A carbon fiber / thermoplastic polyurethane interlayer toughened composite material and a preparation method thereof

By introducing a TPU film between CFRP layers and employing a co-curing process, the problem of insufficient damping performance of CFRP composites under vibration and impact loads is solved, improving the material's energy dissipation and impact resistance, making it suitable for aerospace, marine equipment and other fields.

CN123129576APending Publication Date: 2026-11-20ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611273728.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional CFRP composite materials have insufficient damping performance under vibration and impact loads, which easily leads to matrix damage and interlayer delamination, affecting the load-bearing capacity and service life of the structure.

Method used

A thermoplastic polyurethane film (TPU film) is introduced between CFRP layers and a stable interfacial bond is formed through a co-curing process to construct a composite material that combines damping performance and high impact damage tolerance.

Benefits of technology

It significantly improves the vibration energy dissipation capacity and impact resistance of composite materials, enhances the damping performance and impact damage resistance of structures, and is suitable for high-requirement applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123129576A_ABST
    Figure CN123129576A_ABST
Patent Text Reader

Abstract

The application discloses a kind of carbon fiber / thermoplastic polyurethane interlayer toughened composite material and preparation method thereof, the carbon fiber / thermoplastic polyurethane interlayer toughened composite material includes: plain weave carbon fiber prepreg layer and thermoplastic polyurethane film, plain weave carbon fiber prepreg layer is overlapped and set multiple layers;Thermoplastic polyurethane film is in the form of single layer concentration or multiple layer distribution and is inserted between plain weave carbon fiber prepreg layer;The carbon fiber / thermoplastic polyurethane interlayer toughened composite material proposed in the application has the characteristics such as structural design flexible, preparation process simple, wide application range, etc., can be adjusted the thickness, quantity and spatial distribution position of thermoplastic polyurethane film to realize the synergistic regulation and control of composite material damping performance and impact resistance, has good application prospect in the field such as aerospace, marine equipment, etc. to light weight, damping performance and impact resistance have high requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite material technology, specifically relating to a carbon fiber / thermoplastic polyurethane interlaminar toughened composite material and its preparation method. Background Technology

[0002] As modern equipment continues to develop towards high-end and lightweight designs, carbon fiber reinforced polymer (CFRP) composites, with their advantages of high specific strength, high specific modulus, and good fatigue performance, have been widely used in aerospace, marine equipment, and rail transportation. However, with increasingly complex and harsh service environments, composite structures must not only meet high load-bearing capacity requirements but also possess excellent vibration damping and impact resistance to ensure their reliability under vibration and impact loads. Therefore, how to simultaneously improve the impact damage tolerance and damping performance of composite materials while maintaining their good static mechanical properties has become a key issue in promoting the further application of CFRP composites in modern equipment.

[0003] Currently, traditional CFRP composites mostly use thermosetting epoxy resins as the matrix, relying on carbon fiber reinforcement to achieve excellent mechanical properties. However, after epoxy resin cures, it forms a highly cross-linked three-dimensional network structure, which restricts the movement of molecular chain segments and weakens the material's internal energy dissipation capacity. This results in CFRP composites generally suffering from insufficient damping performance and limited vibration energy dissipation capacity. Furthermore, under impact loads, the composite material is prone to various forms of damage, including matrix damage, interlaminar delamination, and fiber damage, severely weakening the structure's remaining load-bearing capacity and service life. Summary of the Invention

[0004] To address the aforementioned problems, embodiments of the present invention propose a carbon fiber / thermoplastic polyurethane interlaminar toughened composite material and its preparation method.

[0005] The carbon fiber / thermoplastic polyurethane interlaminar toughened composite material (CF / TPU composite material) of the present invention comprises:

[0006] Plain weave carbon fiber prepreg layer, wherein multiple layers of the plain weave carbon fiber prepreg layer are overlapped;

[0007] Thermoplastic polyurethane film (TPU film), wherein the thermoplastic polyurethane film is interspersed between plain weave carbon fiber prepreg layers in a single-layer concentrated or multi-layer distributed manner.

[0008] Plain-weave carbon fiber prepreg is a semi-finished material formed by combining plain-weave carbon fiber fabric with a resin matrix. The carbon fiber fabric is arranged with warp and weft yarns to form a two-dimensional reinforcing structure, and the epoxy resin matrix is ​​pre-impregnated into the fibers to maintain the fabric shape and promote subsequent composite material molding.

