Low thermal resistance aluminum substrate interface sectional compression process
By using a segmented lamination process with modified heat-resistant adhesives and low thermal resistance fillers, the problem of insufficient thermal conductivity of the insulating layer of aluminum substrates was solved, enabling the manufacture of aluminum substrates with high thermal conductivity, low thermal resistance, and high reliability.
Patent Information
- Application Number
- CN202611313135.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-20
AI Technical Summary
In the existing technology, the insulating layer material and lamination technology of aluminum substrates have failed to effectively improve thermal conductivity while maintaining bonding performance, resulting in high thermal resistance of aluminum substrates, which cannot meet the requirements of high thermal conductivity, low thermal resistance and high reliability.
A modified heat-resistant adhesive and a low thermal resistance filler are used to prepare the insulation layer by a segmented pressing process, including the segmented pressing of the aluminum base layer, the thermally conductive insulation layer and the circuit layer. The modified heat-resistant epoxy resin compound and the low thermal resistance filler are used to improve the thermal conductivity and adhesion of the insulation layer.
It improves the thermal conductivity and adhesion of the aluminum substrate, reduces thermal resistance, and enhances the heat resistance and thermal stability of the insulation layer, making it suitable for long-term high-temperature LED operation and avoiding the problem of aluminum substrate warping during lamination.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aluminum substrate manufacturing technology, specifically relating to a segmented lamination process for the interface of a low thermal resistance aluminum substrate. Background Technology
[0002] Aluminum substrates are currently the most widely used type of metal-based heat dissipation substrates. Composed of an aluminum base layer, an insulating layer, and a circuit layer, they possess excellent mechanical strength, dimensional stability, and heat dissipation performance. By utilizing the high thermal conductivity of aluminum, heat generated by electronic components is rapidly conducted to the external heat dissipation structure, effectively reducing operating temperature. Therefore, they are widely used in LED lighting, power modules, and power devices. Currently, epoxy resin is commonly used as the insulating layer matrix for aluminum substrates. However, the inherent thermal conductivity of the resin material often makes the insulating layer a key bottleneck restricting heat transfer. To improve the thermal conductivity of the insulating layer, high-filler-ratio micron-sized alumina or boron nitride particles are often used. Excessive filler content leads to a decrease in the insulation and adhesion properties of the composite material, making it unsuitable for substrate applications. Therefore, improving the thermal conductivity of the insulating layer and reducing the thermal resistance of the insulating layer and interface, without excessively increasing the amount of thermally conductive filler and avoiding a significant decrease in adhesion, is of great significance for obtaining aluminum substrates that combine high thermal conductivity, low thermal resistance, and high reliability.
[0003] Chinese invention patent CN116321732B discloses a single-sided aluminum substrate pressing device and process, including a vacuum chamber and a pressing plate disposed inside the vacuum chamber. An mounting groove is provided above the worktable, and support platforms are symmetrically distributed and movably connected to the worktable, with magnets disposed on opposite sides of the support platforms. A pressure plate is mounted on top of the support platforms, with a placement groove on the top. After the pressing plate is pressed down, the pressure plate and the pressing plate are in clearance fit. A synchronous belt conveyor mechanism is installed in the mounting groove on the worktable via an adjustment device. The synchronous belt conveyor mechanism includes a synchronous belt and synchronous pulleys. The support platform passes through the middle of the synchronous belt, and the pressure plate is mounted on both sides of the synchronous belt. The vacuum chamber and the pressing plate descend synchronously to prepare for pressing. The vacuum chamber evacuates internal air, while simultaneously pulling the synchronous belt to fit against the gap between the vacuum chamber and the pressure plate. The synchronous belt seals the internal space of the vacuum chamber, thereby ensuring a vacuum effect. However, existing technologies have the technical problem of not improving the thermal conductivity of aluminum substrates while maintaining their bonding performance through further improvements to the insulating layer materials and lamination techniques. Summary of the Invention
[0004] The purpose of this invention is to provide a segmented lamination process for the interface of a low thermal resistance aluminum substrate, which solves the technical problem in the prior art that the bonding performance of the aluminum substrate is not improved while the thermal conductivity of the aluminum substrate is improved through further improvements to the insulating layer material and lamination technology.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A low thermal resistance aluminum substrate, comprising, from bottom to top, an aluminum base layer, a thermally conductive insulating layer, and a circuit layer; The aluminum base layer uses 5052 series aluminum alloy with a thickness of 1~1.5mm; The thermally conductive insulating layer has a thickness of 75~120μm and is made from the following raw materials in parts by weight: 50~60 parts heat-resistant adhesive, 10~20 parts organic solvent, 1~3 parts dispersant, 1~5 parts curing agent, 2~3 parts curing accelerator and 20~30 parts low thermal resistance filler. The circuit layer is a copper foil with a thickness of 70~140μm; The curing agent is prepared by mixing bismaleimide and 4,4'-diaminodiphenyl sulfone in a mass ratio of 1:3~5.
[0006] The organic solvent is any one or a combination of ethyl acetate, butanone, and N,N-dimethylacetamide; the curing accelerator is any one or a combination of 2-methylimidazole, dicyandiamide, and 2-ethyl-4-methylimidazole.
[0007] The preparation method of the heat-resistant adhesive includes the following steps: S11. Vanillin and N,N-dimethylacetamide were added to a reaction vessel, 4-amino-o-cresol was added, the mixture was heated and stirred, and after the reaction was completed, the solid was collected by filtration, washed with anhydrous ethanol, and dried to obtain the modified heat-resistant monomer. S12. Add the modified heat-resistant monomer, epichlorohydrin and isopropanol to the reactor, add tetramethylammonium bromide, heat and react in a nitrogen atmosphere, cool down, add 40~50wt% sodium hydroxide aqueous solution while stirring, keep the reaction at the temperature, cool to room temperature, wash with deionized water until neutral, add anhydrous sodium sulfate to remove water, and rotary evaporate to obtain the heat-resistant epoxy resin compound. S13. Heat-resistant adhesive is prepared by mixing heat-resistant epoxy resin compound, E-51 epoxy resin and E-44 epoxy resin.
