A gold foil stamping product and a method for preparing the same

By using a combination of mercapto self-crosslinking core-shell emulsion, aliphatic waterborne polyurethane, and polyvinyl alcohol in gold foil offset printing, the problem of asynchronous interface and cohesive network during semi-dry bonding and offset printing of waterborne gold foil adhesives was solved, improving the cutting and bending integrity of gold foil and the flatness of the paper surface, and enhancing the peel strength after bonding.

CN123129609APending Publication Date: 2026-11-20NANJING JINLING GOLDFOIL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611354253.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing water-based gold leaf adhesives suffer from asynchronous interfacial interactions and cohesive network establishment during semi-dry lamination, film curing, and subsequent offset printing processes. This leads to gold foil defects, boundary migration, and paper warping, affecting the integrity of the decorative layer and the stability of overprinting.

Method used

Gold foil offset printing products using a specific water-based compounding system include a paper substrate, a water-based gold foil layer, and a UV offset printing image layer. Through the combination of thiol self-crosslinking core-shell emulsion, aliphatic water-based polyurethane, and polyvinyl alcohol, a functional hard shell and continuous phase are formed, providing dynamic bonding and flexibility, and improving interfacial adhesion and cohesion retention.

Benefits of technology

It improves the cutting and bending integrity of gold foil, reduces boundary migration, improves paper surface flatness and UV offset printing position stability, enhances post-application peel strength, and reduces warping after conditioning.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application relates to the technical field of offset printing, and particularly discloses a gold foil offset printing product and a preparation method thereof. The gold foil offset printing product comprises a paper base material, a water-based gold sticking adhesive layer, a gold foil layer and a UV offset printing text layer along the thickness direction. The water-based gold sticking adhesive comprises a mercapto self-crosslinking core-shell emulsion, an aliphatic water-based polyurethane, an acrylic modified rosin emulsion and polyvinyl alcohol. The functional hard shell of the core-shell particle is provided with aryl boronic acid side groups and terminal mercapto side chains. During preparation, the water-based gold sticking adhesive is prepared, the paper base is coated, the semi-dry foil sticking is performed, pre-solidification is carried out, UV offset printing overprinting is performed and ultraviolet solidification is carried out in sequence, so that the semi-dry sticking operation window can be prolonged, the foil sticking integrity, the boundary stability after offset printing and the paper surface flatness can be maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of offset printing technology, specifically to a gold foil offset print and its preparation method. Background Technology

[0002] As packaging printing evolves towards more refined decoration and water-based processing, paper-based packaging needs to convey information through offset printing and also utilize metallic layers to create localized visual depth. Metallic decoration is typically achieved through hot stamping, transfer printing, or foil application, and then combined with offset printing. Building upon this, a technique that involves coating the paper base with water-based adhesive, allowing the adhesive layer to dry appropriately, then applying alloy foil and continuing offset printing reduces the impact of continuous heating on the paper base and printing plate, and adapts to the positioning of different graphic areas. The continuous implementation of this technique involves moisture migration to the paper base, changes in the adhesive layer's surface adhesion, gold foil application, and subsequent printing loads; therefore, it imposes interrelated control requirements on the timing of foil application, interface adhesion, and the adhesive layer's film-forming state.

[0003] In recent years, common solutions for water-based gold foil adhesives have primarily used water-based polymers. Common techniques involve compounding different water-based film-forming materials and then using auxiliary film-forming materials to adjust the drying state of the adhesive layer. The initial adhesion required for foil application can be obtained by adjusting the emulsion film-forming temperature, continuous phase tack elasticity, tackifying component ratio, or drying regime. Some technical approaches also introduce crosslinking agents to improve the cohesive strength of the adhesive film after formation. While these solutions can alter surface adhesion, adhesive layer flexibility, or curing speed, the continuous loss of moisture after coating creates a time lag between the surface lamination state and the internal film-forming process. Cutting and bending after foil application create localized stress at the gold foil edges and within the adhesive layer, and subsequent UV printing applies shear loads to the bonded areas. Therefore, simply increasing initial tack, crosslinking degree, or drying speed may still shorten the foil application time, or make it difficult to simultaneously control adhesive layer brittleness, gold foil boundary movement, and paper base moisture absorption and warping.

[0004] Regarding the aforementioned technologies, the inventors believe that in application scenarios where water-based gold foil transitions from a wet to a semi-dry state and continues to bear the offset printing load, although adjusting the initial tack or drying regime can improve the initial state of foil application, the material and process limitations of the adhesive layer surface losing water faster than the internal film formation mean that when the timing of foil application or the degree of pre-curing fluctuates, the interface adhesion and cohesion establishment will become mismatched, leading to gold foil defects, boundary migration, and paper warping, resulting in reduced integrity of the decorative layer and printing stability. Summary of the Invention

[0005] In related technologies, water-based gold foil adhesives suffer from asynchronous interfacial interactions and cohesive network establishment during semi-dry lamination, film formation and curing, and subsequent offset printing. To address this deficiency, this application provides a gold foil offset print and its preparation method.

[0006] In a first aspect, this application provides a gold foil offset print, employing the following technical solution: A gold foil offset print comprises, along its thickness direction, a paper substrate, a water-based gold foil layer, a gold foil layer, and a UV offset printing image layer, stacked sequentially. The water-based gold foil layer is formed by curing the water-based gold foil, which includes a dispersion medium and the following components by mass of polymer solids: 95-105 parts of a thiol self-crosslinking core-shell emulsion, 15-22 parts of an aliphatic waterborne polyurethane, 10-15 parts of an acrylic-modified rosin emulsion, and 2-3.5 parts of polyvinyl alcohol. The thiol self-crosslinking core-shell emulsion contains self-crosslinking core-shell particles, which have a functional hard shell. The functional hard shell has arylboronic acid side groups and terminal thiol side chains. The arylboronic acid side groups are formed by a ring-opening reaction between an amino group and an epoxy group in an amino-arylboronic acid raw material, and the terminal thiol side chains are obtained by a ring-opening reaction between an epoxy group and cysteine.