[0009] The thermoplastic polyurethane film is uniformly coated with FG-767 surface treatment agent on both sides.

[0010] The thickness of the thermoplastic polyurethane film is 0.2 mm, 0.4 mm, or 0.8 mm.

[0011] The plain weave carbon fiber prepreg layer has 10 layers, and the thickness of a single plain weave carbon fiber prepreg layer is 0.2 mm.

[0012] The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material of the present invention includes the following steps:

[0013] S1. Preparation and surface treatment of thermoplastic polyurethane film: Thermoplastic polyurethane particles are prepared by melt extrusion process, and their surface is processed into a frosted surface. Then, the thermoplastic polyurethane film is subjected to surface treatment.

[0014] S2. Layup Design: The thermoplastic polyurethane film is inserted and laid into the plain weave carbon fiber prepreg layer in a single-layer concentrated or multi-layer distributed manner;

[0015] S3. Co-curing molding: After the layup is completed, the pre-fabricated laminate is sent into an autoclave for co-curing molding. During the curing process, the heating rate, curing temperature, holding time, cooling rate and molding pressure are controlled in a coordinated manner to form a stable interfacial bond between the thermoplastic polyurethane film and the epoxy resin matrix in the carbon fiber prepreg.

[0016] The surface treatment method in S1 is as follows: First, the surface of the thermoplastic polyurethane film is cleaned with isopropanol to remove surface oil and impurities; then, FG-767 surface treatment agent is evenly coated on both sides of the thermoplastic polyurethane film and left to stand at room temperature for 5 minutes to allow the FG-767 surface treatment agent to fully adhere to the surface of the thermoplastic polyurethane film.

[0017] The heating rate in S3 is 2℃ / min, the curing temperature is 100℃, the holding time is 5 h, and the cooling rate is 1℃ / min.

[0018] The specific steps of the co-curing molding are as follows: First, the temperature inside the tank is raised to 100°C at a constant heating rate, and the molding pressure is gradually applied to 0.6 MPa to promote resin flow and improve the interfacial wetting between the TPU film and the carbon fiber prepreg; then, it is kept at a constant temperature and pressure for 5 hours to promote the full curing of the epoxy resin and reduce the porosity inside the composite material; after the heat preservation stage, the temperature and pressure inside the tank are slowly reduced at a set rate to avoid residual stress concentration caused by excessive cooling or pressure change, thereby reducing the risk of warping or cracking of the laminate. After curing in the autoclave, the composite material laminate is finally obtained.

[0019] The length of the composite laminate = 450 mm, width = 450 mm, thickness =2~3 mm.

[0020] The beneficial effects of this invention are:

[0021] 1. This invention constructs a composite laminate with both adjustable damping performance and high impact damage tolerance by introducing a flexible TPU film with viscoelastic energy dissipation properties between the layers of a traditional CFRP. This method significantly improves the material's energy dissipation capacity and impact resistance during vibration while maintaining the high stiffness and strength characteristics of CFRP by adjusting the thickness and interlayer distribution of the TPU film.

[0022] 2. This invention effectively improves the interfacial bonding performance between the TPU film and the carbon fiber prepreg by cleaning and coating the TPU film surface with a treatment agent. Simultaneously, the autoclave co-curing process ensures a stable, integrated structure between the TPU film and the prepreg, avoiding the problems of insufficient interfacial bonding and poor structural stability associated with traditional surface bonding or assembly methods. Furthermore, under vibration or impact loads, the interlayer TPU film can dissipate external energy through its viscoelastic deformation and interfacial friction, and suppress the initiation and propagation of interlayer cracks under impact loads, thereby improving the vibration damping performance and impact damage resistance of the composite material.

[0023] 3. Compared with traditional CFRP, the CF / TPU composite material proposed in this invention has the advantages of flexible structural design, simple preparation process and wide applicability. The damping performance and impact resistance of the composite material can be synergistically controlled by adjusting the thickness, quantity and spatial distribution of TPU film. It has good application prospects in fields such as aerospace and marine equipment where there are high requirements for lightweight, damping performance and impact resistance. Attached Figure Description

[0024] Figure 1This is a schematic diagram of the structure of the carbon fiber / thermoplastic polyurethane interlayer toughened composite material of the present invention.

[0025] Figure 2 This is a temperature and pressure change curve of the composite material of the present invention during the curing process.

[0026] Figure 3 This is a schematic diagram of the vibration test platform of the present invention.

