Thermoplastic composite laminate integrated with carbon nanotube film, and self-resistance heating forming method and application thereof

By integrating carbon nanotube membranes with a self-resistance heating method, the problem of insufficient processing window and interlayer interface strengthening caused by the high viscosity of thermoplastic resin was solved, realizing efficient thermoplastic composite material forming and interfacial bonding strengthening, and improving the forming and manufacturing efficiency and mechanical properties of thermoplastic CFRTP laminates.

CN123129556APending Publication Date: 2026-11-20CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611480924.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The high viscosity of thermoplastic resins limits the processing window and the mechanical properties of the molded components. Traditional heating methods have long heating cycles and limited temperatures, making them difficult to apply effectively in the field of high-performance structures, and there is also the problem of insufficient interlayer interface strengthening.

Method used

The self-resistance heating method of integrated carbon nanotube membrane is adopted. By alternating layers of CNT membrane and thermoplastic fiber reinforced composite material, the self-resistance heating of CNT membrane reduces resin viscosity and promotes melt wetting. Combined with mold heating and stamping, a "studded-anchored" structure is formed, which improves the interfacial bonding strength.

Benefits of technology

It significantly improves the heating efficiency and interfacial bonding of thermoplastic CFRTP composites, enhances the crystallization characteristics of thermoplastic resins, and optimizes the forming and manufacturing efficiency of laminated structural components and the mechanical properties of multi-component heterogeneous interfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129556A_ABST
    Figure CN123129556A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of thermoplastic composite laminates and fiber metal composite laminates forming, and particularly relates to a thermoplastic composite laminate integrated with a carbon nanotube film, a self-resistance heating forming method and application thereof. The present application implants a CNT film in a CFRTP composite laminate structure to form a super-hybrid CFRTP composite laminate structure, and prepares a carbon fiber reinforced thermoplastic composite material by electrically heating the CNT film. The high specific surface area and nano-scale pore structure of the CNT can promote the penetration of the PEEK melt, form a 'pinning-anchoring' structure, and improve the mechanical bonding strength. The present application not only improves the heating efficiency of the CFRTP composite material, but also improves the interlaminar resin crystallization characteristics and interfacial bonding force. The present application can form an optimized design of the stacking configuration of the CNT modified CFRTP and the fiber metal hybrid laminate structure, and provides a new method for reducing the forming cost of the CFRTP composite laminate structure and improving the mechanical properties of the multi-element heterogeneous interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of thermoplastic composite laminate and fiber-metal composite laminate forming technology, specifically relating to a thermoplastic composite laminate with integrated carbon nanotube film, its self-resistive heating forming method and application. Background Technology

[0002] Thermoplastic fiber-reinforced composites (CFRTP) and their fiber-metal hybrid laminates (FML) have important application prospects in achieving high-speed and lightweight development in high-precision fields such as aerospace and weaponry due to their advantages such as high specific strength, excellent damage tolerance and reprocessability.

[0003] However, the high viscosity of thermoplastic resins severely restricts the processing window and the mechanical properties of molded components, thus limiting their engineering applications in high-performance structures. On the one hand, thermoplastic resins rely mainly on melt flow and physical wetting to form the bonding interface during molding and bonding. High-viscosity molten resins are prone to problems such as insufficient wetting, residual pores, and inadequate interfacial bonding within a limited processing time. Increasing the molding temperature can significantly reduce resin viscosity, but excessively high temperatures weaken the resin's antioxidant stability, and traditional heating methods have excessively long heating cycles, strictly limiting the process temperature. On the other hand, heating methods such as in-situ self-resistance heating of carbon fibers have been proposed to address the heating efficiency and interface quality issues of thermoplastic composites, but insufficient interlayer interface strengthening still exists in multilayer composites and fiber-metal hybrid structures. Since these methods mainly rely on the conductive heating of the carbon fiber itself, the temperature uniformity in the thickness direction of the layers is limited. Therefore, the resin-rich interface formed between the layers of the woven prepreg has weak performance. At the same time, the higher requirements for resin wettability of the metal-CFRTP heterogeneous interface are also difficult to meet. Summary of the Invention

[0004] The purpose of this invention is to provide a thermoplastic composite laminate with integrated carbon nanotube film, its self-resistive heating forming method, and its application. The forming method provided by this invention can improve the forming efficiency of composite structures, enhance their interlayer bonding performance, and result in composite structures with high interfacial strength and toughness after forming.

