Preparation method of mildew-proof antibacterial reflective film

By setting an antibacterial layer and a protective layer on the microprism reflective film and using a combination of specific antibacterial and antifungal components, the problem of bacteria easily adhering to the surface of the microprism reflective film is solved, achieving broad-spectrum antibacterial and antifungal effects and long-term stability, which is suitable for highway road signs, traffic signs and other fields.

CN123129581APending Publication Date: 2026-11-20JINJIANG LIANXING REFLECTIVE MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611072564.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing microprism reflective films are prone to the adhesion of harmful bacteria and germs on their surface during use, which affects their service life and poses health and safety hazards, especially in applications such as medical and food industries where there is a risk of cross-infection.

Method used

An antibacterial layer is set on the microprism layer. The main component is polyurethane acrylic resin, and silane coupling agent modified nano silver, chitosan quaternary ammonium salt and modified nano silica are added as antibacterial and antifungal functional components. A protective layer is set on the surface to prevent wear and loss of antibacterial components. The layer-by-layer preparation process ensures reliable interlayer bonding.

Benefits of technology

It achieves broad-spectrum antibacterial and anti-mildew effects, has long-lasting anti-mildew performance, and does not affect the optical and mechanical properties of the reflective film, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application relates to a preparation method of a mildewproof and antibacterial reflective film, and the mildewproof and antibacterial reflective film comprises, from top to bottom, a protective layer, a bacteriostatic layer, a micro-prism layer, an encapsulation layer, a back adhesive layer and a release layer; the bacteriostatic layer comprises the following raw materials: polyurethane acrylic resin, silane coupling agent modified nano-silver, chitosan quaternary ammonium salt, modified nano-silicon dioxide, ethyl acetate, trimethylolpropane triacrylate, silicone leveling agent, defoaming agent and photoinitiator; the bacteriostatic layer is arranged on the upper surface of the micro-prism layer; the raw material composition of the bacteriostatic layer is further limited, the polyurethane acrylic resin is used as the main body, the silane coupling agent modified nano-silver, the chitosan quaternary ammonium salt and the modified nano-silicon dioxide are added as antibacterial and mildewproof functional components, the synergistic effect of inorganic antibacterial agents in rapid sterilization and organic antibacterial and mildewproof agents in long-acting bacteriostatic and mildewproof is realized, the antibacterial spectrum is wider, and the mildewproof effect is more durable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of reflective film preparation technology, specifically relating to a method for preparing an anti-mildew and antibacterial reflective film. Background Technology

[0002] Microprism reflective film is a high-performance retroreflective material manufactured based on precision microprism array technology. Its core principle lies in using a micro-scale array of three-sided right-angled pyramidal prisms made of micron-sized transparent engineering plastic. Light is reflected three times on three mutually perpendicular planes before returning along the original incident direction, thus achieving a retroreflective effect. Compared to traditional glass microbead reflective films, microprism reflective films offer higher reflectivity, superior retroreflective performance, and lower manufacturing costs. They are widely used in highway road signs, directional signs, traffic signs, urban roads, railways, fire protection, environmental protection, mining, and personal safety applications.

[0003] Currently available microprism reflective films on the market have complex structures but limited functions, lacking antibacterial properties. This results in a large number of harmful bacteria and germs adhering to their surface during use, affecting the normal operation of the microprism reflective film. Especially in applications with high hygiene and safety requirements, such as medical, food, and public health sectors, the bacteria and mold growing on the reflective film surface not only affect product appearance and lifespan but also pose potential hygiene and safety hazards such as cross-infection, necessitating further improvements. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing an anti-mildew and antibacterial reflective film.

