Waterproof and fireproof cushion material
By using a multi-layer composite structure and modified expandable graphite, the problem of reasonable interlayer coordination between waterproofing, bonding, and construction performance and expansion insulation and flame barrier properties of waterproofing pads has been solved, achieving more efficient fireproofing and bonding stability, and enhancing the continuity and uniformity of construction performance and fireproofing.
Patent Information
- Application Number
- CN202611610910.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies have failed to effectively address the issue of proper interlayer compatibility between waterproofing, bonding, and construction performance and expansion insulation and flame barrier properties of waterproofing gaskets, especially in maintaining expansion performance while improving the compatibility of graphite and butyl rubber.
The product employs a multi-layer composite structure, including a waterproof surface composite layer, an expandable butyl rubber layer, an expandable coating, a fiberglass cloth layer, and a release protective layer. By combining modified expandable graphite with a binder, the synergistic effect of the expandable coating and the fiberglass cloth layer is ensured, forming a symmetrical fireproof structure. Furthermore, the dispersibility and compatibility of graphite are improved through treatment with titanate coupling agents and naphthenic oils.
It improves the fire resistance and heat insulation performance and bonding stability of the padding material, reduces the possibility of flame penetration and heat transfer, and enhances the construction performance and the continuity and uniformity of fire resistance and heat insulation.
Smart Images

Figure CN123129571A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fireproof materials technology, and more specifically to a waterproof and fireproof mat material. Background Technology
[0002] Roofing waterproofing underlayment is placed between the roofing material and the substrate to prevent moisture penetration into the substrate and to withstand tension and tearing during installation and use. For combustible substrates such as wood, the underlayment also needs to have the ability to block flames and delay heat transfer. Therefore, related technologies are gradually adopting composites of waterproof membranes, fiber-reinforced materials, and intumescent flame-retardant materials, enabling the underlayment to simultaneously possess waterproof, reinforcing, and fireproof functions.
[0003] Chinese patent document CN105026660A, entitled "Fire-resistant Roofing System and Membrane Composite Material," discloses a technical solution of incorporating expandable graphite into the reinforcing fabric or fabric backing of a roofing membrane. In this solution, the expandable graphite is dispersed in an adhesive to form a coating, and the adhesive can be materials such as polyurethane. This document indicates that by combining an expandable graphite-containing coating with a fabric, thermal expansion functionality can be introduced into the roofing membrane structure. However, this document focuses on thermoplastic roofing membranes and their fabric reinforcement structures, and does not provide details regarding the interlayer configuration and adhesive layer parameter matching when the expandable coating and the two sides of expandable butyl rubber layers together constitute a fire-resistant structure.
[0004] Chinese patent document CN105238271A, entitled "A Smoke-Suppressing Non-Curing Rubber Asphalt Waterproof Coating," discloses a scheme for modifying a smoke-suppressing material containing expandable graphite, ammonium octamolate, and calcium phosphomolybdate using titanate esters to improve its oleophilicity and dispersibility in asphalt. This document provides a technical approach to improve the compatibility of expandable graphite with organic matrices through surface treatment; however, its application is limited to rubber asphalt waterproof coatings, and it does not provide a comparative evaluation of the expansion volume of expandable graphite before and after modification. Therefore, based solely on improvements in oleophilicity or dispersibility, it is insufficient to determine whether the modified graphite can maintain its performance for expansion insulation, nor can its applicability in butyl rubber layers be directly determined.
[0005] Chinese patent document CN115232577A, entitled "A Fire-Resistant Butyl Rubber and Its Application in Multilayer Composite Fire-Resistant Roll Material," discloses a fire-retardant butyl rubber containing expanded graphite, and a roll material formed by sequentially laminating an isolation layer, a first fire-retardant butyl rubber layer, a first refractory fiber cloth layer, a second fire-retardant butyl rubber layer, and a second refractory fiber cloth layer. The document also proposes that the two fire-retardant butyl rubber layers can use different expanded graphite contents, and points out that in its tests, when the expanded graphite content increased to a certain level, the peel strength of the rubber compound decreased significantly. This indicates that the composite of double-layer expanded butyl rubber with refractory fiber cloth, and the balance between fire resistance and adhesion by adjusting the graphite content, have been studied.
[0006] However, the aforementioned two-layer butyl rubber solution does not further specify the relationship between the adhesive layer thickness, the mass of graphite per unit volume, and the expansion volume of graphite itself in the formulation of the two adhesive layers. For adhesive layers of different thicknesses, even with the same percentage of graphite mass, the mass of graphite per unit area may differ; when using different grades or treated graphite, the expansion volume per unit mass may also vary. Therefore, simply comparing the graphite content of the two adhesive layers is insufficient to fully reflect the amount of graphite material per unit area and its corresponding free expansion capacity, nor is it sufficient to directly determine a formulation that balances substrate adhesion and expansion fireproofing.
[0007] Based on the above-mentioned publicly available information, existing technologies have respectively involved intumescent coatings on fabrics, multilayer fire-retardant butyl rubber structures, and surface modification of expandable graphite. However, when these technologies are applied to padding materials with waterproof surfaces and self-adhesive base layers, two interrelated issues still need to be addressed: first, how to achieve a reasonable interlayer fit between the waterproof structure, fiber skeleton, and intumescent material; and second, how to maintain the expansion performance while improving the compatibility of graphite and butyl rubber, and how to configure graphite materials in combination with different adhesive layer thicknesses and bonding requirements.
[0008] Therefore, it is necessary to further improve the composite layer structure of waterproof and fireproof mat materials and the application of expandable graphite in the adhesive layer, so as to take into account the waterproof, bonding and construction performance at room temperature, as well as the expansion insulation and flame barrier requirements under heat conditions.
[0009] Therefore, further improvements and development are still needed. Summary of the Invention
[0010] To address the shortcomings of existing technologies and solve the aforementioned problems, a waterproof and fireproof mat material is proposed, and the following technical solution is provided: A waterproof and fireproof mat material includes a waterproof surface composite layer, a first intumescent butyl rubber layer, a first intumescent coating layer, a fiberglass cloth layer, a second intumescent coating layer, a second intumescent butyl rubber layer, and a release protective layer, which are sequentially laminated along the thickness direction. The waterproof surface composite layer is a composite layer with waterproof effect; Both the first and second expandable butyl rubber layers comprise expandable graphite and butyl rubber. Both the first and second expanding coatings comprise expandable graphite and a binder; The release protective layer can be peelably applied to the surface of the second expanded butyl rubber layer opposite to the second expanded coating.
[0011] Furthermore, the adhesive is a polyurethane adhesive.
[0012] Furthermore, the thickness ratio of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer is (0.30-0.40):(0.005-0.02):(0.4-0.6):(0.005-0.02):(0.30-0.60).
[0013] Furthermore, the thickness of the second expanded butyl rubber layer is greater than the thickness of the first expanded butyl rubber layer.
[0014] Preferably, the thickness ratio of the first expandable butyl rubber layer, the first expandable coating layer, the glass fiber cloth layer, the second expandable coating layer, and the second expandable butyl rubber layer is 0.35:0.01:0.5:0.01:0.55.
[0015] Furthermore, the expandable graphite is modified expandable graphite, which is obtained by coating expandable graphite with a treatment liquid, wherein the treatment liquid is formed by mixing titanate coupling agent and naphthenic oil.
[0016] Furthermore, the amount of the treatment liquid is 0.1% to 3% of the mass of expandable graphite, and the mass ratio of the titanate coupling agent to the naphthenic oil is 1-3:1.
[0017] Furthermore, the expandable graphite has a particle size of 50-200 mesh and a volume expansion factor of not less than 150.
[0018] Furthermore, the waterproof surface composite layer comprises a non-woven fabric layer, a first waterproof membrane layer, a woven fabric reinforcement layer, and a second waterproof membrane layer sequentially laminated together, wherein the second waterproof membrane layer is bonded to the first expanded butyl rubber layer; The nonwoven fabric layer is a polypropylene nonwoven fabric layer, and the woven fabric reinforcement layer is a polypropylene woven fabric layer; both the first waterproof membrane layer and the second waterproof membrane layer are composite membrane layers containing polypropylene and polyethylene.
[0019] Preferably, the thickness ratio of the nonwoven fabric layer, the first waterproof membrane layer, the woven fabric reinforcement layer, and the second waterproof membrane layer is (0.5-0.6):(0.01-0.05):(0.1-0.2:(0.01-0.05).
[0020] More preferably, the thickness ratio of the nonwoven fabric layer, the first waterproof membrane layer, the woven fabric reinforcement layer, and the second waterproof membrane layer is 0.58:0.02:0.15:0.02.
[0021] Furthermore, the ratio of the expansion volume of the modified expandable graphite to the expansion volume of the expandable graphite raw material used to prepare the modified expandable graphite is not less than 0.90.
