A low dielectric cyanate ester-based composite material and a method for preparing the same

By twisting and surface modification of glass fiber precursors, combined with cyanate ester resin modification, low dielectric cyanate ester-based composite materials were prepared, solving the problems of decreased dielectric properties and interface debonding after reinforcement modification, and achieving excellent performance under high frequency and high temperature environments.

CN123129557APending Publication Date: 2026-11-20XI'AN POLYTECHNIC UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611640570.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing cyanate ester-bismaleimide blended resin composites exhibit decreased dielectric properties, are prone to interfacial debonding, lack sufficient toughness and fatigue performance, and are unsuitable for high-load and high-temperature environments after reinforcement modification.

Method used

Low-dielectric glass fiber cloth was prepared by twisting glass fiber filaments and treating them with special slurry and coupling agent. The cloth was then modified with cyanate ester resin as the main matrix and bismaleimide to form a composite material impregnation solution. The low-dielectric cyanate ester-based composite material was obtained by hot pressing and curing.

Benefits of technology

It significantly reduces the dielectric constant and dielectric loss of composite materials, improves heat distortion temperature and peel strength, and is suitable for high-frequency communication and high-temperature environments, meeting the performance requirements of high-end electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129557A_ABST
    Figure CN123129557A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of composite materials, and particularly relates to a low-dielectric cyanate-based composite material and a preparation method thereof. The low-dielectric glass fiber cloth is obtained by performing twisting treatment on the glass fiber original wire, then performing sizing treatment and surface modification, and then impregnating a composite material impregnating solution obtained by using cyanate resin as a main matrix and bismaleimide modification to obtain the low-dielectric cyanate-based composite material through hot pressing and curing. The single yarn arrangement is regular through the twisting treatment, the yarn bundle internal air interface polarization is reduced, the yarn bundle looseness, the serious interface polarization, the high dielectric constant and the high loss are solved, the obtained fiber cloth has a dielectric constant of less than or equal to 4.2 and a dielectric loss of less than or equal to 0.009 at 1 MHz; the resin compounding system further reduces the overall dielectric parameters of the composite material, and simultaneously improves the heat distortion temperature, the peeling strength and the dimensional stability, and is suitable for high-end scenes such as high-frequency communication PCB, high-speed server substrate and vehicle-mounted radio frequency circuit board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material technology, specifically relating to a cyanate ester-based composite material and its preparation method. Background Technology

[0002] Cyanate ester-bismaleimide (CE-BMI) blends are a class of high-performance thermosetting matrix materials, combining the advantages of cyanate ester resins (low dielectric strength, low moisture absorption, and excellent dimensional stability) with bismaleimide resins (high heat resistance and good mechanical strength). They are widely used in advanced composite material fields such as aerospace, high-speed electronic printed circuit boards, and radar radomes, where high temperature resistance and dielectric properties are critical. However, pure cyanate ester-bismaleimide cured resins have inherent defects: high crosslinking density after curing leads to brittleness, insufficient impact toughness, and susceptibility to microcracks under external forces; simultaneously, the high viscosity of the cured system results in a narrow molding and processing window, and poor crack resistance when used alone as structural components, limiting their application under high load and alternating stress conditions.

[0003] To address the aforementioned issues, existing technologies commonly employ glass fiber to reinforce and modify the cyanate ester-bismaleimide resin matrix. Glass fiber, as an inorganic reinforcing phase, possesses advantages such as high modulus, controllable cost, and good adaptability to molding processes. Introducing it into the CE-BMI system can significantly improve the tensile and flexural static mechanical properties of the composite material, reduce the curing shrinkage rate of the resin matrix, and improve the overall dimensional stability of the product.

