A photovoltaic screen printing plate manufacturing method based on etching and laser removal
By using a metal foil with its own adhesive layer to hot-press and laminate it with a screen substrate, combined with photochemical etching and laser removal technology, the problems of precision and lifespan in photovoltaic screen grid processing have been solved, achieving efficient 5μm-level openings and improved wear resistance.
Patent Information
- Application Number
- CN202611644089.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing photovoltaic grid line processing technology cannot simultaneously achieve the comprehensive requirements of fine opening, long grid life, and low cost. Traditional methods have problems such as limited precision, high cost, and short life.
A metal foil with its own adhesive layer is used to replace the traditional polyimide film. It is fixed to the screen substrate by hot pressing and combined with photochemical etching and laser removal technology to precisely define the grid line openings and form a photovoltaic screen.
It achieves a grid line opening accuracy of 5μm, reduces the grid line light-blocking area and silver paste consumption, improves the printing aspect ratio, extends the screen life, and reduces production costs.
Smart Images

Figure CN123129583A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photovoltaic cell manufacturing technology, specifically to a method for manufacturing photovoltaic screens based on etching and laser removal. Background Technology
[0002] The positive and negative electrode grid lines of crystalline silicon solar cells are generally prepared using screen printing technology. The screen, as the core tooling of screen printing, directly determines the line width, aspect ratio and silver paste consumption of the printed grid lines due to the width of the grid line openings, the morphology of the opening sidewalls, and the wear resistance of the screen itself, which in turn affects the photoelectric conversion efficiency and manufacturing cost of the solar cell.
[0003] Currently, there are three main processing methods for the grid openings of photovoltaic screens in the industry: The first is a polyimide (PI) film composite screen: PI film is laminated onto a metal wire mesh substrate as a pattern layer, and then the grid openings are processed by laser cutting. This is the current mainstream technology route, with high process maturity and good mass production stability. However, due to the limitation of laser thermal processing precision, the opening width can usually only reach 10μm or more, and the average printing life of the screen is about 500,000 times. The second is a photosensitive emulsion screen: Photosensitive emulsion is coated on a stainless steel or polyester wire mesh, and after film exposure and development, the grid openings are formed. This solution has the lowest manufacturing cost, but the emulsion layer is thick and has poor thickness uniformity. After development, the opening taper is large, the line width consistency is poor, and the screen life is shorter than that of the PI film screen. The third is an electroformed nickel mesh / pure metal screen: An all-metal screen is integrally formed using an electroforming process. The opening consistency is good and the life is long, but the investment in electroforming equipment is large, the manufacturing cost is high, the production cycle is long, and the opening size and position accuracy are limited by the electroforming process itself.
[0004] With the continuous advancement of photovoltaic cell technology, the industry's requirements for finer grid lines are constantly increasing. Improving cell efficiency and reducing costs by reducing the grid line shading area, increasing the grid line aspect ratio, and reducing silver paste consumption has become a development trend. The advancement of grid line opening width from the 10μm level to the 5μm level has become a common technical bottleneck in the industry. The three mainstream processes mentioned above cannot simultaneously meet the comprehensive requirements of fine opening, long screen life, and low cost: PI film laser cutting process has a heat-affected zone, and slag and burrs are easily generated at the opening edge, making it impossible to achieve finer line widths. Moreover, PI film itself has insufficient wear resistance and solvent resistance, resulting in a short screen life; photosensitive emulsion screens have poor precision and short life; and electroformed nickel screens are costly and have long production cycles, making them difficult to adapt to the needs of large-scale mass production. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a photovoltaic screen printing method based on etching and laser removal. This method uses a metal foil with a self-adhesive layer to replace the traditional polyimide film as the screen printing pattern layer. The metal foil is fixed to the surface of the screen substrate through hot-pressing. After creating an anti-corrosion pattern on the metal layer surface, photochemical etching is used to precisely remove the metal layer in the opening areas. Finally, the anti-corrosion layer and the exposed adhesive layer are removed to form openings through the grid lines, thus obtaining the photovoltaic screen printing method.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for manufacturing photovoltaic screens based on etching and laser removal, the method comprising the following specific steps: S1: Provide a screen printing substrate and a metal foil, wherein the metal foil includes a metal layer and an adhesive layer bonded to one side of the metal layer; attach the metal foil to the surface of the screen printing substrate with the adhesive layer facing the screen printing substrate, and perform pre-pressing and hot pressing in sequence to make the metal foil firmly bonded to the screen printing substrate through the adhesive layer to obtain a composite screen printing plate; S2: An anti-corrosion layer is formed on the surface of the metal layer of the composite screen. The anti-corrosion layer is exposed and developed according to the preset grid pattern, so that the metal layer in the area where the grid opening is to be formed is exposed, and the metal layer in the remaining area is covered and protected by the anti-corrosion layer. S3: The composite screen after exposure and development is etched with an etching solution. The metal layer in the area not covered by the anti-corrosion layer is etched away, leaving only the adhesive layer in that area. The metal layer in the area covered by the anti-corrosion layer is retained. S4: Remove the anti-corrosion layer, and then remove the adhesive layer exposed after etching, so that the area forms a through grid opening to obtain a photovoltaic screen.