[0022] Furthermore, the first expanded butyl rubber layer and the second expanded butyl rubber layer satisfy the following: Where c1 and c2 are the mass of expandable graphite per unit volume, h1 and h2 are the thickness of the adhesive layer, and E1 and E2 are the expansion volumes of the corresponding expandable graphite materials measured using the same test method and test conditions.
[0023] Due to the adoption of the above technical solutions, the beneficial technical effects of the present invention are as follows: 1. This application employs a multi-layer composite fireproof structure with a fiberglass cloth layer as the intermediate layer. Intumescent coatings are applied to both sides of the fiberglass cloth layer, and intumescent butyl rubber layers are applied to the outer sides of both intumescent coatings, forming a symmetrical fireproof structure of intumescent butyl rubber layer—intumescent coating—fiberglass cloth layer—intumescent coating—intumescent butyl rubber layer. Upon heating, the expandable graphite in the intumescent butyl rubber layers and intumescent coatings on both sides expands in volume, forming a multi-layered, porous heat-insulating barrier structure on both sides of the fiberglass cloth layer. The fiberglass cloth layer acts as a heat-resistant skeleton, supporting and constraining the expanded material, which helps reduce the possibility of cracking, detachment, or local collapse of the expanded layer after heating, and maintains good continuity and integrity of the expanded structure on both sides in the thickness direction. Thus, through the combined effect of expansion insulation and the barrier effect of the fiberglass skeleton, the path of heat transfer along the thickness direction of the pad material to the base layer is extended, reducing the possibility of flame penetration and heat propagation to the wooden base layer, thereby improving the fireproof and heat-insulating performance of the pad material under continuous fire source conditions.
[0024] 2. This application employs a treatment solution formed from a titanate coupling agent and naphthenic oil to surface-modify expandable graphite. The treatment solution coats the surface of the expandable graphite particles. The naphthenic oil acts as a wetting and dispersing carrier for the expandable graphite particles, facilitating the uniform distribution of the titanate coupling agent on the graphite particle surface. After surface treatment, the interfacial compatibility differences between expandable graphite and organic components such as butyl rubber, polyisobutylene, and petroleum resin are reduced, thereby reducing localized agglomeration of graphite particles in the adhesive and improving the uniformity of expansionable graphite dispersion in the butyl rubber system. Therefore, on the one hand, it reduces localized fire-resistant weak areas in the adhesive layer caused by graphite agglomeration, resulting in a more uniform and continuous expanding heat-insulating layer after heating; on the other hand, it reduces the adverse effects of graphite particles on the continuous phase of butyl rubber and the effective bonding area of the adhesive layer, maintaining the expansion flame-retardant capability while also considering the adhesion and workability of the adhesive layer, thus improving the overall fire resistance and service stability of the expandable butyl rubber layer.
[0025] 3. This application further specifies that the ratio of the expansion volume of the modified expandable graphite to the expansion volume of the unmodified expandable graphite raw material is not less than 0.90, and ensures that the potential expansion capacity per unit area of the first expandable butyl adhesive layer and the second expandable butyl adhesive layer meets a predetermined matching relationship. Specifically, the expansion volume retention rate is not less than 0.90, ensuring that while the expandable graphite improves its compatibility with the butyl adhesive system through surface treatment, it still maintains a high proportion of its original expansion capacity, avoiding restricted interlayer expansion and a significant decrease in expansion capacity due to excessive surface treatment. Simultaneously, by comprehensively considering the unit volume of expandable graphite in the two adhesive layers, the adhesive layer thickness, and the expansion volume of the graphite itself, the potential expansion capacity per unit area of the two adhesive layers is kept within a suitable matching range, avoiding stress imbalance, local cracking, or weak insulation areas caused by excessive expansion on one side and insufficient expansion on the other. This allows for a more balanced, continuous, and stable expansion insulation structure on both sides of the fiberglass cloth. While ensuring sufficient adhesion and sealing capabilities on the side closest to the substrate, it also improves the uniformity of thermal barrier and structural stability throughout the thickness of the pad, thereby further reducing the risk of temperature rise on the unexposed side and continuous combustion of the substrate. Attached Figure Description
[0026] Figure 1 This is a structural schematic diagram of the waterproof and fireproof mat material of this application.
[0027] The above figures include the following reference numerals: 1. Non-woven fabric layer; 2. First waterproof membrane layer; 3. Woven fabric reinforcement layer; 4. Second waterproof membrane layer; 5. First expandable butyl rubber layer; 6. First expandable coating layer; 7. Fiberglass cloth layer; 8. Second expandable coating layer; 9. Second expandable butyl rubber layer; 10. Release protective layer. Detailed Implementation
[0028] To enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Based on the embodiments in this application, other similar embodiments obtained by those skilled in the art without creative effort should all fall within the scope of protection of this application.
[0029] Unless otherwise specified in the examples, standard conditions or conditions recommended by the manufacturer should be followed. Reagents or instruments whose manufacturers are not specified are all commercially available products. Unless otherwise specified, all reagents used in the examples are commercially available.
[0030] The specific implementation of this application will be further described below. Unless otherwise stated, the arrangement order of each layer is based on the side away from the base layer and towards the side closer to the base layer after the pad material is installed. The thickness of the adhesive layer is the thickness in the unheated expansion state, and the thickness of the coating layer is the thickness after drying and film formation.
[0031] This embodiment provides a waterproof and fireproof mat material, comprising a waterproof surface composite layer, a first intumescent butyl rubber layer, a first intumescent coating layer, a fiberglass cloth layer, a second intumescent coating layer, a second intumescent butyl rubber layer, and a release protective layer, sequentially laminated along the thickness direction. The waterproof surface composite layer includes a non-woven fabric layer, a first waterproof membrane layer, a woven fabric reinforcing layer, and a second waterproof membrane layer, sequentially laminated. The second waterproof membrane layer is bonded to the first intumescent butyl rubber layer. The first intumescent coating layer and the second intumescent coating layer are respectively disposed on opposite sides of the fiberglass cloth layer, with the first intumescent butyl rubber layer in contact with the first intumescent coating layer, and the second intumescent butyl rubber layer in contact with the second intumescent coating layer. The release protective layer is peelably applied to the surface of the second intumescent butyl rubber layer facing away from the second intumescent coating layer.
[0032] The non-woven fabric layer is made of polypropylene non-woven fabric, the woven reinforcement layer is made of polypropylene woven fabric, and both the first and second waterproof membrane layers are composite membranes containing polypropylene and polyethylene. The non-woven fabric layer forms the outer surface of the pad material, increasing surface friction and aiding in water conduction; the two waterproof membrane layers form two water-blocking structures, and the woven reinforcement layer improves tensile and tear resistance. The fiberglass cloth layer is woven from fiberglass, with expanded coatings on both sides covering the fabric surface and filling the surface pores to reduce the possibility of flame penetration through the pores. The release protective layer is a polypropylene film with a silicone oil release coating on the side facing the second expanded butyl rubber layer.
[0033] The non-woven fabric layer also provides excellent anti-slip and grip properties, ensuring good walking safety and ease of operation for construction workers when working on the roof.
[0034] In a preferred thickness combination, the thicknesses of the nonwoven fabric layer, the first waterproof membrane layer, the woven fabric reinforcement layer, the second waterproof membrane layer, the first expanded butyl rubber layer, the first expanded coating layer, the fiberglass cloth layer, the second expanded coating layer, the second expanded butyl rubber layer, and the release liner are 0.58 mm, 0.02 mm, 0.15 mm, 0.02 mm, 0.35 mm, 0.01 mm, 0.50 mm, 0.01 mm, 0.55 mm, and 0.03 mm, respectively. The thickness of the second expanded butyl rubber layer is greater than that of the first expanded butyl rubber layer. Adding the nominal thicknesses of each layer, the thickness including the release liner is 2.22 mm, and the thickness after peeling off the release liner is 2.19 mm. After laminating all layers, the finished product thickness including the release liner, affected by pressure, is between 1.6 and 2 mm.
[0035] The first and second intumescent butyl rubber layers both use graphite-modified butyl rubber, which is prepared by blending modified expandable graphite with butyl rubber, polyisobutylene, petroleum resin, calcium powder and naphthenic oil.
[0036] Modified expandable graphite was prepared according to the following steps.
[0037] First, expandable graphite raw material is selected. In this embodiment, expandable graphite with a nominal particle size of 100 mesh is used, but the raw material can also be selected within the limited range of 50 to 200 mesh.
[0038] Subsequently, the titanate coupling agent was added to the naphthenic oil and stirred until homogeneous to obtain the treated solution. The naphthenic oil served as the dispersion carrier for the coupling agent in this step. The titanate coupling agent used was TC-114, and the mass ratio of the titanate coupling agent to the naphthenic oil was 1-3:1.
[0039] Preferably, the mass ratio of titanate coupling agent to naphthenic oil is 2:1.