[0005] The present invention adopts the following technical solution: A method for preparing an anti-mildew and antibacterial reflective film, wherein the anti-mildew and antibacterial reflective film comprises, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer; The antibacterial layer comprises the following raw materials in parts by weight: 75-85 parts polyurethane acrylic resin, 2-5 parts silane coupling agent modified nano silver, 8-12 parts chitosan quaternary ammonium salt, 2-4 parts modified nano silica, 18-25 parts ethyl acetate, 15-18 parts trimethylolpropane triacrylate, 0.5-1 part organosilicon leveling agent, 0.5-1 part defoamer, and 2-6 parts photoinitiator; The preparation method of the anti-mildew and antibacterial reflective film specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer, dry and cure to form the backing layer, then apply the encapsulation layer resin adhesive to the backing layer, dry and cure to form the encapsulation layer. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. Step 4: Apply the prepared antibacterial coating liquid to the upper surface of the substrate, and then dry and UV cure to form an antibacterial layer. Step 5: Apply the prepared protective coating liquid to the upper surface of the antibacterial layer, and after curing, form a protective layer. Then, transfer the composite film material into the curing chamber and let it stand at 40°C for 24 hours. Finally, cut and roll it up according to the target specifications to obtain the anti-mildew and antibacterial reflective film.

[0006] Furthermore, the protective layer comprises the following raw materials in parts by weight: 80-90 parts acrylic resin, 8-15 parts polyethylene glycol diacrylate, 3-5 parts nano silica dispersion, 1-2 parts polytetrafluoroethylene micro powder, 0.5-1 parts photoinitiator, 8-12 parts n-butyl acetate, 1-3 parts vinyltrimethoxysilane, 0.05-0.1 parts 2,6-di-tert-butyl-p-cresol, and 0.3-0.5 parts leveling agent.

[0007] Further, the specific operation of step 4 is as follows: the prepared antibacterial coating liquid is coated on the upper surface of the substrate, and the thickness of the dry film is controlled to be 15-20 μm. Then it is sent into a 60℃ hot air circulation channel for pre-drying for 3 minutes, and then subjected to 800mJ / cm 2 UV curing with ultraviolet light forms an antibacterial layer.

[0008] Further, the specific operation of step 5 is as follows: The prepared protective coating solution is coated onto the upper surface of the antibacterial layer, controlling the dry film thickness to be 8-12 μm. It is then pre-dried in a 65℃ hot air circulation channel for 2 minutes, followed by 700 mJ / cm² drying. 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film.

[0009] Furthermore, the encapsulating layer resin adhesive comprises the following raw materials in parts by weight: 40-45 parts of saturated polyester resin, 10-15 parts of ethyl acetate, 20-22 parts of butyl acetate, 8-10 parts of cellulose acetate butyrate, 3-4 parts of curing agent, and 0.15-0.25 parts of dispersant.

[0010] Furthermore, in step 3, the composite temperature of the microprism layer and the encapsulation layer is 120-150℃, the composite pressure is 0.3-0.5MPa, and the pressing rate is 3-6m / min.

[0011] Furthermore, in step 1, the encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 10-20 minutes, the drying temperature is 80-130℃, and the dry film thickness is 20-40μm.

[0012] Furthermore, in the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 3-5min, 3-5min, and 4-10min.

[0013] Furthermore, in step 1, the pressure-sensitive adhesive is dried at 80-120℃ for 5-10 minutes to form the backing layer.

[0014] Furthermore, the thickness of the microprism layer is 50-70 μm, and the thickness of the adhesive layer is 30-50 μm.

