Method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous phase system

By employing a three-step synergistic method in an aqueous system, the efficient and green exfoliation of graphene was achieved through the synergistic effect of quaternary ammonium salt and polymer chains. This method solves the problems of low graphene exfoliation efficiency and easy product aggregation in existing technologies, while maintaining the intrinsic lattice structure of graphene.

CN123130786APending Publication Date: 2026-11-20CHONGQING INST OF GREEN & INTELLIGENT TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611310469.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve efficient and low-cost large-scale exfoliation without damaging the intrinsic lattice of graphene, and physical exfoliation methods suffer from low exfoliation efficiency and easy product agglomeration.

Method used

A three-step synergistic method in an aqueous system, namely "double quaternary ammonium salt high-pressure intercalation - polymer chain steric anchoring - hydrogen peroxide gentle gas exfoliation", is adopted to achieve efficient and green exfoliation of graphite and carbon black by utilizing the synergistic effect of tetramethylammonium hydroxide and tetraethylammonium hydroxide intercalating agents, polyacrylamide aqueous solution and hydrogen peroxide.

Benefits of technology

Efficient graphene exfoliation was achieved in the aqueous phase, preserving the intrinsic lattice structure of graphene, and the product exhibited ultra-long aqueous dispersion stability, solving the problems of low efficiency and easy product agglomeration in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123130786A_ABST
    Figure CN123130786A_ABST
Patent Text Reader

Abstract

The application discloses a method for preparing few-layer graphene by peeling graphite and carbon black in an aqueous phase system, and belongs to the technical field of carbon material preparation, which comprises the following steps: S1: two kinds of prepared quaternary ammonium salts and a carbon source to be peeled are added into water and uniformly mixed to obtain a first mixed solution, and intercalation and peeling are carried out on the first mixed solution under a closed high pressure and shearing condition to obtain a second mixed solution; step S2: polyacrylamide aqueous solution is added into the second mixed solution and stirred to obtain a third mixed solution; step S3: hydrogen peroxide is added into the third mixed solution, the third mixed solution is allowed to react with the hydrogen peroxide until the reaction is completed, and then the third mixed solution is allowed to stand and stratify, the supernatant is taken out and subjected to centrifugal treatment to obtain a graphene powder. The three-step synergistic method of "double quaternary ammonium salt high-pressure intercalation-polymer chain steric hindrance anchoring-mild hydrogen peroxide gas peeling" is adopted, and the efficient and green peeling of graphite and carbon black in the aqueous phase system is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbon material preparation technology, and particularly relates to a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system. Background Technology

[0002] Graphene, a two-dimensional carbon nanomaterial with a single atomic layer thickness, has attracted widespread attention in new energy storage, transparent conductive films, and high-end corrosion protection fields due to its excellent electron mobility, high thermal conductivity, and superior mechanical strength. However, achieving large-scale, low-cost, and green preparation of high-quality graphene remains a major bottleneck restricting its industrial application.

[0003] Traditional chemical oxidation-reduction methods use strong acids and strong oxidants (such as concentrated sulfuric acid and potassium permanganate) to violently penetrate the interlayer of graphite. Although the exfoliation yield is high, this process inevitably introduces a large number of oxygen-containing functional groups and lattice defects into the graphene substrate, which severely damages the intrinsic electrical and thermal conductivity of graphene. Furthermore, the subsequent washing process generates a large amount of acidic and harmful wastewater, causing extremely serious environmental pollution.