[0040] Expandable graphite was added to a high-speed mixer, and stirring was started. The above-mentioned treatment liquid was evenly sprayed onto the graphite while it was being stirred, so that the treatment liquid was distributed on the surface of the graphite particles. The stirring process was carried out for 5 minutes to obtain modified expandable graphite. This step aims to wet and coat the particle surface, and the particle morphology of the graphite is maintained after treatment.
[0041] The resulting modified expandable graphite is stored in a sealed container for later use. The naphthenic oil introduced during pretreatment is uniformly measured in subsequent rubber compound formulations; if the specified amount of naphthenic oil in the rubber compound formulation includes the oil used for pretreatment, then the mass of naphthenic oil added during mixing is the specified mass in the formulation minus the mass introduced during pretreatment.
[0042] Graphite-modified butyl rubber is prepared by kneading and mixing. The raw materials include butyl rubber, calcium powder, polyisobutylene, petroleum resin, naphthenic oil, and the aforementioned modified expandable graphite. By weight, the composition is: 5-20 parts butyl rubber, 20-60 parts calcium powder, 5-30 parts polyisobutylene, 5-30 parts petroleum resin, 1-5 parts naphthenic oil, and 5-30 parts modified expandable graphite.
[0043] During preparation, all raw materials are weighed according to the determined formula. The kneader is started, and the equipment temperature is set to 90℃. The raw materials are put into the kneader for mixing. After mixing for 4 hours, the material is discharged to obtain graphite-modified butyl rubber. During the mixing process, the actual material temperature is monitored and controlled to not exceed 150℃ according to the processing requirements of this formula to reduce the risk of graphite expanding prematurely during processing, forming pores, and affecting the sealing and bonding performance of the rubber compound. 90℃ is the equipment set temperature, and the actual material temperature is recorded separately. Polyisobutylene and petroleum resin in the rubber compound are used to provide and adjust the bonding performance, while the rubber compound used in the second adhesive layer maintains the pressure-sensitive self-adhesive properties required for construction.
[0044] To improve the dispersion of expandable graphite in butyl rubber systems, this application employs a treatment solution composed of a titanate coupling agent and naphthenic oil to surface-treat the expandable graphite. The naphthenic oil wets the surface of the expandable graphite and acts as a dispersion carrier for the titanate coupling agent, ensuring its more uniform distribution on the graphite particle surface. The titanate coupling agent, in turn, helps reduce the interfacial differences between expandable graphite and organic components such as butyl rubber, polyisobutylene, and petroleum resin, reducing graphite particle agglomeration in the rubber compound, thereby improving the continuity of the rubber compound and the effective contact between the adhesive layer and the substrate.
[0045] However, a higher degree of surface treatment for expandable graphite is not always better. When the amount of treatment solution used is excessive or the resulting surface treatment layer is too thick, the layer may hinder the release of interlayer gas and the unfolding of graphite flakes after heating. Simultaneously, the non-expanding components in the treatment solution can increase the mass of the modified material, thereby reducing the expansion volume per unit mass of modified expandable graphite. Therefore, when surface treating expandable graphite, a balance needs to be struck between improving its dispersibility and interfacial compatibility and maintaining its thermal expansion capacity.
[0046] Based on this, this application limits the ratio of the expansion volume of the modified expandable graphite to the expansion volume of the expandable graphite raw material used to prepare the modified expandable graphite to not less than 0.90. This ratio was measured and calculated under the same testing methods, heating temperatures, holding times, sample measurement methods, and volume reading methods for graphite materials before and after modification. A ratio of not less than 0.90 indicates that the expandable graphite, after surface treatment, can still retain at least 90% of its original expansion capacity, thereby avoiding significant damage to its expansion and fire-retardant properties in order to improve the dispersibility of graphite in butyl rubber.
[0047] Within the aforementioned range, the surface treatment layer on graphite improves the wetting and dispersion of graphite particles in the continuous phase of butyl rubber, reduces localized graphite enrichment areas, maintains a larger effective contact area between the adhesive layer and the substrate, and enhances the adhesion performance of the adhesive layer. Simultaneously, because the modified expandable graphite retains a high expansion volume, it can fully expand upon heating to form an expansion barrier layer with a porous structure. With a more uniform distribution of graphite particles, the expansion initiation and degree of expansion in different regions are also more uniform, which is beneficial for forming a continuous and complete thermal insulation structure. Therefore, the aforementioned limitation on the expansion volume retention rate can balance the room-temperature adhesion performance and thermal expansion performance of the adhesive layer.
[0048] Furthermore, the thicknesses of the first and second expanded butyl rubber layers differ somewhat in their primary functions. The first expanded butyl rubber layer is located on the side of the fiberglass cloth layer closest to the waterproof surface composite layer, and is mainly used to form a front-end expansion barrier structure near the fire-exposed side when the padding material is subjected to flames or high temperatures. The second expanded butyl rubber layer is located on the side of the fiberglass cloth layer closest to the substrate, and in addition to forming an end expansion barrier structure near the substrate, it is also used to bond with the substrate and fill the microscopic irregularities and local gaps on the substrate surface.
[0049] For two expandable butyl rubber layers of different thicknesses, even if the mass percentage of expandable graphite in both layers is the same, the mass of expandable graphite material per unit area may differ. Furthermore, expandable graphite of different particle sizes, grades, or degrees of surface treatment may also have different expansion volumes per unit mass. Therefore, simply comparing the thickness or graphite mass percentage of the two layers cannot fully reflect their expansion capacity per unit area.
[0050] Therefore, this application uses the mass of expandable graphite material contained in a unit volume of adhesive layer, the thickness of the adhesive layer, and the expansion volume of the corresponding expandable graphite material to jointly characterize the theoretical expansion capacity per unit area of the two adhesive layers. The first expandable butyl adhesive layer and the second expandable butyl adhesive layer satisfy the following: Wherein, c1 and c2 are the masses of expandable graphite material contained in the first and second expandable butyl rubber layers per unit volume, respectively; h1 and h2 are the thicknesses of the first and second expandable butyl rubber layers in the unheated expansion state, respectively; E1 and E2 are the expansion volumes of the expandable graphite material used to prepare the corresponding rubber layers, measured using the same test method and test conditions.
[0051] Based on the unit area of the adhesive layer, c1 and c2 represent the mass of expandable graphite material contained in the first and second expandable butyl adhesive layers per unit area, respectively. After multiplying by the expansion volume of the corresponding graphite material, c1h1E1 and c2h2E2 are used to characterize the theoretical free expansion volume per unit area of the two adhesive layers. When g / cm3 is used as the unit of c1 and c2, cm is used as the unit of h1 and h2, and cm3 / g is used as the unit of E1 and E2, the unit of cihiEi is cm, which can be understood as the theoretical equivalent thickness of expansion per unit area of the corresponding adhesive layer.
[0052] The theoretical equivalent thickness of expansion mentioned above is used to evaluate the relative expansion potential of the two adhesive layers and is not equivalent to the actual expansion thickness of the gasket after heating. The actual expansion thickness of the gasket is also affected by factors such as the constraint of the butyl rubber matrix, the composition of the expansion coating, the supporting effect of the glass fiber cloth layer, the interlayer bonding state, and the heating conditions.
[0053] The ratio of c1h1E1 to c2h2E2 is limited to not less than 1.0, ensuring that the theoretical expansion capacity per unit area of the first intumescent butyl rubber layer is not less than that of the second intumescent butyl rubber layer. Therefore, when the gasket is subjected to flame or high temperature from the side of the waterproof surface composite layer, the first intumescent butyl rubber layer near the fire-exposed side can form a relatively sufficient front-end expansion barrier structure, providing initial protection against flame and heat, and reducing heat transfer to the fiberglass cloth layer and the base layer.
[0054] The upper limit of the above ratio is set at 1.2, so that the theoretical expansion capacity of the first expandable butyl adhesive layer can be moderately higher than that of the second expandable butyl adhesive layer, but the difference between the two will not be too large. If the theoretical expansion capacity of the first expandable butyl adhesive layer is too high relative to that of the second expandable butyl adhesive layer, the expansion degree of the two adhesive layers after heating may be significantly inconsistent, causing the glass fiber cloth layer to be subjected to uneven expansion forces on both sides, which may cause local cracking, warping or interlayer separation of the expansion structure; at the same time, the end expansion barrier effect of the second expandable butyl adhesive layer may also be relatively insufficient.
[0055] When the above ratio is controlled between 1.0 and 1.2, the first expandable butyl rubber layer can form a front-end expansion capacity that is not lower than and moderately higher than that of the second expandable butyl rubber layer. The second expandable butyl rubber layer can form an end-end thermal insulation structure close to the substrate while maintaining the bonding, filling, and sealing performance of the substrate. The glass fiber cloth layer located between the two rubber layers provides high-temperature resistant skeleton support for the expandable coating and expandable butyl rubber layer on both sides, and bears and constrains the expandable material, so that the expandable materials on both sides together form a relatively continuous and stable composite barrier structure.
