Lightweight material for humanoid robots and method for manufacturing the same
By using a gradient material system and integrated molding process, the mechanical requirements of different parts of the humanoid robot were addressed, achieving lightweight and high-strength material design, and improving the robot's performance and lifespan.
Patent Information
- Application Number
- CN202611493478.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies struggle to precisely design for the varying strength, stiffness, and toughness requirements of different parts of a humanoid robot, and the interfacial compatibility and integrated design issues between high-performance PEEK and lightweight, high-strength magnesium alloys and carbon fiber composites have not been effectively resolved.
A gradient material system is adopted, including an outer continuous carbon fiber reinforced polyether ether ketone composite, a middle short-cut carbon fiber reinforced polyether ether ketone composite, and an inner toughened modified polyether ether ketone and foamed magnesium alloy composite structure. Integrated co-curing molding is achieved through automated fiber laying and autoclave molding processes.
The design achieves multi-scale, multi-material collaborative design for various parts of the humanoid robot, improving material utilization efficiency and structural load-bearing efficiency, reducing overall weight, and enhancing interface bonding strength and structural stability.
Abstract
Description
Technical Field
[0001] This invention relates to the field of structural materials technology for humanoid robots, and more specifically, to a lightweight material for humanoid robots and a method for preparing the same. Background Technology
[0002] Humanoid robots, with their humanoid appearance and movement characteristics, are considered an important carrier for next-generation intelligent terminals. However, one of the key bottlenecks currently restricting their large-scale application and performance leap is their excessive weight. Traditional humanoid robot structural components mostly use metal materials such as aluminum alloys and steel, resulting in a generally heavy overall weight, which leads to a series of chain problems: First, high energy consumption, as the large mass leads to a surge in the power demand of the drive motor, resulting in low energy utilization and seriously affecting the endurance; second, sluggish motion response, as the large inertia slows down the robot's start-up, stopping, and posture adjustment response speed, greatly reducing dynamic stability and flexibility; third, a prominent contradiction between material utilization and cost, with excessively heavy structural components designed to meet local strength requirements increasing material costs and processing difficulty.
[0003] To address the aforementioned issues, researchers have attempted to incorporate high-performance engineering plastics and composites into robot structures. For example, polyetheretherketone (PEEK) has attracted attention due to its excellent specific strength and heat resistance. However, existing technologies are largely limited to preparing single-PEEK-based composites through injection molding. While partial fiber reinforcement has been achieved through methods such as vibration injection molding, it suffers from significant drawbacks:
[0004] While the material properties prepared by this technology are improved in terms of isotropy, it cannot be precisely designed according to the different requirements of strength, stiffness and toughness of different parts of the robot such as torso, limbs and joints, and may instead increase unnecessary weight.
[0005] Injection molding is suitable for complex small-sized parts, but for large-sized, thin-walled robot shells and skeletons, the mold cost is high, the internal stress of the product is large, and the fiber orientation is difficult to control in multiple dimensions.
[0006] Existing technologies have failed to solve the interfacial compatibility and integrated integration problems between high-performance PEEK and lightweight, high-strength magnesium alloys and carbon fiber composites. Summary of the Invention
[0007] To overcome the above-mentioned defects of the prior art, embodiments of the present invention provide a lightweight material for humanoid robots and a method for preparing the same.
[0008] To achieve the above objectives, the present invention provides the following technical solution: a lightweight material for humanoid robots, which adopts a gradient material system. The material is composed of at least three functional layers in a gradient composite, and according to their distribution position in the humanoid robot structural components, it includes, from the outside to the inside or from the main load-bearing area to the secondary load-bearing area, the following:
[0009] Outer / Main Load-Bearing Layer: This is a continuous carbon fiber reinforced polyetheretherketone composite layer, wherein the volume fraction of the continuous carbon fiber is 45% to 65%. This layer provides the main stiffness and strength of the structural component.
[0010] Intermediate / Transitional Connecting Layer: This is a layer of short-cut carbon fiber reinforced polyetheretherketone composite material, wherein the mass fraction of the short-cut carbon fiber is 20% to 40%. This layer is used to connect the outer layer and the inner layer, buffer sudden stress changes, and has good molding fluidity.