[0007] By adopting the above technical solution, this application sets a gold-coating adhesive layer formed by a specific aqueous compound system between the paper substrate and the gold foil layer, and enables the functional hard shell of the core-shell particles to simultaneously support arylboronic acid side groups and terminal thiol side chains. The functional hard shell provides a common carrier for the two types of side groups. The arylboronic acid side groups are located in a continuous phase containing polyvinyl alcohol, providing contact sites for the dynamic bonding of boric acid groups and polyvinyl alcohol hydroxyl groups. When the adhesive layer continues to lose water or is subjected to offset printing shear, this dynamic bonding opportunity helps to limit the local slippage of the continuous phase. The terminal thiol side chains provide sulfur-containing end groups facing the gold foil interface, which helps to maintain the bonding between the gold foil and the adhesive layer. The aliphatic aqueous polyurethane forms a flexible continuous phase in the adhesive layer, which can mitigate the concentration of local deformation under cutting and bending stress. The core-shell particles and polyvinyl alcohol jointly participate in the film formation of the aqueous system, so that the continuous phase is constrained and kept connected to the gold foil interface in the same gold-coating adhesive layer. The acrylic modified rosin emulsion adjusts the surface adhesion in the semi-dry stage, and polyvinyl alcohol participates in the film formation of the continuous phase and restricts water migration. Therefore, the gold foil layer first obtains the surface adhesion required for continuous foil application in the semi-dry stage, and then obtains the cohesive retention ability to withstand cutting, bending and UV offset printing loads after pre-curing. This helps to reduce continuous defects or boundary migration of gold foil, and alleviates warping caused by local moisture and shrinkage differences in the paper matrix, thereby improving the paper surface flatness.

[0008] Preferably, the thiol self-crosslinking core-shell emulsion is prepared by a method comprising the following steps: (1) The acrylate soft core monomer was dispersed in an aqueous phase and emulsion polymerized to obtain a soft core seed emulsion; (2) Add a hard-shell monomer including glycidyl methacrylate, diacetone acrylamide and phosphate functional monomers to the soft-core seed emulsion and perform coating polymerization to obtain a core-shell emulsion with reserved epoxy groups. (3) Add boron-containing amine ring-opening raw material to the core-shell emulsion with reserved epoxy groups and stir to make the amino group of the boron-containing amine ring-opening raw material ring-open with a portion of the reserved epoxy groups; (4) After step (3), add cysteine ​​and stir to open the ring with another portion of the reserved epoxy group; (5) Add adipic acid dihydrazide to obtain the thiol self-crosslinked core-shell emulsion.

[0009] By adopting the above technical solution, this application first forms a soft core and coats it with a functional hard shell containing epoxy groups, diacetone amide groups, and phosphate ester groups, so that the deformation-bearing region and the cohesive reinforcement region are separated at the particle scale. Then, the reserved epoxy groups are distributed in the order of boron-containing amine raw materials first and cysteine ​​later, which can reduce the competitive reaction when the two types of ring-opening raw materials are added at the same time, so that the arylboronic acid side groups and terminal mercapto side chains are more stably assigned to the functional hard shell. The carbonyl groups introduced by adipic acid dihydrazide and diacetone acrylamide crosslink during the film-forming stage, which is beneficial to transform the deformability before foil application into the cohesive retention ability after foil application, thereby maintaining the integrity of the gold foil after cutting and bending and the peel strength after application.

[0010] Preferably, the boron-containing amine ring-opening raw material is an aminoarylboronic acid raw material, which has both an amino group and a borate group on the same aryl skeleton, and the amino group can participate in the ring-opening reaction of the reserved epoxy group.

[0011] By adopting the above technical solution, this application utilizes the amino group in the same molecule to complete the covalent grafting with the hard shell epoxy group, so that the boric acid group is fixed near the particle surface along with the aryl skeleton, avoiding migration with the aqueous phase when added in the form of free small molecules. This is beneficial to keep the polar interface on the functional hard shell of the core-shell particles during the film formation and loading process, and improves the interfacial bonding stability.

[0012] Preferably, the aminoarylboronic acid raw material is selected from at least one of 2-aminophenylboronic acid, 3-aminophenylboronic acid, and 4-aminophenylboronic acid.

[0013] By adopting the above technical solution, this application can adjust the ring-opening grafting accessibility of the raw material and the spatial exposure degree of the borate group after grafting by adjusting the positional relationship between the amino group and the borate group on the aryl skeleton, so as to adapt to different emulsion reaction states and interface bonding requirements.

[0014] Preferably, in step (4) of the method for preparing the thiol self-crosslinking core-shell emulsion, the ring-opening temperature of cysteine ​​and the reserved epoxy group is 40-50°C.

[0015] By adopting the above technical solution, this application enables cysteine ​​to be grafted within a temperature range sufficient to promote epoxy ring opening without excessively inducing side reactions of thiol groups. This is beneficial for retaining the terminal thiol side chains on the functional hard shell and reducing particle aggregation caused by excessively rapid local reactions in the emulsion, thereby improving the preparation stability of the emulsion and the maintenance of the gold foil interface.

[0016] Preferably, the aliphatic waterborne polyurethane is a polyether-type aliphatic waterborne polyurethane.

[0017] By adopting the above technical solution, this application utilizes the flexibility and water-dispersible compatibility of the polyether soft segment to buffer the film-forming shrinkage of the core-shell particles and the bending strain of the paper base. Furthermore, the flexibility of the continuous phase and the cohesive base formed by the core-shell particles complement each other, which helps maintain the continuity of stress transfer during gold foil bonding and subsequent offset printing, thereby improving the integrity of the gold foil after bending. This design also helps improve the flatness of the paper surface after conditioning and maintains the load-bearing stability of the adhesive layer.

[0018] Preferably, the polyether-type aliphatic waterborne polyurethane is selected from at least one of polytetrahydrofuran ether diol-type aliphatic waterborne polyurethane, polypropylene glycol-type aliphatic waterborne polyurethane, and polyethylene glycol / polypropylene glycol copolyether-type aliphatic waterborne polyurethane.

[0019] By adopting the above technical solution, this application can adjust the deformation recovery and moisture release of the continuous phase by taking advantage of the differences in the segment regularity, hydrophilicity and flexibility of different polyether soft segments, which is conducive to obtaining a suitable balance between foil integrity, offset printing boundary stability and paper surface flatness for a specific paper base.

[0020] Preferably, the degree of alcoholysis of the polyvinyl alcohol is 87.0 mol%-99.5 mol%.

[0021] By adopting the above technical solution, this application adjusts the hydroxyl density and residual acetate group ratio by limiting the degree of alcoholysis of polyvinyl alcohol, so that the dissolution and dispersion process of polyvinyl alcohol in the aqueous system is connected with its effect on paper fibers. At the same time, the effect of paper fibers is coordinated with the film formation of the emulsion continuous phase, which helps to reduce the local shrinkage difference caused by uneven drying and improve the boundary stability of gold foil and the smoothness of paper surface.

[0022] Preferably, the degree of alcoholysis of the polyvinyl alcohol is 87.0 mol%-90.0 mol%.

[0023] By adopting the above technical solution, this application retains an appropriate amount of residual acetate groups within the range of hydrolysis degree in the upper position, so that the continuous phase has both the paper-based action ability brought by hydroxyl groups and maintains faster water solubility and lower local crystallization tendency, which is conducive to further improving the uniformity of the semi-dry stage and the boundary stability after offset printing.