[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a self-resistance heating forming method for thermoplastic composite laminates, comprising the following steps: (1) The CNT film and the thermoplastic fiber reinforced composite material layer are stacked according to the preset layup sequence to obtain the fiber composite layer; (2) The CNT film in the fiber composite layer is subjected to self-resistance heating by passing an electric current through it until the thermoplastic resin reaches a molten state; (3) The fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (4) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The preset layup sequence alternates between the first unit and the second unit, with the outermost layer being the first unit; the first unit is an N-layer thermoplastic fiber reinforced composite material layer; and the second unit is a single-layer CNT film.

[0006] Preferably, N is 2 to 20; the self-resistance heating of the CNT film also includes the self-resistance heating of the thermoplastic fiber reinforced composite material layer; the self-resistance heating of the composite material layer also includes external heating provided by mold heating.

[0007] Preferably, the thermoplastic fiber reinforced composite layer comprises a thermoplastic resin and carbon fibers impregnated in the thermoplastic resin, wherein the thermoplastic resin comprises one or more of PEEK, PEKK, PPS, PA6, PA12 and PI.

[0008] Preferably, the thermoplastic composite laminate further includes a thermoplastic resin layer; when the thermoplastic composite laminate includes a thermoplastic resin layer, the thermoplastic resin layer is used as the outermost layer of the thermoplastic composite laminate, and the middle layer consists of alternating first and second units, with the first and last sections of the middle layer being the second unit.

[0009] The present invention also provides a thermoplastic composite laminate prepared by the above-described self-resistance heating forming method, comprising alternating first units and second units; the first unit is an N-layer thermoplastic fiber reinforced composite material layer; the second unit is a single-layer CNT film; the first unit is at both the beginning and end of the thermoplastic composite laminate.

[0010] Preferably, when the thermoplastic composite laminate includes a thermoplastic resin layer, its outermost layer is a thermoplastic resin layer, the middle layer is an alternating first unit and a second unit, and the first and last sections of the middle layer are both second units.

[0011] Preferably, the thickness of the thermoplastic fiber reinforced composite material layer is 0.1~1mm; and the thickness of the single-layer CNT film is 5~100μm.

[0012] The present invention also provides a metal composite workpiece, the metal composite workpiece comprising alternating metal layers and thermoplastic composite plates; the end of the metal composite workpiece is a metal layer; the total number of metal layers in the metal composite workpiece is M+1 layers; the total number of thermoplastic composite plates is M layers; M≥1; the thermoplastic composite plate is a thermoplastic composite plate prepared by the self-resistance heating forming method according to any one of claims 1 to 4 or a thermoplastic composite plate according to claim 5.

[0013] The present invention also provides a method for preparing the above-described metal composite workpiece, comprising the following steps: (1) Perform surface treatment on the metal layer; (2) Stack the CNT film, thermoplastic fiber reinforced composite material layer and metal layer according to the layup sequence of the metal composite workpiece, and then perform hot pressing integration treatment to obtain the metal fiber composite layer; or, stack the metal layer with the CNT film and thermoplastic fiber reinforced composite material layer according to the layup sequence of the metal composite workpiece to obtain the metal fiber composite layer. (3) The CNT film in the metal fiber composite layer is energized and self-heated until the thermoplastic resin reaches the molten state, while the metal layer is subjected to external auxiliary heating to a temperature not higher than that of the thermoplastic composite layer. (4) The metal fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating conditions; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (5) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The steps (2) and (3) are not in any particular order.

[0014] Preferably, the external auxiliary heating includes one or more of the following: mold heating, metal layer self-resistance heating, induction heating, infrared heating, and hot plate contact heating.

[0015] Compared with the prior art, the present invention has the following technical effects: A novel ultrahybrid composite laminate structure is formed by embedding CNT films into thermoplastic CFRTP and its fiber-metal hybrid laminate structure. Thermoplastic composite materials are prepared by electrically heating the CNT film. The local high temperature of in-situ heating of the CNT film can significantly reduce the resin viscosity. At the same time, the high specific surface area and nanoscale pore structure of CNTs can promote the penetration of PEEK melt, forming a "pinning-anchoring" structure and improving the mechanical bonding strength. This not only improves the heating efficiency of thermoplastic CFRTP composite materials, but also improves the crystallization characteristics and interfacial bonding force of thermoplastic resin. It can form a laminate configuration optimization design of CNT-modified thermoplastic CFRTP composite laminate structure, providing a new method for improving the forming and manufacturing efficiency of thermoplastic CFRTP laminate structure and improving the mechanical properties of multi-component heterogeneous interfaces. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 Schematic diagram of the laminated configuration design of ultrahybrid composite materials and the heating method of CNT film; Figure 2 A schematic diagram of the structure of a hot stamping die for integrating carbon nanotube fiber metal layers. Detailed Implementation