[0015] As can be seen from the above description of the present invention, compared with the prior art, the beneficial effects of the present invention are: This application sets an antibacterial layer on the upper surface of a microprism layer and further defines the raw material composition of the antibacterial layer. It uses polyurethane acrylic resin as the main body, and adds silane coupling agent-modified nano-silver, chitosan quaternary ammonium salt, and modified nano-silica as antibacterial and antifungal functional components. This achieves a synergistic effect of rapid sterilization by inorganic antibacterial agents and long-lasting antibacterial and antifungal effects by organic antibacterial and antifungal agents, resulting in a broader antibacterial spectrum and a more durable antifungal effect. The raw material composition of the antibacterial layer is not a simple superposition of the functions of each component, but rather a synergistic unity of multiple functions achieved through reasonable formulation. Specifically, silane coupling agent-modified nano-silver and chitosan quaternary ammonium salt synergistically achieve antibacterial and antifungal effects; modified nano-silica enhances mechanical properties while assisting in antibacterial activity; the cross-linked network of polyurethane acrylic resin and trimethylolpropane triacrylate provides a stable carrier matrix for the functional components; and leveling agents and defoamers ensure coating quality. The synergistic integration of the four functions enables the antibacterial layer to impart excellent antibacterial and antifungal properties to the reflective film without affecting its optical and mechanical properties, thus solving the technical problem of the difficulty in balancing antibacterial and antifungal functions with reflective properties in the existing technology. Secondly, a protective layer is further added to the upper surface of the antibacterial layer, effectively preventing wear and tear and loss of antibacterial and antifungal components caused by external friction and scratching. The protective layer uses acrylic resin as the main film-forming material, with polyethylene glycol diacrylate added as an active diluent monomer to adjust the crosslinking density. The addition of nano-silica dispersion significantly improves the hardness and wear resistance of the coating. The introduction of polytetrafluoroethylene micropowder reduces the friction coefficient of the protective layer surface, giving the coating excellent slip properties and anti-fouling self-cleaning ability. Vinyltrimethoxysilane is added as a silane coupling agent to improve the interfacial bonding between inorganic fillers and organic resins. 2,6-Di-tert-butyl-p-cresol is added to inhibit yellowing caused by excessive free radical polymerization during UV curing, thereby significantly reducing the yellowing tendency of the protective layer and maintaining its optical transparency. Third, the preparation method of this invention, through a bottom-up, layer-by-layer preparation sequence, ensures that the preparation of each layer does not interfere with each other and that the interlayer bonding is reliable. The antibacterial layer and the protective layer are cured by ultraviolet light, avoiding thermal damage to the microprism structure caused by high temperature, while also achieving high curing efficiency and suitability for continuous production. The encapsulation layer is dried and cured by a step-by-step baking method, effectively avoiding coating defects and ensuring the density and sealing effect of the encapsulation layer. The microprism layer and the encapsulation layer are embossed together to form a sealed air pocket structure, achieving efficient retroreflection without the need for a metal plating layer, simplifying the process, and ensuring long-term stability of reflective performance. Subsequent curing treatment makes the interlayer bonding tighter and fully releases internal stress, further improving the overall performance of the film material. The overall process conditions are mild and easy to operate, and each process is mature and reliable, suitable for large-scale industrial production, and has good prospects for industrial application. Detailed Implementation

[0016] The present invention will be further described below through specific embodiments.

[0017] An anti-mildew and antibacterial reflective film comprises, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer; wherein the thickness of the protective layer is 8-12 μm, the thickness of the antibacterial layer is 15-20 μm, the thickness of the microprism layer is 50-70 μm, the thickness of the encapsulation layer is 20-40 μm, and the thickness of the adhesive backing layer is 30-50 μm.

[0018] The protective layer comprises the following raw materials in parts by weight: 80-90 parts acrylic resin, 8-15 parts polyethylene glycol diacrylate, 3-5 parts nano-silica dispersion, 1-2 parts polytetrafluoroethylene (PTFE) micropowder, 0.5-1 part photoinitiator, 8-12 parts n-butyl acetate, 1-3 parts vinyltrimethoxysilane, 0.05-0.1 parts 2,6-di-tert-butyl-p-cresol, and 0.3-0.5 parts leveling agent. The photoinitiator used is photoinitiator 184, the leveling agent is silicone leveling agent BYK-333, and the PTFE micropowder is DuPont PTFE micropowder with a particle size of 0.2 μm. Specifically, the preparation method of the protective coating solution is as follows: acrylic resin, polyethylene glycol diacrylate and n-butyl acetate are added to a mixing tank and stirred at 800 rpm until completely dissolved; then nano silica dispersion, polytetrafluoroethylene micro powder and vinyltrimethoxysilane are added and stirred for another 30 min; then photoinitiator, 2,6-di-tert-butyl-p-cresol and leveling agent are added and stirred at 600 rpm for 20 min. After mixing evenly, the mixture is passed through a 200-mesh sieve to obtain the protective coating solution.