[0008] Preferably, the ratio of vanillin, N,N-dimethylacetamide and 4-amino-o-cresol in S11 is (25~30) g: (150~200) mL: (20~25) g, the temperature is raised to 70~80℃ and the reaction is carried out at 300~500 rpm for 2~4 h, and then dried at 50~60℃ for 4~6 h.
[0009] Preferably, the ratio of modified heat-resistant monomer, epichlorohydrin, isopropanol, tetramethylammonium bromide and sodium hydroxide aqueous solution in S12 is (30~40)g:(150~200)g:(100~150)mL:(3~5)g:(100~150)g. The mixture is heated to 85~90℃ in a nitrogen atmosphere and reacted for 4~6h. The temperature is then lowered to 40~50℃ and sodium hydroxide aqueous solution is added at a rotation speed of 300~500rpm. The mixture is then kept at 60~65℃ and reacted for 1~2h.
[0010] Preferably, the mass ratio of the heat-resistant epoxy resin compound, E-51 epoxy resin and E-44 epoxy resin in S13 is 1.5~2:1.5~2.5:2.5~3.
[0011] The method for preparing the low thermal resistance filler includes the following steps: S21. Add boron nitride to an isopropanol aqueous solution in which isopropanol and deionized water are mixed at a volume ratio of 1:1, sonicate at room temperature, centrifuge and filter, collect the supernatant, and vacuum dry to obtain hexagonal boron nitride. Add hexagonal boron nitride to deionized water and shear and stir to obtain a hexagonal boron nitride dispersion. S22. Tris(hydroxymethyl)aminomethane was added to a hexagonal boron nitride dispersion, dopamine hydrochloride was added, and ammonia was added to adjust the pH to 8.5. The mixture was stirred at room temperature, centrifuged and filtered to collect the solid, washed with deionized water and ethanol in sequence, and dried under vacuum to obtain dopamine-modified boron nitride. S23. Alumina particles are added to an ethanol-water solution prepared by mixing ethanol and deionized water at a volume ratio of 1:1. KH-550 is added for surface modification. The solid is collected by filtration, washed with deionized water, and dried to obtain modified alumina particles. Modified alumina particles, carbon nanotubes, and modified boron nitride are added to N,N-dimethylacetamide for ultrasonic dispersion, heated and stirred, centrifuged and filtered to collect the solid. The solid is washed with deionized water and ethanol in sequence and dried under vacuum to obtain a low thermal resistance filler.
[0012] Preferably, the ratio of boron nitride to isopropanol aqueous solution in S21 is (1~2) g: (80~100) mL. The solution is ultrasonicated at a power of 300~350W and a frequency of 20~40kHz for 6~8 hours, centrifuged at a speed of 800~1200rpm for 10~15 minutes to remove the solid, centrifuged at a speed of 3000~4000rpm for 10~15 minutes, and the supernatant is collected. The solution is then vacuum dried at 60~80℃ for 4~6 hours and stirred at a speed of 1000~2000rpm for 30~60 minutes. The concentration of the hexagonal boron nitride dispersion is 3~5 mg / mL.
[0013] Preferably, the ratio of tris(hydroxymethyl)aminomethane, hexagonal boron nitride dispersion and dopamine hydrochloride in S22 is (0.4~0.5) g : (300~500) mL : (0.8~1) g. The mixture is stirred at 300~500 rpm for 20~24 h, centrifuged at 3000~4000 rpm for 10~15 min, and then vacuum dried at 60~80℃ for 4~6 h.
[0014] Preferably, the average particle size of the alumina particles in S23 is 1~3μm, and the ratio of alumina particles, ethanol aqueous solution and KH-550 is (5~8)g:(100~200)mL:(0.8~1)g. The alumina particles are heated to 50~60℃ for 1~2h, dried at 50~60℃ for 4~6h, and the mass ratio of modified alumina particles, carbon nanotubes, modified boron nitride and N,N-dimethylacetamide is 5~6:0.1~0.2:1~1.5:80~100. The alumina particles are ultrasonically dispersed at 30~50W power and 20~40kHz frequency for 20~30min, heated to 60~70℃ and stirred at 300~500rpm for 4~8h, centrifuged at 3000~4000rpm for 10~15min, and vacuum dried at 60~80℃ for 4~6h.
[0015] A segmented lamination process for the interface of a low thermal resistance aluminum substrate includes the following steps: S1. Add the aluminum alloy plate to a 5-8 wt% sodium hydroxide aqueous solution to remove oil, wash with deionized water, dry, and then grind in a grinding machine to remove the oxide layer. After grinding, wash with deionized water, vacuum dry, and set aside. S2. Add the heat-resistant adhesive, organic solvent and dispersant to the mixing tank and stir at 300~500 rpm for 20~30 min. Then add the low thermal resistance filler and stir at 2000~3000 rpm for 60~120 min. Finally add the curing agent and curing accelerator and stir at 600~800 rpm for 30~60 min. Degas at a vacuum degree of -0.09~-0.1 MPa for 3~5 min to obtain a thermally conductive mixture. Coat the thermally conductive mixture into a film and bake to obtain a semi-cured insulation layer. S3. The aluminum plate, semi-cured insulating layer and copper foil are stacked in sequence, pressed and cured in sections, and cooled to room temperature to obtain a low thermal resistance aluminum substrate.
[0016] Preferably, in step S1, the oil is removed by adding a sodium hydroxide aqueous solution at 40-60°C for 5-10 minutes, drying at 100-110°C for 10-15 minutes, and then polishing with a 400-600 mesh abrasive belt at a belt linear speed of 15-18 m / s and a pressure of 0.1-0.3 MPa. The feed speed is 2-4 m / min, the polishing amount is 10-20 μm, and the surface roughness is polished to 0.4-0.8 μm.
