The thermal desorption tube was connected to a thermal desorption-gas chromatography analysis system for analysis. The retention time and corresponding response value during the chromatographic analysis were recorded. Taking the samples of Example 2 and Comparative Example 3 as examples, the corresponding gas chromatograms were obtained. A quantitative calibration relationship was established using toluene standard material. The responses of each volatile organic component within the specified analytical range were converted to the equivalent mass of toluene and summed to obtain the total volatile organic compounds (TVOC) released by the sample. This was then divided by the corresponding sample mass m to calculate the TVOC release amount, in μg / g. Three parallel samples were prepared for each test group, and the arithmetic mean was taken as the release amount test result for that group.
[0120] (2) Odor Characteristic Evaluation Test: The finished materials from the same batch after demolding were used as the test objects. The cut samples were placed in 1L odorless glass bottles and sealed. The glass bottles were placed in an 80℃ constant temperature drying oven for 2 hours and then cooled to 60℃ at room temperature. The odor evaluators opened the bottle caps and smelled the samples, scoring them according to the odor evaluation scale of 1 to 6 levels specified in VDA270 (05 / 2022). Level 1 represents no odor, Level 2 represents perceptible but no interference, Level 3 represents obvious but no interference, Level 4 represents interference, Level 5 represents strong interference, and Level 6 represents unacceptable. The scores were recorded as the odor levels. Each group of test objects was scored independently by 3 evaluators, and the arithmetic mean was taken as the odor level of the group.
[0121] (3) Fourier transform infrared spectroscopy test: The basalt short fibers without organosilane coupling treatment in Preparation Example 2 and the surface-treated basalt short fibers used in Comparative Example 3 were used as test objects. A Fourier transform infrared spectrometer with attenuated total reflectance accessory was used for the test. The basalt short fibers were directly pressed onto the attenuated total reflectance test crystal, and the scanning wavenumber range was set to 4000 cm⁻¹. -1 Up to 400cm -1 The infrared absorption characteristics of the two types of basalt short fiber surfaces were compared to characterize the additional absorption signal introduced by the organic surface treatment agent on the surface of the basalt short fiber of Comparative Example 3, and the corresponding infrared spectra were obtained and recorded as basalt short fiber of Preparation Example 2 and basalt short fiber of Comparative Example 3.
[0122] The test results are shown in Table 4.
[0123] Table 4. Test Data Table for Emission Performance Evaluation of Materials Inside the Vehicle:
[0124] in conclusion: According to the data in Table 4, the TVOC release levels of Examples 1 to 4 range from 27.8 μg / g to 47.3 μg / g, and the odor ratings range from 2.0 to 3.5.
[0125] The TVOC emission level and odor grade of Comparative Example 3 were higher than those of Examples 1 to 4. Figure 4 It can be seen that the number of chromatographic peaks and the overall response of the Comparative Example 3 sample were higher than those of the Example 2 sample, while Example 2 still showed some response from volatile organic components, but the overall peak response was significantly lower. Combined with... Figure 5 It can be seen that the surface-treated basalt short fibers used in Comparative Example 3 showed additional organic component absorption signals compared with the untreated basalt short fibers in Preparation Example 2. The results suggest that this phenomenon is related to the state of the raw materials using the organic surface treatment agent in Comparative Example 3.
[0126] Comparative Example 3 used basalt short fibers surface-treated with γ-aminopropyltriethoxysilane coupling agent and polyurethane film-forming agent. Combined with infrared spectroscopy results, it was found that the surface-treated basalt short fibers exhibited additional organic component absorption signals introduced by the surface treatment agent. Simultaneously, the TVOC release of Comparative Example 3 was significantly higher than that of Example 2, indicating that this surface treatment system increased the source of volatile organic components in the composite material.
[0127] Example 2 uses basalt short fibers without organosilane coupling treatment. During hot pressing, the surface of the basalt short fibers is wetted and melt-bonded by polypropylene melt, followed by pressure holding and cooling solidification to form a composite skeleton structure. Compared with Comparative Example 3, Example 2 does not introduce any additional organic surface treatment agents, which to some extent helps reduce the source of volatile organic components introduced into the composite material system by such surface treatment agents. Under the test conditions, Example 2 exhibits lower TVOC emissions and odor levels.