[0019] The antibacterial layer comprises the following raw materials in parts by weight: 75-85 parts polyurethane acrylic resin, 2-5 parts silane coupling agent modified nano-silver, 8-12 parts chitosan quaternary ammonium salt, 2-4 parts modified nano-silica, 18-25 parts ethyl acetate, 15-18 parts trimethylolpropane triacrylate, 0.5-1 part silicone leveling agent, 0.5-1 part defoamer, and 2-6 parts photoinitiator; wherein, the chitosan quaternary ammonium salt is hydroxypropyltrimethylammonium chloride chitosan, and the degree of deacetylation of hydroxypropyltrimethylammonium chloride chitosan is ≥95%, and the degree of quaternization substitution is ≥80%; the photoinitiator is photoinitiator 184; the silicone leveling agent is silicone leveling agent BYK-333; and the defoamer is silicone defoamer BYK-024. Specifically, the preparation method of the antibacterial coating solution is as follows: the above raw materials are added to a mixing tank in sequence and stirred at 1000 rpm for 60 minutes. After mixing evenly, the mixture is passed through a 200-mesh sieve to obtain the antibacterial coating solution.

[0020] The modification method of silane coupling agent for nano-silver includes the following steps: S1. Select two portions of silver nanoparticles with an average particle size of 15-20 nm and dry them in a vacuum oven at 105 °C for 2 h. Then, add 98 portions of anhydrous ethanol into a three-necked flask equipped with a reflux condenser and slowly adjust the pH of the system to 5 with glacial acetic acid. S2. The dried silver nanoparticles were slowly added to the pH-adjusted ethanol solution. The mixture was first mechanically stirred at a high speed of 800 r / min for 30 min to initially disperse the silver nanoparticles. Then the mixture was transferred to an ultrasonic disperser at 40 kHz and ultrasonically dispersed for 20 min under ice-water bath conditions. S3, heat the suspension system to 55℃, add 3 parts of silane coupling agent KH-560 at a dropping rate of 1 drop per second, maintain constant temperature after the addition is completed, and stir and reflux at a speed of 300 r / min for 2.5-3 hours. S4. The mixed system after the reaction was completed was transferred into a high-speed centrifuge and centrifuged at 8000 r / min for 15 min. The bottom precipitate was collected. The precipitate was washed three times with anhydrous ethanol. Finally, the purified product was dried in a vacuum oven at 60℃ for 6 h to obtain silane coupling agent modified nano-silver.

[0021] The encapsulation layer comprises the following raw materials in parts by weight: 40-45 parts saturated polyester resin, 10-15 parts ethyl acetate, 20-22 parts butyl acetate, 8-10 parts cellulose acetate butyrate, 3-4 parts curing agent, and 0.15-0.25 parts dispersant; wherein the saturated polyester resin has a molecular weight of 12000 and its hydroxyl value is controlled at 10 mg KOH / g; the butyryl group content of cellulose acetate butyrate is 37-40%; the curing agent is Bayer isocyanate curing agent N75; and the dispersant is BYK-110 dispersant. Specifically, the preparation method of the encapsulation layer resin is as follows: ethyl acetate, butyl acetate, and dispersant are added sequentially to a mixing tank and stirred until homogeneous; cellulose acetate butyrate is then added and stirred until homogeneous; the saturated polyester resin is then added and stirred until homogeneous; finally, the curing agent is added and stirred until homogeneous, and the mixture is passed through a 200-mesh sieve to obtain the encapsulation layer resin.

[0022] Its preparation method specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer and dry it at 80-120℃ for 5-10 minutes to form the backing adhesive layer. Then, apply the encapsulation layer resin adhesive onto the backing adhesive layer and dry and cure it to form the encapsulation layer. The encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 10-20 minutes and the drying temperature is 80-130℃. In the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 3-5 minutes, 3-5 minutes, and 4-10 minutes, respectively. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. The bonding temperature of the microprism layer and the encapsulation layer is 120-150℃, the bonding pressure is 0.3-0.5MPa, and the pressing rate is 3-6m / min. Step 4: Apply the prepared antibacterial coating solution to the upper surface of the substrate, controlling the dry film thickness to be 15-20 μm. Then, pre-dry it in a 60℃ hot air circulation channel for 3 minutes, followed by 800 mJ / cm 2 UV curing with ultraviolet light to form an antibacterial layer; Step 5: Apply the prepared protective coating solution to the upper surface of the antibacterial layer, controlling the dry film thickness to be 8-12 μm. Pre-dry in a 65℃ hot air circulation channel for 2 minutes, then pass through a 700 mJ / cm... 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film. Example

[0023] An anti-mildew and antibacterial reflective film includes, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer; wherein, the thickness of the protective layer is 8μm, the thickness of the antibacterial layer is 15μm, the thickness of the microprism layer is 70μm, the thickness of the encapsulation layer is 20μm, and the thickness of the adhesive backing layer is 30μm.