[0011] Inner / Lightweight Core Layer: A composite structural layer of toughened modified polyether ether ketone and foamed magnesium alloy or magnesium-lithium alloy, wherein the porosity of the foamed metal is 50% to 75% and the pore size is 0.5 to 3 mm. This layer achieves a significant lightweight effect and absorbs impact energy.
[0012] The outer layer, middle layer and inner layer are integrated and co-cured through one or more of the following processes: autoclave molding, resin transfer molding or vacuum-assisted resin infusion, to form an integrated material-structure-function gradient component without adhesive layers.
[0013] In a preferred embodiment, the carbon fiber in the outer continuous carbon fiber reinforced polyetheretherketone composite material layer is one or more of T300, T700 or T800 grade, and the fiber morphology is unidirectional tape or fabric; the polyetheretherketone resin is an injection molding or prepreg grade resin with a crystallinity ≥35% and a melt flow rate of 8-25 g / 10 min (380℃ / 5 kg).
[0014] In a preferred embodiment, the chopped carbon fiber reinforced polyetheretherketone (PEEK) composite material in the intermediate layer has chopped carbon fibers with a length of 0.2–1 mm and a diameter of 5–15 μm, and the fiber surface is oxidized or sized to enhance the interfacial bonding strength with the PEEK matrix; the SCF / PEEK composite material is subjected to a shear rate of 1000 s at 380 °C. -1 The melt viscosity is 150–300 Pa·s.
[0015] In a preferred embodiment, in the composite structure layer of the inner toughened modified PEEK and foamed magnesium alloy, the foamed magnesium alloy is one of the AZ31, AZ91 or WE43 series magnesium alloys, with an open or closed pore structure and a pore wall thickness of 0.1 to 0.5 mm; the toughened modified PEEK is a blend of PEEK and thermotropic liquid crystal polymer (TLCP) or polyetherimide (PEI), wherein the mass fraction of TLCP or PEI is 5% to 15%.
[0016] The present invention also includes a method for preparing a lightweight material for humanoid robots, comprising an automated fiber laying preform forming step, a mold assembly and encapsulation step, a gradient resin infusion and curing step, and a demolding and post-processing step.
[0017] In the automated fiber laying preform forming step, continuous carbon fiber prepreg tape is laid on a laying mold at multiple angles such as 0°, ±45°, and 90° according to the three-dimensional digital model of the structural component using AFP equipment to form a preform with outer and middle layers. Infrared heating is applied during the laying process to maintain the interlayer temperature of the prepreg tape at 280-350°C, the compaction pressure at 200-600N, and the laying head traveling speed at 5-20m / min.
[0018] In the mold assembly and packaging steps, the AFP-molded CF / PEEK outer preform, the middle layer SCF / PEEK prepreg or premix, and the inner layer foam magnesium alloy core are assembled in an integrated molding mold according to the design position. Vacuum bags or rigid molds are used for packaging, the vacuum is drawn to below -0.095MPa, and resin flow channels and overflow ports are set.
[0019] In the gradient resin infusion and curing step, an autoclave molding process is adopted. Under vacuum assistance, molten PEEK resin or low-viscosity PEEK prepolymer is sequentially injected from multiple injection ports of the mold. The injection pressure is 0.3-1.5 MPa, and the injection temperature is 360-390°C. During the injection process, the gradient resin impregnation from the outer layer to the inner layer is achieved by controlling the opening and closing sequence of different injection ports. Subsequently, curing is carried out in an autoclave at a curing pressure of 0.6-2.0 MPa and a curing temperature of 380-400°C. The holding time is 1-4 hours, and finally, the material is cooled to room temperature for demolding.
[0020] The technical effects and advantages of this invention are as follows:
[0021] 1. This invention achieves multi-scale, multi-material collaborative design for the mechanical requirements of different parts of a humanoid robot by constructing a gradient material system. The outer layer provides high strength and high stiffness to resist bending and torsion, the middle layer serves as a transition to effectively alleviate interface stress concentration and improve molding processability, and the inner layer of lightweight foam metal core material achieves significant weight reduction and energy absorption, overcoming the over-design problem caused by the isotropic or homogeneous properties of a single PEEK composite material.