[0007] Furthermore, the specific steps of S1 are as follows: The selected wire mesh substrate is any one of tungsten carbide wire mesh, stainless steel wire mesh, or polyester wire mesh, with the mesh count controlled within the range of 300-900 mesh, selected according to the target grid line precision; the wire mesh substrate can be used directly, or it can be pre-cleaned, roughened, or treated with coupling agent to further improve the adhesion of the adhesive layer. A double-layer composite metal foil is used as the substrate for the screen printing pattern layer. The metal foil is prefabricated and composited with a metal layer and an adhesive layer. The metal layer is any one of nickel foil, stainless steel foil, copper foil, aluminum foil, or an alloy foil of the above metals, with a thickness controlled between 1μm and 10μm, possessing both good etchability and wear resistance. The adhesive layer is bonded to one side of the metal layer and is any one of epoxy adhesive, acrylic adhesive, polyurethane adhesive, or thermosetting adhesive, with a thickness controlled between 2μm and 20μm, used to achieve bonding and fixation between the metal layer and the screen substrate. The metal foil is smoothly adhered to the surface of the screen substrate with the adhesive layer facing towards it and the metal layer facing away from it, ensuring no wrinkles or bubbles. A pre-pressing process is then performed, with a pre-pressing temperature of 100℃-300℃, a pre-pressing pressure of 0.1MPa-0.5MPa, and a pre-pressing time of 100s-3000s, to initially soften the adhesive layer and wet the surface of the screen substrate. After pre-pressing, a hot-pressing curing process is performed, with a hot-pressing temperature of 100℃-300℃, a hot-pressing pressure of 0.2MPa-0.8MPa, and a hot-pressing time of 100s-3000s, to completely cross-link and cure the adhesive layer, firmly bonding the metal foil to the screen substrate to obtain a composite screen printing semi-finished product.
[0008] Furthermore, the specific steps of S2 are as follows: A uniform anti-corrosion layer is formed on the surface of the metal layer of the composite screen. The anti-corrosion layer can be formed by applying liquid photosensitive adhesive through spin coating, roller coating or blade coating, or by transferring dry film photoresist to the surface of the metal layer through hot pressing. The anti-corrosion layer must completely cover the surface of the metal layer, without pinholes, without missing coating, and with uniform thickness. The anti-corrosion layer is selectively exposed according to a preset grid pattern. The exposure method can be laser direct imaging (LDI) scanning exposure or film ultraviolet exposure; the exposure energy is controlled at 10 mJ / cm. 2 -500mJ / cm 2 This causes the anti-corrosion layer in the exposed area to undergo photocrosslinking and curing, giving it etching resistance. A sodium carbonate solution with a mass fraction of 0.3%-2% is used as the developer to develop the exposed resist layer, with the development time controlled between 10s and 300s. After development, the resist layer in the unexposed area to be formed into the grid line opening is dissolved and removed, and the metal layer in this area is completely exposed. The resist layer in the exposed area is retained and tightly covers the metal layer, forming a resist pattern that is complementary to the preset grid line. No post-baking process is required after development to avoid the resist layer being deformed by heat and affecting the pattern accuracy.