[0024] The protective layer comprises the following raw materials in parts by weight: 80 parts acrylic resin, 15 parts polyethylene glycol diacrylate, 3 parts nano silica dispersion, 2 parts polytetrafluoroethylene micro powder, 0.5 parts photoinitiator, 12 parts n-butyl acetate, 1 part vinyltrimethoxysilane, 0.05 parts 2,6-di-tert-butyl-p-cresol, and 0.5 parts leveling agent.

[0025] The antibacterial layer comprises the following raw materials in parts by weight: 75 parts polyurethane acrylic resin, 5 parts silane coupling agent modified nano silver, 8 parts chitosan quaternary ammonium salt, 4 parts modified nano silica, 18 parts ethyl acetate, 18 parts trimethylolpropane triacrylate, 0.5 parts organosilicon leveling agent, 1 part defoamer, and 2 parts photoinitiator.

[0026] The encapsulation layer comprises the following raw materials in parts by weight: 40 parts saturated polyester resin, 15 parts ethyl acetate, 22 parts butyl acetate, 8 parts cellulose acetate butyrate, 4 parts curing agent, and 0.15 parts dispersant.

[0027] Its preparation method specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer and dry it at 80℃ for 10 minutes to form the backing adhesive layer. Then, apply the encapsulation layer resin adhesive onto the backing adhesive layer and dry and cure it to form the encapsulation layer. The encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 10 minutes and the drying temperature is 80-130℃. In the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 3 minutes, 3 minutes, and 4 minutes, respectively. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. The bonding temperature of the microprism layer and the encapsulation layer is 120℃, the bonding pressure is 0.5MPa, and the pressing rate is 6m / min. Step 4: Apply the prepared antibacterial coating solution to the upper surface of the substrate, controlling the dry film thickness to 15 μm. Then, pre-dry it in a 60℃ hot air circulation channel for 3 minutes, followed by 800 mJ / cm... 2 UV curing with ultraviolet light to form an antibacterial layer; Step 5: Apply the prepared protective coating solution to the upper surface of the antibacterial layer, controlling the dry film thickness to 8 μm. Pre-dry in a 65℃ hot air circulation channel for 2 minutes, then pass through a 700 mJ / cm... 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film. Example

[0028] An anti-mildew and antibacterial reflective film includes, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer; wherein, the thickness of the protective layer is 12μm, the thickness of the antibacterial layer is 20μm, the thickness of the microprism layer is 50μm, the thickness of the encapsulation layer is 40μm, and the thickness of the adhesive backing layer is 50μm.

[0029] The protective layer comprises the following raw materials in parts by weight: 90 parts acrylic resin, 8 parts polyethylene glycol diacrylate, 5 parts nano silica dispersion, 1 part polytetrafluoroethylene micro powder, 1 part photoinitiator, 8 parts n-butyl acetate, 3 parts vinyltrimethoxysilane, 0.1 parts 2,6-di-tert-butyl-p-cresol, and 0.3 parts leveling agent.

[0030] The antibacterial layer comprises the following raw materials in parts by weight: 85 parts polyurethane acrylic resin, 2 parts silane coupling agent modified nano silver, 12 parts chitosan quaternary ammonium salt, 2 parts modified nano silica, 25 parts ethyl acetate, 15 parts trimethylolpropane triacrylate, 1 part organosilicon leveling agent, 0.5 parts defoamer, and 6 parts photoinitiator.

