A ship ceiling fireproof cover and a preparation process thereof
By utilizing plasma activation, silicon oxide nanoparticle deposition, and silane coupling agent treatment in the three-layer structure design of the ship's ceiling fireproof cover, the interfacial bonding problem between the non-combustible board and the steel shell was solved, achieving high bonding strength and B15 fire resistance performance, which meets the green requirements of shipbuilding.
Patent Information
- Application Number
- CN202611565433.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-20
AI Technical Summary
The existing fireproof ceiling covers for ships have insufficient interfacial bonding between the non-combustible board material and the steel shell, resulting in poor structural integrity and long-term reliability. In particular, the interface debonding phenomenon is serious under ship navigation vibration, temperature fluctuations and high humidity salt spray environment, and the organic adhesive decomposes and releases toxic fumes at high temperature in a fire.
It adopts a three-layer structure design, including a steel shell, a non-combustible plate and an aluminum foil. By plasma activation treatment on the surface of the non-combustible plate, silicon oxide nanoparticles are deposited and coated with a silane coupling agent to form a continuous silicate ceramic layer, achieving inorganic interface bonding and avoiding the use of organic coatings.
A continuous chemical bonding path is constructed between the non-combustible sheet and the steel shell, which improves the interfacial adhesion strength and flame penetration resistance, meeting the B15 fire resistance requirements. At the same time, no organic coatings release smoke, making it suitable for the green requirements of shipbuilding.
Smart Images

Figure CN123129552A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of fireproof cover technology, and relates to a fireproof cover for ship ceilings and its manufacturing process. Background Technology
[0002] Fireproof ceiling covers are an important component of the fire-resistant compartmentation system of ships. They are usually installed at ceiling openings (such as downlights, speakers, canopy lights, inspection ports, etc.) to prevent flames and high-temperature smoke from spreading between compartments through the ceiling openings.
[0003] Existing fireproof ceiling covers for ships typically employ a multi-layered composite structure, including a steel outer shell, a non-combustible core layer, and an aluminum foil reflective layer. For example, CN222341845U discloses a fireproof ceiling cover for ships that uses a structure of a cover tube and eaves combined with aluminum foil restraint. The aluminum foil causes the fireproof cover to contract inwards during a fire, improving its adaptability and ease of installation. However, these existing solutions primarily focus on the macroscopic structural design of the fireproof cover, lacking specific solutions for the interface bonding between the non-combustible material and the steel outer shell.
[0004] During the manufacturing process of fireproof covers, non-combustible boards (such as calcium silicate boards, rock wool boards, etc.) are typically fixed to the steel outer shell using adhesives and mechanical fasteners. The surfaces of non-combustible boards usually have high surface energy and chemical inertness, resulting in limited interfacial bonding with inorganic adhesives. Under conditions of shipboard vibration, temperature fluctuations, and high humidity and salt spray, interfacial debonding can easily occur, affecting the structural integrity and long-term reliability of the fireproof cover. To address this issue, organic primers or adhesives are often used to improve interfacial bonding. However, organic materials decompose at high temperatures during a fire, releasing toxic fumes and causing interfacial failure.
[0005] Therefore, there is an urgent need to provide a fireproof cover for ship ceilings that can simultaneously achieve enhanced interfacial adhesion and improved fire resistance through an inorganic surface treatment system, as well as its preparation process. Summary of the Invention
[0006] The purpose of this invention is to provide a fireproof cover for ship ceilings and its manufacturing process. Through the combination of a three-layer structure and surface modification, the fireproof cover can meet the B15 fire resistance requirement.
[0007] The objective of this invention can be achieved through the following technical solutions: A fireproof ceiling cover for ships, the fireproof cover being composed of a steel outer shell, a non-combustible plate and an aluminum foil in sequence, wherein the non-combustible plate is disposed between the steel outer shell and the aluminum foil; The surface of the non-combustible sheet facing the steel shell is an activated surface that has undergone plasma activation treatment. The activated surface is deposited with a silicon oxide deposition layer and treated with a silane coupling agent hydrolysate.