[0017] Preferably, in step S2, the sample is baked at 80-90°C for 30-60 minutes, and a sample is scraped from the edge of the aluminum substrate with a sharp blade. The degree of curing is detected by infrared spectroscopy and found to be 70-80%.
[0018] Preferably, in step S3, after evacuating to -0.08 to -0.1 MPa, the temperature is preheated to 80 to 100°C and held for 5 to 10 minutes. Then, the temperature is increased to 130 to 150°C at a rate of 2 to 3°C / min with a pressure of 0.1 to 0.3 MPa and held for 10 to 20 minutes. Next, the temperature is increased to 170 to 180°C at a rate of 2 to 3°C / min. Then, the temperature is compressed at 13 to 16 MPa for 60 to 80 minutes. Finally, the temperature is decreased to 130 to 150°C at a rate of 1 to 1.5°C / min and held for 10 to 20 minutes. The pressure is then released to 8 to 10 MPa, and the temperature is decreased to 80 to 100°C at a rate of 1.5 to 2°C / min and held for 10 to 20 minutes. The pressure is then released to atmospheric pressure, and the temperature is decreased to room temperature at a rate of 2 to 3°C / min.
[0019] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention involves reacting vanillin with 4-amino-o-cresol to form a modified heat-resistant monomer containing imine bonds and phenolic hydroxyl groups, which is then condensed with epichlorohydrin to obtain a heat-resistant epoxy resin compound. Compared with conventional bisphenol A epoxy resin, this heat-resistant epoxy resin compound has a higher aromatic ring density. The imine bonds and bismaleimide crosslink and cure to form a highly crosslinked network, which improves the heat resistance of the resin matrix. The heat-resistant adhesive prepared by mixing this heat-resistant epoxy resin compound, E-51 epoxy resin, and E-44 epoxy resin improves the heat resistance of the insulating layer. The low viscosity of E-51 ensures uniform dispersion under high filling conditions, and the toughening effect of E-44 maintains the integrity of the filler network during long-term thermal cycling, making the obtained aluminum substrate suitable for long-term high-temperature LED operation.
[0020] 2. This invention utilizes dopamine-modified hexagonal boron nitride, kH-550-modified alumina particle surface, and N,N-dimethylacetamide to disperse and assemble modified alumina particles, carbon nanotubes, and modified boron nitride to obtain a low thermal resistance filler. During the baking and semi-curing process, this low thermal resistance filler deposits and arranges itself to form a thermally conductive pathway within the insulation layer. The dopamine-modified hexagonal boron nitride improves the interfacial compatibility between hexagonal boron carbide and resin, reacts and grafts with kH-550 on the surface of modified alumina particles, reduces phonon scattering centers between inorganic fillers and resin, lowers the interfacial thermal resistance between fillers, and inhibits microcrack propagation through carbon nanotube bridging. It is also less prone to desorption at high temperatures, which helps maintain the thermal stability of the insulation layer.
[0021] 3. This invention thoroughly cleans the oxide layer on the surface of the aluminum substrate, reducing the oxide layer, lowering the overall thermal resistance of the aluminum substrate, improving the interfacial bonding performance between the aluminum plate and the insulating layer material, and improving the thermal conductivity of the aluminum substrate. The segmented pressing process involves vacuum preheating to remove moisture and air bubbles, and slow heating to promote resin flow and wet the surface of the aluminum plate and copper foil, reducing residual air bubbles. During the high-pressure and high-temperature stage, maleimide ring-opening polymerization and epoxy-amine curing are carried out. During the stepped cooling and pressure holding stage, some pressure is released before the cross-linked network is completely frozen, allowing the internal stress to gradually relax and avoiding the problem of aluminum substrate warping caused by thermal stress accumulation. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] The dispersant involved in this invention is BYK-110; the carbon nanotubes have an outer diameter of 4.7 nm, a length of 2 μm, a purity of 98.5%, and a carboxyl content of 3.8 wt%; the boron nitride has an average particle size of 5 μm and a purity of 99.5%.
[0024] Example 1: A low thermal resistance aluminum substrate of this embodiment includes, from bottom to top, an aluminum base layer, a thermally conductive insulating layer, and a circuit layer. The aluminum base layer uses 5052 series aluminum alloy with a thickness of 1.2mm; The thermally conductive insulating layer has a thickness of 75 μm and is made from the following raw materials: 50 g heat-resistant adhesive, 15 g organic solvent, 1 g dispersant, 2.5 g curing agent, 3 g curing accelerator and 20 g low thermal resistance filler; The circuit layer is a copper foil with a thickness of 70 μm; The curing agent is prepared by mixing bismaleimide and 4,4'-diaminodiphenyl sulfone in a mass ratio of 1:5.
[0025] The organic solvent is ethyl acetate; the curing accelerator is prepared by mixing dicyandiamide and 2-ethyl-4-methylimidazole in a mass ratio of 1:1.
[0026] The method for preparing the heat-resistant adhesive in this embodiment includes the following steps: S11. Add 25g vanillin and 20.2g 4-amino-o-cresol to 150mL of N,N-dimethylacetamide, heat to 70℃ and stir at 300rpm for 2h, filter to collect solid, wash with anhydrous ethanol, and dry at 50℃ for 4h to obtain modified heat-resistant monomer. S12. Add 30g of modified heat-resistant monomer, 150g of epichlorohydrin and 100mL of isopropanol to a reaction vessel, add 3g of tetramethylammonium bromide, heat to 85℃ in a nitrogen atmosphere and react for 4h, cool to 40℃ and stir at 300rpm, add 100g of 40wt% sodium hydroxide aqueous solution, keep at 60℃ and react for 1h, cool to room temperature, wash with deionized water until neutral, add anhydrous sodium sulfate to remove water, and rotary evaporate to obtain heat-resistant epoxy resin compound; S13. A heat-resistant adhesive is prepared by mixing 15g of heat-resistant epoxy resin compound, 15g of E-51 epoxy resin and 25g of E-44 epoxy resin.