[0128] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A basalt fiber composite reinforced polypropylene material, characterized in that, It includes a backing material, a composite skeleton felt, an adhesive backing layer, and a decorative surface layer, which are stacked from bottom to top and solidified by hot pressing. The composite skeleton felt includes a core fiber felt; Based on the total mass of fibers in the core fiber felt, the core fiber felt comprises the following components by mass percentage: The core layer consists of 50%–70% untreated basalt short fibers, 5%–10% single-component low-melting-point copolyester short fibers, and 20%–45% core layer polypropylene short fibers, with the sum of the mass percentages of each component being 100%.
2. The basalt fiber composite reinforced polypropylene material according to claim 1, characterized in that, The composite skeleton felt is a single-layer composite skeleton felt or a three-layer gradient composite skeleton felt. When the composite skeleton felt is a single-layer composite skeleton felt, the composite skeleton felt is composed of the core fiber felt; When the composite skeleton felt is a three-layer gradient composite skeleton felt, the three-layer gradient composite skeleton felt includes, in order from bottom to top, a bottom surface fiber felt, a core fiber felt, and a top surface fiber felt. Based on the total fiber mass of the bottom or top surface fiber felt, the bottom or top surface fiber felt comprises the following components by mass percentage: The composition consists of 20%–40% untreated surface basalt short fibers, 5%–10% single-component low-melting-point copolyester short fibers, and 50%–75% surface polypropylene short fibers, with the sum of the mass percentages of each component being 100%.
3. The basalt fiber reinforced polypropylene material according to claim 2, characterized in that, The single fiber diameter of the core basalt short fibers that have not undergone organosilane coupling treatment is 13μm to 18.7μm, and the cut length is 64mm. The linear density of the polypropylene short fibers in the core layer is 8D to 11D, and the cut length is 64mm. The single-component low-melting-point copolyester staple fiber has a fiber length of 45.9 mm to 70.4 mm; When the composite skeleton felt is a three-layer gradient composite skeleton felt, the diameter of a single basalt short fiber in the surface layer that has not been treated with organosilane coupling is 8.1μm to 13μm, and the cutting length is 81mm to 121mm; the linear density of the polypropylene short fiber in the surface layer is 5.4D to 8D, and the cutting length is 64mm.
4. The basalt fiber composite reinforced polypropylene material according to claim 1, characterized in that, The backing material has an areal density of 100 g / m³. 2 Polyethylene terephthalate needle-punched nonwoven fabric; The adhesive backing layer is applied at a rate of 45g / m² per unit area. 2 ~110g / m 2 It is composed of low-density polyethylene powder; The decorative surface layer has a surface density of 450 g / m³. 2 Polyethylene terephthalate needle-punched fabric or fabric with a surface density of 750 g / m 2 Polyamide tufted fabric.
5. The basalt fiber reinforced polypropylene material according to claim 1, characterized in that, The single-component low-melting-point copolyester staple fiber is formed from a single low-melting-point modified copolyester, and the heat bonding temperature is 110℃~130℃. The base resin for the core layer polypropylene short fibers is fiber-grade isotactic polypropylene homopolymer, with a melt flow rate of 13.5 g / 10 min to 38.5 g / 10 min and a density of 0.90 g / cm³ under conditions of 230°C and 2.16 kg load. 3 ~0.91g / cm 3 ; The core basalt short fibers that have not undergone organosilane coupling treatment are obtained by completely melting natural basalt ore at 1450℃~1500℃, flowing it out through a platinum-rhodium alloy spinneret and drawing it into continuous fiber filaments. During the drawing process, pure water atomization spray is used for cooling and no organosilane coupling treatment is performed. After drying to remove moisture, the fibers are cut.