[0004] To maintain the integrity of the graphene lattice, existing physical exfoliation methods (such as conventional aqueous ultrasonic exfoliation and high-shear hydromechanical shearing) have been proposed. While these physical exfoliation methods can effectively preserve the intrinsic integrity of the lattice, they often face the following bottlenecks in practical operation: First, the van der Waals forces between graphite layers are too large, resulting in extremely low exfoliation efficiency and single-layer yield when relying solely on external mechanical force; second, the thickness of the exfoliated graphene sheets is uneven, making it impossible to precisely and effectively control the number of layers; third, the high specific surface area of ​​graphene easily leads to secondary recombination and macroscopic agglomeration in water or common solvents, greatly limiting its subsequent dispersion and assembly processing. Furthermore, with the popularization of new energy vehicles, the recycling of graphite from waste lithium-ion battery anodes has become an urgent environmental and resource issue. Therefore, developing a green and environmentally friendly liquid-phase exfoliation technology that does not damage the intrinsic lattice is a pressing issue in this field. Summary of the Invention

[0005] Based on the technical problems existing in the prior art, the present invention provides a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system.

[0006] According to the technical solution of the present invention, a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system is provided, comprising the following steps: Step S1: Add the two prepared quaternary ammonium salts and the carbon source to be stripped to water and mix them evenly to obtain a first mixture. Then, perform intercalation and stripping of the first mixture under closed high pressure and shear conditions to obtain a second mixture. Step S2: Add an aqueous solution of polyacrylamide to the second mixture and stir to obtain a third mixture; Step S3: Add hydrogen peroxide to the third mixture. After the hydrogen peroxide reacts with the third mixture, allow it to stand and separate into layers. Take the supernatant and centrifuge it to obtain graphene powder.

[0007] A further improvement of the present invention is that the two quaternary ammonium salts are tetramethylammonium hydroxide and tetraethylammonium hydroxide, respectively.

[0008] A further improvement of the present invention is that, in step S1, the mass of the carbon source to be stripped is 0.8g to 1.2g, the volume of the tetramethylammonium hydroxide is 160μL to 240μL, the volume of the tetramethylammonium hydroxide is 800μL to 1200μL, and the volume of the water is 40mL to 60mL.

[0009] A further improvement of the present invention is that, in step S1, during the process of intercalation and exfoliation of the mixture under closed high pressure and shear conditions to obtain the second mixture, the reaction temperature is maintained at 120°C to 150°C and the reaction time is 3500 min to 4200 min.

[0010] A further improvement of the present invention is that: in step S1, the closed high pressure and shear conditions are achieved by adding the first mixture into the reaction vessel, the pressure inside the reaction vessel being 0.2MPa~0.35MPa, and the first mixture being continuously mechanically stirred inside the reaction vessel at a speed of 1000r / min~1500r / min.

[0011] A further improvement of the present invention is that, in step S2, a polyacrylamide aqueous solution with a mass fraction of 1% to 5% is added to the second mixture.

[0012] A further improvement of the present invention is that, in step S2, the polyacrylamide aqueous solution is obtained by dissolving polyacrylamide in deionized water and stirring for 60-80 hours.

[0013] A further improvement of the present invention is that, in step S3, the hydrogen peroxide and the third mixture are continuously stirred during the reaction process, and the stirring time is 60h~80h.

[0014] A further improvement of the present invention is that, in step S3, the volume of hydrogen peroxide is 15 mL to 25 mL.

[0015] A further improvement of the present invention is that, in step S3, the settling time is 2 to 3 days.

[0016] Compared with the prior art, the above-mentioned technical solution of the present invention has the following beneficial technical effects: 1. This invention achieves efficient and green exfoliation of graphite and carbon black in an aqueous system through a three-step synergistic method: "double quaternary ammonium salt high-pressure intercalation - polymer chain steric hindrance anchoring - gentle hydrogen peroxide and gas exfoliation". This method completely eliminates strong acids and strong oxidants, fully preserving the intrinsic crystal structure of graphene, while endowing the product with ultra-high aqueous dispersion stability of more than 25 to 35 hours, solving the dual bottlenecks of low exfoliation efficiency and easy product agglomeration in traditional physical methods and severe crystal lattice damage in chemical methods.

