Degradable copper-clad plate and preparation method thereof

By utilizing the labyrinthine structure formed by organically modified montmorillonite and microwave hydrothermal reaction, along with the catalyst slow-release mechanism, the problem of rapid degradation and green recycling of copper clad laminates in low-concentration acidic environments has been solved, achieving efficient and stable degradation results.

CN123129555APending Publication Date: 2026-11-20MEIZHOU WEILIBANG ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611456290.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing biodegradable copper-clad laminates present a contradiction in balancing long-term service stability and degradation performance. They are difficult to degrade rapidly in low-concentration acidic environments with low degradation pollution, and their mechanical properties are insufficient, making them unsuitable for the efficient and green recycling needs of circuit boards.

Method used

Organically modified montmorillonite is used as a degradation-promoting inorganic filler. Hollow mesoporous silica particles and a network silica coating layer are formed through microwave hydrothermal reaction. Combined with the slow-release mechanism of zinc acetate catalyst, a labyrinth barrier structure is formed to ensure that the copper-clad laminate can be used stably in a humid and hot environment and degrade rapidly at high temperatures.

Benefits of technology

It enables rapid degradation of copper-clad laminates in low-concentration acidic environments with low degradation pollution, while also possessing high mechanical toughness and long-term stability under humid heat, thus improving degradation efficiency and uniformity and meeting green recycling requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the technical field of copper-clad plate, and particularly relates to a degradable copper-clad plate and a preparation method thereof, which comprises the following components by weight: 80-100 parts of epoxy resin, 6-10 parts of curing agent, 0.3-0.5 parts of curing accelerator, 4-7 parts of degradation-promoting inorganic filler, 20-25 parts of flame retardant, 1-1.5 parts of silane coupling agent KH-550, and 75-85 parts of acetone-butanone mixed solvent. In the present application, an ester bond-containing degradable epoxy resin is used as a matrix, and is matched with degradation-promoting inorganic filler. The outer layer of the filler is a stable basic zinc carbonate layer, which can lock the catalyst and avoid premature degradation of the plate. When the plate is subjected to high-temperature and high-humidity degradation for scrapping, the internal stress is generated due to the deformation difference of the filler-resin, which induces the generation of connected micro-cracks, forms a mass transfer channel for degradation medium, and improves the degradation uniformity of the plate. Meanwhile, the external acid medium destroys the sealing layer and releases zinc acetate under acidic conditions, and the zinc ion catalyzes the continuous hydrolysis of the resin, so that the rapid degradation is realized. The long-term service stability and efficient green degradation and recycling performance of the copper-clad plate are taken into account.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper clad laminate technology, specifically to a biodegradable copper clad laminate and its preparation method. Background Technology

[0002] Copper clad laminates (CCLs) are the core substrate material for printed circuit boards (PCBs), widely used in consumer electronics, communication equipment, industrial control, and new energy fields. With the rapid pace of electronic product iteration and increasing pressure on the recycling of waste electronic products, traditional thermosetting epoxy resin CCLs, despite their dense and stable cross-linked networks after curing and excellent resistance to chemical corrosion and hydrolysis, are difficult to degrade naturally after disposal. This results in challenges such as high recycling difficulty, high dismantling costs, and severe environmental pollution, making them unsuitable for the current industry demands for green manufacturing and the harmless recycling of waste boards.

[0003] Currently, the industry has gradually begun research on biodegradable copper clad laminates. The mainstream biodegradable solutions are mainly divided into two categories: one is a water-soluble polymer resin system, which relies on the water solubility of the resin itself to achieve hot water degradation. However, this type of board has poor heat resistance, moisture resistance and mechanical properties, and cannot be adapted to circuit board reflow soldering and long-term humid and hot service conditions, so its practical value is limited; the other is a modified epoxy resin system containing hydrolyzable ester bonds, which can take into account both conventional performance and biodegradability, and is the current mainstream research direction for biodegradable copper clad laminates.

[0004] Currently, achieving efficient degradation of copper clad laminates (CCLs) heavily relies on external immersion in high-concentration acid and alkali solutions. This approach limits the applicable scenarios for recycling and is insufficiently environmentally friendly. It requires specialized etching equipment, involves cumbersome recycling processes, and incurs high processing costs. Furthermore, the high-concentration acid and alkali systems can easily cause serious secondary pollution, resulting in poor green recyclability. At the same time, existing biodegradable CCLs generally face a dilemma between service stability and degradation performance: to ensure the long-term reliability of the board, it is usually necessary to increase the resin crosslinking density or use inert fillers, which significantly increases the difficulty of hydrolysis and reduces degradation efficiency after the board is discarded. On the other hand, weakening the resin structure to improve degradation capacity will increase the water absorption rate and reduce the mechanical toughness of the board, making it prone to performance degradation and premature failure in humid service environments. It is difficult to balance practical performance and green recycling characteristics.

[0005] Therefore, developing a biodegradable copper-clad laminate that can adapt to low-concentration acidic environments, degrades rapidly with less pollution, and also has low water absorption, high mechanical toughness, and long-term stability under humid heat has become a technical challenge that urgently needs to be solved in this field. Summary of the Invention

[0006] To address the problems existing in the prior art, the present invention aims to provide a biodegradable copper clad laminate and its preparation method, which can achieve rapid degradation in low-concentration acidic environments with lower degradation pollution, while taking into account the long-term service stability of the copper clad laminate and its efficient green degradation and recycling performance.

[0007] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a biodegradable copper-clad laminate specifically includes the following steps: 1) Weigh the raw materials according to the following parts by weight: 80-100 parts epoxy resin, 6-10 parts curing agent, 0.3-0.5 parts curing accelerator, 4-7 parts degradable inorganic filler, 20-25 parts flame retardant, 1-1.5 parts silane coupling agent KH-550, and 75-85 parts acetone-butanone mixed solvent; 2) Add epoxy resin, curing agent, curing accelerator, degradation-promoting inorganic filler, flame retardant, and silane coupling agent KH-550 to an organic solvent to obtain a resin solution; 3) Impregnate the fiberglass cloth with the adhesive, bake it in sections to obtain a prepreg, and stack at least one prepreg. After stacking, attach electrolytic copper foil to one or both sides to assemble it into a slab. 4) Place the slab in a vacuum hot press, heat and press in stages to solidify, and after cooling and trimming, obtain a biodegradable copper-clad laminate.

[0008] As a further preferred embodiment of the present invention, in step 3), the segmented baking involves baking at 120-130°C for 2-3 minutes, and then raising the temperature to 140-150°C for 3-5 minutes. In step 4), the segmented heating and pressurizing hot pressing curing involves evacuating to a vacuum level of -0.05 to -0.08 MPa, pre-pressing at an initial temperature of 80-90℃ for 10-15 minutes at a pressure of 0.8-1.2 MPa, then heating at a rate of 1-2℃ / min to 120-130℃, holding at that temperature for 15-20 minutes, continuing to heat to 170-175℃, increasing the pressure to 2.5-3.0 MPa, and maintaining constant temperature and pressure for 70-90 minutes.