[0024] Secondly, this application provides a method for preparing gold foil offset printing products, which adopts the following technical solution: The preparation method of gold foil offset printing products according to any one of the above includes the following steps: (1) The prepared mercapto self-crosslinking core-shell emulsion was mixed with aliphatic waterborne polyurethane, acrylic modified rosin emulsion, polyvinyl alcohol, dispersion medium and coating additive to obtain waterborne gold leaf adhesive. (2) Clean and position the paper substrate, and apply the water-based gold leaf adhesive to the paper substrate; (3) Dry the coated water-based gold leaf adhesive until it is semi-dry and does not continuously transfer to the polyester film and continuously adheres to the gold foil under light pressure. Then apply the gold foil and pre-cur it. (4) Perform UV offset printing on the positioning area and then perform UV curing to obtain the gold foil offset print.

[0025] By adopting the above technical solution, this application first completes the cleaning and positioning of the paper base surface, and then determines the foil application time point based on observable surface transfer and continuous foil adhesion state, so that foil application does not depend on a single fixed drying time; after foil application, pre-curing is performed first, so that the cohesive network of the adhesive layer is established before being subjected to offset printing shear, and then UV offset printing and ultraviolet curing are performed according to the positioning area, which helps to reduce the displacement of the gold foil boundary caused by the offset printing load, and maintain the continuity of graphic overprinting and boundary stability across the gold foil area and non-gold foil area.

[0026] In summary, this application has the following beneficial effects: 1. By providing dynamic bonding opportunities in the continuous phase containing polyvinyl alcohol through the arylboronic acid side groups on the functional hard shell, and by providing sulfur-containing action sites for the terminal thiol side chains facing the gold foil interface, the gold foil adhesive can connect the continuous phase constraint and interface bonding during the dehydration process, widen the identifiable semi-dry foil application operation window, and improve the cutting and bending integrity and UV offset printing position stability. 2. The flexible continuous phase of polyether-type aliphatic waterborne polyurethane buffers the shrinkage of the adhesive layer and the deformation of the paper base, which helps to improve the peel strength after bonding and reduce the warping of the paper surface after conditioning, thereby improving the flatness of the paper surface after conditioning. 3. By progressively adjusting the degree of polyvinyl alcohol hydrolysis, the dispersion process in water, the action on paper fibers, and the continuous phase film formation process are seamlessly connected. This reduces localized drying shrinkage differences, decreases the gold foil boundary displacement after UV offset printing, and improves the paper surface smoothness after conditioning. These adjustments contribute to improving the overall performance of offset printing. Detailed Implementation

[0027] The present application will be further described below with reference to preparation examples, embodiments, and comparative examples. The paper substrate, gold foil, and UV ink are all commercially available materials. The paper substrate uses coated paper from the same batch, the gold foil uses gold foil from the same batch without a carrier film and without a pre-coated hot melt adhesive layer, and the UV ink uses offset UV ink from the same batch. The deionized water is commercially available conventional deionized water; the formulation amounts of aqueous emulsions or dispersions are calculated based on the mass of the polymer solids contained therein.

[0028] Aliphatic waterborne polyurethane, acrylic-modified rosin emulsion, and polyvinyl alcohol are all commercially available materials. Aliphatic waterborne polyurethane is accepted based on soft segment type and polymer solids content, while acrylic-modified rosin emulsion is accepted based on resin solids content. The polyvinyl alcohol used in all examples and comparative examples is of a comparable grade with a nominal degree of polymerization of 1700±100, with only the degree of hydrolysis modified according to the corresponding example specifications. Polyvinyl alcohol is accepted based on the degree of hydrolysis stated in the product quality certificate; when verification is required, the same batch is used for saponification titration. Anionic emulsifiers, ammonium persulfate, wetting agents, defoamers, and rheology modifiers are all commercially available materials, and the same batch and the same method of addition are used for similar applications.

[0029] Butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, glycidyl methacrylate, diacetone acrylamide, 2-aminophenylboronic acid, 3-aminophenylboronic acid, 4-aminophenylboronic acid, cysteine, and adipate dihydrazide are all commercially available materials, and are inspected according to their raw material names and effective contents. The phosphate ester functional monomer used in this application is 2-methacryloyloxyethyl phosphate, which contains methacryloyl groups and phosphate groups that can participate in the coating polymerization; nitrogen is a commercially available industrial gas. The thiol self-crosslinking core-shell emulsion is the only component in this application that is prepared separately before use; the "self-crosslinking" in its name refers to the crosslinking relationship formed between diacetone acrylamide and adipate dihydrazide during the film-forming stage, with the terminal thiol side chain providing sulfur-containing action sites facing the gold foil interface; the other formulation components are used directly in their respective commercial forms.

[0030] Preparation example of thiol self-crosslinking core-shell emulsion Preparation Example 1 This preparation example provides a thiol-based self-crosslinking core-shell emulsion, prepared according to the following method: (1) Add 300g of deionized water and 2.0g of anionic emulsifier to a reaction vessel equipped with a stirrer, condenser, thermometer and nitrogen inlet, introduce nitrogen and heat to 75℃. Mix 52g of n-butyl acrylate and 18g of 2-ethylhexyl acrylate to form a soft core monomer, and dissolve 0.8g of ammonium persulfate in 20g of deionized water to form the first initiator solution; add the soft core monomer and the first initiator solution dropwise simultaneously at 75℃, complete the addition within 2h, keep warm for 1h, and obtain a soft core seed emulsion.

[0031] (2) Mix 20g methyl methacrylate, 8g glycidyl methacrylate, 3g diacetone acrylamide, and 1g 2-methacryloyloxyethyl phosphate to form a hard-shell monomer. Dissolve 0.4g ammonium persulfate in 10g deionized water to form a second initiator solution. Heat the soft-core seed emulsion to 80℃ and simultaneously add the hard-shell monomer and the second initiator solution dropwise over 1.5h. Keep warm for 1h to obtain a core-shell emulsion with reserved epoxy groups, wherein the solid mass ratio of the soft-core monomer to the hard-shell monomer is 70:32. Based on the calculation that each mole of glycidyl methacrylate monomer contains one mole of epoxy group, the reserved epoxy group corresponding to 8g of glycidyl methacrylate at the time of feeding is 0.0563mol.