[0017] 2. This invention utilizes two quaternary ammonium salts of different sizes, tetramethylammonium hydroxide and tetraethylammonium hydroxide, as intercalating agents. It leverages the synergistic effect of smaller cations preferentially penetrating into tightly packed interlayer spaces, followed by larger cations that open up the interlayer gaps, thus achieving highly efficient intercalation of graphite layers. This solves the problem that a single intercalating agent, due to its fixed size, cannot adapt to interlayer defects of different initial scales, thus limiting intercalation efficiency. It also significantly weakens the van der Waals forces between carbon layers.

[0018] 3. This invention precisely limits the ratio of carbon source to two quaternary ammonium salts, ensuring that the concentrations of quaternary ammonium salt cations of varying sizes in the system are within the optimal window for synergistic intercalation. This ratio ensures sufficient contact between the two intercalating agents and the carbon source, achieving efficient and uniform interlayer insertion without wasting reagents. Simultaneously, an appropriate amount of water maintains suitable system fluidity, allowing subsequent high-pressure shearing to stably act on the carbon source particles, thus solving the problem of uneven intercalation caused by improper ratios.

[0019] 4. This invention significantly enhances the permeation activity and diffusion rate of quaternary ammonium salt cations by controlling the temperature at 120℃~150℃ and maintaining a reaction time of 3500min~4200min during the intercalation process. The high temperature combined with the self-generated pressure inside the reactor continuously forces the intercalated ions into the deep region, ensuring sufficient pre-expansion of the graphite particles over an extended period. This solves the problem of conventional methods where intercalation only occurs on the particle surface due to insufficient time, laying the foundation for subsequent exfoliation.

[0020] 5. This invention achieves highly efficient synergy between chemical intercalation and physical shearing by creating a pressure of 0.2MPa~0.35MPa within the reactor and coordinating with high-speed stirring at 1000r / min~1500r / min. The slightly positive pressure forces quaternary ammonium salt ions into the interlayer space, while the high shear force induces interlayer slippage and exfoliation. This synergy significantly improves the primary exfoliation efficiency, solving the problem of low efficiency when relying solely on chemical intercalation or mechanical shearing. Furthermore, the entire process is conducted in a closed aqueous environment, ensuring safety and environmental friendliness.

[0021] 6. This invention utilizes a 1%–5% (w / w) aqueous solution of polyacrylamide to induce in-situ adsorption of long-chain polymers on the freshly exfoliated graphene surface, forming a dense steric hindrance protective layer. This concentration effectively prevents secondary agglomeration of the graphene sheets, ensuring uniform dispersion of the slurry during standing for more than 25 hours. Simultaneously, the expanded macromolecular chains can further penetrate into the loose interlayers to achieve secondary expansion, thus solving the core problem of the easy re-agglomeration and precipitation of products from physical exfoliation methods.

[0022] 7. This invention ensures that the polyacrylamide is fully swollen and expanded by pre-dissolving it and stirring it for 60-80 hours, thus eliminating undissolved micelles and entanglements. After this treatment, the expanded molecular chains can quickly and uniformly complete multi-point adsorption and anchoring when in contact with graphene, constructing a continuous spatial steric shielding network. This solves the problems of uneven surface coverage and unstable anti-agglomeration effect caused by insufficient polymer dissolution.

[0023] 8. This invention achieves uniform distribution and full contact with carbon materials by continuously stirring the hydrogen peroxide during the reaction stage for 60-80 hours. Continuous stirring allows the hydrogen peroxide to slowly release oxygen bubbles and gently etch the edges of thick layers. Oxygen nucleates and expands between the expanding layers, pushing the graphite sheets apart layer by layer. This solves the problem of severe lattice damage to the graphene basal plane caused by the violent reaction of traditional strong oxidants, achieving a gentle and controllable exfoliation process while preserving the intrinsic structure of graphene.