[0027] The method for preparing the low thermal resistance filler in this embodiment includes the following steps: S21. Add 1g of boron nitride to 80mL of an isopropanol aqueous solution prepared by mixing isopropanol and deionized water in a volume ratio of 1:1. Sonicate at 300W power and 20kHz frequency for 6h at room temperature. After centrifugation at 800rpm for 10min to remove the solid, centrifuge at 3000rpm for 10min and collect the supernatant. Dry the supernatant under vacuum at 60℃ for 4h to obtain hexagonal boron nitride. Add 1.2g of hexagonal boron nitride to 300mL of deionized water and stir at 1000rpm for 30min to obtain a hexagonal boron nitride dispersion with a concentration of 4mg / mL. S22. Add 0.4g of tris(hydroxymethyl)aminomethane to 300mL of hexagonal boron nitride dispersion, add 0.8g of dopamine hydrochloride, add ammonia to adjust the pH to 8.5, stir at 300rpm for 20h at room temperature, centrifuge at 3000rpm for 10min to collect the solid, wash with deionized water and ethanol in sequence, and dry under vacuum at 60℃ for 4h to prepare dopamine-modified boron nitride. S23. Add 5g of alumina particles with an average particle size of 1μm to 100mL of an ethanol-water solution prepared by mixing ethanol and deionized water in a volume ratio of 1:1. Add 0.8g of KH-550 and heat to 50℃ for 1h to modify the alumina. Filter and collect the solid, wash with deionized water, and dry at 50℃ for 4h to obtain modified alumina particles. Add 5g of modified alumina particles, 0.1g of carbon nanotubes, and 1g of modified boron nitride to 80g of N,N-dimethylacetamide and ultrasonically disperse at 30W power and 20kHz frequency for 20min. Heat to 60℃ and stir at 300rpm for 4h. Centrifuge at 3000rpm for 10min, collect the solid, wash with deionized water and ethanol sequentially, and vacuum dry at 60℃ for 4h to obtain a low thermal resistance filler.
[0028] This embodiment of a segmented lamination process for the interface of a low thermal resistance aluminum substrate includes the following steps: S1. Add the aluminum alloy plate to a 5wt% sodium hydroxide aqueous solution at 40℃ for 5 minutes to remove oil, wash with deionized water, dry at 100℃ for 10 minutes, put it into a grinding machine to remove the oxide layer, use a 400-mesh abrasive belt, a belt linear speed of 15m / s, a pressure of 0.1MPa, a feed speed of 2m / min, a grinding amount of 10μm, grind until the surface roughness is 0.4μm, wash with deionized water after grinding, vacuum dry, and set aside for later use; S2. Heat-resistant adhesive, organic solvent and dispersant are added to a mixing tank and stirred at 300 rpm for 20 min. Then, low thermal resistance filler is added and stirred at 2000 rpm for 60 min. Finally, curing agent and curing accelerator are added and stirred at 600 rpm for 30 min. The mixture is degassed under a vacuum of -0.09 MPa for 3 min to obtain a thermally conductive mixture. The thermally conductive mixture is coated into a film and baked at 80℃ for 30 min. A sample is scraped from the edge of the aluminum substrate with a sharp blade. The degree of curing is detected by infrared spectroscopy and found to be 70%, thus obtaining a semi-cured insulating layer. S3. Stack the aluminum plate, semi-cured insulating layer and copper foil in sequence, evacuate to -0.08MPa, preheat to 80℃ and hold for 5min, heat to 130℃ at a pressure of 0.1MPa and a heating rate of 2℃ / min and hold for 10min, heat to 170℃ at a heating rate of 2℃ / min, press at 13MPa for 60min, cool to 130℃ at a cooling rate of 1℃ / min and hold for 10min, depressurize to 8MPa, cool to 80℃ at a cooling rate of 1.5℃ / min and hold for 10min, depressurize to atmospheric pressure, and cool to room temperature at a cooling rate of 2℃ / min to obtain a low thermal resistance aluminum substrate.
[0029] Example 2: A low thermal resistance aluminum substrate of this example includes, from bottom to top, an aluminum base layer, a thermally conductive insulating layer, and a circuit layer. The aluminum base layer uses 5052 series aluminum alloy with a thickness of 1mm; The thermally conductive insulating layer has a thickness of 120μm and is made from the following raw materials: 55g heat-resistant adhesive, 20g organic solvent, 2g dispersant, 5g curing agent, 3g curing accelerator and 25g low thermal resistance filler; The circuit layer is a copper foil with a thickness of 140μm; The curing agent is prepared by mixing bismaleimide and 4,4'-diaminodiphenyl sulfone in a mass ratio of 1:4.
[0030] The organic solvent is N,N-dimethylacetamide; the curing accelerator is dicyandiamide.
[0031] The method for preparing the heat-resistant adhesive in this embodiment includes the following steps: S11. Add 29g vanillin and 23.5g 4-amino-o-cresol to 188mL of N,N-dimethylacetamide, heat to 78℃ and stir at 450rpm for 3.5h, filter to collect solid, wash with anhydrous ethanol, and dry at 58℃ for 5.5h to obtain modified heat-resistant monomer. S12. Add 38g of modified heat-resistant monomer, 188g of epichlorohydrin and 138mL of isopropanol to a reaction vessel, add 4.5g of tetramethylammonium bromide, heat to 90℃ in a nitrogen atmosphere and react for 5h, cool to 48℃ and stir at 450rpm, add 138g of 48wt% sodium hydroxide aqueous solution, keep at 64℃ and react for 1.5h, cool to room temperature, wash with deionized water until neutral, add anhydrous sodium sulfate to remove water, and rotary evaporate to obtain heat-resistant epoxy resin compound; S13. A heat-resistant adhesive is prepared by mixing 19g of heat-resistant epoxy resin compound, 22g of E-51 epoxy resin and 29g of E-44 epoxy resin.