[0032] (3) 3.08 g of 3-aminophenylboronic acid was dispersed in 17.45 g of deionized water to obtain a 15.0% (w / w) aqueous dispersion of 3-aminophenylboronic acid. The core-shell emulsion was cooled to 55 °C, and the aqueous dispersion was added and stirred for 6 h to allow the amino group to undergo ring-opening with a portion of the reserved epoxy groups. The molar ratio of the amino group of 3-aminophenylboronic acid to the reserved epoxy groups at the time of feeding was 0.40:1. Subsequently, the temperature was adjusted to 45 °C, and 1.74 g of cysteamine was dissolved in 15.66 g of deionized water. The resulting 10.0% (w / w) aqueous solution of cysteamine was added. The molar ratio of cysteamine to the reserved epoxy groups at the time of feeding was 0.40:1. The pH was maintained at 7.5-8.5 and stirred for 4 h to allow the cysteamine to undergo ring-opening with another portion of the reserved epoxy groups. The total molar ratio of the amino group of the two ring-opening raw materials to the reserved epoxy groups at the time of feeding was 0.80:1. After cooling to room temperature, 2.2 g of adipic acid dihydrazide was added, stirred until homogeneous, and the polymer solid content was adjusted to 40% with deionized water to obtain the thiol self-crosslinking core-shell emulsion of Preparation Example 1.

[0033] Referring to Table 1, the difference between Preparation Examples 1-3 lies in the aminoarylboronic acid raw material. The actual feed amount of the three positional isomers was 3.08 g, and an aqueous dispersion with a mass fraction of 15.0% was used. The molar ratio of the amino group to the epoxy group reserved at the time of feeding was 0.40:1. Other raw materials, dosages, and operating conditions were the same as in Preparation Example 1. The ring-opening temperature of cysteine ​​in all three preparation examples was 45°C.

[0034] Table 1. Preparation of aminoarylboronic acid raw materials for Examples 1-3 Preparation Example aminoarylboronic acid raw materials Actual feed weight / g Aqueous dispersion mass fraction / % Preparation Example 1 3-Aminophenylboronic acid 3.08 15.0 Preparation Example 2 2-Aminophenylboronic acid 3.08 15.0 Preparation Example 3 4-Aminophenylboronic acid 3.08 15.0 Preparation Example 4 The difference between this preparation example and Preparation Example 1 is that the ring-opening temperature of cysteine ​​and the reserved epoxy group is 37.5°C, while the other raw materials, amounts and operating conditions are the same as in Preparation Example 1.

[0035] Referring to Table 2, the difference between Preparation Example 1 and Preparation Examples 4-8 lies in the ring-opening temperature of cysteine ​​and the reserved epoxy group; other raw materials, amounts, and operating conditions are the same as in Preparation Example 1. The ring-opening temperatures of each preparation example are shown in Table 2.

[0036] Table 2. Cysteine ​​ring-opening temperature settings for Preparation Examples 1 and 4-8 Preparation Example Cysteine ​​ring-opening temperature / °C Preparation Example 4 37.5 Preparation Example 5 40.0 Preparation Example 6 42.5 Preparation Example 1 45.0 Preparation Example 7 47.5 Preparation Example 8 50.0 Example Example 1

[0037] This embodiment provides a gold foil offset print, comprising, along the thickness direction, a paper substrate, a water-based gold foil layer, a gold foil layer, and a UV offset printing image layer stacked sequentially; the water-based gold foil layer is formed by curing the water-based gold foil, which, based on the polymer solids mass, is prepared using 95g of a mercapto self-crosslinking core-shell emulsion (Preparation Example 1), 15g of a polyester-type aliphatic waterborne polyurethane, 10g of an acrylic-modified rosin emulsion, and 2.0g of polyvinyl alcohol with a degree of hydrolysis of 80.0 mol%; the mercapto self-crosslinking core-shell emulsion contains self-crosslinking core-shell particles, which have a functional hard shell with arylboronic acid side groups and terminal mercapto side chains.

[0038] This embodiment provides a method for preparing gold foil offset printing products, including the following steps: (1) Calculate the wet material dosage based on the polymer solids content of each emulsion or dispersion, and add the equivalent of 95g of polymer solids from the thiol self-crosslinking core-shell emulsion of Preparation Example 1, the equivalent of 15g of polymer solids from polyester-type aliphatic waterborne polyurethane, the equivalent of 10g of polymer solids from acrylic-modified rosin emulsion, and 2.0g of polyvinyl alcohol with a degree of alcoholysis of 80.0 mol%. The thiol self-crosslinking core-shell emulsion of Preparation Example 1 is 237.5g of wet material based on a polymer solids content of 40.0%. First, dilute the polyvinyl alcohol with deionized water to form water. The solution was then sequentially supplemented with a mercapto self-crosslinking core-shell emulsion, an aliphatic waterborne polyurethane, and an acrylic-modified rosin emulsion. Based on a total polymer solid mass of 100 parts for the four film-forming components, 0.30 parts for wetting agent, 0.20 parts for defoamer, and 0.50 parts for rheology modifier were added. The actual amounts added in Example 1 were 0.37 g, 0.24 g, and 0.61 g, respectively. Deionized water was added to ensure the total polymer solid mass of the four film-forming components accounted for 35.0% of the total mass of the waterborne gold leaf adhesive. The mixture was stirred until homogeneous to obtain the waterborne gold leaf adhesive. All examples and comparative examples used the above-mentioned additive ratios based on the total polymer solid mass of their respective four film-forming components, and the polymer solid mass fraction was adjusted to 35.0%. (2) Clean and position the paper substrate. In an environment of 23±2℃ and 50±5% relative humidity, apply the water-based gold plating adhesive obtained in step (1) to the paper substrate using a wire rod. The wet coating amount is 40g / m². (3) Dry the coated water-based gold leaf adhesive in an environment of 23±2℃ and 50±5% relative humidity. Based on the mass of volatile substances in the adhesive layer at the end of coating, when the mass loss rate of volatile substances reaches 50-65%, and the adhesive layer surface does not continuously transfer to the polyester film, and the gold foil can be continuously adhered under light pressure, it is determined to be in a semi-dry state. Then, gold foil without carrier film and without pre-coated hot melt adhesive layer is laminated. A 1.0kg flat roller is used to press back and forth once at a speed of 100mm / s, and then pre-cured for 2 minutes under hot air at 60℃. (4) After pre-curing, UV ink is used for offset printing according to the positioning area, so that the UV offset printed image area spans the gold foil area and the non-gold foil area; the offset printing speed is 0.5m / s, the printing pressure is 0.20MPa, and then UV curing is performed with a cumulative irradiation energy of 800mJ / cm² to obtain the gold foil offset printed product. All examples and comparative examples use the same paper substrate, gold foil and UV ink, and maintain the same wet coating amount, foil bonding conditions, pre-curing conditions, offset printing speed, printing pressure and UV curing energy.