[0027] Figure 4 This is a schematic diagram of the composite material laminate of the present invention.

[0028] Figure 5 This is a schematic diagram of the vibration damping test specimen of the present invention.

[0029] Figure 6 This is a schematic diagram of the low-speed impact test specimen of the present invention.

[0030] Figure 7 These are the FRF curves of CFRP and the CF / TPU composite material specimens of the present invention.

[0031] Figure 8 The present invention is based on the FRF curve and combined with the half-power bandwidth method to calculate the first two bending modes of six composite material specimens.

[0032] Figure 9 The force-displacement curves of CFRP and CF / TPU composite laminates during low-speed impact testing are shown.

[0033] Figure 10 The results show the energy absorption of CFRP and CF / TPU composite laminates during low-speed impact testing. Detailed Implementation

[0034] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.

[0035] like Figure 1 As shown, the carbon fiber / thermoplastic polyurethane interlayer toughened composite material (CF / TPU composite material) of the present invention includes: a plain weave carbon fiber prepreg layer and a thermoplastic polyurethane film (TPU film), wherein multiple layers of the plain weave carbon fiber prepreg layer are overlapped; the thermoplastic polyurethane film is interspersed between the plain weave carbon fiber prepreg layers in a single-layer concentrated or multi-layer distributed manner.

[0036] Plain-weave carbon fiber prepreg is a semi-finished material formed by combining plain-weave carbon fiber fabric with an epoxy resin matrix. The carbon fiber fabric is arranged with warp and weft yarns interlaced to form a two-dimensional reinforcing structure. The resin matrix is ​​pre-impregnated into the fibers to maintain the fabric's shape and promote subsequent composite material molding. (The plain-weave carbon fiber prepreg mentioned here refers to commercially available materials.)

[0037] Both sides of the thermoplastic polyurethane film are uniformly coated with FG-767 surface treatment agent.

[0038] The thickness of the thermoplastic polyurethane film is 0.2 mm, 0.4 mm or 0.8 mm.

[0039] The plain weave carbon fiber prepreg layer has 10 layers, and the thickness of a single plain weave carbon fiber prepreg layer is 0.2mm.

[0040] The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material of the present invention includes the following steps:

[0041] S1. Preparation and Surface Treatment of Thermoplastic Polyurethane Film: The TPU film is prepared by melt extrusion of TPU particles and its surface is processed into a frosted surface to increase the surface roughness and effective contact area of ​​the TPU film, thereby improving the interfacial bonding between the resin matrix and the TPU film. In order to further improve the interfacial bonding performance between the TPU film and the epoxy resin prepreg, the TPU film must be surface treated before layup: First, the surface of the TPU film is cleaned with isopropanol to remove surface oil and impurities; then, FG-767 surface treatment agent is evenly coated on both sides of the TPU film and left to stand at room temperature for 5 minutes to allow the FG-767 surface treatment agent to fully adhere to the surface of the TPU film.

[0042] FG-767 is a surface treatment agent used to improve the interfacial bonding properties of polymers. It mainly comprises coupling components containing active functional groups, organic solvents, and interfacial wetting aids. By introducing an active interfacial layer onto the surface of the TPU film, it enhances the surface polarity and resin wetting ability of the TPU film, promoting the formation of a stable interfacial bond between the TPU film and the epoxy resin matrix.

[0043] S2. Layup Design: The thermoplastic polyurethane film is laid in a single-layer concentrated or multi-layer distributed manner in the plain weave carbon fiber prepreg layer.

[0044] To analyze the influence of TPU film thickness and interlayer distribution on the damping and impact resistance of composite materials, this invention designs six composite laminates by controlling the thickness and interlayer distribution of the TPU film, such as... Figure 1 As shown. The single-layer thickness of the plain-weave carbon fiber prepreg used is 0.2 mm. Among them, Figure 1 (a) Pure CFRP composite laminate without TPU film, serving as a control group; Figure 1 (b) is a CF / TPU composite laminate with a single TPU film laid in the center along the thickness direction of the laminate, denoted as CF / TPU-1. The thickness of the TPU film is 0.2 mm, 0.4 mm and 0.8 mm respectively, and the corresponding configurations are denoted as CF / TPU-1a, CF / TPU-1b and CF / TPU-1c respectively. Figure 1 (c) and Figure 1 (d) CF / TPU composite laminates with two and four layers of 0.2 mm thick TPU film laid symmetrically, respectively, are CF / TPU-2 and CF / TPU-4. It should be noted that the total thickness of the TPU film in CF / TPU-1b and CF / TPU-2 is 0.4 mm, and the total thickness of the TPU film in CF / TPU-1c and CF / TPU-4 is 0.8 mm. Thus, under the condition of the same total TPU usage, a comparison of two interlayer toughening configurations, namely single-layer centralized and multi-layer distributed, is achieved.