[0022] 2. This invention introduces an integrated process of automated fiber placement and autoclave molding, and optimizes the gradient resin infusion sequence. The AFP technology can precisely control the placement angle and path of continuous carbon fibers on a three-dimensional curved surface, realizing the optimized layout of fiber orientation in complex structural components, which greatly improves the material utilization efficiency and structural load-bearing efficiency. Combined with the high temperature and high pressure of the autoclave and the zoned infusion technology, it realizes the chemical co-curing of different gradient layers without adhesives, resulting in high interfacial bonding strength and good overall structural stability.
[0023] 3. The PEEK resin matrix selected in this invention has excellent chemical compatibility and thermophysical property matching with the magnesium alloy core material. By introducing TLCP or PEI toughening components into PEEK, the interfacial wettability and toughness between the inner resin and the foam metal are effectively improved. At the same time, the processing temperature window matches the operating temperature range of the magnesium alloy, avoiding the performance degradation of the magnesium alloy core material during high-temperature molding and ensuring the long-term service reliability of the composite component. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0025] Material preparation and pretreatment
[0026] 1. PEEK resin: Use imported or domestic polyether ether ketone (PEEK) powder or granules with a melt index of 15g / 10min (380℃ / 5kg), glass transition temperature (Tg) of 143℃, and melting temperature (Tm) of 343℃. Dry in a vacuum oven at 150℃ for 4 hours before use.
[0027] 2. Continuous carbon fiber: T700 grade (12K) carbon fiber is selected, with tensile strength ≥4900MPa and modulus ≥230GPa. It adopts a special prepreg form treated with sizing agent, and the resin content is 32%~38%.
[0028] 3. Short-cut carbon fiber: T300 grade short-cut carbon fiber with a length of 0.5 mm and a diameter of 7 μm is selected. Before use, it is oxidized in air at 400℃ for 1 hour to increase the oxygen-containing functional groups on the surface.
[0029] 4. Foamed magnesium alloy: AZ31B foamed magnesium alloy board is selected, with a porosity of 65%, an average pore diameter of 1.5mm, and a thickness of 5-15mm depending on the component design. It is subjected to alkaline washing and acid washing activation treatment before use.
[0030] 5. Toughening modifier: Thermotropic liquid crystal polymer (TLCP) or polyetherimide (PEI) powder, purity ≥98%, used after drying.
[0031] Example 1: Lightweight gradient material for the lower leg component of a humanoid robot
[0032] This embodiment prepares a lightweight gradient material for the lower leg (main load-bearing tubular structure) of a humanoid robot.
[0033] S1. Gradient Structure Design: Design a three-layer structure from the outside in:
[0034] The outer layer is 2mm thick and is a continuous CF / PEEK (T700 / PEEK) unidirectional tape.
[0035] The intermediate layer is 3mm thick and is a short-cut CF / PEEK (SCF content 30wt%) composite material.
[0036] The inner core material is 10mm thick and is made of foamed magnesium alloy, with some of its pores filled with toughened PEEK (containing 10wt% TLCP).
[0037] S2. AFP Precast Molding: Automated fiber layup (AFP) equipment (equipped with an infrared heater and compaction rollers) is used. Based on the three-dimensional curved surface model of the lower leg component, continuous carbon fiber prepreg tape is laid on a steel laying mold. The laying angle alternates between 0° (along the component axis), ±45°, and 90°, with 16 layers laid. The laying head travel speed is 10 m / min, the infrared heating temperature is set to 320℃, and the compaction roller pressure is 400 N. After laying, an outer layer and part of the intermediate layer precast structure are formed.
[0038] S3. Mold Assembly and Packaging: The AFP preform, pre-impregnated chopped CF / PEEK sheet (intermediate layer), and surface-treated and fixed-position magnesium alloy foam core are sequentially assembled into the modular metal mold. After mold closing, a vacuum sealing ring is placed around the mold, and a vacuum pump is connected to evacuate to -0.098 MPa, then the airtightness is checked. The mold has multiple injection ports, corresponding to the resin injection channels for the outer, intermediate, and inner layers, respectively.
[0039] S4. Gradient Resin Injection and Autoclave Curing: The sealed mold is placed into the autoclave. First, PEEK resin is melted at 380℃ and injected into the corresponding outer layer injection port through the pressure vessel at 0.8MPa for 10 minutes to fully impregnate the continuous fibers of the outer layer. Then, the outer layer injection port is closed, and the middle layer injection port is opened to inject a PEEK molten mixture (viscosity adjusted) mixed with chopped fibers. The injection pressure is increased to 1.2MPa and held for 15 minutes. Finally, the inner layer injection port is opened to inject a molten PEEK / TLCP blend (TLCP content 10%), allowing it to penetrate some of the pores of the foamed magnesium alloy. The injection pressure is 0.5MPa and held for 20 minutes. After injection, the autoclave is heated to 390℃ and pressurized to 1.5MPa, and cured under heat and pressure for 2.5 hours. Then, it is cooled to room temperature at a rate of 2℃ / min, and demolded to obtain the leg component blank.