[0039] Referring to Table 3, the difference between Examples 1-5 lies in the solid feeding point of the four film-forming components; the other materials and preparation conditions are the same as in Example 1.

[0040] Table 3. Solid feed settings for film-forming components in Examples 1-5 sample Thiol-based self-crosslinking core-shell emulsion solids / g Aliphatic waterborne polyurethane solids / g Acrylic modified rosin emulsion solids / g Polyvinyl alcohol solids / g Example 1 95 15 10 2.0 Example 2 98 17 11 2.3 Example 3 100 19 12 2.7 Example 4 103 20.5 13.5 3.1 Example 5 105 22 15 3.5 Example 6 The difference between Example 6 and Example 3 is that the thiol self-crosslinking core-shell emulsion of Preparation Example 1 is replaced with the thiol self-crosslinking core-shell emulsion of Preparation Example 2, while the other materials, amounts and operating conditions are the same as in Example 3.

[0041] Referring to Table 4, the difference between Example 3 and Examples 6-12 is that the preparation methods of the thiol self-crosslinking core-shell emulsion are different.

[0042] Except for the preparation of the thiol self-crosslinking core-shell emulsion, the materials, amounts, and operating conditions in Examples 3 and 6-12 are the same.

[0043] Table 4. Source settings of thiol self-crosslinking core-shell emulsions in Examples 3 and 6-12 sample Thiol-based self-crosslinking core-shell emulsion source Example 3 Preparation Example 1 Example 6 Preparation Example 2 Example 7 Preparation Example 3 Example 8 Preparation Example 4 Example 9 Preparation Example 5 Example 10 Preparation Example 6 Example 11 Preparation Example 7 Example 12 Preparation Example 8 Example 13 The difference between Example 13 and Example 10 is that the polyester-type aliphatic waterborne polyurethane is replaced with polytetrahydrofuran ether diol-type aliphatic waterborne polyurethane, while the other materials, dosages and operating conditions are the same as in Example 10.

[0044] Referring to Table 5, the difference between Example 10 and Examples 13-15 is that the type of soft segment of the aliphatic waterborne polyurethane is different, while the other materials, dosages and operating conditions are the same as in Example 10.

[0045] Table 5. Aliphatic waterborne polyurethane soft segment type settings in Examples 10 and 13-15 sample Aliphatic waterborne polyurethane soft segment type Example 10 Polyester type Example 13 Polytetrahydrofuran ether diol type Example 14 Polypropylene glycol type Example 15 Polyethylene glycol / polypropylene glycol copolyether type Example 16 The difference between Example 16 and Example 13 is that the polyvinyl alcohol with a degree of hydrolysis of 80.0 mol% is replaced with polyvinyl alcohol with a degree of hydrolysis of 87.0 mol%, while the other materials, amounts and operating conditions are the same as in Example 13.

[0046] Referring to Table 6, the difference between Example 13 and Examples 16-20 is that the degree of alcoholysis of polyvinyl alcohol is different, while the other materials, amounts and operating conditions are the same as in Example 13.

[0047] Table 6. Polyvinyl alcohol hydrolysis degree settings for Examples 13 and 16-20 sample Polyvinyl alcohol degree of hydrolysis / mol% Example 13 80.0 Example 16 87.0 Example 17 90.0 Example 18 93.0 Example 19 96.0 Example 20 99.5 Example 21 The difference between Example 21 and Example 18 is that the polyvinyl alcohol with a degree of hydrolysis of 93.0 mol% is replaced with polyvinyl alcohol with a degree of hydrolysis of 87.75 mol%, while the other materials, amounts and operating conditions are the same as in Example 18.

[0048] Referring to Table 7, the difference between Example 18 and Examples 16, 17 and 21-23 is that the degree of alcoholysis of polyvinyl alcohol is different, while the other materials, amounts and operating conditions are the same as those in Example 18.

[0049] Table 7. Polyvinyl alcohol hydrolysis degree settings for Examples 16-18 and 21-23 sample Polyvinyl alcohol degree of hydrolysis / mol% Example 18 93.00 Example 16 87.00 Example 21 87.75 Example 22 88.50 Example 23 89.25 Example 17 90.00 Comparative Example 1 The difference between this comparative example and Example 3 is that 3.08g of 3-aminophenylboronic acid was not added when preparing the core-shell emulsion, and 17.45g of deionized water was added in the corresponding steps to maintain the consistency of the dispersion medium feed; cysteine ​​was still fed at 1.74g, and the concentration of cysteine ​​aqueous solution, ring-opening conditions, other core-shell structures and the final aqueous gold foil formulation remained unchanged, resulting in a functional hard shell gold foil offset print without arylboronic acid side groups.

[0050] Comparative Example 2 The difference between this comparative example and Example 3 is that 3-aminophenylboronic acid ring-opening grafting was not performed when preparing the core-shell emulsion, and 17.45g of deionized water was added in the corresponding step; after the core-shell emulsion was prepared, 3.08g of 3-aminophenylboronic acid was dispersed in 17.45g of deionized water, and then the resulting aqueous dispersion with a mass fraction of 15.0% was directly added to the core-shell emulsion, while other materials, amounts and operating conditions remained unchanged.

[0051] Comparative Example 3 The difference between this comparative example and Example 3 is that 1.74g of cysteine ​​was not added when preparing the core-shell emulsion, and 15.66g of deionized water was added in the corresponding steps to maintain consistent feeding of the dispersion medium; the ring-opening grafting of 3.08g of 3-aminophenylboronic acid and the remaining core-shell structure and the final aqueous gold foil formulation were retained to obtain a functional hard shell gold foil offset print without terminal thiol side chains.

[0052] Comparative Example 4 The difference between this comparative example and Example 3 is that, firstly, a 10.0% cysteamine aqueous solution prepared by 1.74g cysteamine and 15.66g deionized water was added at 45°C, maintaining the pH at 7.5-8.5 and stirring for 4 hours; then, the temperature was adjusted to 55°C, and a 15.0% aqueous dispersion prepared by 3.08g 3-aminophenylboronic acid and 17.45g deionized water was added and stirred for 6 hours. The molar ratio of the amino group to the epoxy group reserved at the time of feeding for both raw materials was 0.40:1, and other materials, amounts, and operating conditions remained unchanged.

[0053] Performance testing methods Each embodiment and comparative example prepared three batches of final gold foil offset prints independently. For the semi-dry, adhesive-compatible time window, five independent time series of coated paper strips were set for each batch, with one independent strip used at each testing point; for other indicators, five samples were randomly obtained from each batch. Except for the semi-dry, adhesive-compatible time window, sampling began at the end of coating, all other samples were conditioned for 24 hours at 23±2℃ and 50±5% relative humidity, and tested under the same conditions. For the semi-dry, adhesive-compatible time window, the arithmetic mean of the five independent time series for each batch was calculated first, followed by the arithmetic mean of the three batch averages; for other indicators, the arithmetic mean of the five samples in each batch was calculated first, followed by the reporting of the three batch averages. All results were rounded to the precision shown in Table 8, while retaining single-piece or single-sequence records and batch records.