[0032] The method for preparing the low thermal resistance filler in this embodiment includes the following steps: S21. Add 2g of boron nitride to 100mL of an isopropanol aqueous solution prepared by mixing isopropanol and deionized water at a volume ratio of 1:1. Sonicate the solution at 350W power and 40kHz frequency for 8h at room temperature. After centrifugation at 1200rpm for 15min, remove the solid. Centrifuge at 4000rpm for 15min and collect the supernatant. Dry the supernatant under vacuum at 80℃ for 6h to obtain hexagonal boron nitride. Add 2g of hexagonal boron nitride to 500mL of deionized water and stir at 2000rpm for 60min to obtain a hexagonal boron nitride dispersion with a concentration of 4mg / mL. S22. Add 0.5g of tris(hydroxymethyl)aminomethane to 500mL of hexagonal boron nitride dispersion, add 1g of dopamine hydrochloride, add ammonia water to adjust the pH to 8.5, stir at 500rpm for 24h at room temperature, centrifuge at 4000rpm for 15min to collect the solid, wash with deionized water and ethanol in sequence, and dry under vacuum at 80℃ for 6h to prepare dopamine-modified boron nitride. S23. Add 8g of alumina particles with an average particle size of 3μm to 200mL of an ethanol-water solution prepared by mixing ethanol and deionized water in a volume ratio of 1:1. Add 1g of KH-550 and heat to 60℃ for 2h to modify. Filter and collect the solid, wash with deionized water, and dry at 60℃ for 6h to obtain modified alumina particles. Add 6g of modified alumina particles, 0.2g of carbon nanotubes and 1.5g of modified boron nitride to 100g of N,N-dimethylacetamide and ultrasonically disperse at 50W power and 40kHz frequency for 30min. Heat to 70℃ and stir at 500rpm for 8h. Centrifuge at 4000rpm for 15min, collect the solid, wash with deionized water and ethanol sequentially, and vacuum dry at 80℃ for 6h to obtain a low thermal resistance filler.
[0033] This embodiment of a segmented lamination process for the interface of a low thermal resistance aluminum substrate includes the following steps: S1. Add the aluminum alloy plate to an 8wt% sodium hydroxide aqueous solution at 60℃ for 10 minutes to remove oil, wash with deionized water, dry at 110℃ for 15 minutes, and grind in a grinding machine to remove the oxide layer. Use a 600-mesh abrasive belt at a belt linear speed of 18m / s and a pressure of 0.3MPa, a feed speed of 4m / min, and a grinding depth of 20μm until the surface roughness is 0.8μm. After grinding, wash with deionized water, vacuum dry, and set aside for later use. S2. Heat-resistant adhesive, organic solvent and dispersant are added to a mixing tank and stirred at 500 rpm for 30 min. Then low thermal resistance filler is added and stirred at 3000 rpm for 120 min. Finally, curing agent and curing accelerator are added and stirred at 800 rpm for 60 min. Degassing is carried out at -0.1 MPa vacuum for 5 min to obtain a thermally conductive mixture. The thermally conductive mixture is coated into a film and baked at 90℃ for 60 min. A sample is scraped from the edge of the aluminum substrate with a sharp blade. The degree of curing is detected by infrared spectroscopy and it is 80%, thus obtaining a semi-cured insulating layer. S3. Stack the aluminum plate, semi-cured insulating layer and copper foil in sequence, evacuate to -0.1MPa, preheat to 100℃ and hold for 10min, heat to 150℃ at a pressure of 0.3MPa and a heating rate of 3℃ / min and hold for 20min, heat to 180℃ at a heating rate of 3℃ / min, press at 16MPa for 80min, cool to 150℃ at a cooling rate of 1.5℃ / min and hold for 20min, depressurize to 10MPa, cool to 100℃ at a cooling rate of 2℃ / min and hold for 20min, depressurize to atmospheric pressure, and cool to room temperature at a cooling rate of 3℃ / min to obtain a low thermal resistance aluminum substrate.
[0034] Example 3: A low thermal resistance aluminum substrate of this embodiment includes, from bottom to top, an aluminum base layer, a thermally conductive insulating layer, and a circuit layer. The aluminum base layer uses 5052 series aluminum alloy with a thickness of 1.5mm; The thermally conductive insulating layer has a thickness of 105 μm and is made from the following raw materials: 60 g heat-resistant adhesive, 20 g organic solvent, 3 g dispersant, 3 g curing agent, 2 g curing accelerator and 30 g low thermal resistance filler; The circuit layer is a copper foil with a thickness of 140μm; The curing agent is prepared by mixing bismaleimide and 4,4'-diaminodiphenyl sulfone in a mass ratio of 1:3.
[0035] The organic solvent is prepared by mixing butanone and N,N-dimethylacetamide in a mass ratio of 1:1; the curing accelerator is 2-methylimidazole.
[0036] The method for preparing the heat-resistant adhesive in this embodiment includes the following steps: S11. Add 30g vanillin and 24.3g 4-amino-o-cresol to 200mL of N,N-dimethylacetamide, heat to 80℃ and stir at 500rpm for 4h, filter to collect solid, wash with anhydrous ethanol, and dry at 60℃ for 6h to obtain modified heat-resistant monomer. S12. Add 40g of modified heat-resistant monomer, 200g of epichlorohydrin and 150mL of isopropanol to a reaction vessel, add 5g of tetramethylammonium bromide, heat to 90℃ in a nitrogen atmosphere and react for 6h, cool to 50℃ and stir at 500rpm, add 150g of 50wt% sodium hydroxide aqueous solution, keep at 65℃ and react for 2h, cool to room temperature, wash with deionized water until neutral, add anhydrous sodium sulfate to remove water, and rotary evaporate to obtain heat-resistant epoxy resin compound; S13. A heat-resistant adhesive is prepared by mixing 20g of heat-resistant epoxy resin compound, 25g of E-51 epoxy resin and 30g of E-44 epoxy resin.