[0024] 9. This invention achieves precise control over the oxidation etching intensity and oxygen generation rate by precisely controlling the amount of hydrogen peroxide used to 15mL~25mL. This dosage only provides limited weak oxidation modification to the edges of thick layers, generating sufficient interlayer force while simultaneously generating enough oxygen to complete pneumatic stripping. This solves the dilemma of insufficient stripping due to insufficient oxidant dosage and lattice damage due to excessive dosage, achieving the optimal balance between yield and quality.

[0025] 10. This invention allows for natural sedimentation and classification after the reaction, with the remaining thick layers and aggregates allowed to settle naturally, while the highly dispersed few-layer graphene remains stably suspended. High-purity powder can be obtained by centrifuging the supernatant, thus solving the problem of mechanical damage and breakage of graphene sheets that may occur during direct separation by high-speed centrifugation, and maximizing the preservation of the integrity of the few-layer graphene sheets and the quality of the product. Attached Figure Description

[0026] The accompanying drawings are provided to better understand the invention and are not intended to unduly limit the scope of the invention. Wherein: Figure 1 This is a flowchart of a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to the present invention. Figure 2This is a schematic diagram of the structure of the graphite powder raw material and the prepared graphene under a scanning electron microscope in Embodiment 2 of the present invention; Figure 3 Transmission electron microscope images of graphite powder raw materials and graphene; Figure 4 This is an atomic force microscope image of the graphene prepared in Example 2. Detailed Implementation

[0027] The following description, in conjunction with the accompanying drawings, illustrates exemplary embodiments of the present invention, including various details to aid understanding. These details should be considered merely exemplary. Therefore, those skilled in the art will recognize that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the invention. Similarly, for clarity and brevity, descriptions of well-known functions and structures are omitted in the following description.

[0028] This invention discloses a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system, belonging to the field of carbon material preparation technology. The method includes the following steps: S1: Two prepared quaternary ammonium salts and the carbon source to be exfoliated are added to water and mixed evenly to obtain a first mixture. The first mixture is subjected to intercalation and exfoliation under closed high pressure and shear conditions to obtain a second mixture; S2: An aqueous solution of polyacrylamide is added to the second mixture and stirred to obtain a third mixture; S3: Hydrogen peroxide is added to the third mixture. After the hydrogen peroxide reacts with the third mixture, the mixture is allowed to stand and separate into layers. The supernatant is then centrifuged to obtain graphene powder. This invention achieves efficient and green exfoliation of graphite and carbon black in an aqueous system by employing a three-step synergistic method of "double quaternary ammonium salt high-pressure intercalation - polymer chain steric anchoring - gentle gas exfoliation with hydrogen peroxide". This method completely eliminates strong acids and strong oxidants, fully preserving the intrinsic lattice structure of graphene, while endowing the product with ultra-high aqueous phase dispersion stability for more than 25 to 35 hours, solving the dual bottlenecks of low exfoliation efficiency, easy product agglomeration, and severe lattice damage in traditional physical methods.

[0029] The following examples further illustrate the technical solution of the method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to the present invention.

[0030] Example 1 like Figure 1 As shown, this embodiment provides a method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system, which includes the following steps: Step S1: Add the two prepared quaternary ammonium salts and the carbon source to be stripped to water and mix them evenly to obtain a first mixture. Then, perform intercalation and stripping of the first mixture under closed high pressure and shear conditions to obtain a second mixture. Step S2: Add an aqueous solution of polyacrylamide to the second mixture and stir to obtain a third mixture; Step S3: Add hydrogen peroxide to the third mixture. After the hydrogen peroxide reacts with the third mixture, allow it to stand and separate into layers. Take the supernatant and centrifuge it to obtain graphene powder.