[0040] S5. Post-processing: The blank is deburred, polished, and subjected to fluorescent penetrant non-destructive testing to obtain the final lightweight lower leg component.
[0041] The performance of the component prepared in this embodiment was tested: the density was 1.65 g / cm³, the axial tensile strength was 850 MPa, the bending modulus was 62 GPa, the weight was reduced by 38% compared with the aluminum alloy (6061-T6) component of the same size, and the first natural frequency was increased by 22% through modal analysis.
[0042] Example 2: Lightweight gradient material for the torso frame of a humanoid robot
[0043] Unlike Example 1, this example prepares a flat, thin-walled, large-area torso shell structure.
[0044] The outer CF / PEEK layer uses plain weave prepreg with a layup angle of 0° / 90° orthogonal. During layup, AFP is used in conjunction with a cutting device to stack the sheets.
[0045] The intermediate SCF / PEEK layer contains 25 wt% short-cut fibers and 5 wt% carbon nanotubes to improve conductivity.
[0046] The inner layer of foamed magnesium alloy has been changed to the WE43 series with a porosity of 70%, and a heat-conducting copper tube has been pre-embedded to facilitate heat management.
[0047] The resin infusion process adopts the vacuum-assisted resin infusion (VARI) process, which uses the vacuum pressure difference to drive the resin flow. The curing regime is adjusted to be: heat preservation at 385℃ for 3 hours and pressure of 1.0MPa.
[0048] The final torso component had a surface density reduced to 4.2 kg / m², and an overall bending stiffness of 2.1 × 10⁻⁶. 6N·m², which is 42% lighter than aluminum alloy.
[0049] Example 3: Lightweight gradient material for humanoid robot joint connectors
[0050] Unlike Example 1, this example adapts and adjusts the gradient structure to accommodate complex forces (multi-axis torsion and impact) at the joints.
[0051] The outer CF / PEEK layer is locally thickened in critical stress areas (such as around bolt holes) and reinforced with circumferential fiber winding via AFP.
[0052] 10wt% of molybdenum disulfide (MoS2) solid lubricant is added to the intermediate SCF / PEEK layer to reduce the coefficient of friction during relative joint movement.
[0053] The inner layer of magnesium alloy foam is not filled with PEEK, retaining an open pore structure for storing grease or serving as a channel for cooling medium.
[0054] During autoclave curing, a segmented curing process is adopted: first, pre-curing at 360℃ for 1 hour, and then heating to 395℃ for high-temperature curing for 1.5 hours to optimize the bonding between the resin and the metal interface.
[0055] The resulting joint connectors achieved a 35% weight reduction while maintaining a tensile strength of ≥700MPa, and their lifespan exceeded 2 million cycles in simulated swing fatigue tests.
[0056] Performance comparison test
[0057] The present invention conducted systematic mechanical property tests on the lightweight gradient material components prepared in Examples 1-3, and set up comparative examples.
[0058] Comparative Example 1
[0059] Homogeneous standard specimens of 30wt% short-cut carbon fiber reinforced PEEK composite material were prepared using traditional injection molding processes (without using gradient structures and continuous fibers).
[0060] Comparative Example 2
[0061] 6061-T6 aluminum alloy components of the same size were prepared using conventional machining methods.
[0062] The test results are shown in the table below:
[0063] Test Project Example 1 Comparative Example 1 Comparative Example 2 Density (g / cm³) 1.65 1.42 2.70 Tensile strength (MPa) 850 180 310 Flexural modulus (GPa) 62 8.5 69 Impact toughness (kJ / m²) 45 55 30 Weight reduction ratio (vs. aluminum alloy) 38% 47% -
[0064] As shown in the table above, the gradient material of Example 1 maintains a flexural modulus comparable to that of aluminum alloy, while its tensile strength far exceeds that of aluminum alloy and homogeneous injection molded parts, and achieves a weight reduction of nearly 38%.