[0054] 1. Semi-dry, bondable time window: For each independent time series, coated paper strips 25mm wide and 100mm long were prepared along the paper machine direction. Starting from the end of coating, one strip was taken every 1 minute. Under constant temperature and humidity conditions, the polyester film was pressed back and forth once with a 1.0kg flat roller, then peeled off. The alloy foil was then bonded under the same pressure. The pass criterion was that the adhesive layer did not continuously transfer to the polyester film, and the gold foil continuously covered 95% of the effective length of the test strip after light pressure. The difference between the last pass time point and the first pass time point was the semi-dry, bondable time window for that time series, in minutes. The results of each batch of 5 time series and 3 independent batches were averaged according to the above two levels and rounded to 0.1 minutes.

[0055] 2. Initial Gold Foil Area Ratio: Using a 100mm×100mm sample, after foil application and pre-curing, and before UV offset printing, the central 50mm×50mm gold foil area was photographed using a ring light source with a color temperature of 5500±200K, a vertical imaging stand, and a camera with a resolution of no less than 20μm / pixel. The two sets of edges of this area were parallel to the paper machine direction and the transverse direction, respectively. Before each batch was tested, white balance and exposure calibration were performed using a neutral gray card. Subsequently, the white balance, exposure parameters, light source, and object distance were locked, and the same batch of complete gold foil, exposed adhesive layer, and exposed paper base were photographed under the same imaging conditions as three types of reference images. The reference image and the image to be tested are converted to the CIELAB color space. The mean values ​​of L*, a*, and b* of the three types of pixels in the reference image are calculated respectively. For each pixel in the target area, the distance between it and the three mean values ​​is calculated using CIEDE2000 color difference. Only when the color difference between the pixel and the mean value of the complete gold foil is strictly less than the color difference between the pixel and the mean values ​​of the exposed adhesive layer and the exposed paper base is the pixel identified as a gold foil pixel. If the color difference is equal, the pixel is identified as a non-gold foil pixel. Eight-neighbor connected component analysis is performed on the identified gold foil pixels. Only connected components with a converted physical area of ​​not less than 0.01 mm² are included. No manual point filling, hole filling, or boundary interpolation is performed. The initial proportion of the complete gold foil area is calculated by dividing the number of included gold foil pixels by the total number of pixels in the target area and multiplying by 100%, in percentages (%).

[0056] 3. Proportion of Complete Gold Foil Area After Cutting: Using the same test piece and imaging system as the initial complete area, the edge of the gold foil area is cut along a straight line parallel to the paper machine direction at a speed of 100 mm / s using the same cutter. After standing for 10 minutes, imaging is performed. Taking the cut edge as the x=0 line and the side retaining the gold foil as the positive x-axis, 25 mm is taken on each side along the cut edge direction from the midpoint of the cut edge, and then 50 mm is extended vertically from the cut edge to the side retaining the gold foil. This forms a unique target area with an edge coinciding with the cut edge and a size of 50 mm × 50 mm. Identification is performed according to the same batch of three-class references, CIELAB conversion, CIEDE2000 minimum color difference judgment, classification of equal color difference into non-gold foil, eight-neighbor connected domain, and 0.01 mm² area threshold as described in the initial complete gold foil area proportion. The percentage of the number of gold foil pixels included in the target area is used as the proportion of the complete gold foil area after cutting, in units of %.

[0057] 4. Proportion of Complete Gold Foil Area After Bending: With the fold line perpendicular to the paper machine direction, bend the sample 180° three times along the fold line around a 2mm diameter circular axis. Unfold and let stand for 10 minutes before imaging. Using the midpoint of the fold line as the center, extend 25mm to each side along the fold line direction, and then extend 25mm to each side along the normal direction of the fold line, thus forming a unique target area of ​​50mm × 50mm, equally divided by the fold line. Identify the target area according to the initial gold foil complete area proportion, using three reference types from the same batch, CIELAB conversion, CIEDE2000 minimum color difference judgment, classification of equal color differences into non-gold foil, eight-neighbor connected domains, and a 0.01mm² area threshold. The percentage of gold foil pixels included in the target area relative to the total number of pixels is used as the proportion of the complete gold foil area after bending, in units of %. The initial, cut, and bent areas of the gold foil in Table 8 are all calculated using the above-mentioned fixed identification rules and their respective fixed target areas, without adjusting the reference category, color difference criterion, connectivity mode, or area threshold for different samples.

[0058] 5. Post-attach peel strength: Prepare strip specimens 25 mm wide and with an effective peel length of 100 mm along the paper machine direction. Attach a 25 mm wide polyester reinforcing tape to the gold foil surface to form the traction end. Use an electronic universal testing machine with a force sensor range of 0-50 N and a 180° peel fixture to peel at a speed of 100 mm / min. Integrate the force value over the 20-80 mm stable section and divide by the displacement length. Report the average peel force based on the 25 mm strip width, in N / 25 mm.

[0059] 6. Gold foil boundary displacement after UV offset printing: Using a 100mm×150mm specimen, a straight gold foil boundary with a length of not less than 50mm and four positioning marks were set on the specimen. Using a digital microscopic imaging system with a planar resolution of 0.01mm, the same 10 boundary points and positioning marks were imaged before UV offset printing and after UV curing. The planar displacement vector of each point relative to the positioning marks was calculated, and the maximum displacement modulus among the 10 points was reported in mm.

[0060] 7. Paper surface flatness after conditioning: Use a 150mm×150mm test piece. Place the test piece naturally on the granite platform without applying external pressure. Use a height gauge with a resolution of 0.01mm to measure the height of the four corner points and the four midpoints of the sides relative to the platform. Report the maximum value among the eight measuring points in mm. The smaller the value, the flatter the paper surface.