[0008] The fireproof cover of this invention consists of a three-layer structure: a steel outer shell, a non-combustible board, and aluminum foil. The steel outer shell enhances the mechanical strength of the fireproof cover and provides the first line of fire protection. The non-combustible board serves as the main heat insulation layer, and the aluminum foil helps to reflect heat and provide moisture protection. Together, these three elements meet the B15 fire rating requirement for ship ceilings. The non-combustible board undergoes a three-step surface modification treatment involving atmospheric pressure plasma activation, silicon oxide nanoparticle deposition, and silane coupling agent hydrolysis. This process solves the interfacial adhesion problem between the non-combustible board and the steel outer shell without introducing any organic coatings and improves the flame penetration resistance of the board surface.
[0009] The silicon oxide deposited layer on the non-combustible surface can sinter with the surface layer of the non-combustible board at high temperature to form a continuous silicate ceramic protective layer, which further improves the flame penetration resistance. At the same time, the inorganic silicon-oxygen structure left after the silane coupling agent decomposes at high temperature still maintains the interface integrity.
[0010] As a preferred embodiment of the present invention, the non-combustible board is one of calcium silicate board, rock wool board, aerogel board and basalt fiber board.
[0011] As a preferred embodiment of the present invention, the thickness of the steel outer shell is 0.3~1.0mm; the thickness of the non-combustible plate is 3~10mm; and the thickness of the aluminum foil is 0.05~0.2mm.
[0012] The non-combustible boards used in this invention are calcium silicate boards, rock wool boards, aerogel boards, and basalt fiber boards. These materials are all Class A non-combustible materials with excellent fire resistance, making them suitable for marine fire protection applications. Furthermore, the surfaces of these boards contain abundant silanol groups or inorganic polar groups, which can effectively complement atmospheric pressure plasma activation treatment, ensuring uniform deposition of silicon oxide nanoparticles and effective bonding of silane coupling agents, resulting in strong process versatility.
[0013] As a preferred embodiment of the present invention, the silicon oxide nanoparticles in the silicon oxide deposition layer have a particle size of 8~36nm, and the thickness of the silicon oxide deposition layer is 20~200nm.
[0014] The silicon oxide nanoparticles deposited on the surface possess high specific surface area and nanoscale roughness, providing numerous anchoring sites for silane coupling agents. This also facilitates the penetration of adhesives during subsequent fireproof cover assembly, forming a mechanical interlock. By controlling the thickness to 20–200 nm, the silicon oxide deposited layer can be fully sintered with the substrate surface at high temperatures, forming a continuous ceramicized layer without shrinkage cracking due to excessive thickness.
[0015] In a preferred embodiment of the present invention, the silane coupling agent is at least one of KH550, KH560, and KH570, the concentration of the silane coupling agent hydrolysate is 0.5~2wt%, and the coating amount is 5~20g / m². 2 .
[0016] After hydrolysis, silane coupling agents produce silanol groups, which can condense with Si-OH on the surface of silicon oxide nanoparticles to form Si-O-Si bonds. At the same time, their organic functional groups (such as amino and epoxy groups) can form hydrogen bonds or physical adsorption with silanol or phosphate groups in inorganic high-temperature adhesives, thereby improving interfacial wettability and adhesive strength.
[0017] A manufacturing process for a fireproof ceiling cover for ships includes the following steps: S1. Prepare a steel casing, non-combustible sheet metal, and aluminum foil; S2. The surface of the non-combustible board is subjected to plasma activation treatment; S3. On the surface treated by S2, silicon oxide nanoparticles are deposited on the surface using a silicon-containing precursor by plasma-enhanced chemical vapor deposition to form a silicon oxide deposition layer. S4. Coat the surface of the non-combustible board treated with S3 with silane coupling agent hydrolysate and dry. S5. The non-combustible sheet material treated in S4 is placed between the steel shell and the aluminum foil. After assembly, the edges are sealed with inorganic sealant. The assembly method is at least one of adhesive and mechanical fastening, thus obtaining the ship ceiling fireproof cover.