[0009] Furthermore, the specific steps of S3 are as follows: The composite screen after exposure and development is placed in an etching solution for etching. The etching solution can be any one of acidic ferric chloride etching solution, acidic copper chloride etching solution, nitric acid etching solution, or alkaline etching solution, selected according to the material of the metal layer. The etching method can be static immersion etching or circulating spray etching, wherein spray etching can improve etching uniformity and processing efficiency.
[0010] Etching is performed at room temperature, with the etching time controlled between 1 min and 30 min. The etching time is precisely adjusted according to the material and thickness of the metal layer to ensure that the exposed metal layer is completely removed and the amount of lateral etching is minimized.
[0011] After etching, the composite screen is removed and rinsed with water to remove residual etching solution and etching byproducts. After etching, the metal layer in the exposed area is completely removed, leaving only the adhesive layer underneath. The metal layer in the area covered by the anti-corrosion layer is not eroded by the etching solution and is completely preserved. The pattern boundary of the gate opening is precisely defined by the edge of the etched metal layer, and the edge quality is guaranteed by the photochemical etching process.
[0012] Furthermore, the specific steps of S4 are as follows: The etched composite screen is placed in a stripping solution to remove the residual anti-corrosion layer. The stripping solution is a sodium hydroxide aqueous solution with a mass fraction of 5%-15%. The stripping temperature is controlled at 40℃-60℃. The screen is soaked until the anti-corrosion layer on the surface of the metal layer is completely removed. After stripping, the screen is rinsed with clean water to remove the residual stripping solution.
[0013] The adhesive layer in the exposed area after etching is removed by means of laser cutting, plasma etching or chemical dissolution; among them, laser processing can be any one of picosecond laser, nanosecond laser, ultraviolet laser or CO2 laser. The laser beam only acts on the exposed adhesive layer area. The metal layer acts as a self-aligned mask during the processing, which strictly limits the laser heat-affected zone within the opening of the metal layer and does not damage the opening edge.
[0014] After the adhesive layer is completely removed, a grid opening is formed in the area that penetrates the screen substrate, and the final photovoltaic screen is obtained; the width of the final grid opening is 5μm-30μm, preferably controlled between 8μm-10μm.
[0015] The order of the above-mentioned steps for removing the anti-corrosion layer and removing the exposed adhesive layer can be interchanged. That is, the exposed adhesive layer can be removed first by laser or plasma method, and then the anti-corrosion layer can be removed by film stripping. This can be flexibly adjusted according to the layout of the production line equipment without affecting the final opening quality and screen performance.
[0016] Compared with existing technologies, this photovoltaic screen fabrication method based on etching and laser removal has the following advantages: This invention replaces traditional polyimide film with a metal foil with a self-adhesive layer as the screen printing pattern layer. Through a processing method that combines etching and laser adhesive removal, it achieves a comprehensive performance improvement in photovoltaic screen grid line processing. The grid line openings are precisely defined by a photochemical etching process, eliminating the precision limitations of laser thermal processing. It can stably achieve fine openings at the 5μm level, with no heat-affected zone or slag burrs at the opening edges. The steep sidewalls with a small taper effectively reduce the grid line shading area and silver paste consumption, while significantly improving the aspect ratio of the printed grid lines. In addition, the metal layer itself has excellent wear resistance and solvent resistance, extending the printing life of the screen and significantly reducing the frequency of screen replacements during production, thus reducing the manufacturing cost of solar cells.