[0061] Table 8 Performance test results of each embodiment and comparative example sample Semi-dry adhesive time window / min Initial gold foil complete area / % Complete area after cutting / % Complete area after bending / % Post-application peel strength (N / 25mm) Boundary displacement after UV offset printing / mm Maximum warping height after humidification / mm Example 1 9.6 85.4 84.2 83.2 0.76 0.77 1.89 Example 2 10.9 88.1 86.0 83.0 0.89 0.65 2.26 Example 3 11.2 90.8 88.8 88.1 0.94 0.50 1.62 Example 4 10.6 88.4 86.6 86.6 0.91 0.60 2.37 Example 5 10.2 87.8 85.0 84.6 0.83 0.68 3.27 Example 6 10.5 89.7 86.8 85.8 0.90 0.64 2.05 Example 7 11.1 89.6 88.4 86.9 0.92 0.52 2.28 Example 8 9.7 86.4 83.8 82.5 0.77 0.74 2.14 Example 9 10.3 87.9 87.3 84.3 0.83 0.66 1.61 Example 10 11.4 92.1 88.7 87.7 1.01 0.48 1.79 Example 11 10.9 91.4 87.6 87.1 0.90 0.59 2.74 Example 12 10.2 90.1 87.1 85.8 0.86 0.64 2.25 Example 13 11.2 93.8 91.1 90.2 1.05 0.46 1.77 Example 14 11.3 92.7 90.4 88.2 1.00 0.51 2.78 Example 15 10.8 91.5 87.2 87.9 0.97 0.55 1.44 Example 16 11.8 93.5 91.8 90.6 1.03 0.39 1.56 Example 17 11.8 95.7 93.0 91.1 1.04 0.27 1.95 Example 18 12.2 93.9 93.0 91.2 1.11 0.30 2.25 Example 19 11.4 92.0 89.9 88.4 0.97 0.49 2.58 Example 20 10.3 90.3 87.6 87.5 0.88 0.65 2.98 Example 21 12.0 95.4 93.2 90.4 1.06 0.33 1.43 Example 22 12.1 94.9 93.4 92.1 1.10 0.18 1.56 Example 23 12.0 95.0 93.4 90.9 1.10 0.33 1.89 Comparative Example 1 8.7 83.0 80.4 79.6 0.70 1.03 2.08 Comparative Example 2 9.2 84.4 82.3 81.1 0.71 0.97 3.10 Comparative Example 3 10.2 77.7 75.6 74.1 0.61 0.73 1.89 Comparative Example 4 9.1 85.2 83.6 83.9 0.78 0.87 2.74 Referring to Table 8, Examples 1-5 only changed the compatibility of the four film-forming components within a predetermined range. The semi-dry lamination time window of Example 3 was 11.2 min, with initial, cut, and bent intact gold foil areas of 90.8%, 88.8%, and 88.1%, respectively. The peel strength after lamination was 0.94 N / 25 mm, all higher than Example 1. Its boundary displacement after UV offset printing decreased from 0.77 mm in Example 1 to 0.50 mm, and the maximum lift-off height decreased from 1.89 mm to 1.62 mm. When the dosage of each component was further increased to Examples 4 and 5, many indicators did not continue to improve in the same direction, and the maximum lift-off height increased to 2.37 mm and 3.27 mm, respectively, indicating that the compatibility of the four film-forming components affected the overall balance of semi-dry lamination, cohesion retention, and paper shrinkage.

[0062] Referring to Table 8, compared with Example 3, Examples 6-12 only changed the source of the self-made emulsion, while keeping other conditions the same. Examples 6 and 7 used different aminophenylboronic acid positional isomers; Examples 8-12 and Example 3 corresponded to cysteine ​​ring-opening temperatures of 37.5℃, 40℃, 42.5℃, 45℃, 47.5℃, and 50℃, respectively. The semi-dry adhesive time window of Examples 9, 10, 3, 11, and 12, which were in the 40-50℃ range, was 10.2-11.4 min, with initial, cut, and bent intact areas of 87.9-92.1%, 87.1-88.8%, and 84.3-88.1%, respectively. The peel strength after application was 0.83-1.01 N / 25 mm, the boundary displacement after UV offset printing was 0.48-0.66 mm, and the maximum lift height was 1.61-2.74 mm. The corresponding data for Example 8, below this range, are 9.7 min, 86.4%, 83.8%, 82.5%, 0.77 N / 25 mm, 0.74 mm, and 2.14 mm, respectively. Therefore, under the fixed conditions in this group, the samples in the 40-50°C range generally outperformed the samples at 37.5°C in terms of semi-drying time, gold foil retention after cutting and bending, peel strength, and boundary displacement; however, the optimal points for each indicator are not entirely consistent. These results indicate that the ring-opening temperature affects the formation state of functional groups on the hard shell surface and their matching with the continuous phase film formation, but the indicators within this temperature range do not change monotonically with increasing temperature.

[0063] Referring to Table 8, compared with Example 10, Examples 13-15 only changed the type of soft segment of the aliphatic waterborne polyurethane, while keeping other conditions the same. In Example 13, the intact area after cutting increased from 88.7% to 91.1%, the intact area after bending increased from 87.7% to 90.2%, the peel strength after application increased from 1.01 N / 25 mm to 1.05 N / 25 mm, and the boundary displacement decreased from 0.48 mm to 0.46 mm. Example 15 had the lowest maximum warp height at 1.44 mm, but its intact area and peel strength were lower than those of Example 13. This data indicates that different polyether soft segments will adjust the continuous phase flexibility, moisture release, and deformation recovery to varying degrees, thus exhibiting different emphases between interface maintenance and paper surface flatness.

[0064] Referring to Table 8, compared with Example 13, Examples 16-20 only changed the degree of polyvinyl alcohol hydrolysis, while keeping other conditions the same. When the degree of hydrolysis increased from 87.0 mol% to 93.0 mol%, the semi-dry bondable time window increased from 11.8 min to 12.2 min, and the peel strength after bonding increased from 1.03 N / 25 mm to 1.11 N / 25 mm; when it continued to increase to 99.5 mol%, both data decreased to 10.3 min and 0.88 N / 25 mm, the boundary displacement increased to 0.65 mm, and the maximum lift height increased to 2.98 mm. This change is consistent with the changes in hydroxyl density, dissolution state, and local crystallization tendency of the continuous phase when the degree of hydrolysis increases, indicating that there is no monotonically improving relationship between the various indicators and the degree of hydrolysis within the upper range.

[0065] Referring to Table 8, compared with Example 18, Examples 16, 17, and 21-23 only changed the degree of polyvinyl alcohol hydrolysis, while keeping other conditions the same. Example 22 had a boundary displacement of 0.18 mm and a 92.1% intact area after bending, while Example 21 had a maximum warp height of 1.43 mm, representing superior values ​​in different evaluation dimensions. Examples 16 and 17, located at the endpoints of the range, maintained a semi-dry, platable time window of 11.8 min and an intact area after bending of no less than 90.6%. These results indicate that the balance between the density of residual acetate groups and hydroxyl groups within the narrowed range is beneficial for connecting the dispersion process in water, the action on paper fibers, and the continuous phase film formation process, and improves the boundary stability after UV offset printing. However, different indicators still exhibit identifiable trade-offs.