[0056] Therefore, by limiting the expansion volume retention rate of modified expandable graphite and further limiting the relative relationship of the theoretical expansion capacity per unit area of the two expandable butyl adhesive layers, it is possible to maintain the thermal expansion capacity of graphite while improving the dispersibility and adhesive bonding performance of graphite. This also allows the fire-retardant effect at the front end, the heat insulation effect at the end, and the bonding effect of the base layer of the two adhesive layers to work together, thereby improving the fireproof and heat-insulating performance, bonding stability, and integrity of the expanded structure after heating of the pad material.
[0057] The padding material is prepared by composite process according to the following route.
[0058] First, a waterproof surface composite layer is prepared. Polypropylene nonwoven fabric is prepared using a spunbond method, and polypropylene woven fabric is prepared using a fiber weaving method; alternatively, pre-made materials of corresponding specifications can be used. A film containing polypropylene and polyethylene is melt-extruded from the raw materials, and then laminated using a casting process and roller press to form a first waterproof membrane layer between the nonwoven and woven fabrics. A second waterproof membrane layer is formed on the side of the woven fabric facing away from the nonwoven fabric. After cooling, a four-layer waterproof surface composite layer is obtained. This melt-lamination step is completed before laminating with the adhesive layer containing expandable graphite. Next, a glass fiber cloth with expandable coatings on both sides is prepared. A polyurethane binder and expandable graphite are mixed evenly to form a coating material, which is then applied to one side of the glass fiber cloth using a roller coating method, ensuring the coating material covers the fabric surface and penetrates the surface pores. After drying, a first expandable coating is obtained. The other side of the glass fiber cloth is then roller-coated and dried to obtain a second expandable coating. The nominal dry film thickness of each expandable coating is 0.01 mm. The expandable coating contains 30%–70% polyurethane binder and 20%–50% expandable graphite. After the double-sided coating is dried and cooled, the adhesive layers are laminated. The graphite-modified butyl rubber used for the first adhesive layer is applied by extrusion coating or calendering to form a 0.35 mm thick first expanded butyl rubber layer. One side of this layer is bonded to the second waterproof membrane layer of the waterproof surface composite layer, and the other side is bonded to the first expanded coating on the fiberglass cloth. This is then laminated using a pressure roller to obtain the upper composite. The graphite-modified butyl rubber used for the second adhesive layer is applied to the second expanded coating of the upper composite to form a 0.55 mm thick second expanded butyl rubber layer. The exposed adhesive surface of this second layer is then bonded to the release surface of the release liner. This is further laminated using a pressure roller to bond the second expanded coating to the second expanded butyl rubber layer. The bonding surface can be adjusted according to the production equipment, but the final layer sequence must remain consistent. The actual material temperature of the adhesive should not exceed 150℃ as required by this formula, and it must be confirmed that the drying of the coating will not cause premature expansion of the graphite contained within. After lamination, the material is cooled, trimmed, and wound up to ensure that the release liner continuously covers the bottom adhesive surface, resulting in a waterproof and fireproof mat material.
[0059] When the padding material is heated, the expandable graphite in the two expandable butyl rubber layers expands, forming a porous heat-insulating structure; the two expandable coatings further form an expandable barrier structure, and the fiberglass cloth provides a heat-resistant skeleton and prevents flame penetration, allowing the intermediate layers to collectively delay heat transfer to the substrate. In the unheated state, the waterproof surface composite layer provides surface water resistance and reinforcement, while the second expandable butyl rubber layer provides substrate adhesion and sealing.
[0060] This set of examples is used to verify the influence of the interlayer relationship of the padding material on its flame retardant and fireproof performance. Example 1 This embodiment provides a waterproof and fireproof mat material.
[0061] The waterproof and fireproof mat material comprises, in sequence along the thickness direction, a waterproof surface composite layer, a first intumescent butyl rubber layer, a first intumescent coating layer, a fiberglass cloth layer, a second intumescent coating layer, a second intumescent butyl rubber layer, and a release protective layer.
[0062] The waterproof surface composite layer comprises, in sequence along the thickness direction, a non-woven fabric layer, a first waterproof membrane layer, a woven fabric reinforcement layer, and a second waterproof membrane layer.
[0063] Specifically, the thicknesses of the nonwoven fabric layer, the first waterproof membrane layer, the woven fabric reinforcement layer, the second waterproof membrane layer, the first expandable butyl rubber layer, the first expandable coating layer, the fiberglass cloth layer, the second expandable coating layer, the second expandable butyl rubber layer, and the release protective layer are 0.58 mm, 0.02 mm, 0.15 mm, 0.02 mm, 0.35 mm, 0.01 mm, 0.50 mm, 0.01 mm, 0.55 mm, and 0.03 mm, respectively.
[0064] Both the first and second expanded butyl rubber layers use graphite-modified butyl rubber.
[0065] The expandable graphite in the graphite-modified butyl rubber undergoes pre-surface modification treatment. A treatment solution is formed by mixing a titanate coupling agent with naphthenic oil. This treatment solution is then uniformly applied to the surface of the expandable graphite particles under stirring, allowing the treatment solution to distribute and coat the surface of the expandable graphite particles, thus obtaining modified expandable graphite. Subsequently, the modified expandable graphite is compounded with butyl rubber, polyisobutylene, petroleum resin, calcium powder, and naphthenic oil to obtain graphite-modified butyl rubber.
[0066] Both the first and second expanding coatings comprise expandable graphite and polyurethane binder, respectively formed on both sides of the glass fiber cloth layer.
[0067] Following the aforementioned method for preparing the padding material, the layers are sequentially laminated to obtain the waterproof and fireproof padding material of this embodiment.
[0068] In this embodiment, the butyl rubber is designated as HRB0810FR.
[0069] The prepared waterproof and fireproof padding material was used in the roofing system for fire performance testing. The tests were conducted according to ICC-ES AC 188-12 (Rev.15) and with reference to ASTM E108-25.
[0070] The test used 15 / 32-inch thick AC-grade fir plywood as the base layer. A layer of waterproof and fireproof underlayment, as described in this embodiment, was laid on the plywood base layer through its own self-adhesive layer. The transverse joints of adjacent underlayment layers overlapped by approximately 4 inches. A 26 Ga vertically interlocking metal roof was then laid on top of the underlayment. Four roofs were used for Class A flammability brand testing, and two roofs were used for Class A intermittent flame exposure testing.
[0071] During the combustion tests in groups 1 to 4, although some samples exhibited phenomena such as smoke, discoloration, localized reddening, or deformation of the metal surface, no sustained flames appeared on the sample surface or the back of the substrate at the end of the test. The tests in groups 1, 2, 3, and 4 ended at 30 min, 25 min, 30 min, and 30 min respectively, all meeting the acceptance requirement of Class A test that no flames should appear on the back of the substrate.
[0072] For the intermittent flame exposure tests in groups 5 and 6, no surface flames appeared after the 56-minute flame exposure cycle. When the observation continued for 80 minutes, there was no smoke, redness or flames on the sample surface and the back of the substrate. The test results were all passed.
[0073] The final test result is that the roofing system in which the padding material is located in this embodiment meets the modified ICC-ES AC 188-12 (Rev.15) Class A requirements, with a test slope of 5:12.
[0074] Comparative Example 1 This comparative example uses the conventional waterproof matting material used by the applicant before the fireproof structure improvement. This matting material, along its thickness direction, comprises, in sequence, a non-woven fabric layer, a waterproof membrane layer, a woven fabric reinforcement layer, another waterproof membrane layer, a plain butyl rubber layer, and a release protective layer. Notably, the plain butyl rubber layer does not contain the expandable flame-retardant system formed from expandable graphite as described in this application, nor does it contain the first and second expandable coatings located on both sides of the fiberglass cloth.
[0075] The aforementioned underlayment was used in the roofing system for fire performance testing. The test was conducted on September 26, 2024, using a Class A burning wood block test according to ASTM E108-20a. The test system used 3 / 8-inch thick AC-grade fir plywood as the base layer, on which a layer of underlayment was laid, and on top of the underlayment were three-piece asphalt shingles conforming to ASTM D3018.
[0076] In the fourth test, the right side of the joint turned red at 18 minutes and 47 seconds, the redness increased at 23 minutes, and a persistent flame appeared on the back of the substrate at 25 minutes, so the test was terminated. Ultimately, three of the four test roofs passed and one failed. The fourth test roof did not obtain ASTM E108 rating due to the persistent flame on the back.
[0077] The above results indicate that waterproof padding materials consisting solely of ordinary butyl rubber layers and conventional non-woven fabrics, waterproof membranes, and woven fabrics are still insufficient in their ability to transfer heat to the wood substrate and to inhibit the continuous burning of the substrate's unexposed surface when exposed to a fire source for an extended period of time.