[0017] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 A flowchart illustrating a photovoltaic screen fabrication method based on etching and laser removal; Figure 2 This is a schematic diagram of the layer structure of the screen printing plate; In the figure, a- is a schematic diagram of the layer structure after hot pressing and lamination; b- is a schematic diagram of the layer structure after exposure and development; c- is a schematic diagram of the layer structure after etching; d- is a schematic diagram of the layer structure after the finished product has been opened. Figure 3 This is a magnified view of a portion of the grid opening. Detailed Implementation
[0020] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0021] Example 1 This embodiment uses a nickel metal layer plus an epoxy adhesive layer composite foil paired with a tungsten steel wire mesh substrate, employing a laser direct imaging exposure and immersion etching process, such as... Figure 1 As shown, the specific processing procedure is as follows: S1: 500-mesh tungsten carbide wire mesh is selected as the wire mesh substrate, with a wire diameter of 18μm and a tension of 28N / cm. The wire mesh surface is subjected to plasma roughening treatment to improve the adhesion of the adhesive layer. A prefabricated double-layer nickel-epoxy composite foil is used, wherein the metal layer is high-purity nickel foil with a thickness of 3μm; the adhesive layer is thermosetting epoxy adhesive, which is pre-coated evenly on one side of the nickel foil with a thickness of 5μm. The metal foil is laid flat on the surface of the wire mesh substrate with the epoxy adhesive layer facing the wire mesh and the nickel layer facing outwards. Figure 2As shown, the interface air is removed by roller pressing to ensure no wrinkles, no bubbles, and no misalignment. Then, it is sent to a flatbed hot press for pre-pressing. The pre-pressing temperature is set at 180℃, the pre-pressing pressure is 0.3MPa, and the pre-pressing time is 300s, which allows the epoxy adhesive layer to soften initially and fully impregnate the surface fibers of the mesh. After pre-pressing, the pressure and temperature are directly increased for hot pressing and curing. The hot pressing temperature is set at 200℃, the hot pressing pressure is 0.5MPa, and the hot pressing time is 600s, which allows the epoxy adhesive layer to fully cross-link and cure. After hot pressing, the composite mesh is taken out, and the adhesion is tested using the cross-cut adhesion test. The metal layer does not peel off or curl, and the adhesion level reaches 0.
[0022] S2: Liquid acid-resistant photosensitive emulsion is coated onto the nickel layer surface of the composite screen using a roller coating method. After drying, a uniform anti-corrosion layer with a thickness of 2μm is formed, with no pinholes, missed coatings, or flow marks on the surface. A laser direct imaging device is used to scan and expose the photosensitive emulsion layer line by line according to a preset grid pattern file. The exposure wavelength is 405nm, and the exposure energy is 80mJ / cm². 2 The photosensitive emulsion in the exposed area undergoes photocrosslinking and curing. The exposed screen is then immersed in a 1% sodium carbonate aqueous solution for development at 25°C for 40 seconds. After development, the photosensitive emulsion in the unexposed grid line opening area is completely dissolved, exposing the nickel layer in that area. The photosensitive emulsion in the exposed area is cured and retained, tightly covering the nickel layer surface to form an anti-corrosion mask pattern complementary to the preset grid lines. No post-baking is performed after development to avoid thermal deformation of the emulsion layer affecting the pattern accuracy.
[0023] S3: The developed composite screen is horizontally immersed in an acidic ferric chloride etching solution for etching. The concentration of ferric ions in the etching solution is 1.2 mol / L, the pH value is 1.5, the etching temperature is 25℃ (room temperature), and the etching time is 8 min. During the etching process, the nickel layer in the exposed area reacts with the etching solution and is gradually etched away, while the nickel layer in the area covered by photosensitive emulsion is protected from etching. After etching for the predetermined time, the screen is removed and immediately rinsed with high-pressure deionized water to remove residual etching solution and reaction byproducts. Then, it is dried with compressed air. After etching, the nickel layer in the exposed area is completely removed with no residual metal. The etching depth on the grid line opening side does not exceed 1 μm, and the metal layer opening edge is neat with no serrations or gaps.
[0024] S4: Immerse the etched screen printing plate in a 10% sodium hydroxide aqueous solution for film removal at 50℃ for 8 minutes to completely dissolve and remove the residual photosensitive adhesive layer. After removal, rinse thoroughly with water and dry. Use a picosecond laser to scan and cut away the exposed epoxy adhesive layer after etching. The laser wavelength is 355nm, and the laser power and scanning speed are matched to a 5μm adhesive layer thickness. Using the edge of the metal layer opening as a self-aligning mask, the laser beam acts only on the adhesive layer area without damaging the edge of the metal layer opening. After complete removal of the adhesive layer, a grid line opening penetrating the screen substrate is formed, such as... Figure 3 As shown, the finished photovoltaic grid plate is obtained.