[0066] Referring to Table 8, compared with Example 3, all comparative examples maintained the same conditions as in Example 3 except for the registration changes. In Comparative Example 1, after omitting the arylboronic acid side groups on the hard shell, the initial intact area decreased from 90.8% to 83.0%, the intact area after cutting decreased from 88.8% to 80.4%, the intact area after bending decreased from 88.1% to 79.6%, and the boundary displacement increased from 0.50 mm to 1.03 mm. In Comparative Example 2, when an equimolar amount of 3-aminophenylboronic acid was introduced by adding free small molecules, the initial intact area was 84.4%, the intact area after cutting was 82.3%, the intact area after bending was 81.1%, and the maximum warp height was 3.10 mm. Compared with the arylboronic acid side groups covalently fixed on the functional hard shell, free 3-aminophenylboronic acid cannot stably maintain the boron-containing action sites near the core-shell particles, nor can it continuously participate in the local confinement of the continuous phase containing polyvinyl alcohol. In Comparative Example 3, after omitting the terminal thiol side chain, the initial intact area was 77.7%, the intact area after cutting was 75.6%, the intact area after bending was 74.1%, and the peel strength after application was 0.61 N / 25 mm. In Comparative Example 4, after changing the order of addition of the two types of ring-opening raw materials, the boundary displacement was 0.87 mm, and the maximum lift height was 2.74 mm. The above comparisons show that the covalently fixed arylboronic acid side group, the terminal thiol side chain, and their formation order all affect interfacial bonding and film retention under load after formation.

[0067] Referring to Table 8, overall, the comparisons of each group regarding basic formulation, source of self-made emulsion, type of polyether soft segment, and degree of polyvinyl alcohol hydrolysis maintained consistent conditions for paper base, gold foil, coating, foil application, pre-curing, and UV offset printing. The data from each group collectively presented multi-indicator relationships between semi-dry application time, intact gold foil area, peel strength, boundary displacement, and paper warpage, with some variables showing slightly different optimal points across different indicators. Therefore, the dual-type side groups of the functional hard shell respectively address the continuous phase constraint and gold foil interface maintenance; waterborne polyurethane and polyvinyl alcohol regulate the toughness and moisture release of the continuous phase; and the semi-dry criterion and pre-curing in the process allow the above materials to be gradually established before the offset printing load. These three factors form a technical path corresponding to the test results.

[0068] The above are merely preferred embodiments of this application and are not intended to limit the scope of protection of this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the scope of protection of this application.

Claims

1. A gold foil offset printed product, characterized in that, The material comprises, along its thickness direction, a paper substrate, a water-based gold leaf adhesive layer, a gold foil layer, and a UV offset printing image layer, which are sequentially stacked. The water-based gold leaf adhesive layer is formed by curing the water-based gold leaf adhesive, which includes a dispersion medium and the following components by mass of polymer solids: 95-105 parts of thiol self-crosslinking core-shell emulsion, 15-22 parts of aliphatic waterborne polyurethane, 10-15 parts of acrylic-modified rosin emulsion, and 2-3.5 parts of polyvinyl alcohol. The thiol self-crosslinking core-shell emulsion contains self-crosslinking core-shell particles, which have a functional hard shell. The functional hard shell has arylboronic acid side groups and terminal thiol side chains. The arylboronic acid side groups are formed by the ring-opening reaction of amino groups and epoxy groups in aminoarylboronic acid raw materials, and the terminal thiol side chains are obtained by the ring-opening reaction of epoxy groups and cysteine.

2. The gold foil offset printing product according to claim 1, characterized in that, The thiol self-crosslinking core-shell emulsion is prepared by a method comprising the following steps: (1) The acrylate soft core monomer was dispersed in an aqueous phase and emulsion polymerized to obtain a soft core seed emulsion; (2) Add a hard-shell monomer including glycidyl methacrylate, diacetone acrylamide and phosphate functional monomers to the soft-core seed emulsion and perform coating polymerization to obtain a core-shell emulsion with reserved epoxy groups. (3) Add boron-containing amine ring-opening raw material to the core-shell emulsion with reserved epoxy groups and stir to make the amino group of the boron-containing amine ring-opening raw material ring-open with a portion of the reserved epoxy groups; (4) After step (3), add cysteine ​​and stir to open the ring with another portion of the reserved epoxy group; (5) Add adipic acid dihydrazide to obtain the thiol self-crosslinked core-shell emulsion.

3. The gold foil offset printed product according to claim 2, characterized in that, The boron-containing amine ring-opening raw material is an aminoarylboronic acid raw material, which has both an amino group and a borate group on the same aryl skeleton, and the amino group can participate in the ring-opening reaction of the reserved epoxy group.

4. The gold foil offset printed product according to claim 3, characterized in that, The aminoarylboronic acid raw materials are selected from at least one of 2-aminophenylboronic acid, 3-aminophenylboronic acid, and 4-aminophenylboronic acid.

5. The gold foil offset printed product according to claim 2, characterized in that, In step (4) of the method for preparing the thiol self-crosslinking core-shell emulsion, the ring-opening temperature of cysteine ​​and the reserved epoxy group is 40-50°C.

6. The gold foil offset printing product according to claim 1, characterized in that, The aliphatic waterborne polyurethane is a polyether-type aliphatic waterborne polyurethane.

7. The gold foil offset printed product according to claim 6, characterized in that, The polyether-type aliphatic waterborne polyurethane is selected from at least one of polytetrahydrofuran ether diol-type aliphatic waterborne polyurethane, polypropylene glycol-type aliphatic waterborne polyurethane, and polyethylene glycol / polypropylene glycol copolyether-type aliphatic waterborne polyurethane.

8. The gold foil offset printed product according to claim 1, characterized in that, The degree of alcoholysis of the polyvinyl alcohol is 87.0 mol%-99.5 mol%.

9. The gold foil offset printed product according to claim 8, characterized in that, The degree of alcoholysis of the polyvinyl alcohol is 87.0 mol%-90.0 mol%.

10. A method for preparing gold foil offset printing according to any one of claims 1-9, characterized in that, Includes the following steps: (1) The prepared mercapto self-crosslinking core-shell emulsion was mixed with aliphatic waterborne polyurethane, acrylic modified rosin emulsion, polyvinyl alcohol, dispersion medium and coating additive to obtain waterborne gold leaf adhesive. (2) Clean and position the paper substrate, and apply the water-based gold leaf adhesive to the paper substrate; (3) Dry the coated water-based gold leaf adhesive until it is semi-dry and does not continuously transfer to the polyester film and continuously adheres to the gold foil under light pressure. Then apply the gold foil and pre-cur it. (4) Perform UV offset printing on the positioning area and then perform UV curing to obtain the gold foil offset print.