[0078] Comparative Example 2 This comparative example is the padding material obtained by making the first fireproof structural improvement based on Comparative Example 1.
[0079] The padding material comprises, in sequence along its thickness, a non-woven fabric layer, a waterproof membrane layer, a woven fabric reinforcement layer, a waterproof membrane layer, a first flame-retardant butyl rubber layer, a first intumescent coating, a fiberglass cloth layer, a second intumescent coating, a second flame-retardant butyl rubber layer, and a release protective layer.
[0080] Compared to Comparative Example 1, this comparative example adds a multi-layer fireproof structure consisting of a flame-retardant butyl rubber layer, an intumescent coating, and fiberglass cloth between the waterproof surface composite layer and the release protective layer. Specifically, the first and second flame-retardant butyl rubber layers are flame-retardant modified butyl rubbers, but the graphite-modified butyl rubber used in Example 1 is not employed.
[0081] The method for preparing the flame retardant-modified butyl rubber in this application involves blending a flame retardant and butyl rubber. The flame retardant is designated as Hi-D308, and the butyl rubber is designated as HRB0810FR.
[0082] The aforementioned underlayment was used in a roofing system for fire performance testing. Testing was conducted according to ICC-ES AC 188-12 (Rev.15) and with reference to ASTM E108-25. The test system used 15 / 32-inch thick AC-grade fir plywood. A layer of underlayment was laid on the plywood surface through its self-adhesive layer, with adjacent underlayments overlapping by approximately 4 inches laterally. A 26Ga vertically interlocking metal roof was installed on top of the underlayment.
[0083] The original plan was to conduct four combustion brand tests and two intermittent flame exposure tests.
[0084] The first test result for the roof in the fire test was a failure; a continuous flame appeared on the back of the wooden base during the test, which did not meet the acceptance criteria of ASTM E108-25, and subsequent tests were not carried out.
[0085] Comparative Example 1 shows the conventional waterproofing material used by the applicant before the fire resistance improvement. It mainly consists of non-woven fabric, a waterproof membrane, woven fabric, ordinary butyl rubber, and a release liner. In the fire resistance test, a sustained flame appeared on the back of the substrate of one of the four tested roofs, resulting in the roof failing to obtain the corresponding rating. This demonstrates that while conventional waterproofing materials provide waterproofing and substrate adhesion, their ability to inhibit heat and flame propagation to the wooden substrate under strong fire conditions is limited.
[0086] It should be noted that there are differences in the roofing materials and plywood thickness used in Comparative Example 1, Comparative Example 2, and Example 1. Comparative Example 1 uses 3 / 8-inch thick AC-grade fir plywood and three-piece asphalt shingles, while Comparative Example 2 and Example 1 use 15 / 32-inch thick AC-grade fir plywood and 26 Ga stand-fit metal roofing. Therefore, Comparative Example 1 is mainly used to illustrate the applicant's technical background of improving conventional waterproofing materials to waterproof and fireproofing materials with specialized fire-resistant structures, and is not used as a quantitative performance comparison under strictly single-factor conditions with the results of subsequent tests.
[0087] The test conditions for Comparative Example 2 and Example 1 are comparable. Both used 15 / 32-inch thick AC-grade fir plywood as the base layer, with a layer of self-adhesive padding laid on the base layer surface, and a 26 Ga vertically interlocking metal roof installed on top of the padding. The test slope was 5:12 for both, and the Class A fire resistance performance was tested according to ICC-ES AC 188-12 (Rev.15) and with reference to ASTM E108-25.
[0088] Regarding the padding structure, both Comparative Example 2 and Example 1 have intumescent coatings on both sides of the glass fiber cloth and flame-retardant butyl rubber layers on the outside of the two intumescent coatings. The main difference between the two is that the flame-retardant butyl rubber used in Comparative Example 2 is not modified by the graphite method described in this application, while the first and second intumescent butyl rubber layers in Example 1 use graphite-modified butyl rubber. The expandable graphite is pre-treated with a treatment solution formed by titanate coupling agent and naphthenic oil before being mixed with the butyl rubber system.
[0089] Test results showed that Comparative Example 2 failed the first combustion brand test due to a continuous flame on the back of the substrate, and subsequent tests were stopped immediately; while Example 1 passed all four combustion brand tests and two intermittent flame exposure tests, and no continuous combustion was observed on the back of the substrate.
[0090] This demonstrates that, based on a composite fireproof structure comprising fiberglass cloth and a double-sided intumescent coating, further employing the graphite-modified butyl rubber described in this application to form a first intumescent butyl rubber layer and a second intumescent butyl rubber layer can further improve the fire-resistant barrier performance of the composite structure under continuous fire source conditions.
[0091] Its mechanism of action is that after surface treatment, the dispersion and interfacial bonding of expandable graphite in the butyl rubber organic system are improved. While maintaining the thermal expansion capacity of expandable graphite, it helps to reduce the fire-resistant weak areas caused by local graphite aggregation. During the heating process, the expandable graphite in the first and second expandable butyl rubber layers expands and together with the expansion structure formed by the expansion coatings on both sides of the fiberglass cloth, it forms a multi-layer heat insulation barrier area. The fiberglass cloth continues to provide heat-resistant skeleton support after the expansion material is heated, thereby reducing the possibility of flames and heat continuing to spread to the wood substrate along the thickness direction.
[0092] Example 2 This embodiment is basically the same as Embodiment 1, except for the thickness of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer.
[0093] In this embodiment, the thicknesses of the first expandable butyl rubber layer, the first expandable coating layer, the glass fiber cloth layer, the second expandable coating layer, and the second expandable butyl rubber layer are 0.30 mm, 0.005 mm, 0.40 mm, 0.005 mm, and 0.30 mm, respectively, and their thickness ratio is 0.30∶0.005∶0.40∶0.005∶0.30.
[0094] Except for the thickness parameters mentioned above, the composition of the waterproof surface composite layer, the type and modification method of expandable graphite, the formulation of the expandable butyl rubber, the composition of the expandable coating, and the preparation method of the padding material are all the same as in Example 1.
[0095] The test results showed that the expanded barrier layer thickness of the pad material obtained in this embodiment was approximately 2.7 mm, the highest temperature on the unexposed side was approximately 182°C, and there was no sustained flame within 30 minutes. The fire resistance test result was passed.
[0096] Example 3 This embodiment is basically the same as Embodiment 1, except for the thickness of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer.
[0097] In this embodiment, the thicknesses of the first expandable butyl rubber layer, the first expandable coating layer, the glass fiber cloth layer, the second expandable coating layer, and the second expandable butyl rubber layer are 0.40 mm, 0.020 mm, 0.60 mm, 0.020 mm, and 0.60 mm, respectively, and their thickness ratio is 0.40∶0.020∶0.60∶0.020∶0.60.
[0098] Except for the thickness parameters mentioned above, the other raw materials, composition and preparation conditions are the same as in Example 1.
[0099] The test results showed that the expanded barrier layer thickness of the pad material obtained in this embodiment was approximately 4.8 mm, the highest temperature on the unexposed side was approximately 148°C, and there was no sustained flame within 30 minutes. The fire resistance test result was passed.
[0100] Example 4 This embodiment is used to examine the effect of the thickness of the second expanded butyl rubber layer relative to the thickness of the first expanded butyl rubber layer.
[0101] Except for the thickness of the second expanded butyl rubber layer, all other conditions in this embodiment are the same as in Example 1.
[0102] The thickness of the first expanded butyl rubber layer remains at 0.35 mm, and the thickness of the second expanded butyl rubber layer is adjusted to 0.40 mm; the thicknesses of the first expanded coating, the glass fiber cloth layer, and the second expanded coating remain at 0.01 mm, 0.50 mm, and 0.01 mm, respectively.
[0103] Therefore, the thickness ratio of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer is 0.35∶0.01∶0.50∶0.01∶0.40.
[0104] Compared with Example 1, this example only reduces the thickness of the second intumescent butyl adhesive layer to examine the effect of the adhesive layer thickness near the substrate on the substrate's bonding performance and heat barrier performance.
[0105] The test results showed that the expanded barrier layer thickness of the pad material obtained in this embodiment was about 3.5 mm, the highest temperature on the unexposed side was about 165°C, and there was no sustained flame within 30 minutes. The fire resistance test result was passed. Its 180° peel strength decreased by about 8% compared with Example 1.
[0106] Table 1. Influence of different combinations of fire-resistant functional layer thicknesses on the fire-resistant and heat-insulating performance of the padding material. Note: The five middle layers in the table are, in order, the first intumescent butyl rubber layer, the first intumescent coating layer, the fiberglass cloth layer, the second intumescent coating layer, and the second intumescent butyl rubber layer; "Pass" indicates that the sample did not exhibit a sustained flame within the 30-minute test period.