[0025] The photovoltaic screen prepared in this embodiment has an average grid line opening width of 7μm, a line width tolerance of no more than ±0.8μm, and an opening sidewall perpendicularity of no less than 88°. After printing life test, the grid lines showed no obvious wear or edge chipping after 850,000 continuous printing cycles, and the printing line width change rate did not exceed 3%.
[0026] Example 2 This embodiment uses a stainless steel metal layer plus an acrylic adhesive layer composite foil paired with a stainless steel wire mesh substrate, and employs film ultraviolet exposure and spray etching processes. The specific processing steps are as follows: S1: 400 mesh stainless steel wire mesh is selected as the wire mesh substrate, with a wire diameter of 20μm and a tension of 25N / cm. The wire mesh surface is degreased and cleaned to remove surface oil and impurities, ensuring a clean adhesive bonding interface. A prefabricated double-layer stainless steel-acrylic composite foil is used, where the metal layer is 304 stainless steel foil with a thickness of 5μm and a matte roughening treatment to improve adhesive adhesion. The adhesive layer is a thermosetting acrylic adhesive, pre-coated evenly on one side of the stainless steel foil with a thickness of 8μm and a coating thickness deviation ≤±0.5μm. The metal foil is laid flat on the wire mesh with the acrylic adhesive layer facing the wire mesh and the stainless steel layer facing outwards. On the surface of the mesh substrate, air at the interface is removed using vacuum adsorption to ensure no wrinkles, bubbles, or misalignments. It is then fed into a flatbed hot press for pre-pressing at 150℃, 0.2MPa, and 500s to initially soften the acrylic adhesive layer and fully impregnate the warp and weft fibers of the mesh. After pre-pressing, the pressure and temperature are directly increased for hot-pressing curing at 170℃, 0.4MPa, and 900s to completely cross-link and cure the acrylic adhesive layer. After hot-pressing, the composite mesh is removed, and the adhesion is tested using a tape peeling method. No large pieces of the metal layer peel off, and the adhesion meets the requirements for mass production.
[0027] S2: An anti-corrosion layer is prepared using a dry film photoresist hot-press bonding process. The dry film is a negative acid-resistant dry film photoresist with a total thickness of 3μm. The dry film is then applied to the stainless steel layer surface of the composite screen and fed into a hot-press laminator. The lamination temperature is 110℃, the lamination pressure is 0.3MPa, and the lamination speed is 1.5m / min, ensuring a tight bond between the dry film and the stainless steel layer surface without bubbles or curling. Exposure is performed using a film alignment UV exposure machine. The film pattern is a preset grid line pattern, the exposure wavelength is 365nm, and the exposure energy is 200mJ / cm². 2 The exposure alignment accuracy is ≤±1μm, which causes the dry film photoresist in the exposed area to undergo photocrosslinking and curing. The exposed screen is immersed in a sodium carbonate aqueous solution with a mass fraction of 0.8% for development at a development temperature of 23℃ for 60s, with spray stirring to assist development. After development, the dry film in the unexposed grid opening area is completely dissolved and removed, and the stainless steel layer in this area is completely exposed. The dry film in the exposed area is cured and retained, tightly covering the surface of the stainless steel layer, forming an anti-corrosion mask pattern that is complementary to the preset grid lines.
[0028] S3: Etching is performed using a horizontal spray etching production line. The etching solution is an acidic copper chloride etching solution with a copper ion concentration of 1.0 mol / L, a hydrochloric acid concentration of 0.5 mol / L, and an oxidant content of 0.2 mol / L. The etching temperature is controlled at 30℃, the upper and lower spray pressures are both 0.2 MPa, the screen transmission speed is 0.8 m / min, and the total etching time is 12 min. During the etching process, the upper and lower sprayed etching solutions act evenly on the screen surface. The exposed stainless steel layer undergoes an oxidation-reduction reaction with the etching solution and is gradually etched away. The stainless steel layer in the area covered by the dry film is protected from etching. After etching, the screen is sequentially rinsed in a primary water washing tank and a secondary pure water washing tank to remove residual etching solution and reaction byproducts from the surface. It is then dried by an air knife. Post-etching inspection shows that the exposed stainless steel layer is completely removed with no metal residue. The etching depth on the grid line opening side does not exceed 1.5 μm, and the metal layer opening edge is neat with no obvious serrations or gaps.