[0009] As a further preferred embodiment of the present invention, the epoxy resin is selected from at least one of diglycidyl adipate, diglycidyl isophthalate, diglycidyl hexahydrophthalate, and diglycidyl 4,5-epoxytetrahydrophthalate. The curing agent is dicyandiamide; The curing accelerator is selected from 2-methylimidazole; The flame retardant is selected as a halogen-free phosphate flame retardant. The acetone-butanone mixed solvent is prepared by mixing equal volumes of acetone and butanone.

[0010] As a further preferred embodiment of the present invention, the degradation-promoting inorganic filler is prepared by the following method: S1 uses hexadecyltrimethylammonium bromide to modify montmorillonite, resulting in organically modified montmorillonite; S2-1: Hexadecyltrimethylammonium bromide is dissolved in deionized water to obtain a template agent solution. Then, organically modified montmorillonite is dispersed in the template agent solution to obtain an aqueous phase. Tween-80 is added to dodecane and stirred until completely dissolved to obtain an oil phase. Then, the oil phase is added to the aqueous phase at a volume ratio of (4.0-4.5):1, and an emulsion is obtained by shear emulsification. S2-2 After pre-cooling the prepared silicon source solution to 10-15℃, the silicon source solution is added dropwise to the emulsion, the pH value is adjusted to 9-10, and then transferred to a reaction vessel. The reaction is carried out at 120-130℃ for 40-60 min under microwave action. After the reaction is completed, the mixture is cooled to room temperature. The product is washed and dispersed in an acidic ethanol solution. After reflux extraction for 12-16 h, the product is dried to obtain the montmorillonite support. S2-3 Under continuous stirring, ethyl orthosilicate ethanol solution was added dropwise to montmorillonite carrier suspension. After the addition was complete, the temperature was raised to 65-68℃, and the mixture was stirred and aged at normal pressure for 3-4 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed and dried to obtain composite carrier. S3-1 The composite carrier is activated under vacuum for 1-2 hours, then the vacuum-activated composite carrier is dispersed in an ethanol solution of zinc acetate dihydrate, vacuumed and impregnated for 30-40 minutes, then allowed to stand for 4-6 hours and centrifuged, washed and dried to obtain the powder product for later use. S3-2 The above powder product is dispersed in an ethanol-water mixed solution to obtain a suspension. Then, it is stirred at 100-150 r / min for 10-15 min at 40-45℃. Then, an ammonium bicarbonate aqueous solution is added dropwise to adjust the pH value to 6.5-6.8. The reaction is continued to be stirred for 1.5-2.0 h. After the reaction is completed, the product is centrifuged, washed, dried, ground, and passed through a 200-mesh sieve to obtain the desired degradation-promoting inorganic filler.

[0011] As a further preferred embodiment of the present invention, in S2-1, the concentration of the template agent solution is 0.020-0.025 mol / L; The aqueous phase contains 0.5-1.0 wt% organically modified montmorillonite. In the oil phase, Tween-80 accounts for 4-5% of the mass of dodecane; The shear emulsification is performed by emulsifying at 6000-8000 r / min for 10-15 min in a water bath at 25-30℃.

[0012] As a further preferred embodiment of the present invention, in S2-2, the silicon source solution is obtained by taking a silica sol with a SiO2 concentration of 10-13wt%, adjusting the pH value of the system to 8.0-8.5 with a 3wt% dilute ammonia solution, and stirring. The silicon source solution and emulsion have a mass ratio of 1:(1.5-2.5). The dropping process is carried out at a rate of 0.06-0.09% of the total volume of the emulsion per minute, representing the volume of the silicon source solution added. The microwave action has a power of 200-300W; The acidic ethanol solution has a pH value of 5.0-5.5; The reflux extraction is performed at a temperature of 80-85℃.

[0013] As a further preferred embodiment of the present invention, in S2-3, the continuous stirring speed is 150-180 r / min; The montmorillonite carrier suspension is prepared by dispersing the montmorillonite carrier in anhydrous ethanol, adding deionized water, and adjusting the pH value to 9.0 according to the ratio of montmorillonite carrier, anhydrous ethanol, and deionized water as (10-15) g: (800-1000) mL: (15-25) mL. The tetraethyl orthosilicate ethanol solution is prepared by weighing tetraethyl orthosilicate and adding it to anhydrous ethanol at a mass ratio of tetraethyl orthosilicate to montmorillonite carrier of (0.28-0.42):1, and controlling the volume ratio of tetraethyl orthosilicate to anhydrous ethanol to be 1:(4-10). The dropping rate is 0.04-0.06% of the total volume of the montmorillonite carrier suspension, representing the volume of tetraethyl orthosilicate ethanol solution added per minute.

[0014] As a further preferred embodiment of the present invention, in S3-1, the vacuum activation is carried out at 110-130°C and -0.05 to -0.1 MPa. The mass-to-volume ratio of the vacuum-activated composite carrier and the zinc acetate dihydrate ethanol solution is 1g:(10-20)mL. The zinc acetate dihydrate ethanol solution has a concentration of 0.5-1.0 mol / L; The process involves impregnation after vacuuming, with a vacuum level of -0.05 to -0.1 MPa, and the application of 120-150 W of ultrasound.

[0015] As a further preferred embodiment of the present invention, in S3-2, the ethanol-water mixed solution is composed of anhydrous ethanol and deionized water in a volume ratio of (1.2-1.5):1; The powder product and the ethanol-water mixed solution have a mass-to-volume ratio of 1g:(15-20)mL; The ammonium bicarbonate aqueous solution has a concentration of 0.8-1.2 mol / L, and the dropping rate is such that the volume of the ammonium bicarbonate aqueous solution dropped per minute is 0.08-0.16% of the total volume of the suspension.

[0016] A biodegradable copper-clad laminate is prepared using the method described above.