[0004] However, conventional glass fiber reinforced cyanate ester-bismaleimide composites still have significant shortcomings. While using conventional E glass fiber to reinforce CE-BMI can improve mechanical properties, the high dielectric constant and dielectric loss of E glass fiber itself, when introduced into the system, increase the overall dielectric constant and high-frequency dielectric loss of the composite, compromising the excellent low-dielectric properties of the CE-BMI resin matrix. Even with low-dielectric glass fibers (such as patent CN102976620A), their dielectric properties are still inferior to those of a pure resin matrix, and the interfacial bonding between the fiber and the resin matrix is ​​limited, making them prone to interfacial debonding under external loads. This results in limited improvement in material toughness and insufficient fatigue performance and resistance to damp heat aging. Furthermore, conventional glass fibers have a relatively high density, which is unfavorable for the fabrication of lightweight components; their poor matching of thermal expansion coefficients with the resin matrix at high temperatures makes them prone to microcracks at the interface during thermal cycling, limiting long-term service reliability. Summary of the Invention

[0005] To address the aforementioned technical shortcomings, this invention involves twisting glass fiber filaments, followed by sizing and surface modification to obtain a low-dielectric glass fiber cloth. This cloth is then impregnated with a composite material impregnation solution modified with cyanate ester resin as the main matrix and bismaleimide, and finally cured by hot pressing to obtain a low-dielectric cyanate ester-based composite material. The twisting process ensures a regular arrangement of the monofilaments, reducing interfacial polarization within the yarn bundle and solving the defects of loose yarn bundles, severe interfacial polarization, and high dielectric constant and loss. The resulting fiber cloth exhibits a dielectric constant ≤4.2 and a dielectric loss ≤0.009 at 1MHz. The resin compounding system further reduces the overall dielectric parameters of the composite material while improving heat distortion temperature, peel strength, and dimensional stability, making it suitable for high-end applications such as high-frequency communication PCBs, high-speed server substrates, and automotive RF circuit boards.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a method for preparing a low-dielectric cyanate-based composite material, comprising the following steps: S1 Preparation of low dielectric twisted glass fiber yarn: Select glass fiber filaments with a single filament diameter of 5-7 μm and put them into a twisting machine for twisting treatment. The twist is 30-45 twists / m to obtain low dielectric twisted glass fiber yarn. S2 Special Sizing Material Preparation and Sizing: PVA-based sizing material containing quaternary ammonium salt softener is prepared and applied to the warp yarns through initial sizing after drawing and subsequent re-sizing after warping. The yarns are then dried and separated to make the weaving beam. S3 Weaving and pretreatment of greige fabric: Plain weaving of fiber greige fabric is carried out using an air-jet loom, followed by first-stage high-temperature pre-desizing and long-term burning depth desizing to obtain fiber greige fabric with residual sizing ≤0.07%; S4 Surface Modified Fiber Opening: The fiber opening is achieved by impregnation with coupling agent solution and drying to obtain low dielectric glass fiber cloth; S5 Composite Material Impregnation Solution Preparation: The composite material impregnation solution is prepared by using cyanate ester resin as the main matrix, bismaleimide as the modifying component, and adding additives, low dielectric inorganic fillers and organic solvents. S6 Prepreg and Hot Press Composite: The low dielectric glass fiber cloth obtained in S4 is impregnated with the composite material impregnation liquid of S5 to make a semi-cured sheet. The multi-layer semi-cured sheets are stacked and hot-pressed to obtain a low dielectric cyanate ester-based composite material.

[0007] For step S1, the twisting process makes the monofilaments more regular, reduces the polarization of the air interface inside the yarn bundle, and solves the defects of loose yarn bundle, severe interface polarization, and high dielectric constant and loss. The glass fiber can be a commonly used glass fiber in the field, such as type A glass fiber, type C glass fiber, type D glass fiber, type E glass fiber, type S glass fiber, etc. In order to prepare a low dielectric composite material, type D glass fiber is preferred. More preferably, the glass fiber precursor comprises 60.4–65 wt% SiO2, 10–14 wt% Al2O3, 22–26 wt% B2O3, and 0.5–2 wt% Li2O, with a total trace impurity content ≤2 wt%. Specifically, this invention not only uses twisting treatment to eliminate interfacial polarization and reduce dielectric constant and dielectric loss, but also optimizes the twisting process by using 30 to 45 twists / m for moderate twisting. While ensuring effective reduction of dielectric constant and dielectric loss, it also ensures that the glass fiber yarn has excellent mechanical properties; preferably, the twist is 35 to 40 twists / m.