[0045] S3. Co-curing and molding: After the layup is completed, the precast laminate is placed in an autoclave for co-curing and molding. The temperature and pressure change curves during the curing process are shown in the figure. Figure 2 As shown, during the curing process, by synergistically controlling the heating rate, curing temperature, holding time, cooling rate, and molding pressure, a stable interfacial bond is formed between the thermoplastic polyurethane film and the epoxy resin matrix in the carbon fiber prepreg.

[0046] The specific steps of co-curing molding are as follows: First, the temperature inside the tank is raised to the curing temperature of 100℃ at a constant heating rate of 2℃ / min, and the molding pressure is gradually applied to 0.6 MPa to promote resin flow and improve the interfacial wetting between the TPU film and the carbon fiber prepreg. Then, the mixture is kept at a constant temperature and pressure for 5 hours to promote full curing of the epoxy resin and reduce the porosity inside the composite material. After the holding period, the temperature and pressure inside the tank are slowly reduced at a set rate of 1℃ / min to avoid residual stress concentration caused by rapid cooling or sudden pressure changes, thereby reducing the risk of warping or cracking of the laminate. Compared with traditional surface-bonded damping layers or assembly processes, the co-curing process has significant advantages in terms of interfacial bonding quality, service durability, and overall structural consistency. After curing in an autoclave, the aforementioned six types of composite material laminates are finally obtained.

[0047] To evaluate the vibration damping performance of CFRP and CF / TPU composite laminates, this invention conducts vibration damping tests according to ASTM E756 standard, and performs modal damping characteristic analysis on the laminates. The experimental platform is as follows: Figure 3As shown in the figure. In the experiment, an electromagnetic exciter was used to apply a fixed amplitude sweep frequency excitation to the specimen, and an accelerometer was used to collect the time-domain acceleration signals of the excitation end and the response end of the specimen.

[0048] The time-domain acceleration signals acquired at both ends of the specimen were converted into frequency-domain signals using a Fast Fourier Transform (FFT). A frequency response function (FRF) was constructed based on the frequency-domain excitation and response signals, and its expression is as follows:

[0049]

[0050] In the formula, Indicates FRF, This represents the frequency domain acceleration signal at the free end (response end). This represents the frequency-domain acceleration signal at the loading end (excitation end).

[0051] Based on the resonance peak in the frequency response function curve, the damping ratio of the first two bending modes of the composite laminate is calculated using the half-power bandwidth method. The half-power bandwidth method is based on the resonance peak bandwidth. With natural frequency Calculate the modal damping ratio, where the bandwidth Determined by the following formula:

[0052]

[0053] In the formula, and These represent the frequency response function amplitude decreasing to the resonant peak value, respectively. When the frequency is doubled, the corresponding low-frequency side frequency and high-frequency side frequency on both sides of the resonance peak.

[0054] According to the half-power bandwidth method, the modal damping ratio of the composite material It can be represented as:

[0055]

[0056] By comparing the damping ratios of the first two bending modes of CFRP and various CF / TPU composite laminates, the influence of the thickness and interlayer distribution of TPU film on the damping performance of composite materials was investigated.

[0057] Furthermore, to evaluate the impact of the introduction of TPU film on the impact resistance of the composite material, this invention conducted low-velocity impact tests on the composite laminate according to ASTM D7136 standard, extracted the force-displacement curves during the impact process, and calculated the absorbed energy using the following formula:

[0058]

[0059] In the formula, This represents the energy absorbed during the impact. and These represent the impact force and displacement during the impact process, respectively. By analyzing the force-displacement curves and energy absorption of the impact test, and combining the results of ultrasonic C-scan detection of the internal damage area of ​​the specimen, the impact resistance of composite laminates with different configurations is comprehensively evaluated.