[0107] As can be seen from Examples 1 to 4, under the same or basically the same conditions and other components and test conditions, as the overall thickness of the first intumescent butyl rubber layer, the intumescent coating, the glass fiber cloth layer and the second intumescent butyl rubber layer increases, the overall thickness of the barrier layer formed after expansion increases, and the highest temperature of the unexposed surface decreases accordingly.
[0108] In Example 2, the overall thickness of the fire-resistant functional layer is relatively small, with an expanded barrier layer thickness of approximately 2.7 mm and a maximum temperature on the unexposed surface of approximately 182°C. In Example 1, increasing the overall thickness of the fire-resistant functional layer increased the expanded barrier layer thickness to approximately 4.2 mm, and reduced the maximum temperature on the unexposed surface to approximately 154°C. In Example 3, further increasing the thickness of each fire-resistant functional layer further increased the expanded barrier layer thickness to approximately 4.8 mm, and reduced the maximum temperature on the unexposed surface to approximately 148°C. These results indicate that increasing the overall thickness of the fire-resistant functional layer is beneficial for increasing the thickness of the heated barrier layer and reducing heat transfer to the unexposed surface.
[0109] The possible mechanism of action lies in the fact that the expandable graphite in the expandable butyl rubber layer and the expandable coating expands along the thickness direction after being heated, forming a barrier layer with a porous structure. As the initial amount of expandable material increases, the amount of expandable graphite participating in the expansion per unit area of the pad increases accordingly, thereby forming a thicker heat-resistant barrier structure. This barrier structure can extend the heat transfer path between the flame and the substrate, and reduce the heat transfer rate by utilizing its internal pores, thereby slowing down the transfer of heat to the unexposed surface and the substrate.
[0110] Meanwhile, the fiberglass cloth layer in the middle does not primarily rely on its own expansion for heat insulation, but rather acts as a high-temperature resistant skeleton to support the expanding materials on both sides. The barrier structure formed by the thermal expansion of expandable graphite may crack, detach, or locally shrink under the influence of flame erosion and hot air currents. The fiberglass cloth layer can bear and constrain the expanding structure, helping to maintain the continuity and integrity of the barrier layer. Therefore, the fireproof and heat-insulating effect of this application does not simply originate from an increase in material thickness, but is achieved by a composite barrier structure formed by the expandable butyl rubber layer, the expandable coating, and the fiberglass cloth layer.
[0111] Example 4 further demonstrates that the thickness of the second intumescent butyl rubber layer has a significant impact on the fireproof and heat-insulating performance of the gasket and the adhesion performance of the substrate. Compared with Example 1, Example 4 only reduced the thickness of the second intumescent butyl rubber layer from 0.55 mm to 0.40 mm, resulting in a reduction in the thickness of the expanded barrier layer from approximately 4.2 mm to approximately 3.5 mm, an increase in the maximum temperature on the unexposed side from approximately 154°C to approximately 165°C, and a decrease in the 180° peel strength of approximately 8%.
[0112] The reason for this may be that the second expandable butyl rubber layer is located on the side of the pad material closest to the substrate, simultaneously serving as both an expansion barrier and a substrate adhesive. When this layer has an appropriate thickness, it can, on the one hand, increase the amount of expandable graphite per unit area near the substrate, creating a more sufficient end-barrier structure in front of the substrate; on the other hand, a thicker pressure-sensitive butyl rubber layer can more fully fill the microscopic irregularities and local gaps on the substrate surface, increasing the actual contact area between the rubber layer and the substrate, thereby improving the substrate adhesion stability. Therefore, setting the second expandable butyl rubber layer to be thicker than the first expandable butyl rubber layer is beneficial for balancing both adhesion performance and expansion barrier performance near the substrate.
[0113] The results of Examples 1 and 3 also show that the performance improvement resulting from increasing the thickness of the fire-resistant functional layers does not increase proportionally. In Example 3, the thickness of each fire-resistant functional layer was increased compared to Example 1, but the thickness of the expanded barrier layer only increased from approximately 4.2 mm to approximately 4.8 mm, and the maximum temperature on the unexposed surface decreased from approximately 154°C to approximately 148°C. Simultaneously, the product thickness and material usage also increased accordingly. Therefore, the thickness combination of 0.35∶0.01∶0.50∶0.01∶0.55 used in Example 1 achieves a better overall balance between fire-resistant and heat-insulating performance, substrate adhesion performance, product thickness, and material usage.
[0114] This set of examples is used to verify the effect of expandable graphite on the padding layer. Example 5 This embodiment is basically the same as Embodiment 1, except for the amount of treatment liquid used in the preparation of modified expandable graphite.
[0115] Based on the mass of expandable graphite before treatment, the amount of treatment liquid added is 0.10% of the mass of expandable graphite. During the treatment process, the expandable graphite is placed in a high-speed mixer, and the treatment liquid is sprayed in evenly while stirring. Stirring is continued for 5 minutes to obtain modified expandable graphite.
[0116] Except for the amount of treatment liquid, the other raw materials, formula, mixing conditions, padding layer structure and preparation method are the same as in Example 1.
[0117] Example 6 This embodiment is basically the same as embodiment 5, except that the amount of treatment liquid added is 3% of the mass of expandable graphite before treatment.
[0118] Except for the amount of treatment solution used, all other conditions were the same as in Example 5.
[0119] Example 7 This Example 7 is basically the same as Example 5, except that the expandable graphite is not treated with a treatment liquid and is used directly to prepare expandable butyl rubber.
[0120] Except for whether or not a treatment liquid is used to treat the expandable graphite, the other raw materials, formulation, mixing conditions, padding layer structure and preparation method are the same as in Example 5.
[0121] Comparative Example 3 This comparative example is basically the same as Example 5, except that the amount of treatment liquid added is 5.0% of the mass of expandable graphite before treatment.
[0122] Except for the amount of treatment solution used, all other conditions were the same as in Example 5.
[0123] Comparative Example 4 This comparative example is basically the same as Example 5, except that the amount of treatment liquid added is 10.0% of the mass of expandable graphite before treatment.
[0124] Except for the amount of treatment solution used, all other conditions were the same as in Example 5.
[0125] Table 2. Effect of treatment solution dosage on the expansion properties of expandable graphite and the adhesion properties of the adhesive layer. Note: The expansion volume retention rate R is the ratio of the expansion volume of expandable graphite after treatment with the corresponding amount of treatment solution to the expansion volume of untreated expandable graphite raw material. The expansion volume of each group was determined using the same sample measurement method, heating temperature, holding time, and volume reading method. Example 7 was untreated, and its R was recorded as 1.00 as a baseline.
[0126] Examples 1, 5-7, and Comparative Examples 3-4 are used to illustrate the effect of the amount of treatment solution composed of titanate coupling agent and naphthenic oil on the expansion performance of expandable graphite and the bonding performance of expandable butyl rubber.
[0127] As shown in Table 2, the expansion volume of untreated expandable graphite is 220 mL / g, and the 180° peel strength of the adhesive layer made from this graphite is 11.2 N / mm. When the amount of treatment solution is 0.10% of the mass of expandable graphite, the expansion volume of the treated graphite is 213 mL / g, with an expansion volume retention rate of 0.97, and the 180° peel strength of the adhesive layer is 11.3 N / mm. When the amount of treatment solution is increased to 1.0%, the expansion volume of the treated graphite is 208 mL / g, with an expansion volume retention rate of 0.95, and the 180° peel strength of the adhesive layer increases to 12.3 N / mm. When the amount of treatment solution is further increased to 1.5%, the expansion volume of the treated graphite is 200 mL / g, the expansion volume retention rate still reaches 0.91, and the 180° peel strength of the adhesive layer increases to 12.8 N / mm, which is the highest value in this group of experiments.
[0128] The above results indicate that within the range of increasing treatment solution dosage from 0.10% to 3%, the overall 180° peel strength of the adhesive layer improves with increasing treatment solution dosage. Although the expansion volume of graphite gradually decreases after treatment, its expansion volume retention rate remains no less than 0.90, indicating that this dosage range can improve the adhesive layer bonding performance while maintaining a high expansion capacity of expandable graphite. Specifically, when the treatment solution dosage is 1.5%, the 180° peel strength of the adhesive layer reaches 12.8 N / mm, while the expansion volume retention rate is 0.91, thus exhibiting good comprehensive performance under the experimental conditions.
[0129] The possible mechanism of action lies in the fact that expandable graphite, being a layered carbon material, exhibits interfacial compatibility differences with organic components such as butyl rubber, polyisobutylene, petroleum resins, and naphthenic oils. When untreated expandable graphite is directly added to the adhesive compound, graphite particles easily form localized agglomerates, resulting in graphite-rich and graphite-depleted regions within the compound. Graphite-rich regions may disrupt the continuous phase of the butyl rubber and reduce the effective contact area between the adhesive layer and the bonded surface, thereby limiting the adhesive bonding performance.