[0008] For step S2, the present invention uses initial sizing and subsequent sizing after warping. The two sizing processes ensure that the yarn is fully wetted, effectively remove dust and other impurities from the yarn surface, ensure the yarn surface is clean, reduce yarn hairiness, and obtain a good adhesion effect. Preferably, the PVA-based slurry comprises, by mass percentage: 5-10% PVA, 0.5-1% quaternary ammonium salt softener, and the remainder being deionized water; the preparation method of the PVA-based slurry is as follows: after adding PVA to deionized water, heat to 85-95°C and stir until completely dissolved, then add quaternary ammonium salt softener, stir for 10-30 minutes until uniform, and then keep warm for 20-40 minutes for later use; The PVA used can be of commonly used types in this field, such as PVA1788, PVA0588, and PVA2488. Adding a quaternary ammonium salt softener to PVA can further wet the yarn, causing the yarn hairs to adhere tightly to the yarn core, reducing the increase in air caused by the excessive hair growth, which in turn increases the dielectric constant and dielectric loss. The quaternary ammonium salt softener can be a commonly used quaternary ammonium salt softener in the art. Preferably, the quaternary ammonium salt softener is an ester-based quaternary ammonium salt softener, specifically a triethanolamine stearate quaternary ammonium salt.

[0009] For step S3, the present invention first weaves the greige fabric, and then uses two pre-desizing processes to effectively remove organic matter, so that the residual sizing of the greige fabric is ≤0.07%; Preferably, the first-stage high-temperature pre-desizing involves high-temperature treatment at 380–420°C for 10–20 minutes to remove 92–96% of the pulp, and the long-term sintering depth desizing involves sintering at 320–360°C for 40–60 minutes to remove residual organic matter until the residual pulp is ≤0.07%. Preferably, the weaving density is 40-50 threads / cm. 2 .

[0010] For step S4, the coupling agent solution is used for impregnation, which can effectively improve the surface bonding between the fiber cloth and the impregnating resin. Preferably, the coupling agent solution is a coupling agent solution with a mass percentage of 0.5 to 1.0 wt%. The coupling agent is selected from one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents. Specifically, silane coupling agents can be KH550, KH560, KH570, etc., titanate coupling agents can be GR-300, GR-101, GR-102, GR-105, etc., and aluminate coupling agents can be GR-AL18, etc. The dipping time is 2 to 5 minutes, and the drying temperature for drying and opening the fibers is 120 to 150°C.

[0011] For step S5, a composite impregnation solution is prepared using cyanate ester resin as the main matrix and bismaleimide as the modifying component. This ensures that the composite material has low dielectric properties and excellent mechanical properties. At the same time, bismaleimide as a modifying component can improve thermal stability. In order to improve the performance of the composite material, other additives and fillers can also be added. For example, to increase the curing rate, a curing accelerator can be added; to increase the toughness and processing window of the composite resin, diallyl bisphenol A can be added; and to reduce the dielectric constant, spherical low-dielectric silica powder can be added. Specifically, the composite material impregnation solution comprises, by weight, 80-120 parts of cyanate ester, 20-60 parts of bismaleimide, 5-25 parts of diallyl bisphenol A, 0.1-2 parts of organometallic curing catalyst, 30-80 parts of spherical low-dielectric silicon micropowder, 0.2-1 parts of coupling agent, and an appropriate amount of organic solvent. The cyanate ester can be any type of cyanate commonly used in the field, specifically bisphenol A cyanate ester, tetramethylbisphenol F cyanate ester, dicyclopentadiene bisphenol cyanate ester, bisphenol M cyanate ester, bisphenol E cyanate ester, etc.; the organometallic curing catalyst can be an acetylacetone metal chelate salt, naphthenate, isooctanoate, and organotin compounds, etc., where the acetylacetone metal chelate salt can be cobalt acetylacetone, copper acetylacetone, zinc acetylacetone, manganese acetylacetone, etc., the naphthenate can be cobalt naphthenate, zinc naphthenate, copper naphthenate, manganese naphthenate, etc., and the isooctanoate can be zinc isooctanoate, cobalt isooctanoate, isooctanoic acid, etc. Manganese, etc., and organotin compounds such as dibutyltin dilaurate and dibutyltin dioctanoate can be used; coupling agents can be one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents. Specifically, silane coupling agents can be KH550, KH560, KH570, etc., titanate coupling agents can be GR-300, GR-101, GR-102, GR-105, etc., and aluminate coupling agents can be GR-AL18, etc.; organic solvents can be commonly used in this field, such as acetone and methyl ethyl ketone; the solid content of the composite material impregnation solution is 50-70%.