[0018] This invention provides a self-resistance heating forming method for thermoplastic composite laminates, comprising the following steps: (1) The CNT film and the thermoplastic fiber reinforced composite material layer are stacked according to the preset layup sequence to obtain the fiber composite layer; (2) The CNT film in the fiber composite layer is subjected to self-resistance heating by passing an electric current through it until the thermoplastic resin reaches a molten state; (3) The fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (4) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The preset layup sequence alternates between the first unit and the second unit, with the outermost layer being the first unit; the first unit is an N-layer thermoplastic fiber reinforced composite material layer; and the second unit is a single-layer CNT film.

[0019] The present invention stacks CNT film and thermoplastic fiber reinforced composite material layer according to a preset layup sequence to obtain fiber composite layer.

[0020] In this invention, the preset layup sequence alternates between a first unit and a second unit, with the outermost layer being the first unit; the first unit is an N-layer thermoplastic fiber-reinforced composite material layer; the second unit is a single-layer CNT film; N≥1, specifically, N can be 2~20.

[0021] In this invention, the thermoplastic composite laminate further includes a thermoplastic resin layer; when the thermoplastic composite laminate includes a thermoplastic resin layer, the thermoplastic resin layer is used as the outermost layer of the thermoplastic composite laminate, and the middle layer consists of alternating first and second units, with the first and last sections of the middle layer being the second unit.

[0022] In this invention, the thermoplastic fiber reinforced composite material layer may include a thermoplastic resin and carbon fibers impregnated in the thermoplastic resin; the thermoplastic resin may include one or more of PEEK, PEKK, PPS, PA6, PA12 or PI.

[0023] In this invention, the CNT film in the fiber composite layer is subjected to self-resistance heating by passing an electric current through it until the thermoplastic resin reaches a molten state.

[0024] In this invention, the thermoplastic fiber reinforced composite material layer can be self-heated simultaneously with the CNT film to improve heating efficiency; the input voltage and current of the self-heating are adjusted according to the size, resistance and number of layers of the self-heating element.

[0025] In this invention, while the composite material layer is subjected to self-resistance heating, external heating can be provided through mold heating.

[0026] In this invention, the self-resisting heating to the point where the thermoplastic resin reaches a molten state can achieve resin melt wetting and interfacial bonding of the CNT film.

[0027] This invention places a fiber composite layer in a convex and concave mold, and sequentially performs stamping, hot pressing, in-mold cooling, and demolding on the fiber composite layer under heating. During stamping, the punch preferably moves downwards at a stamping speed of 5-10 mm / s to close with the concave mold; in this invention, the above stamping speed ensures smooth mold closing. In this invention, the pressure of the hot pressing treatment can be 0.5-3 MPa, specifically 0.7-1 MPa. Setting the hot pressing pressure within the above range allows the molten resin to form a dense interfacial bond between the fiber layers; the in-mold cooling is below the glass transition temperature of the thermoplastic resin; the cooling rate of the in-mold cooling is <10℃ / min, specifically 1℃ / min. In this invention, in-mold cooling can be performed through a water-cooling channel. Near the CNT film layer, a PID controller adjusts the power supply to gradually cool to room temperature at a cooling rate below 10℃ / s, ensuring interfacial bonding strength. When the laminated hybrid layer cools below the glass transition temperature of the resin and completes curing, the composite workpiece is finally demolded.

[0028] The present invention also provides a thermoplastic composite laminate obtained by the above-described self-resistance heating forming method, comprising alternating first units and second units; the first unit is an N-layer thermoplastic fiber reinforced composite material layer; the second unit is a single-layer CNT film; the first unit is at both the beginning and end of the thermoplastic composite laminate.

[0029] In this invention, the total thickness of the N-layer thermoplastic fiber-reinforced composite material can be 50 μm; the PEEK film can provide insulation and prevent potential corrosion.

[0030] In this invention, when the thermoplastic composite laminate includes a thermoplastic resin layer, its outermost layer is a thermoplastic resin layer, the middle layer is an alternating first unit and a second unit, and the first and last sections of the middle layer are both second units.

[0031] The present invention also provides a metal composite workpiece, the metal composite workpiece comprising alternating metal layers and thermoplastic composite plates; both ends of the metal composite workpiece are metal layers; the total number of metal layers in the metal composite workpiece is M+1 layers; the total number of thermoplastic composite plates is M layers; and M≥1.