[0060] Example

[0061] To highlight the damping and impact resistance properties of CF / TPU composite materials, pure CFRP composite materials were selected as a control. Figure 4 This is a schematic diagram of composite laminates, showing the lengths of six different composite laminates. =450mm, width =450mm, thickness =2~3mm (slightly varies depending on the thickness and number of layers of the TPU film). Specimens for vibration damping tests and low-velocity impact tests are as follows: Figure 5 and Figure 6 As shown, all specimens were prepared by waterjet cutting of laminated plates, therefore the specimen thickness is consistent with the corresponding laminate thickness. The length of the vibration damping specimen... =300mm, width =20mm. Length of the low-velocity impact specimen. =150mm, width =100mm.

[0062] Figure 7 FRF curves of CFRP and CF / TPU composite specimens. Figure 8 The damping ratios of the first two bending modes of six composite material specimens are calculated based on FRF curves and the half-power bandwidth method. Figure 8 It was found that, compared with traditional CFRP composites, the damping ratios of the first and second bending modes of all CF / TPU composites were improved, indicating that the introduction of TPU flexible film between carbon fiber composite layers can effectively enhance the damping performance and vibration suppression capability of the laminate during vibration.

[0063] Analysis of vibration damping test results for CF / TPU-1a, CF / TPU-1b, and CF / TPU-1c composites reveals that as the TPU film thickness increases from 0.2 mm to 0.8 mm, the damping ratios of both the first and second bending modes of the composite specimens gradually increase. This is because the TPU film, centrally laid along the thickness direction of the laminate, can form a locally high-damping region. Under alternating loads, the TPU layer undergoes periodic shear deformation. Benefiting from the viscoelastic characteristics of TPU, its stress response lags behind its strain response, causing some vibration energy to dissipate as heat. Therefore, with increasing TPU film thickness, the effective damping region expands accordingly, and the damping performance of the CF / TPU composite material is enhanced.

[0064] Further analysis of the experimental results of CF / TPU-2 and CF / TPU-4 composites reveals that CF / TPU-4 exhibits a higher modal damping ratio. Compared to CF / TPU-2, CF / TPU-4 has more TPU layers and interlayer interfaces, resulting in more energy dissipation and vibration suppression pathways within the composite material. Unlike CF / TPU-1, CF / TPU-2 and CF / TPU-4 can further improve the damping performance of the composite material by increasing the number of interfaces, allowing more regions to participate in energy dissipation during vibration.

[0065] It should be noted that the damping enhancement mechanisms of single-layer centralized and multi-layer distributed CF / TPU composite materials differ. Single-layer structures primarily rely on the TPU layers to create larger localized high-damping regions for energy dissipation, while multi-layer structures mainly improve damping performance by increasing the number of interlayer energy-dissipating interfaces. Under the condition of the same total TPU film thickness (i.e., CF / TPU-1b vs. CF / TPU-2, CF / TPU-1c vs. CF / TPU-4), comparing the damping ratios of the first two bending modes reveals that, within the design scope of this invention, constructing larger localized high-damping regions is more effective in improving damping performance than increasing the number of interlayer energy-dissipating interfaces.

[0066] To analyze the impact resistance of CFRP and CF / TPU composite laminates, this invention employs a drop-weight low-velocity impact test, setting the impact energy to 10 J and recording the force-displacement curves during the impact process. By analyzing the absorbed energy and interlaminar damage area of ​​different specimens, the influence of TPU film thickness and interlaminar distribution on the impact resistance of the composite material is evaluated.

[0067] Figure 9 The force-displacement curves of CFRP and CF / TPU composite laminates during low-speed impact testing are shown. Figure 10 This represents the corresponding energy absorption result. (From...) Figure 9 and Figure 10It can be seen that, compared with CFRP composites, all five CF / TPU composites showed improved energy absorption, indicating that the introduction of TPU film can enhance the composite's ability to dissipate impact energy. Comparing the experimental results of CF / TPU-1a, CF / TPU-1b, and CF / TPU-1c composites, it can be found that the energy absorption of the composite gradually increases with the increase of TPU film thickness. This is because a thicker TPU layer can provide a larger flexible deformation space, allowing for more complete viscoelastic deformation under impact loads, thus dissipating more impact energy through the viscoelastic deformation of the TPU layer. Multilayer distributed CF / TPU-2 and CF / TPU-4 composites also exhibited good impact energy absorption effects. Compared with CF / TPU-1 composites, CF / TPU-2 and CF / TPU-4 composites increased the number of internal flexible interfaces, allowing more areas to participate in deformation and energy dissipation during the impact process. Furthermore, the multilayer structure can disperse and transfer impact loads, improving the interlayer stress distribution, thereby further suppressing the propagation of delamination damage in the laminate.