[0018] As a preferred technical solution of the present invention, in step S2, the conditions for plasma activation treatment are: oxygen / argon mixed atmosphere, processing power of 100~500W, and processing time of 30~300s.
[0019] As a preferred embodiment of the present invention, in step S3, the silicon-containing precursor is hexamethyldisiloxane or tetramethylsilane.
[0020] In a preferred embodiment of the present invention, in step S3, the concentration of the silicon-containing precursor is 100-500 ppm based on the carrier gas carrying capacity, and the deposition power density is 0.5-2 W / cm³. 2 The deposition time is 30~90s.
[0021] As a preferred embodiment of the present invention, in step S5, the adhesive is a silicate-based adhesive or a phosphate-based adhesive.
[0022] As a preferred embodiment of the present invention, the silicon-containing precursor is hexamethyldisiloxane, and argon is used as the carrier gas with a flow rate of 0.05~0.10 SCCM.
[0023] As a preferred embodiment of the present invention, the silicon-containing precursor is tetramethylsilane, and oxygen is introduced as an oxidant at a flow rate of 0.3~0.8 slm.
[0024] This invention provides a specific manufacturing process for fireproof covers. First, non-combustible panels are treated with atmospheric pressure plasma, which effectively cleans the panel surface, introduces Si-OH functional groups, and increases surface energy, resulting in a water contact angle ≤30°, thus providing uniform nucleation sites for subsequent silicon oxide deposition. This process requires no vacuum equipment, making it suitable for continuous processing of large-size marine ceiling panels. The equipment investment and operating costs are lower than those of low-pressure plasma or vacuum deposition processes.
[0025] After surface activation via plasma, deposition occurs, allowing the silicon-containing precursor to fully decompose in the plasma discharge region. Controlling the concentration prevents excessive gas-phase nucleation, avoiding the accumulation of large amounts of powder particles on the substrate surface, thus ensuring uniform deposition. A moderate deposition power density enables silicon oxide nanoparticles to nucleate on the activated surface in an island-like growth pattern, gradually forming a continuous layer that bonds strongly to the substrate surface via Si-O-Si bonds. The sequence of activation-deposition-coupling maximizes the effectiveness of each step, ensuring good process repeatability and suitability for mass production.
[0026] The entire process does not use organic solvents, and the silane coupling agent hydrolysate is a water-based system with good environmental performance, meeting the requirements for green shipbuilding.
[0027] The beneficial effects of this invention are: (1) This invention constructs a continuous chemical bonding path between a non-combustible sheet and a steel shell through a three-step synergistic surface modification process involving atmospheric pressure plasma activation, silicon oxide nanoparticle deposition, and silane coupling agent treatment. First, plasma activation introduces high-density Si-OH functional groups into the surface of the sheet, providing nucleation sites for silicon oxide nanoparticles. The silicon oxide nanoparticles bond with the activated surface via Si-O-Si bonds, forming a strong chemical anchor. The silanols obtained after hydrolysis by the silane coupling agent condense with the Si-OH groups on the surface of the nanoparticles. The organic functional groups of the silanols form hydrogen bonds and physical adsorption with the inorganic high-temperature resistant adhesive, improving the interfacial wettability and bonding strength.
[0028] (2) The fireproof cover of the present invention is composed of a steel shell, a non-combustible plate and an aluminum foil in sequence. The three-layer structure works together to form a clear gradient division of labor in fire protection function. The three-layer structure works together with surface modification to enable the fireproof cover to meet the B15 fire resistance requirement under the conditions of controlled weight, thickness and cost. Attached Figure Description
[0029] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to the accompanying drawings.
[0030] Figure 1 This is a schematic diagram of the structure of the fireproof cover of the present invention; Figure 2 This is a photograph of the fireproof cover prepared in Example 1. Detailed Implementation
[0031] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.