[0017] Compared with the prior art, the beneficial effects of the present invention are: In this invention, firstly, organic modification of sodium-based montmorillonite provides sufficient nucleation sites for subsequent in-situ growth of nanoparticles, allowing nanoparticles to be uniformly immobilized on the surface of the lamellae. Furthermore, the organic modification weakens the interlayer forces of the montmorillonite. Under the synergistic effect of thermo- and mechanical shear during subsequent resin composite and hot-press curing, the stacked lamellae structure is easily peeled and dispersed. The peeled montmorillonite lamellae are evenly distributed in the resin matrix, forming a dense labyrinthine barrier structure that effectively extends the water vapor permeation path, significantly reducing the overall water absorption rate of the copper-clad laminate and preventing premature failure caused by excessive water vapor intrusion into the filler interface under service conditions. On the other hand, it can deflect cracks... First, the energy absorption mechanism improves the brittleness of epoxy resin and effectively enhances the mechanical toughness of copper-clad laminates. Simultaneously, this labyrinthine structure provides a stable path for the diffusion of degradation media into the deeper layers of the board under high-temperature degradation conditions, ensuring uniform degradation. Second, hollow mesoporous silica particles are formed on organically modified montmorillonite sheets through microwave hydrothermal reaction, resulting in a montmorillonite carrier. This hollow mesoporous structure provides high-specific-surface-area mesoporous channels and internal cavities as a catalyst reservoir, capable of accommodating a large amount of zinc acetate catalyst and ensuring its stable crystalline existence within the cavities. Furthermore, the mesoporous channels serve as rapid channels for the dissolution of degradation media and catalysts, ensuring the uniform degradation of Zn after degradation is triggered. 2+It can rapidly diffuse outward, thus significantly improving the degradation reaction rate. Then, a network of silica coating is formed on the surface of the montmorillonite carrier. This network coating has an open-pore structure, ensuring that the mesoporous channels are not blocked, allowing the catalyst to be released smoothly later. Furthermore, the network coating strengthens the mechanical strength of the hollow mesoporous silica particles, preventing the hollow cavities within the silica particles from collapsing or deforming under pressure and high temperature during the subsequent high-temperature hot-pressing curing of the copper-clad laminate, thus ensuring the cavities can store the catalyst effectively. On the other hand, the rough network coating increases the effective contact area between the degradation-promoting inorganic filler and the epoxy resin matrix, improving the interfacial bonding strength. This allows the filler to effectively bear and disperse bending loads, significantly improving the bending strength of the board. Simultaneously, the denser interfacial bonding reduces the original seams at the filler-resin interface. The gaps cut off the channels for water to seep in along the interface, thereby further reducing the water absorption rate of the board. Under humid and hot degradation conditions, the resin absorbs water and swells. Due to the difference in thermal expansion and water absorption deformation at the resin-inorganic filler interface, internal stress is generated, which in turn induces a large number of interconnected microcracks around the filler. This provides a rapid transport channel for water molecules and other degradation media to penetrate into the interior of the board. The degradation media can act on both the surface layer and the core resin of the board, effectively avoiding the phenomenon that the residue generated after the preferential degradation of the surface resin blocks the penetration channels and makes it difficult to degrade inside the board, thus improving the overall degradation rate and degradation uniformity of the copper-clad laminate. Moreover, the mesh structure can effectively prevent the zinc acetate loaded inside the cavity from dissolving outward under mild conditions. Finally, the zinc acetate is pressed into the hollow cavity and mesoporous channels through vacuum impregnation to achieve the effect of catalyst internal slow release. 2+ Firmly anchored to the carrier surface and mesoporous inner wall through ion exchange and electrostatic adsorption, zinc acetate inside the pores slowly dissolves outward. Zinc ions diffuse to the solid-liquid interface and undergo heterogeneous nucleation reaction with the dripped ammonium bicarbonate, forming a dense basic zinc carbonate nano-coating layer that grows in situ on the outer surface of the filler particles and the mesoporous pore openings. This coating layer effectively blocks water vapor from entering the cavity, preventing premature dissolution and seepage of the built-in zinc acetate catalyst, ensuring the long-term stable performance of the board. When the copper-clad laminate is disposed of and placed in an acidic high-temperature aqueous solution for recycling and degradation, the external acidic medium can directly dissolve the outer basic zinc carbonate sealing layer, opening the mesoporous channels, allowing water molecules to enter the cavity, dissolving zinc acetate and releasing zinc ions. The zinc ions efficiently catalyze the hydrolysis of epoxy resin ester bonds, achieving efficient degradation of the copper-clad laminate.

[0018] In this invention, a biodegradable epoxy resin containing ester bonds is used as the matrix, combined with a biodegradable inorganic filler. The outer basic zinc carbonate layer of the biodegradable inorganic filler has a stable structure, which can effectively lock in the catalyst, prevent premature degradation of the board, and ensure reliability. When the board is scrapped and degraded, the high temperature and humidity cause the resin to absorb water and swell. The difference between the thermal expansion and water absorption deformation of the filler and resin phases generates internal stress, which induces the formation of interconnected microcracks around the filler, forming a mass transfer channel for the degradation medium and improving the uniformity of board degradation. At the same time, under acidic conditions, the external acid medium destroys the sealing layer and releases zinc acetate. Zinc ions catalyze the continuous hydrolysis of the resin, achieving rapid degradation, thus taking into account both the long-term service stability of the copper-clad laminate and the efficient green degradation and recycling performance. Detailed Implementation

[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0020] In this embodiment of the invention, the epoxy resin is composed of diglycidyl hexahydrophthalic acid and diglycidyl 4,5-epoxytetrahydrophthalic acid in a mass ratio of 17:3. Diglycidyl hexahydrophthalate, grade CY184 (S-184), epoxy equivalent 155-175 g / eq, provided by Hubei Xinjing New Materials Co., Ltd. 4,5-Epoxytetrahydrophthalic acid diglycidyl ester, grade TDE-85 (S-186), epoxy equivalent 110-130 g / eq, provided by Wuhan Haishan Technology Co., Ltd. The curing agent used is dicyandiamide, specifically electronic-grade dicyandiamide, provided by Ningxia Dadi Circular Development Co., Ltd. The curing accelerator is 2-methylimidazole, industrial electronic grade, provided by Ningxia Changhe Chemical Co., Ltd. The flame retardant is a halogen-free phosphate flame retardant, specifically resorcinol bis(2,6-dimethylphenyl) diphosphate, brand name PX-200, with a phosphorus content of approximately 9% and a thermal decomposition temperature >450℃, provided by Shaorui Chemical (Shanghai) Co., Ltd. Sodium-based montmorillonite, grade DK-NF, cation exchange capacity 90-100 mmol / 100g, provided by Zhejiang Fenghong New Material Co., Ltd. The fiberglass cloth is made of 2116 type electronic grade alkali-free fiberglass cloth, with a thickness of 0.10mm and a unit area weight of 100g / m². 2 The fabric has a plain weave and is supplied by Langfang Anlang Sealing Materials Co., Ltd.

[0021] Example 1 A method for preparing a biodegradable copper-clad laminate includes the following steps: 1) Weigh the raw materials according to the following parts by weight: 80 parts epoxy resin, 6 parts curing agent, 0.3 parts curing accelerator, 4 parts degradable inorganic filler, 20 parts flame retardant, 1 part silane coupling agent KH-550, and 75 parts acetone-butanone mixed solvent. 2) Add the curing agent and curing accelerator to the acetone-butanone mixed solvent, then add the epoxy resin, followed by the silane coupling agent KH-550, flame retardant, and degradable inorganic filler. Stir at 500 r / min for 40 min at 45℃, and then ultrasonically disperse at 300 W for 20 min to obtain a degradable epoxy resin solution. 3) Continuously immerse the fiberglass cloth in the biodegradable epoxy resin solution to fully impregnate it, control the glue application speed to 2m / min, and after impregnation, send it into a hot air oven for segmented baking. Bake at 120℃ for 2min, and then increase to 140℃ for 3min to obtain a semi-cured sheet. 4) Cut the prepreg and stack the corresponding number of prepregs according to the target board thickness. Cover the upper and lower surfaces of the stacked prepregs with electrolytic copper foil (18μm roughened side facing the prepreg), align and stack them, and lay release films on the top and bottom to obtain the hot-pressed board blank. 5) The slab is fed into a vacuum hot press and evacuated to a vacuum degree of -0.08MPa. At an initial temperature of 80℃, it is pre-pressed for 10 minutes at a pressure of 0.8MPa. Then, the temperature is increased to 120℃ at a rate of 2℃ / min and held for 15 minutes. The temperature is then increased to 170℃ and the pressure is increased to 2.5MPa. The temperature and pressure are maintained for 70 minutes. After the process is completed, the furnace is slowly cooled down at a rate of 3℃ / min. The pressure is released when the temperature drops to 50℃. The board is then removed, the release film on the surface is removed, and the edges are trimmed, the board surface is polished and dust is removed, and it is cut to the specified size to obtain the biodegradable copper-clad laminate.