[0130] The naphthenic oil in the treatment solution wets the surface of expandable graphite and acts as a dispersion carrier for the titanate coupling agent, ensuring a more uniform distribution of the agent on the graphite particle surface. The titanate coupling agent helps reduce the interfacial differences between graphite and the organic binder, improving the dispersion of graphite in the butyl rubber continuous phase. As the amount of treatment solution increases within a suitable range, graphite agglomerates in the binder decrease, improving the integrity of the butyl rubber continuous phase and the effective contact between the binder layer and the substrate, thus gradually increasing the 180° peel strength of the binder layer. Uniform graphite distribution also facilitates more uniform expansion of graphite in different regions upon heating, resulting in a more continuous expansion barrier structure.
[0131] However, a higher amount of treatment solution is not necessarily better. When the amount of treatment solution increased to 5.0%, the 180° peel strength of the adhesive layer decreased to 10.5 N / mm; when the amount of treatment solution was further increased to 10.0%, the 180° peel strength of the adhesive layer decreased to 7.5 N / mm, both of which were lower than the peel strength of the corresponding adhesive layer for untreated graphite.
[0132] The reason may be that, exceeding the amount required for effective wetting and coating of the graphite surface, the excess treatment liquid cannot be completely and stably bound or distributed on the surface of the graphite particles, but remains in the continuous phase of the rubber compound, and may migrate or precipitate to the surface of the rubber layer during mixing, molding, or placement. Excess naphthenic oil will have a strong plasticizing effect on the rubber compound, reducing the cohesive strength of the rubber layer; excessive titanate coupling agent and its carried oily components may also form a low-strength interface between the rubber layer and the substrate, reducing the effective contact between the butyl rubber and the substrate, ultimately leading to a decrease in peel strength.
[0133] On the other hand, as the amount of treatment solution increases, the organic treatment layer on the surface of the graphite particles thickens, which may hinder the release of interlayer gas and the unfolding of the sheets after the expandable graphite is heated, resulting in a decrease in the expansion volume of the treated graphite. Therefore, the amount of treatment solution needs to be balanced between improving the dispersibility and adhesive bonding properties of graphite and maintaining the graphite's expansion capacity.
[0134] Based on the results of this group of experiments, when the amount of treatment liquid is 0.10% to 3% of the mass of expandable graphite, it can improve the adhesion performance of the adhesive layer while maintaining the expansion volume retention rate of the modified expandable graphite at no less than 0.90. Among them, the overall performance is better when the amount of treatment liquid is 1.0% to 1.5%, and the 180° peel strength of the adhesive layer is the highest when the amount of treatment liquid is 1.5%.
[0135] This set of examples is used to verify the influence of expandable graphite particle size on expansion performance, adhesive bonding performance, and thermal insulation layer formation. Example 8 This embodiment is basically the same as Embodiment 1, except that the particle size of the expandable graphite used is 50 mesh.
[0136] The 50-mesh expandable graphite used had an expansion volume of 260 mL / g measured under the specified test conditions. Except for the particle size of the expandable graphite, the other modification conditions, binder formulation, composition of the expanded coating, thickness of each layer, and preparation method of the pad material were the same as in Example 1.
[0137] According to the test, the 180° peel strength of the adhesive obtained in this embodiment is 7.4 N / mm, and the thickness of the heat insulation layer of the obtained pad material after heating is about 3.7 mm.
[0138] Example 9 This embodiment is basically the same as Embodiment 1, except that the particle size of the expandable graphite used is 200 mesh.
[0139] The 200-mesh expandable graphite used had an expansion volume of 165 mL / g measured under the specified test conditions. Except for the particle size of the expandable graphite, the other modification conditions, adhesive formulation, composition of the expanded coating, thickness of each layer, and preparation method of the pad material were the same as in Example 1.
[0140] According to the test, the 180° peel strength of the adhesive obtained in this embodiment is 13.2 N / mm, and the thickness of the heat insulation layer of the obtained pad material after heating is about 1.2 mm.
[0141] Table 3. Effect of expandable graphite particle size on expansion performance and adhesive properties As can be seen from Table 3, the particle size of expandable graphite mainly affects two mutually restrictive properties: first, the expansion capacity of expandable graphite after heating and the thickness of the heat insulation layer formed by it; second, the dispersion state of expandable graphite in the butyl rubber system and the bonding performance of the adhesive layer.
[0142] Example 8 used 50-mesh expandable graphite, with an expansion volume of 260 mL / g, the highest among the three groups of tests. The resulting insulation layer thickness after expansion was approximately 3.7 mm. However, the 180° peel strength of the adhesive layer made with this graphite was only 7.4 N / mm, significantly lower than that of Examples 1 and 9. Example 9 used 200-mesh expandable graphite, with an expansion volume reduced to 165 mL / g. The insulation layer thickness after expansion was approximately 1.2 mm, but the 180° peel strength of the adhesive layer increased to 13.2 N / mm.
[0143] The above results indicate that as the mesh size of expandable graphite increases, i.e., the graphite particles gradually decrease, its expansion volume and the thickness of the expanded insulation layer gradually decrease, while the 180° peel strength of the adhesive layer gradually increases. This suggests that graphite particle size has opposite effects on the expansion insulation performance and the adhesive bonding performance.
[0144] The possible mechanism of action is that 50-mesh expandable graphite has a relatively large particle size, a relatively complete graphite sheet structure, and a long sheet unfolding path. After being exposed to sufficient heat, the expansion components between the sheets release gas and drive the graphite sheets to unfold, allowing individual particles to form a large expansion volume, thus exhibiting a high expansion volume and forming a thicker insulation layer after the pad is heated.
[0145] However, 50-mesh graphite particles are relatively large, and their size is close to the initial thickness of the expanded butyl adhesive layer, making it difficult to form a uniform and continuous dispersion in the adhesive. Larger graphite particles can easily cause local particle enrichment, surface undulation of the adhesive layer, and stress concentration, and reduce the effective contact area between the continuous butyl adhesive phase and the substrate, thus reducing the 180° peel strength of the adhesive layer.
[0146] Furthermore, larger graphite particles can negatively impact the processing performance of the adhesive compound. During extrusion, coating, or calendering, 50-mesh graphite particles tend to accumulate at the die or in narrow flow channels, causing die blockage, uneven material output, and fluctuations in adhesive layer thickness. In severe cases, this can disrupt the production process. Therefore, although 50-mesh graphite has a high expansion volume, its adhesive bonding and processing performance are relatively poor.
[0147] When the particle size of expandable graphite is reduced to 200 mesh, the number of particles per unit mass of graphite increases. Smaller particles can be more uniformly dispersed in the continuous phase of butyl rubber, making it less likely to form large local defects. At the same time, smaller particles have less impact on the surface smoothness of the adhesive layer and the effective contact area between the adhesive layer and the substrate. As a result, the 180° peel strength of the adhesive layer increases to 13.2 N / mm, and its performance through the die and flow channel is relatively good.
[0148] However, when the graphite particle size is too small, the effective structural size of a single particle that can participate in interlayer expansion decreases accordingly. The possibility of graphite particles being sheared during processing also increases, thus reducing its volume of expansion per unit mass after heating. Therefore, although 200-mesh graphite is beneficial for improving the adhesion and processing stability of the adhesive layer, its expansion volume is only 165 mL / g, and the thickness of the expanded insulating layer is only about 1.2 mm, making its insulating layer forming ability weaker than that of 50-mesh and 100-mesh graphite.
[0149] Example 10 This embodiment is used to examine the degree to which expandable graphite retains its expansion properties after surface treatment.
[0150] Using the same expandable graphite as in Example 1 as the raw material, the surface was treated with a treatment solution formed by titanate coupling agent and naphthenic oil according to the method described in Example 1.
[0151] The expansion volume of unmodified and modified expandable graphite of the same mass was measured under the same test temperature, heating time and test device conditions.
[0152] Let E0 be the expansion volume of graphite before modification and E1 be the expansion volume of graphite after modification. The expansion volume retention rate R is calculated according to the following formula: R = E1 / E0.
[0153] In this embodiment, R is controlled to be no less than 0.90.
[0154] The mechanism is that the main purpose of surface modification of expandable graphite in this application is to improve the wettability and dispersibility of graphite in butyl rubber, rather than to change the expansion and flame retardant mechanism of graphite itself. The basis for the fire-retardant function of expandable graphite is still its rapid expansion along the interlayer direction after being heated, forming a low-density, porous worm-like expanded structure.
[0155] If the surface treatment is too strong, although it may further improve the interfacial compatibility between graphite and the adhesive, excessive treatment agents covering the graphite particles may restrict the rapid unfolding of the interlayer structure, resulting in a significant decrease in the expansion volume per unit mass of graphite. In this case, although graphite is easier to mix into the adhesive, the core high-temperature expansion insulation capability of this application is lost.