[0032] It should be noted that in the following examples and comparative examples, the adhesive used is a silicate-based adhesive (HK-SN type fire retardant sealant, Shanghai Huoke New Material Co., Ltd.); unless otherwise specified, the present invention does not specifically limit the source of the raw materials used, and commercially available products or products prepared by conventional preparation methods well known to those skilled in the art can be used. Experimental methods without specific conditions are all conventional methods and conditions well known in the art.
[0033] Example 1
[0034] S1. Prepare a steel outer shell (0.5mm thick), a calcium silicate board (5mm thick), and aluminum foil (0.1mm thick). S2. The surface of the calcium silicate board is subjected to atmospheric pressure plasma activation treatment. The plasma activation treatment is carried out in an oxygen / argon mixed atmosphere (O2 volume ratio of 20%, Ar as the balance gas), with a treatment power of 300W and a treatment time of 150s. S3. On the surface treated in S2, plasma-enhanced chemical vapor deposition (PECVD) is performed using a DBD plasma source. The silicon precursor is hexamethyldisiloxane. The deposition is carried out via a bubbling method with argon as the carrier gas at a flow rate of 0.08 SCCM and a deposition power density of 1.0 W / cm³. 2 The deposition time was 60s, the substrate temperature was 80℃, and a silicon oxide deposition layer was formed with a thickness of 80nm.
[0035] S4. Coat the surface of the non-combustible board treated in S3 with KH550 silane coupling agent hydrolysate. The hydrolysate is a mixture of KH550, deionized water, and anhydrous ethanol in a volume ratio of 1:3:6, with the pH adjusted to 3.5 by acetic acid. The concentration is 1.0 wt%, and the coating amount is 10 g / m². 2 Dry at 80℃ for 15 minutes.
[0036] S5. Place the non-combustible sheet material treated with S4 between the steel shell and the aluminum foil, assemble them with adhesive, and seal the edges with inorganic sealant to obtain the fireproof ceiling cover for the ship.
[0037] Example 2
[0038] S1. Prepare a steel outer shell (0.3mm thick), a calcium silicate board (3mm thick), and aluminum foil (0.05mm thick). S2. The surface of the non-combustible board is activated by atmospheric pressure plasma under an oxygen / argon mixed atmosphere (O2 volume percentage 20%, Ar as the balance gas), with a processing power of 100W and a processing time of 30s.
[0039] S3. On the surface treated in S2, silicon oxide nanoparticles are deposited on its surface using atmospheric pressure plasma-enhanced chemical vapor deposition (PECVD) with a DBD plasma source and hexamethyldisiloxane as the silicon precursor, forming a silicon oxide deposition layer. Argon is used as the carrier gas with a flow rate of 0.05 SCCM and a deposition power density of 1.0 W / cm³. 2 The deposition time was 60 seconds.
[0040] S4. Coat the surface of the non-combustible board treated in S3 with KH550 silane coupling agent hydrolysate. The hydrolysate is a mixture of KH550, deionized water, and anhydrous ethanol in a volume ratio of 1:3:6, with the pH adjusted to 3.5 by acetic acid, and the concentration is 0.5wt%. The coating amount is 5g / m². 2 Dry at 80℃ for 15 minutes.
[0041] S5. Place the non-combustible sheet material treated with S4 between the steel shell and the aluminum foil, assemble them with adhesive, and seal the edges with inorganic sealant to obtain the fireproof ceiling cover for the ship.
[0042] Example 3
[0043] S1. Prepare a steel outer shell (1.0mm thick), a calcium silicate board (10mm thick), and aluminum foil (0.2mm thick). S2. The surface of the non-combustible board is subjected to atmospheric pressure plasma activation treatment under an oxygen / argon mixed atmosphere (O2 volume percentage 20%, Ar as balance gas), with a treatment power of 500W and a treatment time of 300s.