[0029] S4: The exposed acrylic adhesive layer after etching is removed by scanning and cutting using an ultraviolet laser device. The laser wavelength is 266nm, the laser spot diameter is 3μm, and the scanning speed is 200mm / s. The edge of the stainless steel layer opening is used as a self-aligning mask, and the laser beam only acts on the adhesive layer area without damaging the edge of the metal layer opening. The laser-removed screen is then immersed in an 8% sodium hydroxide aqueous solution for stripping at a stripping temperature of 45℃ for 10 minutes to completely dissolve and remove the residual dry film photoresist. After removal, it is rinsed with clean water and dried with compressed air. After the adhesive layer and the anti-corrosion layer are completely removed, grid openings are formed that penetrate the screen substrate, resulting in the finished photovoltaic screen.
[0030] The photovoltaic screen prepared in this embodiment has an average grid line opening width of 11μm, a line width tolerance of no more than ±1.0μm, and an opening sidewall verticality of no less than 86°. After printing life test, the grid lines showed no obvious wear or edge chipping after 820,000 consecutive printing cycles, and the printing line width change rate did not exceed 3.5%, making it suitable for mass production scenarios.
[0031] Example 3 This embodiment uses an aluminum metal layer plus a polyurethane adhesive layer composite foil paired with a polyester wire mesh substrate. The exposed adhesive layer is removed by chemical dissolution. The specific processing procedure is as follows: S1: 600-mesh polyester mesh is selected as the mesh substrate, with a wire diameter of 15μm and a tension of 22N / cm. The mesh surface is treated with plasma hydrophilication to enhance the adhesion between the adhesive layer and the polyester fibers. A prefabricated double-layer aluminum-polyurethane composite foil is used, in which the metal layer is high-purity aluminum foil with a thickness of 2μm, and the surface is treated with an anodized thin layer to improve corrosion resistance and adhesive adhesion. The adhesive layer is a thermosetting polyurethane adhesive, which is pre-coated evenly on one side of the aluminum foil with a thickness of 4μm and a coating uniformity deviation ≤±0.3μm. The metal foil is laid flat on the mesh substrate with the polyurethane adhesive layer facing the mesh and the aluminum layer facing outwards. On the material surface, soft rollers are used to remove interfacial air, ensuring no wrinkles, bubbles, or tensile deformation. Then, it is fed into a flatbed hot press for pre-pressing. The pre-pressing temperature is set at 120℃, the pre-pressing pressure at 0.15MPa, and the pre-pressing time at 200s, allowing the polyurethane adhesive layer to initially soften and impregnate the polyester fiber surface. After pre-pressing, the pressure and temperature are directly increased for hot-pressing curing. The hot-pressing temperature is set at 140℃, the hot-pressing pressure at 0.3MPa, and the hot-pressing time at 400s, allowing the polyurethane adhesive layer to fully cross-link and cure. After hot-pressing, the composite mesh is removed, and the adhesion is tested using the cross-cut adhesion test. The metal layer shows no peeling or curling, and the adhesion level reaches grade 0.
[0032] S2: Liquid alkaline corrosion-resistant photosensitive emulsion is coated onto the aluminum layer surface of the composite screen using a spin coating method at a speed of 3000 r / min and a spin coating time of 30 s. After coating, it is dried in an 80℃ oven for 5 min to form a uniform anti-corrosion layer with a thickness of 1.5 μm, free of pinholes, missed coatings, and flow marks. Laser direct imaging equipment is used for scanning exposure at a wavelength of 405 nm and an exposure energy of 60 mJ / cm². 2The laser spot diameter is 2μm, causing photocrosslinking and curing of the photosensitive emulsion in the exposed area, giving it resistance to alkali etching. The exposed screen is then immersed in a 0.5% sodium carbonate aqueous solution for development at 25℃ for 30 seconds. After development, the photosensitive emulsion in the unexposed grid opening areas completely dissolves, exposing the aluminum layer in these areas. The photosensitive emulsion in the exposed areas remains cured and tightly covers the aluminum layer surface, forming an anti-corrosion mask pattern complementary to the preset grid lines. No post-baking is performed after development to avoid thermal deformation of the emulsion layer, which could affect the pattern accuracy.