[0031] The encapsulation layer comprises the following raw materials in parts by weight: 45 parts saturated polyester resin, 10 parts ethyl acetate, 20 parts butyl acetate, 10 parts cellulose acetate butyrate, 3 parts curing agent, and 0.25 parts dispersant.

[0032] Its preparation method specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer and dry it at 120℃ for 5 minutes to form the backing adhesive layer. Then, apply the encapsulation layer resin adhesive onto the backing adhesive layer and dry and cure it to form the encapsulation layer. The encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 20 minutes and the drying temperature is 80-130℃. In the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 5 minutes, 5 minutes, and 10 minutes, respectively. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. The bonding temperature of the microprism layer and the encapsulation layer is 150℃, the bonding pressure is 0.3MPa, and the pressing rate is 3m / min. Step 4: Apply the prepared antibacterial coating solution to the upper surface of the substrate, controlling the dry film thickness to 20 μm. Then, pre-dry it in a 60℃ hot air circulation channel for 3 minutes, followed by 800 mJ / cm 2 UV curing with ultraviolet light to form an antibacterial layer; Step 5: Apply the prepared protective coating solution to the upper surface of the antibacterial layer, controlling the dry film thickness to 12 μm. Pre-dry in a 65℃ hot air circulation channel for 2 minutes, then pass through a 700 mJ / cm... 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film. Example

[0033] An anti-mildew and antibacterial reflective film includes, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer; wherein, the thickness of the protective layer is 10 μm, the thickness of the antibacterial layer is 18 μm, the thickness of the microprism layer is 60 μm, the thickness of the encapsulation layer is 30 μm, and the thickness of the adhesive backing layer is 40 μm.

[0034] The protective layer comprises the following raw materials in parts by weight: 85 parts acrylic resin, 12 parts polyethylene glycol diacrylate, 4 parts nano silica dispersion, 1.5 parts polytetrafluoroethylene micro powder, 0.8 parts photoinitiator, 10 parts n-butyl acetate, 2 parts vinyltrimethoxysilane, 0.08 parts 2,6-di-tert-butyl-p-cresol, and 0.4 parts leveling agent.

[0035] The antibacterial layer comprises the following raw materials in parts by weight: 80 parts polyurethane acrylic resin, 3 parts silane coupling agent modified nano silver, 10 parts chitosan quaternary ammonium salt, 3 parts modified nano silica, 22 parts ethyl acetate, 16 parts trimethylolpropane triacrylate, 0.7 parts organosilicon leveling agent, 0.8 parts defoamer, and 4 parts photoinitiator.

[0036] The encapsulation layer comprises the following raw materials in parts by weight: 42 parts saturated polyester resin, 12 parts ethyl acetate, 21 parts butyl acetate, 9 parts cellulose acetate butyrate, 3.5 parts curing agent, and 0.20 parts dispersant.

[0037] Its preparation method specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer and dry it at 100℃ for 8 minutes to form the backing adhesive layer. Then, apply the encapsulation layer resin adhesive onto the backing adhesive layer and dry and cure it to form the encapsulation layer. The encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 15 minutes and the drying temperature is 80-130℃. In the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 4 minutes, 4 minutes, and 7 minutes, respectively. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. The bonding temperature of the microprism layer and the encapsulation layer is 135℃, the bonding pressure is 0.4MPa, and the pressing rate is 4.5m / min. Step 4: Apply the prepared antibacterial coating solution to the upper surface of the substrate, controlling the dry film thickness to 18 μm. Then, pre-dry it in a 60℃ hot air circulation channel for 3 minutes, followed by 800 mJ / cm 2 UV curing with ultraviolet light to form an antibacterial layer; Step 5: Apply the prepared protective coating solution to the upper surface of the antibacterial layer, controlling the dry film thickness to 10 μm. Pre-dry in a 65℃ hot air circulation channel for 2 minutes, then pass through a 700 mJ / cm... 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film.

[0038] Comparative Example 1 Its layer composition and preparation method are basically the same as those in Example 3. The main difference is that no antibacterial layer is set. The anti-mildew and antibacterial reflective film includes a protective layer, a microprism layer, an encapsulation layer, an adhesive backing layer and a release layer arranged from top to bottom.