[0044] S3. On the surface treated in S2, a silicon oxide deposition layer is formed using plasma-enhanced chemical vapor deposition (PECVD) with a DBD plasma source and hexamethyldisiloxane as the silicon precursor. Argon is used as the carrier gas at a flow rate of 0.10 SCCM, and the deposition power density is 1.0 W / cm³. 2 The deposition time was 60 seconds.
[0045] S4. Coat the surface of the non-combustible board treated in S3 with KH550 silane coupling agent hydrolysate. The hydrolysate is a mixture of KH550, deionized water, and anhydrous ethanol in a volume ratio of 1:3:6, with the pH adjusted to 3.5 by acetic acid. The concentration is 2wt%, and the coating amount is 20g / m². 2 Dry at 80℃ for 15 minutes.
[0046] S5. Place the non-combustible sheet material treated with S4 between the steel shell and the aluminum foil, assemble them with adhesive, and seal the edges with inorganic sealant to obtain the fireproof ceiling cover for the ship.
[0047] Example 4
[0048] This example is essentially the same as Example 1, except that the non-combustible board used in this example is rock wool board (5mm thick, 100kg / m³). 3 ).
[0049] Example 5
[0050] Steps S1, S2, S4, and S5 are the same as in Example 1, except for step S3: S3. Silicon oxide nanoparticles were deposited on the activated surface using plasma-enhanced chemical vapor deposition (PECVD). Tetramethylsilane was used to deposit the nanoparticles, and Ar was introduced as the carrier gas via a bubbling method at a flow rate of 0.06 SCCM. O2 was simultaneously introduced as an oxidant at a flow rate of 0.5 SCCM. The deposition power density was 1.0 W / cm³. 2 The deposition time was 60 seconds.
[0051] Example 6
[0052] This is basically the same as Example 1, except that the silane coupling agent used in this example is KH570.
[0053] Comparative Example 1 This is basically the same as Example 1, except that the surface of the non-combustible board is not treated in any way in this comparative example.
[0054] Comparative Example 2 This is basically the same as Example 1, except that the surface of the non-combustible board in this comparative example is only subjected to plasma activation treatment.
[0055] Comparative Example 3 This is basically the same as Example 1, except that in this comparative example, only silicon oxide is deposited on the surface of the non-combustible board.
[0056] Comparative Example 4 This is basically the same as Example 1, except that the surface of the non-combustible board in this comparative example is only coated with silane coupling agent hydrolysate.
[0057] Comparative Example 5 This is basically the same as Example 1, except that in this comparative example, the surface of the non-combustible board is treated with an epoxy resin primer instead of the three-step treatment, and the epoxy primer thickness is 50μm.
[0058] Performance testing: Fire resistance: The fireproof cover was subjected to a B15 fire resistance test according to IMO FTP Code Part 3: B15 requires insulation for 15 minutes, integrity for 30 minutes, and the maximum temperature rise of any thermocouple not exceeding 225℃. The data obtained are shown in the table below:
[0059] Figure 1 This is a schematic diagram of the ceiling fireproof cover prepared according to the present invention. It consists of a three-layer structure: a steel outer shell, a non-combustible board, and aluminum foil. A physical image of the completed product is shown below. Figure 2 As shown above, the embodiments of the present invention all meet the B15 fire resistance requirements. Example 4 uses rock wool board, with a maximum temperature rise of 106.2℃, and its performance is slightly lower than that of calcium silicate board. Example 5's performance is close to that of Example 1, illustrating the applicability of different silicon-containing precursors.
[0060] This invention achieves high bonding strength, B15 fire resistance, and zero smoke release through a three-step synergistic treatment of "plasma activation + silicon oxide nanoparticle deposition + silane coupling agent" without introducing an organic coating.
[0061] The three-layer structure of Comparative Example 1 was not surface-treated, and its maximum temperature rise was 238.6℃, heat insulation was 13 min, and integrity was 28 min, which did not meet the B15 fire resistance requirements.