[0031] Specifically, in step S1, the two prepared quaternary ammonium salts and the carbon source to be stripped are added to water and mixed evenly to obtain a first mixture. The first mixture is then subjected to intercalation and stripping under closed high pressure and shear conditions to obtain a second mixture. This step utilizes the differences in molecular size and charge density between tetramethylammonium hydroxide and tetraethylammonium hydroxide, two quaternary ammonium salts. The smaller tetramethylammonium cation preferentially penetrates into the relatively tightly packed defect sites between graphite or carbon black layers to initially expand them, while the larger tetraethylammonium cation subsequently enters the slightly expanded interlayer gaps to further widen the interlayer spacing. The two form a complementary size synergistic intercalation effect, effectively weakening the van der Waals forces between carbon layers. Simultaneously, during the closed heating process in the reactor, the solvent vapor pressure creates a micro-positive pressure environment of 0.2~0.35MPa, forcibly pressing the intercalated ions into a deeper interlayer region. Combined with the strong fluid shear force generated by high-speed mechanical stirring at 1000~1500r / min and the collision friction between particles, mechanical energy is efficiently transferred to the graphite interlayers, initiating interlayer slip and exfoliation. The reaction is continued at a temperature of 120~150℃ for 3500~4200 minutes, allowing the graphite or carbon black particles to complete sufficient deep pre-expansion and initial exfoliation, laying a good foundation for subsequent macromolecular intervention and gas exfoliation. The carbon source to be stripped is graphite powder.

[0032] Specifically, in step S2, an aqueous solution of polyacrylamide is added to the second mixture and stirred to obtain a third mixture. This step introduces an aqueous solution of polyacrylamide with a mass fraction of 1% to 5%. Its long-chain polymers can be adsorbed and wrapped in situ onto the surface of the initially exfoliated graphene sheets, forming a dense steric hindrance protective layer. This effectively prevents secondary aggregation and recombination of the high surface energy graphene sheets, giving the product slurry ultra-long-term dispersion stability. Simultaneously, these extended macromolecular chains, as a mild macromolecular intercalating agent, can further penetrate into the graphite interlayers loosened by small-molecule quaternary ammonium salts to achieve secondary intercalation and expansion, further increasing the interlayer spacing of the carbon layers and creating more favorable conditions for final gas exfoliation. The polyacrylamide aqueous solution is pre-dissolved and stirred for 60 to 80 hours to ensure complete swelling and expansion of the macromolecules, eliminating undissolved micelles and entanglements. This allows it to rapidly and uniformly complete multi-point adsorption and entanglement anchoring when in contact with the second mixture, constructing a large-area three-dimensional steric hindrance shielding network.

[0033] Specifically, in step S3, hydrogen peroxide is added to the third mixture. After the hydrogen peroxide reacts with the third mixture, the mixture is allowed to stand and separate into layers. The supernatant is then centrifuged to obtain graphene powder. This step utilizes the dual effects of hydrogen peroxide to achieve final exfoliation and purification: on the one hand, hydrogen peroxide exerts a mild oxidative etching effect, selectively eroding the active sites at the edges of incompletely exfoliated thick graphite or carbon black aggregates, weakening the remaining interlayer bonding forces. Its oxidation degree is extremely low, thus preserving the intrinsic lattice structure of graphene intact. On the other hand, during continuous stirring for 60-80 hours, hydrogen peroxide slowly decomposes and releases tiny oxygen bubbles, which nucleate, aggregate, and continuously expand in the expanded interlayer spaces, pushing the graphite sheets apart layer by layer in a gas-assisted manner to obtain the lattice. Few-layer graphene with few defects and excellent electrical and thermal conductivity; after the reaction is completed, stirring is stopped and the mixture is left to stand for 2-3 days. The thick graphite, carbon black particles and a small amount of agglomerates that were not fully exfoliated slowly settle to the bottom under gravity, while the highly stable and dispersed few-layer graphene remains uniformly suspended in the supernatant due to the synergistic effect of steric hindrance and edge hydrophilic microgroups. The supernatant can be collected by centrifugation to obtain high-purity graphene powder. This natural sedimentation classification method can avoid mechanical damage to the graphene sheets caused by high centrifugal force and maintain the integrity of the few-layer graphene to the greatest extent.