[0039] Comparative Example 2 Its layer composition and preparation method are basically the same as those in Example 3. The main difference is that no protective layer is set. The anti-mildew and antibacterial reflective film includes an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer and a release layer arranged from top to bottom.

[0040] Comparative Example 3 Its layer composition and preparation method are basically the same as those in Example 3. The main difference is that the antibacterial layer does not include chitosan quaternary ammonium salt.

[0041] The reflective films prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests. Specific results are shown in Table 1. The antibacterial performance was tested according to GB / T 21866-2008; the antifungal test clause in GB / T 21866-2008 "Determination of Antibacterial Properties and Antibacterial Effects of Antibacterial Coatings (Films)" was also tested; the retroreflective coefficient was tested according to GB / T 18833; the adhesion was tested according to GB / T 9286; and the aging resistance was tested as follows: the reflective film was placed in a xenon lamp aging chamber for accelerated aging testing at an irradiance of 0.55 W / m². 2 1000 hours.

[0042] Table 1 Performance Test Table

[0043] As shown in the table above, the antibacterial and antifungal reflective films prepared in Examples 1-3 all exhibit excellent performance in terms of antibacterial rate, antifungal grade, adhesion, and retroreflection coefficient. Furthermore, the antibacterial rate retention rate after aging is ≥90%, indicating that the technical solution of this invention has excellent antibacterial and antifungal durability. Comparative Example 1, lacking an antibacterial layer, has no antibacterial and antifungal effect, proving that the antibacterial layer is the key layer for imparting antibacterial and antifungal functions to the reflective film. Comparative Example 2, lacking a protective layer, shows a significant decrease in antibacterial rate to 65% after aging, demonstrating that the protective layer has a significant protective effect on the antibacterial layer and can effectively prolong the durability of the antibacterial and antifungal function. Comparative Example 3, lacking chitosan quaternary ammonium salt in its antibacterial layer, has an antifungal grade of only level 2, far inferior to level 0 of Example 1, proving that the combined use of inorganic antibacterial agents and organic antibacterial and antifungal agents has a synergistic effect, significantly improving antifungal performance.

[0044] This application sets an antibacterial layer on the upper surface of a microprism layer and further defines the raw material composition of the antibacterial layer. It uses polyurethane acrylic resin as the main body, and adds silane coupling agent-modified nano-silver, chitosan quaternary ammonium salt, and modified nano-silica as antibacterial and antifungal functional components. This achieves a synergistic effect of rapid sterilization by inorganic antibacterial agents and long-lasting antibacterial and antifungal effects by organic antibacterial and antifungal agents, resulting in a broader antibacterial spectrum and a more durable antifungal effect. The raw material composition of the antibacterial layer is not a simple superposition of the functions of each component, but rather a synergistic unity of multiple functions achieved through reasonable formulation. Specifically, silane coupling agent-modified nano-silver and chitosan quaternary ammonium salt synergistically achieve antibacterial and antifungal effects; modified nano-silica enhances mechanical properties while assisting in antibacterial activity; the cross-linked network of polyurethane acrylic resin and trimethylolpropane triacrylate provides a stable carrier matrix for the functional components; and leveling agents and defoamers ensure coating quality. The synergistic integration of four functions enables the antibacterial layer to impart excellent antibacterial and antifungal properties to the reflective film without affecting its optical and mechanical properties, thus solving the technical problem of balancing antibacterial and antifungal functions with reflective properties in existing technologies.

[0045] The above description is merely a preferred embodiment of the present invention and should not be construed as limiting the scope of the present invention. All equivalent changes and modifications made in accordance with the scope of the patent application and the contents of the specification of the present invention should still fall within the scope of the patent of the present invention.