[0022] The basic zinc carbonate sealing layer on the outer surface of the degradable inorganic filler undergoes only a very small amount of decomposition during the hot pressing process of the copper clad laminate. The trace amount of CO2 generated escapes from the edge of the board or dissolves in the resin matrix under high pressure, and does not form a continuous and interconnected porous channel inside the copper clad laminate. Therefore, it does not affect the low water absorption rate of the copper clad laminate. Moreover, the nano zinc oxide generated by the decomposition fills the sealing layer surface in situ, which can further enhance the interfacial compactness.

[0023] The preparation method of the degradation-promoting inorganic filler is as follows: S1. Sodium-based montmorillonite was dispersed in deionized water and stirred in a water bath at 400 r / min for 2 h at 80 °C to prepare a 5% (w / w) suspension. Then, hexadecyltrimethylammonium bromide was added to the suspension at an amount of 18% of the total weight of sodium-based montmorillonite. The reaction was continued for 6 h. After the reaction was completed, the mixture was centrifuged and washed alternately with deionized water and anhydrous ethanol until no bromide ion precipitate was detected by silver nitrate. The mixture was then dried at 60 °C for 3 h and ground through a 300-mesh sieve to obtain organically modified montmorillonite. S2-1: Hexadecyltrimethylammonium bromide was dissolved in deionized water and stirred until completely dissolved to obtain a template agent solution with a concentration of 0.02 mol / L. Then, organically modified montmorillonite was dispersed in the template agent solution to obtain an aqueous phase with an organically modified montmorillonite content of 0.5 wt%. Tween-80 at a mass of 4% was added to dodecane and stirred until completely dissolved to obtain an oil phase. Then, the oil phase was added to the aqueous phase at a volume ratio of 4:1 and emulsified in a 25°C water bath at 6000 r / min for 10 min to obtain an emulsion. S2-2: A silica sol with a SiO2 concentration of 10 wt% was prepared. The pH of the system was adjusted to 8.0 using 3 wt% dilute ammonia. After stirring continuously at 150 r / min for 1 h, a silicon source solution was obtained. After pre-cooling to 10℃, the silicon source solution was added dropwise to the emulsion at a mass ratio of 1:1.5, with the volume of silicon source solution added per minute being 0.06% of the total emulsion volume. The pH was adjusted to 9 using 3 wt% dilute ammonia, and the solution was transferred to a reaction vessel and heated at 200 W. Under microwave irradiation, the reaction was carried out at 120℃ for 40 min. After the reaction was completed, the mixture was naturally cooled to room temperature. After centrifugation, the supernatant was discarded. The lower layer product was washed three times alternately with deionized water and anhydrous ethanol, and then dispersed in an acidic ethanol solution with a pH of 5. The mass-to-volume ratio of the lower layer product to the acidic ethanol solution was 1 g: 100 mL. The mixture was refluxed at 80℃ for 12 h. After repeated washing with ethanol and deionized water until the pH of the filtrate was close to neutral, the mixture was dried at 60℃ for 10 h to obtain the montmorillonite carrier. S2-3 was prepared by dispersing the montmorillonite carrier in anhydrous ethanol at a ratio of 10g:800mL:15mL, followed by the addition of deionized water. Then, 3wt% dilute ammonia solution was added dropwise while monitoring the pH value until the pH stabilized at 9.0. This resulted in a montmorillonite carrier suspension with a mass ratio of tetraethyl orthosilicate to montmorillonite carrier of 0.28:1. Ethyl tetrasilicate was weighed and added to anhydrous ethanol, with the volume ratio of ethyl tetrasilicate to anhydrous ethanol controlled at 1:4 to prepare an ethyl tetrasilicate-ethanol solution. Under continuous stirring at 150 r / min, the ethyl tetrasilicate-ethanol solution was added dropwise to the montmorillonite carrier suspension at a uniform rate. The volume of the ethyl tetrasilicate-ethanol solution added per minute was 0.04% of the total volume of the montmorillonite carrier suspension. After the addition was completed, the temperature was raised to 65℃, and the mixture was stirred and aged at normal pressure for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed three times with anhydrous ethanol, and dried under vacuum at 60℃ for 8 hours to obtain the composite carrier. S3-1 The composite carrier was vacuum activated for 1 h at 110 °C and -0.05 MPa. Then, the vacuum-activated composite carrier was dispersed in a 0.7 mol / L zinc acetate dihydrate ethanol solution at a mass-to-volume ratio of 1 g: 10 mL. The solution was then vacuum-impregnated to -0.05 MPa and ultrasonically at 120 W for 30 min. After returning to normal pressure, the vacuum-impregnation cycle was repeated 3 times. After standing for 4 h, the mixture was centrifuged and washed twice with anhydrous ethanol. Each time, anhydrous ethanol was added at a mass-to-volume ratio of 1 g: 20 mL. After stirring for 2 min, the mixture was immediately centrifuged and the supernatant was discarded. The mixture was then dried at 50 °C for 4 h to obtain a powder product for later use. S3-2 The powdered product was dispersed in an ethanol-water mixture of anhydrous ethanol and deionized water at a mass-to-volume ratio of 1 g:15 mL to obtain a suspension. The suspension was stirred at 100 r / min for 10 min in a water bath at a temperature of 40 °C. Then, 0.7 mol / L ammonium bicarbonate aqueous solution was slowly added dropwise at a rate of 0.16% of the total volume of the suspension per minute. Simultaneously, 0.3 mol / L dilute acetic acid solution was added dropwise. The pH of the system was monitored online, and the dropping rate of dilute acetic acid was adjusted to maintain a stable pH of 6.8 throughout the reaction. After the ammonium bicarbonate was added, the reaction was stirred for another 1.5 h. The pH was continuously monitored and maintained at 6.8 throughout the reaction. After the reaction was completed, the product was centrifuged, washed twice with anhydrous ethanol, dried under vacuum at 45 °C for 5 h, and then ground through a 200-mesh sieve to obtain the final product.