[0068] To further analyze the impact damage tolerance of the composite material due to the introduction of TPU film, ultrasonic C-scan technology was used to detect internal damage in the composite laminate after impact. The C-scan results showed that the interlaminar damage area of ​​CFRP was 156.3 mm². 2 The interlaminar damage area of ​​CF / TPU-1a was 26.36 mm², and that of CF / TPU-2 was 21.03 mm². 2 No significant continuous interlaminar damage was observed in the other composite laminates. This indicates that the CFRP laminate formed a large interlaminar damage area after impact, while the interlaminar damage area of ​​the composite material was significantly reduced after the introduction of the TPU film, suggesting that the TPU interlaminar structure can effectively improve the impact damage tolerance of the composite material. The main reason for this is that the TPU film can dissipate some of the impact energy through its own deformation during impact, improving the interlaminar stress distribution and thus reducing the possibility of interlaminar crack initiation and propagation.

[0069] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.

Claims

1. A carbon fiber / thermoplastic polyurethane interlaminar toughened composite material, characterized in that, include: Plain weave carbon fiber prepreg layer, wherein multiple layers of the plain weave carbon fiber prepreg layer are overlapped; Thermoplastic polyurethane film, wherein the thermoplastic polyurethane film is interspersed between plain weave carbon fiber prepreg layers in a single-layer concentrated or multi-layer distributed manner. Plain weave carbon fiber prepreg is a semi-finished material formed by combining plain weave carbon fiber fabric with an epoxy resin matrix.

2. The carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 1, characterized in that, The thermoplastic polyurethane film is uniformly coated with FG-767 surface treatment agent on both sides.

3. The carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 1, characterized in that, The thickness of the thermoplastic polyurethane film is 0.2 mm, 0.4 mm, or 0.8 mm.

4. The carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 1, characterized in that, The plain weave carbon fiber prepreg layer has 10 layers, and the thickness of a single plain weave carbon fiber prepreg layer is 0.2 mm.

5. A method for preparing a carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to any one of claims 1-4, characterized in that, Includes the following steps: S1. Preparation and surface treatment of thermoplastic polyurethane film: Thermoplastic polyurethane particles are prepared by melt extrusion process, and their surface is processed into a frosted surface. Then, the thermoplastic polyurethane film is subjected to surface treatment. S2. Layup Design: The thermoplastic polyurethane film is laid in a single-layer concentrated or multi-layer distributed manner in the plain weave carbon fiber prepreg layer; S3. Co-curing molding: After the layup is completed, the pre-fabricated laminate is sent into an autoclave for co-curing molding. During the curing process, the heating rate, curing temperature, holding time, cooling rate and molding pressure are controlled in a coordinated manner to form a stable interfacial bond between the thermoplastic polyurethane film and the epoxy resin matrix in the carbon fiber prepreg.

6. The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 5, characterized in that, The surface treatment method in S1 is as follows: First, the surface of the thermoplastic polyurethane film is cleaned with isopropanol to remove surface oil and impurities; then, FG-767 surface treatment agent is evenly coated on both sides of the thermoplastic polyurethane film and left to stand at room temperature for 5 minutes to allow the FG-767 surface treatment agent to fully adhere to the surface of the thermoplastic polyurethane film.

7. The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 5, characterized in that, The heating rate in S3 is 2℃ / min, the curing temperature is 100℃, the holding time is 5 h, and the cooling rate is 1℃ / min.

8. The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 5, characterized in that, The specific steps of the co-curing molding are as follows: First, the temperature inside the tank is raised to 100°C at a constant heating rate, and the molding pressure is gradually applied to 0.6 MPa to promote resin flow and improve the interfacial wetting between the TPU film and the carbon fiber prepreg; then, it is kept at a constant temperature and pressure for 5 hours to promote the full curing of the epoxy resin and reduce the porosity inside the composite material; after the heat preservation stage, the temperature and pressure inside the tank are slowly reduced at a set rate to avoid residual stress concentration caused by excessive cooling or pressure change, thereby reducing the risk of warping or cracking of the laminate. After curing in the autoclave, the composite material laminate is finally obtained.

9. The method for preparing the carbon fiber / thermoplastic polyurethane interlaminar toughened composite material according to claim 8, characterized in that, The length of the composite laminate = 450 mm, width = 450 mm, thickness =2~3 mm.