Claims

1. A method for preparing an anti-mildew and antibacterial reflective film, characterized in that: The anti-mildew and antibacterial reflective film includes, from top to bottom, a protective layer, an antibacterial layer, a microprism layer, an encapsulation layer, an adhesive backing layer, and a release layer. The antibacterial layer comprises the following raw materials in parts by weight: 75-85 parts polyurethane acrylic resin, 2-5 parts silane coupling agent modified nano silver, 8-12 parts chitosan quaternary ammonium salt, 2-4 parts modified nano silica, 18-25 parts ethyl acetate, 15-18 parts trimethylolpropane triacrylate, 0.5-1 part organosilicon leveling agent, 0.5-1 part defoamer, and 2-6 parts photoinitiator; The preparation method of the anti-mildew and antibacterial reflective film specifically includes the following steps: Step 1: Apply pressure-sensitive adhesive to the surface of the release layer, dry and cure to form the backing layer, then apply the encapsulation layer resin adhesive to the backing layer, dry and cure to form the encapsulation layer. Step 2: Coat the lower surface of the substrate with photosensitive resin, heat press and UV cure the substrate in a mold, and obtain a microprism layer with a microprism structure after demolding. Step 3: The microprism layer and the release layer with the encapsulation layer are bonded together by embossing. After bonding, the microprism structure of the microprism layer is embedded in the surface of the encapsulation layer. Step 4: Apply the prepared antibacterial coating liquid to the upper surface of the substrate, and then dry and UV cure to form an antibacterial layer. Step 5: Apply the prepared protective coating liquid to the upper surface of the antibacterial layer, and after curing, form a protective layer. Then, transfer the composite film material into the curing chamber and let it stand at 40°C for 24 hours. Finally, cut and roll it up according to the target specifications to obtain the anti-mildew and antibacterial reflective film.

2. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: The protective layer comprises the following raw materials in parts by weight: 80-90 parts acrylic resin, 8-15 parts polyethylene glycol diacrylate, 3-5 parts nano silica dispersion, 1-2 parts polytetrafluoroethylene micro powder, 0.5-1 part photoinitiator, 8-12 parts n-butyl acetate, 1-3 parts vinyltrimethoxysilane, 0.05-0.1 parts 2,6-di-tert-butyl-p-cresol, and 0.3-0.5 parts leveling agent.

3. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: Step 4 is performed as follows: The prepared antibacterial coating solution is applied to the upper surface of the substrate, and the thickness of the dry film is controlled to be 15-20 μm. Then, it is pre-dried in a 60℃ hot air circulation channel for 3 minutes, and then subjected to 800 mJ / cm 2 UV curing with ultraviolet light forms an antibacterial layer.

4. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: Step 5 is performed as follows: The prepared protective coating solution is applied to the upper surface of the antibacterial layer, and the thickness of the dry film is controlled to be 8-12 μm. The film is then pre-dried in a 65℃ hot air circulation channel for 2 minutes, followed by a 700 mJ / cm... 2 UV curing is performed using ultraviolet light to form a protective layer; then the composite film is transferred into a curing chamber and left to stand at 40°C for 24 hours, and then cut and rolled up according to the target specifications to obtain the anti-mildew and antibacterial reflective film.

5. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: The encapsulation layer resin adhesive comprises the following raw materials in parts by weight: 40-45 parts saturated polyester resin, 10-15 parts ethyl acetate, 20-22 parts butyl acetate, 8-10 parts cellulose acetate butyrate, 3-4 parts curing agent, and 0.15-0.25 parts dispersant.

6. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: In step 3, the composite temperature of the microprism layer and the encapsulation layer is 120-150℃, the composite pressure is 0.3-0.5MPa, and the pressing rate is 3-6m / min.

7. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: In step 1, the encapsulation layer resin adhesive is dried and cured using a step-by-step drying method to form the encapsulation layer. The drying time is 10-20 minutes, the drying temperature is 80-130℃, and the dry film thickness is 20-40μm.

8. The method for preparing an anti-mildew and antibacterial reflective film according to claim 7, characterized in that: In the step-by-step drying method, the baking temperature is set to three temperature gradients: 80-90℃, 100-110℃, and 120-130℃, and the baking time is set to 3-5min, 3-5min, and 4-10min.

9. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: In step 1, the pressure-sensitive adhesive is dried at 80-120℃ for 5-10 minutes to form the backing layer.

10. The method for preparing an anti-mildew and antibacterial reflective film according to claim 1, characterized in that: The thickness of the microprism layer is 50-70 μm, and the thickness of the adhesive layer is 30-50 μm.