[0024] Example 2 A biodegradable copper-clad laminate includes the following steps: 1) Weigh the raw materials according to the following parts by weight: 90 parts epoxy resin, 8 parts curing agent, 0.4 parts curing accelerator, 5 parts degradable inorganic filler, 23 parts flame retardant, 1.2 parts silane coupling agent KH-550, and 80 parts acetone-butanone mixed solvent. 2) According to the weight parts, add the curing agent and curing accelerator to the acetone-butanone mixed solvent, then add the epoxy resin, followed by the silane coupling agent KH-550, flame retardant, and degradable inorganic filler. Stir at 500 r / min for 40 min at 45℃, and then ultrasonically disperse at 300 W for 20 min to obtain the degradable epoxy resin solution. 3) Continuously immerse the fiberglass cloth in the biodegradable epoxy resin solution to fully impregnate it, control the glue application speed to 2m / min, and after impregnation, send it into a hot air oven for segmented baking. Bake at 120℃ for 2min, and then increase to 140℃ for 3min to obtain a semi-cured sheet. 4) Cut the prepreg and stack the corresponding number of prepregs according to the target board thickness. Cover the upper and lower surfaces of the stacked prepregs with electrolytic copper foil (18μm roughened side facing the prepreg), align and stack them, and lay release films on the top and bottom to obtain the hot-pressed board blank. 5) The slab is fed into a vacuum hot press and evacuated to a vacuum degree of -0.08MPa. At an initial temperature of 80℃, it is pre-pressed for 10 minutes at a pressure of 0.8MPa. Then, the temperature is increased to 120℃ at a rate of 2℃ / min and held for 15 minutes. The temperature is then increased to 170℃ and the pressure is increased to 2.5MPa. The temperature and pressure are maintained for 70 minutes. After the process is completed, the furnace is slowly cooled down at a rate of 3℃ / min. The pressure is released when the temperature drops to 50℃. The board is then removed, the release film on the surface is removed, and the edges are trimmed, the board surface is polished and dust is removed, and it is cut to the specified size to obtain the biodegradable copper-clad laminate.

[0025] The preparation method of the degradation-promoting inorganic filler is as follows: S1. Sodium-based montmorillonite was dispersed in deionized water and stirred in a water bath at 450 r / min for 2.5 h at 82 °C to prepare a suspension with a mass fraction of 7%. Then, hexadecyltrimethylammonium bromide was added to the suspension, with the amount added being 21% of the total weight of sodium-based montmorillonite. The reaction was continued to be stirred for 7 h. After the reaction was completed, the mixture was separated by centrifugation and washed alternately with deionized water and anhydrous ethanol until no bromide ion precipitate was detected by silver nitrate. The mixture was dried at 65 °C for 4 h and ground through a 300-mesh sieve to obtain organically modified montmorillonite. S2-1: Hexadecyltrimethylammonium bromide was dissolved in deionized water and stirred until completely dissolved to obtain a template agent solution with a concentration of 0.023 mol / L. Then, organically modified montmorillonite was dispersed in the template agent solution to obtain an aqueous phase with an organically modified montmorillonite content of 0.7 wt%. Tween-80 at a mass of 4.5% was added to dodecane and stirred until completely dissolved to obtain an oil phase. Then, the oil phase was added to the aqueous phase at a volume ratio of 4.2:1 and emulsified in a 28°C water bath at 7000 r / min for 12 min to obtain an emulsion. S2-2: A silica sol with a SiO2 concentration of 12 wt% was prepared. The pH of the system was adjusted to 8.5 using 3 wt% dilute ammonia. After continuous stirring at 150 r / min for 1.5 h, a silicon source solution was obtained. After pre-cooling to 12℃, the silicon source solution was added dropwise to the emulsion at a mass ratio of 1:2, with the volume of silicon source solution added per minute being 0.08% of the total emulsion volume. The pH was adjusted to 9.5 using 3 wt% dilute ammonia. The solution was then transferred to a reaction vessel and heated at 300 W. Under microwave irradiation, the reaction was carried out at 125℃ for 50 min. After the reaction was completed, the mixture was naturally cooled to room temperature. After centrifugation, the supernatant was discarded. The lower layer product was washed three times alternately with deionized water and anhydrous ethanol, and then dispersed in an acidic ethanol solution with a pH of 5.5. The mass-to-volume ratio of the lower layer product to the acidic ethanol solution was 1 g: 100 mL. The mixture was refluxed at 82℃ for 15 h. After repeated washing with ethanol and deionized water until the pH of the filtrate was close to neutral, the mixture was dried at 65℃ for 12 h to obtain the montmorillonite carrier. S2-3 was prepared by dispersing the montmorillonite carrier in anhydrous ethanol at a ratio of 12g:900mL:20mL, followed by the addition of deionized water. Then, 3wt% dilute ammonia solution was added dropwise while monitoring the pH value until the pH stabilized at 9.0. This resulted in a montmorillonite carrier suspension with a mass ratio of tetraethyl orthosilicate to montmorillonite carrier of 0.34:1. Ethyl tetrasilicate was weighed and added to anhydrous ethanol, with the volume ratio of ethyl tetrasilicate to anhydrous ethanol controlled at 1:7 to prepare an ethyl tetrasilicate-ethanol solution. Under continuous stirring at 150 r / min, the ethyl tetrasilicate-ethanol solution was added dropwise to the montmorillonite carrier suspension at a uniform rate. The volume of the ethyl tetrasilicate-ethanol solution added per minute was 0.05% of the total volume of the montmorillonite carrier suspension. After the addition was completed, the temperature was raised to 65℃, and the mixture was stirred and aged at normal pressure for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed three times with anhydrous ethanol, and dried under vacuum at 60℃ for 8 hours to obtain the composite carrier. S3-1 The composite carrier was vacuum activated for 1.5 h at 120 °C and -0.08 MPa. Then, the vacuum-activated composite carrier was dispersed in a 0.8 mol / L zinc acetate dihydrate ethanol solution at a mass-to-volume ratio of 1 g: 15 mL. The solution was then vacuum-impregnated to -0.08 MPa and ultrasonically at 150 W for 35 min. After restoring to normal pressure, the vacuum-impregnation cycle was repeated 3 times. After standing for 5 h, the product was centrifuged. For each wash, anhydrous ethanol was added at a mass-to-volume ratio of 1 g: 20 mL. After stirring for 2 min, the product was immediately centrifuged and the supernatant was discarded. The product was dried at 50 °C for 4 h to obtain a powder product for later use. S3-2 The powdered product was dispersed in an ethanol-water mixture of anhydrous ethanol and deionized water at a mass-to-volume ratio of 1 g: 20 mL to obtain a suspension. The suspension was stirred at 100 r / min for 10 min in a water bath at 45 °C. Then, 0.7 mol / L ammonium bicarbonate aqueous solution was slowly added dropwise at a rate of 0.16% of the total suspension volume per minute. Simultaneously, 0.3 mol / L dilute acetic acid solution was added dropwise. The pH of the system was monitored online, and the dropping rate of dilute acetic acid was adjusted to maintain a stable pH of 6.8 throughout the reaction. After the ammonium bicarbonate was added, the reaction was stirred for another 2.0 h. The pH was continuously monitored and maintained at 6.8 throughout the reaction. After the reaction was completed, the mixture was centrifuged, washed twice with anhydrous ethanol, dried under vacuum at 45 °C for 5 h, and then ground through a 200-mesh sieve to obtain the final product.