[0012] For step S6, glass fiber cloth is pre-impregnated to form a semi-cured sheet, and then multiple layers of semi-cured sheets are stacked and hot-pressed to form a composite material. Preferably, the content of the matrix resin in the prepreg is 45-55 wt%, and the content of the low dielectric glass fiber cloth is 45-55 wt%; the number of layers in the prepreg is 5-10 layers, and the hot pressing curing is performed by first pre-pressing at 150-180℃ for 20-30 min at 3.0-5.0 MPa, and then curing at 190-210℃ for 90-150 min.

[0013] Secondly, the present invention provides a low-dielectric cyanate-based composite material, which is prepared by any of the above preparation methods, wherein the composite material impregnation solution in step S5 has a dielectric constant ≤3.8 at 1MHz and a thermal decomposition temperature Td5% ≥410℃; the composite material obtained in step S6 has a dielectric constant Dk ≤4.0 at 1MHz, a dielectric loss Df ≤0.005, a peel strength ≥1.3N / mm, a Z-axis thermal expansion coefficient ≤22ppm / ℃, and a UL94 flame retardant V-0 rating.

[0014] Thirdly, the present invention provides an application of a low-dielectric cyanate-based composite material, which is used in 5G / 6G high-frequency printed circuit boards, high-speed computing substrates, automotive radio frequency copper-clad laminates, and high-end electronic packaging substrates.

[0015] Compared with the prior art, the present invention has the following technical effects: 1. This invention improves dielectric properties from the root by using twisting treatment, reducing dielectric constant and dielectric loss. Twisting treatment makes the monofilament arrangement regular, reduces the polarization of the air interface inside the yarn bundle, and solves the defects of loose yarn bundle, severe interface polarization, and high dielectric constant and loss. Using 30 to 45 twists / m for moderate twisting, while ensuring effective reduction of dielectric constant and dielectric loss, it can also ensure that the glass fiber yarn has excellent mechanical properties. Compared with the use of 20 twists / m ultra-low twist yarn, the fiber cloth Dk is reduced by 0.4 to 0.7 and Df is reduced by more than 30% at 1MHz, solving the pain point of high high frequency loss of ultra-low twist glass fiber; 2. This invention utilizes the synergistic effect of matching sizing agents and segmented desizing and fiber opening, employing two sizing processes to reduce weaving fuzz and defects per 100 meters by 40%. After removing residual sizing base through two-stage high-temperature desizing, the fabric surface is uniform after surface modification and fiber opening, resin impregnation efficiency is significantly improved, and the composite material is free from delamination and void defects. 3. Using cyanate ester as the main matrix and bismaleimide as the modifying component solves the problems of poor toughness and slow curing of pure cyanate ester and narrow processing window of pure bismaleimide. The two are combined to form an interpenetrating cross-linked network. The resin matrix Dk ≤ 3.8 at 1MHz, the 5% thermal weight loss ≥ 410℃, and the peel strength is improved by 15%, taking into account low dielectric, high heat resistance, and high toughness. 4. The product of this invention has excellent comprehensive performance. The finished composite material has Dk≤4.0 and Df≤0.005 at 1MHz; Z-CTE≤22ppm / ℃; no delamination or bubbling when immersed in tin at 260℃; UL94 V-0; and meets the stringent requirements of high-frequency and high-speed PCBs. 5. The invention has strong process compatibility and can be adapted to existing glass fiber twisting, sizing, weaving and hot pressing equipment. It does not require large-scale production line modification, the increase in mass production costs is low, and it is suitable for large-scale industrial production. Attached Figure Description

[0016] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below.