6. A method for preparing a basalt fiber composite reinforced polypropylene material, characterized in that, The method for preparing a basalt fiber composite reinforced polypropylene material as described in any one of claims 1-5 comprises the following steps: The composite skeleton felt is prepared by mixing, web-laying and needle-punching the short fibers of each component that make up the composite skeleton felt according to the formula. The composite skeleton felt was individually subjected to low-temperature pre-bonding treatment and then cooled to room temperature; From bottom to top, the backing material, the composite skeleton felt that has undergone low-temperature pre-bonding treatment, the low-density polyethylene powder used to form the adhesive layer, and the decorative surface layer are laid in sequence to obtain the composite blank to be molded. The composite blank to be molded is placed into a mold for preheating and hot pressing. After hot pressing is completed, the mold cooling cycle is started under pressure to cool it down. The pressure is released and the mold is demolded to obtain the basalt fiber reinforced polypropylene material.
7. The preparation method according to claim 6, characterized in that, The process for obtaining the composite skeleton felt is as follows: When preparing a single-layer composite skeleton felt, the core layer basalt short fibers, single-component low-melting-point copolyester short fibers, and core layer polypropylene short fibers without organosilane coupling treatment are weighed out and mixed according to the corresponding mass percentages. The mixture is then carded to form a continuous fiber web and cross-laid to form a mixed fiber web. The mixed fiber web is then directly needle-punched to obtain a single-layer composite skeleton felt. When preparing a three-layer gradient composite skeleton felt, the corresponding mass percentages of untreated basalt short fibers, single-component low-melting-point copolyester short fibers and surface polypropylene short fibers are weighed, opened and mixed, and then formed into a continuous fiber web by a carding machine and cross-laid to form two surface mixed fiber webs. Weigh out the corresponding mass percentages of the untreated basalt short fiber core, the single-component low-melting-point copolyester short fiber, and the core polypropylene short fiber, open and mix them, and form a continuous fiber web by carding and cross-laying to form a core mixed fiber web. Two surface layer mixed fiber webs are pre-needled to obtain two surface layer fiber mats, and the two surface layer fiber mats are respectively used as the bottom surface layer fiber mat and the top surface layer fiber mat. The core layer mixed fiber web is pre-needled to obtain the core layer fiber mat. The layers are stacked in the order of the bottom surface fiber felt, the core fiber felt, and the top surface fiber felt, and then subjected to overall secondary needle punching to obtain a three-layer gradient composite skeleton felt.
8. The preparation method according to claim 7, characterized in that, The total areal density of the composite skeleton felt is 900 g / m³. 2 ~2200g / m 2 The needle density of the integral needle punching of the single-layer composite skeleton felt or the integral secondary needle punching of the three-layer gradient composite skeleton felt is 45 needles / cm. 2 ~110 stitches / cm 2 The needle insertion depth is 8mm to 11mm; When preparing the three-layer gradient composite skeleton felt, the areal density of the bottom surface fiber felt is 225 g / m². 2 ~550g / m 2 The areal density of the top surface fiber felt is 225 g / m³. 2 ~550g / m 2 The areal density of the core fiber felt is 450 g / m³. 2 ~1100g / m 2 ; The pre-needling of the surface hybrid fiber web and the core hybrid fiber web has a needle density of 27 needles / cm. 2 ~66 stitches / cm 2 The needle insertion depth is 5.4mm to 8mm.
9. The preparation method according to claim 6, characterized in that, The specific process of the low-temperature pre-bonding treatment is as follows: the composite skeleton felt is placed in the upper and lower mesh belt heating equipment, the low-temperature pre-bonding temperature of the heating mesh belt is set to 120℃~135℃, and a pre-bonding pressure of 0.09MPa~0.33MPa is applied for heating; after the central area of the composite skeleton felt is heated to 120℃~135℃, it is held for 27s~132s.
10. The preparation method according to claim 6, characterized in that, During the preheating process, the mold temperature is set to 170℃~180℃, a low preheating pressure of 0.09MPa~0.55MPa is applied, and the time is 54s~198s; During the hot pressing and consolidation, the molding pressure is increased to 0.9 MPa to 3.3 MPa, and the pressure is held at 170°C to 180°C for 27 to 132 seconds. During the cooling process, the pressure is released when the temperature of the basalt fiber reinforced polypropylene material drops to 60°C to 80°C.