[0033] S3: The developed composite screen is horizontally immersed in an alkaline etching solution for etching. The etching solution is a sodium hydroxide-sodium aluminate system, with a sodium hydroxide mass fraction of 5% and a sodium aluminate mass fraction of 3%, and a pH value of 12. The etching temperature is 25℃ (room temperature), and the etching time is 5 minutes. During the etching process, low-speed stirring is used to ensure the uniformity of the etching solution. During the etching process, the aluminum layer in the exposed area reacts with the alkaline etching solution and is gradually etched away, while the aluminum layer in the area covered by photosensitive emulsion is protected from etching. After etching for the predetermined time, the screen is removed and immediately neutralized with dilute nitric acid. Then, the surface is rinsed with high-pressure deionized water to remove residual etching solution and reaction byproducts. Finally, it is dried with compressed air. Post-etching inspection shows that the aluminum layer in the exposed area is completely removed, with no residual metal; the etching depth on the grid line opening side does not exceed 0.8μm, and the opening edge of the metal layer is neat and smooth, without serrations or gaps.
[0034] S4: Immerse the etched screen in a 12% sodium hydroxide aqueous solution for film removal at 55°C for 6 minutes to completely dissolve and remove the residual photosensitive adhesive and anti-corrosion layer. After removal, rinse thoroughly with water and dry. Remove the polyurethane adhesive layer from the exposed areas using a chemical dissolution method. Transfer the screen to an N-methylpyrrolidone organic solvent and immerse it at 40°C for 10 minutes with gentle agitation to fully dissolve and remove the exposed polyurethane adhesive layer. After removal, wash sequentially with anhydrous ethanol and deionized water to remove residual organic solvent. After the adhesive layer and anti-corrosion layer are completely removed, grid openings penetrating the screen substrate are formed, resulting in the finished photovoltaic screen.
[0035] The photovoltaic screen prepared in this embodiment has an average grid line opening width of 6μm, a line width tolerance of no more than ±0.7μm, and an opening sidewall perpendicularity of no less than 89°. After printing life test, the grid lines showed no obvious wear or edge chipping after 780,000 continuous printing cycles, and the printing line width change rate was no more than 4%, demonstrating high line width accuracy, making it suitable for ultra-fine grid line printing scenarios.
[0036] Example 4 The process in this embodiment is basically the same as that in Embodiment 1, except that the order of steps in step S4 is reversed: First, a picosecond laser is used to remove the exposed epoxy adhesive layer after etching. Then, the screen is placed in a sodium hydroxide stripping solution to remove the anti-corrosion layer. The remaining process parameters are completely consistent with those in Example 1.
[0037] The photovoltaic screen prepared in this embodiment has no significant difference in grid opening width, edge quality and printing life compared with that of Example 1, proving that the process sequence can be flexibly adjusted according to the production line layout without affecting the performance of the final product.
[0038] Comparative Example 1 The screen was prepared using mainstream industry processes: a 500-mesh tungsten wire mesh was laminated with an 8μm thick polyimide film via an adhesive layer, and the openings were directly cut using a UV laser to form the grid lines. The opening width was the same as in Example 1. The resulting screen grid lines had an average opening width of 12μm, with heat-affected zones and slag burrs at the opening edges, and a sidewall taper of approximately 15°. After printing life testing, significant wear appeared on the grid lines after 520,000 consecutive prints, with the printed linewidth change rate exceeding 8%, reaching the scrap threshold.