[0017] Figure 1 The low-dielectric glass fiber cloth obtained in S4 of Example 1; Figure 2 This is a super-depth-of-field photograph of the composite material obtained in S6 of Example 1; Figure 3 The dielectric constant of the glass fiber cloth obtained in S4 of Examples 4-5 and Comparative Example 2; Figure 4 The dielectric loss of the glass fiber cloth obtained in S4 of Examples 4-5 and Comparative Example 2; Figure 5 This is a super depth-of-field photograph of the low dielectric twisted glass fiber yarn obtained in Comparative Example 2, S1. Figure 6 This is a super depth-of-field photograph of the low dielectric twisted glass fiber yarn obtained in S1 of Example 4; Figure 7 This is a super depth-of-field photograph of the low dielectric twisted glass fiber yarn obtained in S1 of Example 5. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0019] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.

[0021] All raw materials used in this invention were purchased from the market.

[0022] Example 1: A method for preparing a low-dielectric cyanate-based composite material includes the following steps: Preparation of S1 low dielectric twisted glass fiber yarn: Select glass fiber precursors with a composition of 62% SiO2, 12.3% Al2O3, 24.2% B2O3, 1% Li2O, and the balance being impurities, and put them into a twisting machine for twisting treatment with a twist of 35 twists / m to obtain low dielectric twisted glass fiber yarn; S2 Special Sizing Material Preparation and Sizing: Add 70 parts by weight of PVA1788 to 922 parts by weight of deionized water, heat to 90℃ and stir until completely dissolved, then add 8 parts by weight of triethanolamine stearate quaternary ammonium salt, stir for 20 minutes until uniform, and then keep warm for 30 minutes for later use; then perform initial sizing on the warp yarns after drawing and re-sizing after warping, dry and separate the yarns to make the weaving beam; S3 Weaving and Pre-treatment of Greige Fabric: The greige fabric is woven in plain weave using an air-jet loom (2116) with a weaving density of 48 threads / cm. 2 The fiber fabric was subjected to a first-stage high-temperature pre-desizing treatment at 400℃ for 15 minutes, followed by a long-term burning desizing treatment at 340℃ for 50 minutes, to obtain a fiber fabric with 0.05% residual sizing material. S4 surface-modified fiber opening: The fiber is opened by immersion in 0.8wt% KH550 aqueous solution for 3 min and then dried at 135℃ to obtain low dielectric glass fiber cloth. S5 Composite Material Impregnation Solution Preparation: 100 parts by weight of bisphenol A cyanate, 35 parts by weight of bismaleimide, 12 parts by weight of diallyl bisphenol A, 0.8 parts by weight of zinc naphthenate, 50 parts by weight of spherical low-dielectric silicon micro powder, and 0.5 parts by weight of KH550 are compounded and then butanone is added to obtain a composite material impregnation solution with a solid content of 65%. S6 Prepreg and Hot-Pressure Composite: The low-dielectric glass fiber cloth obtained in S4 is impregnated with the composite material impregnation liquid of S5 to make a semi-cured sheet with a composite material content of 50%. Six layers of semi-cured sheets are stacked and pre-pressed at 160℃ for 30 min under a pressure of 4 MPa, and then cured at 200℃ for 120 min to obtain a low-dielectric cyanate ester-based composite material.

[0023] Example 2: The difference from Example 1 is that the twist in S1 is 30 twists / m, the slurry in S2 is 70 parts by weight of PVA0588, 6 parts by weight of triethanolamine stearate quaternary ammonium salt, and 924 parts by weight of deionized water, and the cyanate ester resin in S5 is 90 parts by weight of bisphenol M cyanate ester, and the bismaleimide is adjusted to 45 parts by weight, while the others remain unchanged.