[0065] Finally, the following points should be noted: First, in the description of this application, it should be noted that, unless otherwise specified and limited, the terms "installation", "connection", and "linkage" should be interpreted broadly, and can be mechanical or electrical connections, or internal connections between two components, or direct connections. "Up", "down", "left", "right", etc. are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may change.
[0066] Secondly: In the embodiments disclosed in this invention, only the structures involved in the embodiments disclosed in this invention are involved. Other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of this invention can be combined with each other.
[0067] In conclusion, the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lightweight material for humanoid robots, characterized in that: The material has a gradient composite structure, consisting of the following components from the outside to the inside: Outer layer: A continuous carbon fiber reinforced polyetheretherketone composite layer, with a continuous carbon fiber volume fraction of 45% to 65%; Intermediate layer: This is a layer of short-cut carbon fiber reinforced polyetheretherketone composite material, with the mass fraction of short-cut carbon fiber being 20%–40%. Inner layer: It is a composite structural layer of toughened modified polyether ether ketone and foamed magnesium alloy or magnesium-lithium alloy. The porosity of the foamed metal is 50% to 75% and the pore size is 0.5 to 3 mm. The outer layer, middle layer and inner layer are integrated and co-cured through one or more of the following processes: autoclave molding, resin transfer molding or vacuum-assisted resin infusion.
2. The lightweight material for humanoid robots according to claim 1, characterized in that: In the outer layer, the continuous carbon fibers are one or more of T300, T700 or T800 grade, and the fiber morphology is unidirectional tape or fabric; the melt flow rate of the polyether ether ketone resin is 8-25 g / 10 min, and the crystallinity is ≥35%.
3. The lightweight material for humanoid robots according to claim 1, characterized in that: In the intermediate layer, the chopped carbon fibers have a length of 0.2–1 mm and a diameter of 5–15 μm, and the fiber surface is treated with oxidation or sizing. The chopped carbon fiber reinforced polyetheretherketone composite layer is subjected to a shear rate of 1000 s at 380 °C. -1 The melt viscosity is 150–300 Pa·s.
4. The lightweight material for humanoid robots according to claim 1, characterized in that: In the inner layer, the foamed magnesium alloy is one of the AZ31, AZ91 or WE43 series magnesium alloys, and its pore structure is open or closed, with a pore wall thickness of 0.1 to 0.5 mm; the toughened modified polyetheretherketone is a blend of polyetheretherketone and thermotropic liquid crystal polymer or polyetherimide, wherein the mass fraction of thermotropic liquid crystal polymer or polyetherimide is 5% to 15%.
5. A method for preparing a lightweight material for a humanoid robot as described in any one of claims 1-4, characterized in that, Includes the following steps: S1. Automated fiber laying preform forming: The continuous carbon fiber prepreg tape is laid on the laying mold with a multi-angle layering design according to the three-dimensional digital model of the structural component using an automated fiber laying equipment to form a preform with an outer layer and part of the middle layer. S2. Mold assembly and packaging: The preform obtained in step S1, the short carbon fiber reinforced polyether ether ketone prepreg or premix, and the foamed magnesium alloy core material are assembled in an integrated molding mold according to the design position and vacuum-sealed. S3. Gradient Resin Injection and Curing: In an autoclave, under vacuum assistance, molten polyether ether ketone resin is sequentially injected from multiple injection ports of the mold. By controlling the opening and closing sequence of different injection ports, gradient resin impregnation from the outer layer to the inner layer is achieved. Subsequently, the material is pressurized and cured in the autoclave, cooled and demolded to obtain the lightweight material.
6. A method for preparing a lightweight material for humanoid robots according to claim 5, characterized in that: In step S1, infrared heating is applied during the automated fiber laying process to maintain the interlayer temperature of the prepreg tape at 280-350°C, the compaction pressure at 200-600N, and the laying head travel speed at 5-20m / min; the multi-angle layup design includes layup angles of 0°, ±45°, and 90°.
7. A method for preparing a lightweight material for humanoid robots according to claim 5, characterized in that: In step S3, the resin injection temperature is 360–390°C, the injection pressure is 0.3–1.5 MPa, the curing pressure is 0.6–2.0 MPa, the curing temperature is 380–400°C, and the holding time is 1–4 hours.