[0037] The method for preparing the low thermal resistance filler in this embodiment includes the following steps: S21. Add 1.2g of boron nitride to 85mL of an isopropanol aqueous solution prepared by mixing isopropanol and deionized water at a volume ratio of 1:1. Sonicate the solution at 310W power and 25kHz frequency for 6h at room temperature. After centrifugation at 900rpm for 11min, remove the solid. Centrifuge at 3200rpm for 10min and collect the supernatant. Dry the supernatant under vacuum at 65℃ for 4h to obtain hexagonal boron nitride. Add 1.2g of hexagonal boron nitride to 400mL of deionized water and stir at 1200rpm for 35min to obtain a hexagonal boron nitride dispersion with a concentration of 3mg / mL. S22. Add 0.42g of tris(hydroxymethyl)aminomethane to 350mL of hexagonal boron nitride dispersion, add 0.85g of dopamine hydrochloride, add ammonia water to adjust the pH to 8.5, stir at 350rpm for 21h at room temperature, centrifuge at 3200rpm for 11min to collect the solid, wash with deionized water and ethanol in sequence, and dry under vacuum at 65℃ for 5h to prepare dopamine-modified boron nitride. S23. Add 6g of alumina particles with an average particle size of 1.5μm to 120mL of an ethanol-water solution prepared by mixing ethanol and deionized water in a volume ratio of 1:1. Add 0.85g of KH-550 and heat to 52℃ for 1.2h to modify the alumina. Filter and collect the solid, wash with deionized water, and dry at 52℃ for 4.5h to obtain modified alumina particles. Add 5.2g of modified alumina particles, 0.12g of carbon nanotubes and 1.1g of modified boron nitride to 85g of N,N-dimethylacetamide and ultrasonically disperse at 35W power and 25kHz frequency for 22min. Heat to 62℃ and stir at 350rpm for 5h. Centrifuge at 3200rpm for 11min, collect the solid, wash with deionized water and ethanol sequentially, and vacuum dry at 65℃ for 4h to obtain a low thermal resistance filler.
[0038] This embodiment of a segmented lamination process for the interface of a low thermal resistance aluminum substrate includes the following steps: S1. Add the aluminum alloy plate to a 6wt% sodium hydroxide aqueous solution at 45℃ for 10 min to remove oil, wash with deionized water, dry at 105℃ for 11 min, put it into a grinding machine to remove the oxide layer, use a 450-mesh abrasive belt, a belt linear speed of 15.5 m / s, a pressure of 0.15 MPa, a feed speed of 2.5 m / min, a grinding amount of 12 μm, grind until the surface roughness is 0.5 μm, wash with deionized water after grinding, vacuum dry, and set aside for later use; S2. Heat-resistant adhesive, organic solvent and dispersant are added to a mixing tank and stirred at 350 rpm for 20 min. Then, low thermal resistance filler is added and stirred at 2200 rpm for 70 min. Finally, curing agent and curing accelerator are added and stirred at 650 rpm for 35 min. The mixture is degassed under a vacuum of -0.092 MPa for 3.5 min to obtain a thermally conductive mixture. The thermally conductive mixture is coated into a film and baked at 82℃ for 35 min. A sample is scraped from the edge of the aluminum substrate with a sharp blade. The degree of curing is detected by infrared spectroscopy and found to be 75%, thus obtaining a semi-cured insulating layer. S3. Stack the aluminum plate, semi-cured insulating layer and copper foil in sequence, evacuate to -0.085MPa, preheat to 85℃ and hold for 6min, heat to 135℃ at a pressure of 0.15MPa and a heating rate of 2.2℃ / min and hold for 12min, heat to 172℃ at a heating rate of 2.2℃ / min, press at a pressure of 13.5MPa for 65min, cool to 135℃ at a cooling rate of 1.1℃ / min and hold for 12min, depressurize to 8.5MPa, cool to 85℃ at a cooling rate of 1.6℃ / min and hold for 12min, depressurize to atmospheric pressure, and cool to room temperature at a cooling rate of 2.2℃ / min to obtain a low thermal resistance aluminum substrate.
[0039] Comparative Example 1 differs from Example 1 in that the pressing process does not use segmented pressing. After being evacuated to -0.08 MPa, it is preheated to 80°C and held for 5 minutes. The temperature is then increased to 170°C at a rate of 2°C / min, and the pressure is maintained at 13 MPa for 60 minutes. Finally, the pressure is released directly to atmospheric pressure.
[0040] Comparative Example 2 differs from Example 1 in that the heat-resistant adhesive is replaced with E-51 epoxy resin.
[0041] Comparative Example 3 differs from Example 1 in that the low thermal resistance filler is replaced with alumina particles with an average particle size of 10 μm.
[0042] Performance testing According to GB / T 36476-2018 "General Specification for Metal-Based Copper-Clad Laminates for Printed Circuits", samples with a length of 25mm and a width of 25mm were cut from the aluminum substrates prepared in each embodiment and comparative example. The samples were sandwiched between the upper and lower thermal test blocks. The upper hot plate was set to a temperature of 80℃, and the lower hot plate was set to a temperature of 20℃. A temperature gradient was applied between the two parallel isothermal interfaces of the sample to ensure that the heat flow passed perpendicularly through the sample without lateral heat diffusion. Data was recorded after the system reached steady state, and the thermal resistance was calculated according to the following formula: R 总 Thermal resistivity of aluminum substrate, in meters (m). 2 ×K / W; T H Temperature of the high-temperature isothermal surface, in Kelvin (K). T C Temperature of the low-temperature isothermal surface, in Kelvin (K). Q represents the heat flow between two isothermal surfaces, expressed in W.