[0032] The present invention also provides a method for preparing the above-described metal composite workpiece, comprising the following steps: (1) Perform surface treatment on the metal layer; (2) Stack the CNT film, thermoplastic fiber reinforced composite material layer and metal layer according to the layup sequence of the metal composite workpiece, and then perform hot pressing integration treatment to obtain the metal fiber composite layer; or, stack the metal layer with the CNT film and thermoplastic fiber reinforced composite material layer according to the layup sequence of the metal composite workpiece to obtain the metal fiber composite layer. (3) The CNT film in the metal fiber composite layer is energized and self-heated until the thermoplastic resin reaches the molten state, while the metal layer is subjected to external auxiliary heating to a temperature not higher than that of the thermoplastic composite layer. (4) The metal fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating conditions; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (5) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The steps (2) and (3) are not in any particular order.

[0033] This invention stacks a CNT film, a thermoplastic fiber reinforced composite material layer, and a metal layer according to the layup sequence of a metal composite workpiece, and then performs a hot-pressing integrated treatment to obtain a metal fiber composite layer. Alternatively, the metal layer is stacked with the CNT film and the thermoplastic fiber reinforced composite material layer according to the layup sequence of a metal composite workpiece to obtain a metal fiber composite layer.

[0034] In this invention, the surface treatment can be one or more of mechanical polishing, anodizing, acid and alkali treatment, and sandblasting.

[0035] In this invention, before stacking, the CNT film and thermoplastic fiber reinforced composite material are pretreated. The pretreatment involves soaking the CNT film and thermoplastic fiber reinforced composite material in anhydrous ethanol and then placing them in a clean room with a lint-free cloth to air dry.

[0036] The present invention places the metal fiber composite layer in a convex and concave mold, and performs stamping, hot pressing, in-mold cooling and demolding on the fiber composite layer in a heated state; the in-mold cooling is below the glass transition temperature of the thermoplastic resin.

[0037] In this invention, the aging treatment includes heating in an aging furnace, or a combination of aging furnace heating and self-resistive electric heating. In this invention, the aging treatment can be performed under pressure; in this invention, the above-mentioned aging methods can maximize the improvement of the mechanical properties of the composite hybrid component.

[0038] To further illustrate the present invention, the following detailed description of the invention's solutions, in conjunction with the accompanying drawings and embodiments, is provided, but should not be construed as limiting the scope of protection of the present invention.

[0039] Example 1 1. Cut the 2024 aluminum alloy plate, CNT film, PEEK film, and CF / PEEK unidirectional prepreg after solution aging (495℃×30min water quenching) and pre-aging treatment (80℃×12h) to standard sample size of 300×28mm. Clean the surface oil with acetone ultrasonically for 10min, and then mechanically polish the aluminum alloy plate with 600-grit sandpaper to remove the surface oxide layer.

[0040] 2. After ultrasonically cleaning the 2024 aluminum alloy plate with deionized water (40kHz, 5min), dry it with hot air at 60℃ for 30min. After soaking the CNT film and PEEK film in anhydrous ethanol (≥99.7%), place it in a clean room to air dry using a lint-free cloth.

[0041] 3. Stack the CNT membrane, CF-PEEK unit, and PEEK membrane in the manner of “PEEK membrane (50μm) / CNT membrane / / CF-PEEK unit (8 CF-PEEK layers) / CNT membrane / PEEK membrane (50μm)” to obtain a fiber composite layer. One layer of CF-PEEK fiber is laid along the 0° direction (horizontal direction), and the next layer of fiber is laid by rotating 90° (vertical direction).

[0042] First, the aluminum alloy plate is heated to 300℃ using a contact heating plate (heating rate of 30℃ / s), and then quickly transferred to a mold preheated to 300℃. The stacked fiber composite layers are then quickly transferred to the 2024 aluminum alloy plate in the order of "aluminum alloy / fiber composite layer / aluminum alloy". The CNT film is heated to 390℃ within 30 seconds using self-resistance heating (DC 15V, 40A), and the temperature data is fed back through an embedded thermocouple.

[0043] 4. Before stamping, a high-temperature boron nitride release agent is uniformly sprayed onto the mating surfaces of the punch and die. The punch pressure is set to 2 MPa, and the punch downward speed is kept constant at 10 mm / s. The mold temperature is rapidly raised to 300℃ (not higher than the external metal temperature of the hybrid layer) through the built-in heating system (ceramic heating rod) at a rate of 50℃ / min. After mold closing, a pressure of 1 MPa is applied, and the holding time is controlled at 30s. Then, the stamped component is cooled in the mold through the cooling channel at an average cooling rate of about 1℃ / s. Near the CNT film layer, the power supply is adjusted by a PID controller to gradually cool the material to below 143℃ (the glass transition temperature of PEEK resin) at a linear cooling rate of 0.5℃ / s to ensure the interfacial bonding strength. When the fiber-metal hybrid layer cools to room temperature and completes curing, the composite workpiece is finally demolded.