[0024] Example 3: The difference from Example 1 is that the twist in S1 is 40 twists / m, the sizing agent in S2 is 70 parts by mass of PVA2488, 10 parts by mass of triethanolamine stearate quaternary ammonium salt, and 920 parts by mass of deionized water, in S3 a first-stage high-temperature pre-desizing treatment at 390°C for 12 min followed by a long-term smoldering desizing treatment at 330°C for 60 min is performed to obtain a fiber fabric with 0.04% residual sizing agent, and in S6 the composite material content in the semi-cured sheet is 55%, while the others remain unchanged.

[0025] Comparative Example 1: The difference from Example 1 is that the twist in S1 is 20 twists / m, and no triethanolamine stearate quaternary ammonium salt is added in S2.

[0026] Performance testing: The test content and standards were as follows: The dielectric properties of the glass fiber cloth obtained in S4 and the composite material containing glass fiber cloth obtained in S6 of each embodiment and comparative example were tested according to ASTM D150; the peel strength of the final composite material obtained in each embodiment and comparative example to the copper plate was tested according to IPC-TM-650; the thermal weight loss (TG), Z-axis thermal expansion (TMA), and flame retardancy (UL94) of the final composite material obtained in each embodiment and comparative example were tested; and the resin penetration time was calculated using the chronometry method. The test results are as follows: Table 1: Composite material performance data for each example and comparative example:

[0027] from Figure 1 As can be seen from the present invention, the fiber cohesion of the glass fiber cloth is high, the warp and weft yarns are evenly arranged, the mesh pore distribution is consistent, there are no obvious local yarn breaks or yarn agglomeration defects, the overall flatness of the fabric is high, and the surface of the fiber cloth has evenly distributed micro gaps, which facilitates subsequent resin impregnation.

[0028] from Figure 2 As can be seen from the present invention, the glass fibers in the final composite material are arranged regularly, fully impregnated, and have an excellent product appearance.

[0029] As can be seen from the data in the table above, both the glass fiber cloth and the final composite material of Examples 1-3 of the present invention have low dielectric constant and low dielectric loss. Compared with Comparative Example 1, the dielectric properties are superior. At the same time, the peel strength and weight loss temperature of the examples are higher, the Z-axis thermal expansion coefficient is lower, the flame retardant grade is higher, and the resin penetration time is shorter.

[0030] Example 4: The difference from Example 1 is that the twist in S1 is 30 twists / m, while the others remain unchanged.

[0031] Example 5: The difference from Example 1 is that the twist in S1 is 40 twists / m, while the others remain unchanged.

[0032] Comparative Example 2: The difference from Example 1 is that the twist in S1 is 20 twists / m, while the others remain unchanged.

[0033] The dielectric properties of the glass fiber cloth obtained in Examples 4-5 and Comparative Example 2 (S4 and S6) were tested according to ASTM D150, and the glass fiber cloth-containing composite materials were observed using ultra-depth-of-field observation. The results are as follows: Figure 3-7 As shown.

[0034] from Figure 3-4It can be seen that the twist (30 twists / m and 40 twists / m) of the present invention, compared with the ultra-low twist (20 twists / m), has a lower dielectric constant and dielectric loss at different frequencies. Figure 5-7 It can be seen that the glass fiber yarns with 30 twists / m and 40 twists / m are more densely arranged than the glass fiber yarns with 20 twists / m, with smaller gaps between fibers and fewer fly feathers.

[0035] In summary, the composite material obtained by this invention has excellent dielectric properties, heat resistance, dimensional stability, and wettability, meeting the requirements of various applications such as 5G / 6G high-frequency printed circuit boards, high-speed computing substrates, automotive RF copper-clad laminates, and high-end electronic packaging substrates.