[0026] Example 3 A biodegradable copper-clad laminate includes the following steps: 1) Weigh the raw materials according to the following parts by weight: 100 parts epoxy resin, 10 parts curing agent, 0.5 parts curing accelerator, 7 parts degradable inorganic filler, 25 parts flame retardant, 1.5 parts silane coupling agent KH-550, and 85 parts acetone-butanone mixed solvent. 2) According to the weight parts, add the curing agent and curing accelerator to the acetone-butanone mixed solvent, then add the epoxy resin, followed by the silane coupling agent KH-550, flame retardant, and degradable inorganic filler. Stir at 500 r / min for 40 min at 45℃, and then ultrasonically disperse at 300 W for 20 min to obtain the degradable epoxy resin solution. 3) Continuously immerse the fiberglass cloth in the biodegradable epoxy resin solution to fully impregnate it, control the glue application speed to 2m / min, and after impregnation, send it into a hot air oven for segmented baking. Bake at 120℃ for 2min, and then increase to 140℃ for 3min to obtain a semi-cured sheet. 4) Cut the prepreg and stack the corresponding number of prepregs according to the target board thickness. Cover the upper and lower surfaces of the stacked prepregs with electrolytic copper foil (18μm roughened side facing the prepreg), align and stack them, and lay release films on the top and bottom to obtain the hot-pressed board blank. 5) The slab is fed into a vacuum hot press and evacuated to a vacuum degree of -0.08MPa. At an initial temperature of 80℃, it is pre-pressed for 10 minutes at a pressure of 0.8MPa. Then, the temperature is increased to 120℃ at a rate of 2℃ / min and held for 15 minutes. The temperature is then increased to 170℃ and the pressure is increased to 3MPa. The temperature and pressure are maintained for 70 minutes. After the process is completed, the furnace is slowly cooled down at a rate of 3℃ / min. The pressure is released when the temperature drops to 50℃. The board is then removed, the release film on the surface is removed, and the edges are trimmed, the board surface is polished and dust is removed, and it is cut to the specified size to obtain the biodegradable copper-clad laminate.

[0027] The preparation method of the degradation-promoting inorganic filler is as follows: S1. Sodium-based montmorillonite was dispersed in deionized water and stirred in a water bath at 500 r / min for 3 h at 85 °C to prepare a suspension with a mass fraction of 8%. Then, hexadecyltrimethylammonium bromide was added to the suspension, with the amount added being 25% of the total weight of sodium-based montmorillonite. The reaction was continued to be stirred for 8 h. After the reaction was completed, the mixture was separated by centrifugation and washed alternately with deionized water and anhydrous ethanol until no bromide ion precipitate was detected by silver nitrate. The mixture was dried at 70 °C for 5 h and ground through a 300-mesh sieve to obtain organically modified montmorillonite. S2-1: Hexadecyltrimethylammonium bromide was dissolved in deionized water and stirred until completely dissolved to obtain a template agent solution with a concentration of 0.025 mol / L. Then, organically modified montmorillonite was dispersed in the template agent solution to obtain an aqueous phase with an organically modified montmorillonite content of 1.0 wt%. Tween-80 at a mass of 5% was added to dodecane and stirred until completely dissolved to obtain an oil phase. Then, the oil phase was added to the aqueous phase at a volume ratio of 4.5:1 and emulsified in a 30°C water bath at 8000 r / min for 15 min to obtain an emulsion. S2-2 A silica sol with a SiO2 concentration of 13 wt% was prepared. The pH of the system was adjusted to 8.5 using 3 wt% dilute ammonia. After continuous stirring at 150 r / min for 2 h, a silicon source solution was obtained. After pre-cooling to 15℃, the silicon source solution was added dropwise to the emulsion at a mass ratio of 1:2.5, with the volume of silicon source solution added per minute being 0.09% of the total emulsion volume. The pH was adjusted to 10 using 3 wt% dilute ammonia, and the solution was transferred to a reaction vessel and heated at 300 W. Under the influence of wave, the reaction was carried out at 130℃ for 60 min. After the reaction was completed, it was naturally cooled to room temperature. After centrifugation, the supernatant was discarded. The lower layer product was washed three times alternately with deionized water and anhydrous ethanol, and then dispersed in an acidic ethanol solution with a pH of 5.5. The mass-to-volume ratio of the lower layer product to the acidic ethanol solution was 1 g: 100 mL. The mixture was refluxed at 85℃ for 16 h. After repeated washing with ethanol and deionized water until the pH of the filtrate was close to neutral, it was dried at 70℃ for 15 h to obtain the montmorillonite carrier. S2-3 was prepared by dispersing the montmorillonite carrier in anhydrous ethanol at a ratio of 15g:1000mL:25mL, followed by the addition of deionized water. Then, 3wt% dilute ammonia solution was added dropwise while monitoring the pH value until the system pH stabilized at 9.0. The resulting montmorillonite carrier suspension was prepared at a mass ratio of tetraethyl orthosilicate to montmorillonite carrier of 0.42:1. Tetraethyl orthosilicate was weighed and added to anhydrous ethanol, with the volume ratio of tetraethyl orthosilicate to anhydrous ethanol controlled at 1:10 to prepare a tetraethyl orthosilicate ethanol solution. Under continuous stirring at 150 r / min, the tetraethyl orthosilicate ethanol solution was added dropwise to the montmorillonite carrier suspension at a uniform rate. The volume of the tetraethyl orthosilicate ethanol solution added per minute was 0.06% of the total volume of the montmorillonite carrier suspension. After the addition was completed, the temperature was raised to 65℃, and the mixture was stirred and aged at normal pressure for 3 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed three times with anhydrous ethanol, and dried under vacuum at 60℃ for 8 hours to obtain the composite carrier. S3-1 The composite carrier was vacuum activated for 2 h at 130 °C and -0.1 MPa. Then, the vacuum-activated composite carrier was dispersed in a 1.0 mol / L zinc acetate dihydrate ethanol solution at a mass-to-volume ratio of 1 g: 20 mL. The solution was then vacuum-impregnated to -0.1 MPa and ultrasonically at 150 W for 40 min. After restoring to normal pressure, the vacuum-impregnation cycle was repeated 3 times. After standing for 6 h, the product was centrifuged. For each wash, anhydrous ethanol was added at a mass-to-volume ratio of 1 g: 20 mL. After stirring for 2 min, the product was immediately centrifuged and the supernatant was discarded. The product was dried at 50 °C for 4 h to obtain a powder product for later use. S3-2 The powdered product was dispersed in an ethanol-water mixture of anhydrous ethanol and deionized water at a mass-to-volume ratio of 1 g: 20 mL to obtain a suspension. The suspension was stirred at 100 r / min for 10 min under a water bath temperature of 45 °C. Then, 0.7 mol / L ammonium bicarbonate aqueous solution was slowly added dropwise at a rate of 0.16% of the total suspension volume per minute. Simultaneously, 0.3 mol / L dilute acetic acid solution was added dropwise. The pH of the system was monitored online, and the dropping rate of dilute acetic acid was adjusted to maintain a stable pH of 6.8 throughout the reaction. After the ammonium bicarbonate was added, the reaction was stirred for another 2.0 h. The pH was continuously monitored and maintained at 6.8 throughout the reaction. After the reaction was completed, the product was centrifuged, washed twice with anhydrous ethanol, dried under vacuum at 45 °C for 5 h, and then ground through a 200-mesh sieve to obtain the final product.