[0156] This set of examples is used to verify the effect of the treatment solution on modified expandable graphite. This was used to investigate the relationship between the expansion materials of the first and second expanded butyl rubber layers.
[0157] The first and second expanded butyl rubber layers respectively satisfy the following formulas: Wherein, c1 and c2 are the unit volume expandable graphite masses in the first and second expandable butyl rubber layers, respectively; h1 and h2 are the thicknesses of the first and second expandable butyl rubber layers, respectively; and E1 and E2 are the expansion volumes of the corresponding expandable graphite measured under the same test methods and conditions.
[0158] Example 11 By adjusting the amount of expandable graphite added in the first expandable butyl rubber layer, Rc is made to be approximately 1.00.
[0159] Except for the amount of expandable graphite added in the first expandable butyl rubber layer, all other conditions were the same as in Example 1.
[0160] Example 12 This embodiment is basically the same as Embodiment 10, except that the amount of expandable graphite added in the first expandable butyl rubber layer is adjusted so that Rc is about 1.20.
[0161] The remaining conditions are the same as in Example 11.
[0162] Comparative Example 3 This embodiment is basically the same as embodiment 10, except that the amount of expandable graphite added in the first expandable butyl rubber layer is adjusted so that Rc is about 0.8.
[0163] The remaining conditions are the same as in Example 11.
[0164] Comparative Example 4 This embodiment is basically the same as Embodiment 10, except that the amount of expandable graphite added in the first expandable butyl rubber layer is adjusted so that Rc is about 1.20.
[0165] The remaining conditions are the same as in Example 1.3.
[0166] Table 4. Influence of the relationship between the expansion capacity of the two intumescent butyl rubber layers on fire resistance. When Rc is approximately 0.80, the potential expansion capacity of the first intumescent butyl rubber layer is significantly lower than that of the second intumescent butyl rubber layer. During heating, the expansion on both sides is asynchronous, with insufficient expansion support formed on the side closer to the waterproof surface, while the expansion is stronger on the side closer to the substrate. This easily leads to uneven expansion stress on both sides of the fiberglass cloth. Such uneven expansion may cause local cracking, displacement, or weak areas in the expansion layer, making it easier for high-temperature gases and heat to propagate to the substrate through local defects. Therefore, the highest temperature on the unexposed surface of Comparative Example 3 rising to approximately 218°C and exhibiting a sustained flame is consistent with this mechanism.
[0167] When Rc is increased to 1.00–1.20, the potential expansion capacity per unit area of the two adhesive layers is relatively close. After flame treatment, the first and second adhesive layers can form a more coordinated expansion structure on both sides of the fiberglass cloth. The expansion force on both sides of the fiberglass cloth is more balanced, making it easier to stay in the middle position of the expansion barrier layer and continue to play a supporting role.
[0168] This two-sided matching has another important effect: it can reduce the tearing or detachment of the expansion layer caused by excessive expansion on one side, and also reduce the local weak areas formed by insufficient expansion on the other side. Therefore, the final adhesive layer expansion body - coating expansion body - glass fiber skeleton - coating expansion body - adhesive layer expansion body is more continuous in the thickness direction.
[0169] This explains why, when Rc is 1.00, 1.10, and 1.20, the proposed maximum temperature on the back surface remains around 151–163°C, and there is no sustained flame within 30 minutes.
[0170] The best performance was observed when Rc was approximately 1.10, which is technically sound. Since the second expanding butyl adhesive layer is close to the wood substrate, it also needs to bond, seal, and fill microscopic unevenness on the substrate surface; therefore, the second adhesive layer often needs to have a relatively large actual thickness. To avoid the potential expansion capacity of the second adhesive layer being significantly higher than that of the first adhesive layer simply because it is thicker, the graphite content per unit volume and the graphite expansion capacity in both adhesive layers can be adjusted to make the potential expansion of the first adhesive layer slightly higher or close to that of the second adhesive layer, thus achieving overall balance.
[0171] When Rc further increases to 1.40, the opposite imbalance occurs. The expansion effect of the first intumescent butyl rubber layer is significantly higher than that of the second rubber layer, resulting in excessive expansion near the fire-exposed side, while the insulation capacity at the end near the base layer is relatively insufficient. Excessive expansion on the first side may also exert a large unidirectional displacement on the intermediate fiberglass cloth and intumescent coating, causing local misalignment, cracking, or interlayer separation in the multilayer structure, thereby weakening the continuous insulation barrier throughout the thickness direction. Therefore, although the total graphite content in Comparative Example 4 may not have decreased, its effective fire resistance performance has actually decreased, with the highest temperature on the unexposed side rising to approximately 211°C and persistent flames appearing.
[0172] The fire-retardant effect of the first and second intumescent butyl adhesive layers is not solely determined by the graphite content of a single layer, but is jointly related to the adhesive layer thickness, the mass of graphite per unit volume, and the expansion properties of the graphite itself. When the potential expansion capacity per unit area of the two adhesive layers is appropriately matched, a relatively balanced, continuous, and stable expansion insulation structure can be formed on both sides of the fiberglass cloth. When the difference in potential expansion capacity between the two sides is too large, uneven expansion, local cracking, or weak areas are likely to occur, leading to increased heat transfer to the substrate. Therefore, controlling Rc within the range of 1.0 to 1.2 is beneficial for balancing the balance of the expansion structure on both sides as well as the bonding and insulation requirements on the side closer to the substrate.
[0173] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A waterproof and fireproof mat material, characterized in that, It includes a waterproof surface composite layer, a first intumescent butyl rubber layer, a first intumescent coating layer, a fiberglass cloth layer, a second intumescent coating layer, a second intumescent butyl rubber layer, and a release protective layer, which are sequentially laminated along the thickness direction. The waterproof surface composite layer is a composite layer with waterproof effect; Both the first and second expandable butyl rubber layers comprise expandable graphite and butyl rubber. Both the first and second expanding coatings comprise expandable graphite and a binder; The release protective layer can be peelably applied to the surface of the second expanded butyl rubber layer opposite to the second expanded coating.
2. The waterproof and fireproof mat material according to claim 1, characterized in that, The thickness ratio of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer is (0.30-0.40):(0.005-0.02):(0.4-0.6):(0.005-0.02):(0.30-0.60).
3. The waterproof and fireproof mat material according to claim 2, characterized in that, The thickness of the second expanded butyl rubber layer is greater than the thickness of the first expanded butyl rubber layer.
4. The waterproof and fireproof mat material according to claim 2, characterized in that, The thickness ratio of the first expanded butyl rubber layer, the first expanded coating layer, the glass fiber cloth layer, the second expanded coating layer, and the second expanded butyl rubber layer is 0.35:0.01:0.5:0.01:0.
55.
5. The waterproof and fireproof mat material according to claim 1, characterized in that, The expandable graphite is modified expandable graphite, which is obtained by coating expandable graphite with a treatment liquid, which is formed by mixing titanate coupling agent and naphthenic oil.
6. The waterproof and fireproof mat material according to claim 5, characterized in that, The amount of the treatment liquid is 0.1% to 3% of the mass of expandable graphite, and the mass ratio of the titanate coupling agent to the naphthenic oil is 1-3:
1.
7. The waterproof and fireproof mat material according to claim 1, characterized in that, The expandable graphite has a particle size of 50-200 mesh and a volume expansion ratio of not less than 150.
8. The waterproof and fireproof mat material according to claim 1, characterized in that, The waterproof surface composite layer comprises a non-woven fabric layer, a first waterproof membrane layer, a woven fabric reinforcement layer, and a second waterproof membrane layer, which are sequentially laminated together. The second waterproof membrane layer is bonded to the first expandable butyl rubber layer. The nonwoven fabric layer is a polypropylene nonwoven fabric layer, and the woven fabric reinforcement layer is a polypropylene woven fabric layer; both the first waterproof membrane layer and the second waterproof membrane layer are composite membrane layers containing polypropylene and polyethylene.
9. The waterproof and fireproof mat material according to claim 5, characterized in that, The ratio of the expansion volume of the modified expandable graphite to the expansion volume of the expandable graphite raw material used to prepare the modified expandable graphite is not less than 0.
90.
10. The waterproof and fireproof mat material according to claim 1, characterized in that, The first expanded butyl rubber layer and the second expanded butyl rubber layer satisfy the following: Where c1 and c2 are the mass of expandable graphite per unit volume, h1 and h2 are the thickness of the adhesive layer, and E1 and E2 are the expansion volumes of the corresponding expandable graphite materials measured using the same test method and test conditions.
Citation Information
Patent Citations
Fire-resistant roof system and membrane composite
CN105026660A
Smoke-suppression non-cured rubber bitumen waterproof coating material
CN105238271A
Fireproof butyl rubber and application thereof in multilayer composite fireproof coiled material
CN115232577A