[0036] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a low-dielectric cyanate-based composite material, characterized in that, Includes the following steps: S1 Preparation of low dielectric twisted glass fiber yarn: Select glass fiber filaments with a single filament diameter of 5-7 μm and put them into a twisting machine for twisting treatment. The twist is 30-45 twists / m to obtain low dielectric twisted glass fiber yarn. S2 Special Sizing Material Preparation and Sizing: PVA-based sizing material containing quaternary ammonium salt softener is prepared and applied to the warp yarns through initial sizing after drawing and subsequent re-sizing after warping. The yarns are then dried and separated to make the warp beam. S3 Weaving and pretreatment of greige fabric: Plain weaving of fiber greige fabric is carried out using an air-jet loom, followed by first-stage high-temperature pre-desizing and long-term burning depth desizing to obtain fiber greige fabric with residual sizing ≤0.07%; S4 Surface Modified Fiber Opening: The fiber opening is achieved by impregnation with coupling agent solution and drying to obtain low dielectric glass fiber cloth; S5 Composite Material Impregnation Solution Preparation: The composite material impregnation solution is prepared by using cyanate ester resin as the main matrix, bismaleimide as the modifying component, and adding additives, low dielectric inorganic fillers and organic solvents. S6 Prepreg and Hot Press Composite: The low dielectric glass fiber cloth obtained in S4 is impregnated with the composite material impregnation liquid of S5 to make a semi-cured sheet. The multi-layer semi-cured sheets are stacked and hot-pressed to obtain a low dielectric cyanate ester-based composite material.

2. The preparation method according to claim 1, characterized in that, The glass fiber precursor in S1 comprises SiO2 60.4-65wt%, Al2O3 10-14wt%, B2O3 22-26wt%, Li2O 0.5-2wt%, and trace impurities ≤2wt%; the twist is 35-40 twists / m.

3. The preparation method according to claim 1, characterized in that, The PVA-based slurry described in S2 comprises, by mass percentage: 5-10% PVA, 0.5-1% quaternary ammonium salt softener, and the remainder being deionized water. The preparation method of the PVA-based slurry is as follows: after adding PVA to deionized water, heat the mixture to 85-95℃ and stir until completely dissolved. Then, add the quaternary ammonium salt softener and stir for 10-30 minutes until homogeneous. Afterward, keep the mixture warm for 20-40 minutes for later use.

4. The preparation method according to claim 1, characterized in that, The first-stage high-temperature pre-desizing in S3 refers to high-temperature treatment at 380-420℃ for 10-20 minutes, and the long-term smoldering depth desizing refers to smoldering at 320-360℃ for 40-60 minutes to remove residual organic matter.

5. The preparation method according to claim 1, characterized in that, The coupling agent solution in S4 is a coupling agent solution with a mass percentage of 0.5 to 1.0 wt%, wherein the coupling agent is selected from one or more of silane coupling agents, titanate coupling agents, and aluminate coupling agents.

6. The preparation method according to claim 1, characterized in that, The composite material impregnation solution in S5 includes, by weight, 80-120 parts of cyanate ester, 20-60 parts of bismaleimide, 5-25 parts of diallyl bisphenol A, 0.1-2 parts of organometallic curing catalyst, 30-80 parts of spherical low-dielectric silicon micropowder, 0.2-1 parts of coupling agent, and an appropriate amount of organic solvent.

7. The preparation method according to claim 1, characterized in that, The semi-cured sheet in S6 contains 45-55 wt% matrix resin and 45-55 wt% low dielectric fiber cloth; the hot-press curing is performed by first pre-pressing at 150-180℃ for 20-30 min at 3.0-5.0 MPa, and then curing at 190-210℃ for 90-150 min.

8. A low-dielectric cyanate-based composite material, characterized in that, The composite material is prepared by the preparation method described in any one of claims 1-7. The composite material has a dielectric constant Dk≤4.0 and a dielectric loss Df≤0.005 at 1MHz; a peel strength ≥1.3N / mm; a Z-axis thermal expansion coefficient ≤22ppm / ℃; and a UL94 flame retardant V-0 rating.

9. The use of the low-dielectric cyanate-based composite material according to claim 8, characterized in that, The composite material is used in 5G / 6G high-frequency printed circuit boards, high-speed computing substrates, automotive RF copper-clad laminates, and high-end electronic packaging substrates.

Citation Information

Patent Citations

  • Composition for preparing glass fibers and low-dielectric constant glass fibers thereof