[0044] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for self-resistance heating forming of a thermoplastic composite laminate, comprising the following steps: (1) The CNT film and the thermoplastic fiber reinforced composite material layer are stacked according to the preset layup sequence to obtain the fiber composite layer; (2) The CNT film in the fiber composite layer is subjected to self-resistance heating by passing an electric current through it until the thermoplastic resin reaches a molten state; (3) The fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (4) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The preset layup sequence alternates between first unit and second unit, with the outermost layer being the first unit; the first unit is an N-layer thermoplastic fiber reinforced composite material layer; The second unit is a single-layer CNT film.

2. The self-resistance heating forming method as described in claim 1, characterized in that, The value of N is 2 to 20; the self-resistance heating of the CNT film also includes the self-resistance heating of the thermoplastic fiber reinforced composite material layer; the self-resistance heating of the composite material layer also includes external heating provided by mold heating.

3. The self-resistance heating forming method as described in claim 1, characterized in that, The thermoplastic fiber reinforced composite layer includes a thermoplastic resin and carbon fibers impregnated in the thermoplastic resin, wherein the thermoplastic resin includes one or more of PEEK, PEKK, PPS, PA6, PA12 and PI.

4. The self-resistance heating forming method as described in claim 1, characterized in that, The thermoplastic composite laminate also includes a thermoplastic resin layer; when the thermoplastic composite laminate includes a thermoplastic resin layer, the thermoplastic resin layer is used as the outermost layer of the thermoplastic composite laminate, and the middle layer consists of alternating first and second units, with the first and last sections of the middle layer being the second unit.

5. The thermoplastic composite laminate prepared by the self-resistance heating forming method according to any one of claims 1 to 3, characterized in that, It includes alternating first and second units; the first unit is an N-layer thermoplastic fiber-reinforced composite material layer; the second unit is a single-layer CNT film; The first and last ends of the thermoplastic composite laminate are both the first unit.

6. The thermoplastic composite laminate as described in claim 5, characterized in that, When the thermoplastic composite laminate includes a thermoplastic resin layer, its outermost layer is a thermoplastic resin layer, and the middle layer consists of alternating layers of a first unit and a second unit, with the first and last sections of the middle layer being the second unit.

7. The thermoplastic composite laminate as described in claim 5 or 6, characterized in that, The thickness of the thermoplastic fiber reinforced composite material layer is 0.1~1mm; the thickness of the single-layer CNT film is 5~100μm.

8. A metal composite workpiece, the metal composite workpiece comprising alternating metal layers and thermoplastic composite plates; the end of the metal composite workpiece being a metal layer; the total number of metal layers in the metal composite workpiece being M+1 layers; the total number of thermoplastic composite plates being M layers; wherein M≥1; the thermoplastic composite plate being a thermoplastic composite plate prepared by the self-resistance heating forming method according to any one of claims 1 to 4 or a thermoplastic composite plate according to claim 5.

9. The method for preparing the metal composite workpiece according to claim 7, characterized in that, Includes the following steps: (1) Perform surface treatment on the metal layer; (2) Stack the CNT film, thermoplastic fiber reinforced composite material layer and metal layer according to the layup sequence of the metal composite workpiece, and then perform hot pressing integration treatment to obtain the metal fiber composite layer; or, stack the metal layer with the CNT film and thermoplastic fiber reinforced composite material layer according to the layup sequence of the metal composite workpiece to obtain the metal fiber composite layer. (3) The CNT film in the metal fiber composite layer is energized and self-heated until the thermoplastic resin reaches the molten state, while the metal layer is subjected to external auxiliary heating to a temperature not higher than that of the thermoplastic composite layer. (4) The metal fiber composite layer is placed in a convex and concave mold, and the fiber composite layer is sequentially stamped, hot-pressed, cooled in the mold and demolded under heating conditions; the in-mold cooling is below the glass transition temperature of the thermoplastic resin. (5) After demolding, the component is subjected to aging treatment to obtain the formed thermoplastic composite laminate; The steps (2) and (3) are not in any particular order.

10. The preparation method according to claim 9, characterized in that, The external auxiliary heating includes one or more of the following: mold heating, metal layer self-resistance heating, induction heating, infrared heating, and hot plate contact heating.