[0039] Comparative Example 2 A 400-mesh stainless steel wire mesh is used, coated with a diazo photosensitive emulsion. The mesh is exposed to film and developed to form the grid lines, with a total emulsion thickness of 15 μm. The resulting screen grid lines have an average width of 15 μm, a large taper, and poor line width uniformity; the printing life is only about 150,000 cycles.
[0040] The core performance indicators of each embodiment and comparative example are summarized in the table below: In summary, the photovoltaic screen grid line micro / nano fabrication method proposed in this invention achieves a firm bond between the metal foil and the screen substrate through hot-pressing composite, precisely defines the metal boundary of the grid line opening through photolithography-etching process, and then removes the residual adhesive layer by laser or chemical means to form the final opening. Each embodiment uses different screen substrates, metal layer materials, adhesive layer systems, exposure methods, etching modes and adhesive removal processes, and can stably achieve a grid line processing accuracy of 5μm. Moreover, the wear resistance of the metal pattern layer is significantly better than that of traditional organic thin film materials.
[0041] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for manufacturing photovoltaic screens based on etching and laser removal, characterized in that, The method includes the following specific steps: S1: Provide a screen printing substrate and a metal foil, wherein the metal foil includes a metal layer and an adhesive layer bonded to one side of the metal layer; attach the metal foil to the surface of the screen printing substrate with the adhesive layer facing the screen printing substrate, and perform pre-pressing and hot pressing in sequence to make the metal foil firmly bonded to the screen printing substrate through the adhesive layer to obtain a composite screen printing plate; S2: An anti-corrosion layer is formed on the surface of the metal layer of the composite screen. The anti-corrosion layer is exposed and developed according to the preset grid pattern, so that the metal layer in the area where the grid opening is to be formed is exposed, and the metal layer in the remaining area is covered and protected by the anti-corrosion layer. S3: The composite screen after exposure and development is etched with an etching solution. The metal layer in the area not covered by the anti-corrosion layer is etched away, leaving only the adhesive layer in that area. The metal layer in the area covered by the anti-corrosion layer is retained. S4: Remove the anti-corrosion layer, and then remove the adhesive layer exposed after etching, so that the area forms a through grid opening to obtain a photovoltaic screen.
2. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In S1, the wire mesh substrate is any one of tungsten steel wire mesh, stainless steel wire mesh, or polyester wire mesh, and the mesh count is 300-900 mesh.
3. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S1, the metal layer is any one of nickel foil, stainless steel foil, copper foil, aluminum foil, or an alloy foil of the above metals, with a thickness of 1μm-10μm; the adhesive layer is any one of epoxy adhesive, acrylic adhesive, polyurethane adhesive, or thermosetting adhesive, with a thickness of 2μm-20μm.
4. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In S1, the pre-pressing temperature is 100℃-300℃ and the pre-pressing time is 100s-3000s; the hot-pressing temperature is 100℃-300℃ and the hot-pressing time is 100s-3000s.
5. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S2, the anti-corrosion layer is a liquid photoresist or a dry film photoresist; the exposure is laser direct imaging exposure or film ultraviolet exposure, and the exposure energy is 10mJ-500mJ.
6. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S2, the developing process uses a sodium carbonate solution with a mass fraction of 0.3%-2% as the developing solution, and the developing time is 10s-300s.
7. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S3, the etching solution is any one of acidic ferric chloride etching solution, acidic copper chloride etching solution, nitric acid-based etching solution, or alkaline etching solution; the etching temperature is room temperature, and the etching time is 1 min to 30 min.
8. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S3, the etching method is either immersion etching or spray etching, and the screen is rinsed with clean water after etching is completed.
9. The photovoltaic screen fabrication method based on etching and laser removal according to claim 1, characterized in that, In step S4, a sodium hydroxide stripping solution with a mass concentration of 5%-15% is used to remove the anti-corrosion layer at a temperature of 40℃-60℃.
10. A method for manufacturing a photovoltaic screen based on etching and laser removal according to claim 1, characterized in that, In step S4, the exposed adhesive layer after etching is removed by laser cutting, plasma etching, or chemical dissolution; wherein the laser is any one of picosecond laser, nanosecond laser, ultraviolet laser, or CO2 laser.