[0062] Comparative Example 2, after plasma activation only, met the B15 fire resistance requirement; Comparative Example 3, after deposition only, had a maximum temperature rise of 215.7℃ and a heat insulation time of 14 minutes, failing to meet the B15 fire resistance requirement; and the deposited layer had poor adhesion.
[0063] Comparative Example 4, treated with coupling agent only: maximum temperature rise of 208.1℃, heat insulation for 14 minutes, did not meet the B15 fire resistance requirement.
[0064] Comparative Example 5, coated with an epoxy primer, experienced a rapid temperature rise after being exposed to fire for 8 minutes. It provided only 9 minutes of heat insulation and 25 minutes of integrity, and released a large amount of white smoke. Its performance was far inferior to that of Example 1 of the present invention.
[0065] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A fireproof ceiling cover for ships, characterized in that, The fireproof cover is composed of a steel outer shell, a non-combustible plate, and an aluminum foil, with the non-combustible plate disposed between the steel outer shell and the aluminum foil. The surface of the non-combustible sheet facing the steel shell is an activated surface that has undergone plasma activation treatment. The activated surface is deposited with a silicon oxide deposition layer and treated with a silane coupling agent hydrolysate.
2. The fireproof ceiling cover for ships according to claim 1, characterized in that, The non-combustible board material is one of calcium silicate board, rock wool board, aerogel board, and basalt fiber board.
3. The fireproof ceiling cover for ships according to claim 1, characterized in that, The steel outer shell has a thickness of 0.3~1.0mm; the non-combustible board has a thickness of 3~10mm; and the aluminum foil has a thickness of 0.05~0.2mm.
4. The fireproof ceiling cover for ships according to claim 1, characterized in that, The silicon oxide nanoparticles in the silicon oxide deposition layer have a particle size of 8~36nm, and the thickness of the silicon oxide deposition layer is 20~200nm.
5. The fireproof ceiling cover for ships according to claim 1, characterized in that, The silane coupling agent is at least one of KH550, KH560, and KH570, the concentration of the silane coupling agent hydrolysate is 0.5~2wt%, and the coating amount is 5~20g / m². 2 .
6. A manufacturing process for a fireproof ceiling cover for ships as described in any one of claims 1-5, characterized in that, Includes the following steps: S1. Prepare a steel casing, non-combustible sheet metal, and aluminum foil; S2. The surface of the non-combustible board is subjected to plasma activation treatment; S3. On the surface treated by S2, silicon oxide nanoparticles are deposited on the surface using a silicon-containing precursor by plasma-enhanced chemical vapor deposition to form a silicon oxide deposition layer. S4. Coat the surface of the non-combustible board treated with S3 with silane coupling agent hydrolysate and dry. S5. The non-combustible sheet material treated in S4 is placed between the steel shell and the aluminum foil. After assembly, the edges are sealed with inorganic sealant. The assembly method is at least one of adhesive and mechanical fastening, thus obtaining the ship ceiling fireproof cover.
7. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, In step S2, the conditions for plasma activation treatment are: oxygen / argon mixed atmosphere, processing power of 100~500W, and processing time of 30~300s.
8. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, In step S3, the silicon-containing precursor is hexamethyldisiloxane or tetramethylsilane.
9. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, In step S3, the concentration of the silicon-containing precursor is 100~500 ppm based on the carrier gas carrying capacity, and the deposition power density is 0.5~2 W / cm³. 2 The deposition time is 30~90s.
10. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, In step S5, the adhesive is a silicate-based adhesive or a phosphate-based adhesive.
11. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, The silicon-containing precursor is hexamethyldisiloxane, with argon as the carrier gas and a carrier gas flow rate of 0.05~0.10 SCCM.
12. The manufacturing process of the fireproof cover for ship ceilings according to claim 6, characterized in that, The silicon-containing precursor is tetramethylsilane, and oxygen is introduced as an oxidant at a flow rate of 0.3~0.8 slm.