[0028] Comparative Example 1: This comparative example is basically the same as Example 1, except that steps S2-3 are omitted and the composite carrier in S3-1 is replaced with montmorillonite carrier.

[0029] Comparative Example 2: This comparative example is basically the same as Example 1, except that steps S2-1 to S3-1 are omitted, and the powder product in S3-2 is replaced with organic modified montmorillonite.

[0030] Comparative Example 3: This comparative example is basically the same as Example 1, except that step S3-1 is omitted and the powder product in S3-2 is replaced with a composite carrier.

[0031] Comparative Example 4: This comparative example is basically the same as Example 1, except that step S3-2 is omitted and the powder product in S3-1 is used as a degradation-promoting inorganic filler.

[0032] Comparative Example 5: This comparative example is basically the same as Example 1, except that steps S1 to S2-2 are omitted, and porous silica (multi-level porous silica microspheres, XFF30, provided by Jiangsu Xianfeng Nanomaterials Technology Co., Ltd.) is used instead of the montmorillonite carrier in the subsequent steps.

[0033] Comparative Example 6: This comparative example is basically the same as Example 1, except that organic modified montmorillonite is used to replace the degradable inorganic filler, and an equal amount of zinc acetate powder is directly physically mixed into the epoxy resin adhesive system to obtain copper-clad laminate.

[0034] Control group: This control group is basically the same as Example 1, except that silica (spherical silica powder, provided by Shijiazhuang Donghao Chemical Research Institute Co., Ltd.) is used instead of the degradation-promoting inorganic filler.

[0035] Test experiment: The copper-clad laminates prepared in Examples 1-3 and Comparative Examples 1-5 were cut into 10cm × 10cm samples. After etching away the copper foil, the samples were washed, dried, and their total weight (including the epoxy resin matrix and fiberglass cloth) was measured. Since the fiberglass cloth does not degrade, the mass m of the fiberglass cloth used in the copper-clad laminate was subtracted. g (The mass m of the fiberglass cloth used in this copper-clad laminate) g The amount of glass fiber cloth used during the preparation of the board can be used to obtain the mass of the resin matrix as m0, and then the following tests are performed; Resin phase acidic degradation performance test: The sample was placed in a deionized water system adjusted to pH=5 with hydrochloric acid, immersed in 100℃ for 1 hour, then removed, washed with water, dried, and the residual total weight m of the sample was measured. t总0 Deducting the mass of the fiberglass cloth (m) g The residual mass m of the resin after degradation was obtained. t0 =m t总0 -m g The degradability rate was calculated by measuring the change in mass before and after degradation. Five parallel samples were used in each group, and the average result was taken. Degradability rate = (m0 - m...) t0 ) / m0×100%.

[0036] Toughness test: The toughness of the sample was tested by the falling weight impact method, where the falling weight was 1m high and the falling weight was 1kg. The crack propagation area (impact area, mm²) after the impact was recorded. 2 The larger the impact area value, the more severe the crack propagation and the worse the toughness of the plate. Five parallel samples were used in each group, and the average value of the results was taken.

[0037] Bending strength test: Refer to Part 7.3 of GB / T 4722-2017 standard for testing the bending strength of samples. The three-point bending method is used to test the bending strength of copper-clad laminate. The span of the support point is 16 times the thickness of the sample. The sample is pretreated for 24 hours at 23±2℃ and 50±5% relative humidity. The loading speed is 1 mm / min. The test is carried out along the longitudinal and transverse directions of the board. There are 5 parallel samples in each group. The result is the arithmetic mean.

[0038] Moisture and heat resistance test: Place the sample in an oven and bake at 105℃ for 2 hours. After cooling, weigh it (m1). Then treat it in an 80℃ distilled water bath for 528 hours. Take out the sample, blot the residual moisture on the surface with qualitative filter paper, weigh it immediately and record it (m2). Calculate the water absorption rate of the sample by the change in mass before and after. There are 5 parallel samples in each group. Take the average value of the results. Water absorption rate (%) = (m2-m1) / m1×100%.

[0039] The experimental results are shown in Table 1.

[0040] Table 1 As shown in Table 1, the copper-clad laminate of the present invention has the advantages of low water absorption, high mechanical properties and stability in long-term humid and hot service environments, and has broad market application prospects.

[0041] Comparative Example 4, by omitting the outer basic zinc carbonate sealing shell, allows zinc acetate to directly contact the epoxy resin during the 170℃ hot-pressing curing stage, resulting in Zn... 2+ Premature catalytic hydrolysis of ester bonds in the resin consumes degradable groups and causes coordination reactions with the curing agent, disrupting the resin crosslinking network and leading to catalyst deactivation. This prevents the effective release of active Zn in subsequent degradation tests. 2+ This resulted in a lower degradation rate than the control group 3 without a catalyst.

[0042] Comparative Example 4, by omitting the outer basic zinc carbonate sealing layer, allows zinc acetate to directly contact the epoxy resin during the 170℃ hot-pressing curing stage. 2+ Premature catalysis of ester bonds and coordination reaction with curing agent severely damages the filler-resin interface, leading to an increase in interface defects. This interface damage effect exceeds the toughening contribution of the montmorillonite sheets themselves. Therefore, the impact area of ​​Comparative Example 4 is actually larger than that of Comparative Example 5.

[0043] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a biodegradable copper-clad laminate, characterized in that, Specifically, the steps include the following: 1) Weigh the raw materials according to the following parts by weight: 80-100 parts epoxy resin, 6-10 parts curing agent, 0.3-0.5 parts curing accelerator, 4-7 parts degradable inorganic filler, 20-25 parts flame retardant, 1-1.5 parts silane coupling agent KH-550, and 75-85 parts acetone-butanone mixed solvent; 2) Add epoxy resin, curing agent, curing accelerator, degradation-promoting inorganic filler, flame retardant, and silane coupling agent KH-550 to an organic solvent to obtain a resin solution; 3) Impregnate the fiberglass cloth with the adhesive, bake it in sections to obtain a prepreg, and stack at least one prepreg. After stacking, attach electrolytic copper foil to one or both sides to assemble it into a slab. 4) Place the slab in a vacuum hot press, heat and press in stages to solidify, and after cooling and trimming, obtain a biodegradable copper-clad laminate.