[0043] According to GB / T 1408.1-2016 "Electrical Strength Test Methods for Insulating Materials - Part 1: Tests at Power Frequency", a continuously and uniformly increasing power frequency AC voltage was applied to the aluminum substrates prepared in each example and comparative example until the sample broke down. The breakdown voltage was recorded, and the breakdown strength was calculated using the following formula: E b Breakdown strength, in kV / mm; U b This is the breakdown voltage, expressed in kV. b represents the thickness of the insulating layer on the aluminum substrate, in mm.
[0044] According to GB / T 4722-2017 "Test Method for Copper-Clad Laminates for Printed Circuits", samples of 120 mm in length and 10 mm in width were cut from the aluminum substrates prepared in each embodiment and comparative example. The copper foil layer was peeled off at 180° at a speed of 50 mm / min at 85°C, and the peel strength was recorded.
[0045] The test results are shown in Table 1 below: Table 1 Test Results According to the data in Table 1, the thermal resistance of the aluminum substrates prepared in Examples 1-3 is 0.63~0.71 μm. 2 ×K / W, the insulation layer thickness of Example 1 is 75μm, resulting in the lowest thermal resistance. While the insulation layer thickness increases the thermal resistance of the aluminum substrate, increasing the proportion of low-thermal-resistance filler slows the rate of increase in the overall thermal resistance of the aluminum substrate with increasing insulation layer thickness. Comparative Example 1 involves direct lamination with no stepless cooling, resulting in residual air bubbles between layers and insufficient resin filling, leading to increased interfacial thermal resistance of 0.92μm. 2 ×K / W; The breakdown strength of the aluminum substrates prepared in Examples 1-3 is 22.6~25.4kV / mm. In Comparative Example 1, direct lamination without stepless cooling results in residual bubbles in the interlayer becoming electric field concentration points, with the shortest breakdown path along the defect, and its breakdown strength is 16.4kV / mm. The peel strength of the aluminum substrates prepared in Examples 1-3 at 85℃ is 1.6~1.8N / mm, indicating that the aluminum substrates prepared by the present invention have excellent breakdown resistance, low thermal resistance and high temperature peel resistance, and are suitable for the heat dissipation requirements of large LEDs.
[0046] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
[0047] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A low thermal resistance aluminum substrate, characterized in that, From bottom to top, it includes an aluminum base layer, a thermally conductive insulating layer, and a circuit layer; The thermally conductive insulating layer has a thickness of 75~120μm and is made from the following raw materials in parts by weight: 50~60 parts heat-resistant adhesive, 10~20 parts organic solvent, 1~3 parts dispersant, 1~5 parts curing agent, 2~3 parts curing accelerator and 20~30 parts low thermal resistance filler. The preparation method of the heat-resistant adhesive includes the following steps: S11. Vanillin and N,N-dimethylacetamide were added to a reaction vessel, 4-amino-o-cresol was added, the mixture was heated and stirred, and after the reaction was completed, the solid was collected by filtration, washed with anhydrous ethanol, and dried to obtain the modified heat-resistant monomer. S12. Add the modified heat-resistant monomer, epichlorohydrin and isopropanol to the reactor, add tetramethylammonium bromide, heat and react in a nitrogen atmosphere, cool down, add 40~50wt% sodium hydroxide aqueous solution while stirring, keep the reaction at the temperature, cool to room temperature, wash with deionized water until neutral, add anhydrous sodium sulfate to remove water, and rotary evaporate to obtain the heat-resistant epoxy resin compound. S13. Heat-resistant adhesive is prepared by mixing heat-resistant epoxy resin compound, E-51 epoxy resin and E-44 epoxy resin.
2. The low thermal resistance aluminum substrate according to claim 1, characterized in that, The aluminum base layer uses 5052 series aluminum alloy with a thickness of 1~1.5mm, and the circuit layer is a copper foil with a thickness of 70~140μm; the organic solvent is any one or a combination of ethyl acetate, butanone, and N,N-dimethylacetamide; the curing agent is prepared by mixing bismaleimide and 4,4'-diaminodiphenyl sulfone in a mass ratio of 1:3~5; the curing accelerator is any one or a combination of 2-methylimidazole, dicyandiamide, and 2-ethyl-4-methylimidazole.
3. The low thermal resistance aluminum substrate according to claim 1, characterized in that, The ratio of vanillin, N,N-dimethylacetamide and 4-amino-o-cresol in S11 is (25~30) g: (150~200) mL: (20~25) g. The mixture is heated to 70~80℃ and reacted at 300~500 rpm for 2~4 hours, and then dried at 50~60℃ for 4~6 hours.
4. The low thermal resistance aluminum substrate according to claim 1, characterized in that, In S12, the ratio of modified heat-resistant monomer, epichlorohydrin, isopropanol, tetramethylammonium bromide, and sodium hydroxide aqueous solution is (30~40) g : (150~200) g : (100~150) mL : (3~5) g : (100~150) g. The mixture is heated to 85~90℃ in a nitrogen atmosphere and reacted for 4~6 h. The mixture is then cooled to 40~50℃ and sodium hydroxide aqueous solution is added at a speed of 300~500 rpm. The mixture is then kept at 60~65℃ and reacted for 1~2 h. In S13, the mass ratio of heat-resistant epoxy resin compound, E-51 epoxy resin, and E-44 epoxy resin is 1.5~2 : 1.5~2.5 : 2.5~3.