2. The method for preparing a biodegradable copper-clad laminate according to claim 1, characterized in that, In step 3), the segmented baking involves baking at 120-130℃ for 2-3 minutes, and then increasing the temperature to 140-150℃ for 3-5 minutes. In step 4), the segmented heating and pressurizing hot pressing curing involves evacuating to a vacuum level of -0.05 to -0.08 MPa, pre-pressing at an initial temperature of 80-90℃ for 10-15 minutes at a pressure of 0.8-1.2 MPa, then heating at a rate of 1-2℃ / min to 120-130℃, holding at that temperature for 15-20 minutes, continuing to heat to 170-175℃, increasing the pressure to 2.5-3.0 MPa, and maintaining constant temperature and pressure for 70-90 minutes.

3. The method for preparing a biodegradable copper-clad laminate according to claim 1, characterized in that, The epoxy resin is selected from at least one of diglycidyl adipate, diglycidyl isophthalate, diglycidyl hexahydrophthalate, and diglycidyl 4,5-epoxytetrahydrophthalate. The curing agent is dicyandiamide; The curing accelerator is selected from 2-methylimidazole; The flame retardant is selected as a halogen-free phosphate flame retardant. The acetone-butanone mixed solvent is prepared by mixing equal volumes of acetone and butanone.

4. The method for preparing a biodegradable copper-clad laminate according to claim 1, characterized in that, The degradation-promoting inorganic filler is prepared by the following method: S1 uses hexadecyltrimethylammonium bromide to modify montmorillonite, resulting in organically modified montmorillonite; S2-1: Hexadecyltrimethylammonium bromide is dissolved in deionized water to obtain a template agent solution. Then, organically modified montmorillonite is dispersed in the template agent solution to obtain an aqueous phase. Tween-80 is added to dodecane and stirred until completely dissolved to obtain an oil phase. Then, the oil phase is added to the aqueous phase at a volume ratio of (4.0-4.5):1, and an emulsion is obtained by shear emulsification. S2-2 After pre-cooling the prepared silicon source solution to 10-15℃, the silicon source solution is added dropwise to the emulsion, the pH value is adjusted to 9-10, and then transferred to a reaction vessel. The reaction is carried out at 120-130℃ for 40-60 min under microwave action. After the reaction is completed, the mixture is cooled to room temperature. The product is washed and dispersed in an acidic ethanol solution. After reflux extraction for 12-16 h, the product is dried to obtain the montmorillonite support. S2-3 Under continuous stirring, ethyl orthosilicate ethanol solution was added dropwise to montmorillonite carrier suspension. After the addition was complete, the temperature was raised to 65-68℃, and the mixture was stirred and aged at normal pressure for 3-4 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed and dried to obtain composite carrier. S3-1 The composite carrier is activated under vacuum for 1-2 hours, then the vacuum-activated composite carrier is dispersed in an ethanol solution of zinc acetate dihydrate, vacuumed and impregnated for 30-40 minutes, then allowed to stand for 4-6 hours and centrifuged, washed and dried to obtain the powder product for later use. S3-2 The above powder product is dispersed in an ethanol-water mixed solution to obtain a suspension. Then, it is stirred at 100-150 r / min for 10-15 min at 40-45℃. Then, an ammonium bicarbonate aqueous solution is added dropwise to adjust the pH value to 6.5-6.

8. The reaction is continued to be stirred for 1.5-2.0 h. After the reaction is completed, the product is centrifuged, washed, dried, ground, and passed through a 200-mesh sieve to obtain the desired degradation-promoting inorganic filler.

5. The method for preparing a biodegradable copper-clad laminate according to claim 4, characterized in that, In S2-1, the template agent solution has a concentration of 0.020-0.025 mol / L; The aqueous phase contains 0.5-1.0 wt% organically modified montmorillonite. In the oil phase, Tween-80 accounts for 4-5% of the mass of dodecane; The shear emulsification is performed by emulsifying at 6000-8000 r / min for 10-15 min in a water bath at 25-30℃.

6. The method for preparing a biodegradable copper-clad laminate according to claim 4, characterized in that, In S2-2, the silicon source solution is obtained by taking a silica sol with a SiO2 concentration of 10-13wt%, adjusting the pH value of the system to 8.0-8.5 with 3wt% dilute ammonia water, and stirring. The silicon source solution and emulsion have a mass ratio of 1:(1.5-2.5). The dropping process is carried out at a rate of 0.06-0.09% of the total volume of the emulsion per minute, representing the volume of the silicon source solution added. The microwave action has a power of 200-300W; The acidic ethanol solution has a pH value of 5.0-5.5; The reflux extraction is performed at a temperature of 80-85℃.

7. The method for preparing a biodegradable copper-clad laminate according to claim 4, characterized in that, In S2-3, the continuous stirring is carried out at a speed of 150-180 r / min; The montmorillonite carrier suspension is prepared by dispersing the montmorillonite carrier in anhydrous ethanol, adding deionized water, and adjusting the pH value to 9.0 according to the ratio of montmorillonite carrier, anhydrous ethanol, and deionized water as (10-15) g: (800-1000) mL: (15-25) mL. The tetraethyl orthosilicate ethanol solution is prepared by weighing tetraethyl orthosilicate and adding it to anhydrous ethanol according to the mass ratio of tetraethyl orthosilicate to montmorillonite carrier of (0.28-0.42):1, and controlling the volume ratio of tetraethyl orthosilicate to anhydrous ethanol to be 1:(4-10). The dropping rate is 0.04-0.06% of the total volume of the montmorillonite carrier suspension, representing the volume of tetraethyl orthosilicate ethanol solution added per minute.

8. The method for preparing a biodegradable copper-clad laminate according to claim 4, characterized in that, In S3-1, the vacuum activation is carried out at 110-130℃ and -0.05 to -0.1MPa. The mass-to-volume ratio of the vacuum-activated composite carrier and the zinc acetate dihydrate ethanol solution is 1g:(10-20)mL. The zinc acetate dihydrate ethanol solution has a concentration of 0.5-1.0 mol / L; The process involves impregnation after vacuuming, with a vacuum level of -0.05 to -0.1 MPa, and the application of 120-150 W of ultrasound.

9. The method for preparing a biodegradable copper-clad laminate according to claim 4, characterized in that, In S3-2, the ethanol-water mixed solution is composed of anhydrous ethanol and deionized water in a volume ratio of (1.2-1.5):1; The powder product and the ethanol-water mixed solution have a mass-to-volume ratio of 1g:(15-20)mL; The ammonium bicarbonate aqueous solution has a concentration of 0.8-1.2 mol / L, and the dropping rate is such that the volume of the ammonium bicarbonate aqueous solution dropped per minute is 0.08-0.16% of the total volume of the suspension.

10. A biodegradable copper-clad laminate, characterized in that, It is prepared by the method described in any one of claims 1-9.