5. The low thermal resistance aluminum substrate according to claim 1, characterized in that, The method for preparing the low thermal resistance filler includes the following steps: S21. Add boron nitride to an isopropanol aqueous solution in which isopropanol and deionized water are mixed at a volume ratio of 1:1, sonicate at room temperature, centrifuge and filter, collect the supernatant, and vacuum dry to obtain hexagonal boron nitride. Add hexagonal boron nitride to deionized water and shear and stir to obtain a hexagonal boron nitride dispersion. S22. Tris(hydroxymethyl)aminomethane was added to a hexagonal boron nitride dispersion, dopamine hydrochloride was added, and ammonia was added to adjust the pH to 8.
5. The mixture was stirred at room temperature, centrifuged and filtered to collect the solid, washed with deionized water and ethanol in sequence, and dried under vacuum to obtain dopamine-modified boron nitride. S23. Alumina particles are added to an ethanol-water solution prepared by mixing ethanol and deionized water at a volume ratio of 1:
1. KH-550 is added for surface modification. The solid is collected by filtration, washed with deionized water, and dried to obtain modified alumina particles. Modified alumina particles, carbon nanotubes, and modified boron nitride are added to N,N-dimethylacetamide for ultrasonic dispersion, heated and stirred, centrifuged and filtered to collect the solid. The solid is washed with deionized water and ethanol in sequence and dried under vacuum to obtain a low thermal resistance filler.
6. The low thermal resistance aluminum substrate according to claim 5, characterized in that, The ratio of boron nitride to isopropanol aqueous solution in S21 is (1~2) g: (80~100) mL. The solution is ultrasonicated at 300~350 W power and 20~40 kHz frequency for 6~8 h, centrifuged at 800~1200 rpm for 10~15 min to remove the solid, then centrifuged at 3000~4000 rpm for 10~15 min. The supernatant is collected and vacuum dried at 60~80℃ for 4~6 h, then centrifuged at 1000~2000 rpm. Stir at a speed of 30-60 min to obtain a concentration of 3-5 mg / mL of hexagonal boron nitride dispersion; the ratio of tris(hydroxymethyl)aminomethane, hexagonal boron nitride dispersion and dopamine hydrochloride in S22 is (0.4-0.5) g: (300-500) mL: (0.8-1) g, stir at 300-500 rpm for 20-24 h, centrifuge at 3000-4000 rpm for 10-15 min, and vacuum dry at 60-80℃ for 4-6 h.
7. A low thermal resistance aluminum substrate according to claim 5, characterized in that, The average particle size of the alumina particles in S23 is 1~3μm. The ratio of alumina particles, ethanol aqueous solution and KH-550 is (5~8)g:(100~200)mL:(0.8~1)g. The alumina particles are heated to 50~60℃ for 1~2h and dried at 50~60℃ for 4~6h. The mass ratio of modified alumina particles, carbon nanotubes, modified boron nitride and N,N-dimethylacetamide is 5~6:0.1~0.2:1~1.5:80~100. The alumina particles are ultrasonically dispersed at 30~50W power and 20~40kHz frequency for 20~30min. The alumina particles are heated to 60~70℃ and stirred at 300~500rpm for 4~8h. The alumina particles are centrifuged at 3000~4000rpm for 10~15min and dried under vacuum at 60~80℃ for 4~6h.
8. A segmented lamination process for the interface of a low thermal resistance aluminum substrate according to any one of claims 1-7, characterized in that, Includes the following steps: S1. Add the aluminum alloy plate to a 5-8 wt% sodium hydroxide aqueous solution to remove oil, wash with deionized water, dry, and then grind in a grinding machine to remove the oxide layer. After grinding, wash with deionized water, vacuum dry, and set aside. S2. Add the heat-resistant adhesive, organic solvent and dispersant to the mixing tank and stir at 300~500 rpm for 20~30 min. Then add the low thermal resistance filler and stir at 2000~3000 rpm for 60~120 min. Finally add the curing agent and curing accelerator and stir at 600~800 rpm for 30~60 min. Degas at a vacuum degree of -0.09~-0.1 MPa for 3~5 min to obtain a thermally conductive mixture. Coat the thermally conductive mixture into a film and bake to obtain a semi-cured insulation layer. S3. The aluminum plate, semi-cured insulating layer and copper foil are stacked in sequence, pressed and cured in sections, and cooled to room temperature to obtain a low thermal resistance aluminum substrate.
9. The segmented lamination process for the interface of a low thermal resistance aluminum substrate according to claim 8, characterized in that, In step S1, the sample is degreased in a sodium hydroxide aqueous solution at 40-60°C for 5-10 minutes, dried at 100-110°C for 10-15 minutes, and then polished with a 400-600 mesh abrasive belt at a linear speed of 15-18 m / s and a pressure of 0.1-0.3 MPa, with a feed rate of 2-4 m / min and a polishing depth of 10-20 μm, until the surface roughness is 0.4-0.8 μm. In step S2, the sample is baked at 80-90°C for 30-60 minutes, and a sample is scraped from the edge of the aluminum substrate with a sharp blade. The degree of curing is determined to be 70-80% using an infrared spectrometer. In step S3, the sample is evacuated to -0.08 to -0.1 MPa, preheated to 80-100°C and held for 5-10 minutes, and then heated to 130-150°C at a pressure of 0.1-0.3 MPa and a heating rate of 2-3°C / min. Hold at 50℃ for 10-20 min, heat to 170-180℃ at a rate of 2-3℃ / min, press at 13-16MPa for 60-80 min, cool to 130-150℃ at a rate of 1-1.5℃ / min and hold for 10-20 min, depressurize to 8-10MPa, cool to 80-100℃ at a rate of 1.5-2℃ / min and hold for 10-20 min, depressurize to atmospheric pressure, and cool to room temperature at a rate of 2-3℃ / min.
Citation Information
Patent Citations
A single-sided aluminum substrate lamination device and process
CN116321732B