[0034] Specifically, the two quaternary ammonium salts are tetramethylammonium hydroxide and tetraethylammonium hydroxide. This combination utilizes the differences in molecular size and charge density between the two organic quaternary ammonium salt cations. Tetramethylammonium, with its smaller volume, can preferentially penetrate into the relatively tightly packed defect sites between graphite or carbon black layers, while tetraethylammonium, with its larger volume, can subsequently expand the slightly expanded interlayer gaps. The two work synergistically to exert a complementary intercalation effect, effectively weakening the van der Waals forces between carbon layers, significantly reducing the exfoliation energy barrier, and providing sufficient chemical driving force for the primary expansion of graphite.

[0035] Specifically, in step S1, the mass of the carbon source to be stripped is 0.8g~1.2g, the volume of tetramethylammonium hydroxide is 160μL~240μL, the volume of tetramethylammonium hydroxide is 800μL~1200μL, and the volume of water is 40mL~60mL. Under the above dosage ratios, the concentrations of small and large quaternary ammonium salt cations reach the optimal window for synergistic intercalation, ensuring sufficient contact between the carbon source surface and interlayer in the aqueous medium, such as graphite, waste battery negative electrode graphite, or carbon black. This achieves efficient and uniform interlayer insertion without excessive reagent waste. Simultaneously, the amount of water maintains suitable system fluidity, allowing subsequent high-pressure shearing to function stably and ensuring the carbon source remains well dispersed throughout the process.

[0036] Specifically, in step S1, during the intercalation and exfoliation of the mixture under closed high pressure and shear conditions to obtain the second mixture, the reaction temperature is maintained at 120℃~150℃, and the reaction time is 3500min~4200min. This temperature range can significantly enhance the molecular thermal motion in the liquid environment, increase the penetration activity and diffusion rate of quaternary ammonium salt cations into the graphite interlayer, and form self-generated pressure in the closed reactor, forcing the intercalated ions into a deeper interlayer region. Combined with a continuous reaction lasting thousands of minutes, this allows the graphite or carbon black particles to undergo sufficient and deep pre-expansion and initial slip exfoliation, laying a good foundation for subsequent macromolecular intervention and gas exfoliation.

[0037] Specifically, in step S1, the closed high pressure and shear conditions are achieved by adding the first mixture to a reactor, where the pressure inside the reactor is 0.2 MPa to 0.35 MPa. The first mixture is continuously mechanically stirred within the reactor at a speed of 1000 r / min to 1500 r / min. During the sealed heating process, a micro-positive pressure environment of 0.2 to 0.35 MPa is naturally formed in the reactor due to solvent vapor pressure and gas release. This pressure helps to force quaternary ammonium salt ions into the interlayer. Simultaneously, the high-speed mechanical stirring generates strong fluid shear force and interparticle collision friction, efficiently transferring mechanical energy to the graphite interlayer and inducing interlayer slip exfoliation. The synergistic effect of high pressure and high shear greatly improves the efficiency of a single primary exfoliation, and the entire process is carried out in a closed aqueous environment, ensuring safety and environmental friendliness.

[0038] Specifically, in step S2, a 1% to 5% (w / w) aqueous solution of polyacrylamide is added to the second mixture. Upon introduction of this concentration of polyacrylamide aqueous solution, its long-chain polymers can be adsorbed and wrapped in situ onto the surface of the initially exfoliated graphene sheets, forming a dense steric hindrance protective layer. This effectively prevents secondary aggregation and recombination of the high surface energy graphene sheets. Simultaneously, these extended macromolecular chains can also act as a mild macromolecular intercalating agent, further penetrating into the graphite interlayers loosened by the small-molecule quaternary ammonium salt, achieving secondary intercalation expansion and further increasing the interlayer spacing of the carbon layers, creating more favorable conditions for the final gas exfoliation.

[0039] Specifically, in step S2, the polyacrylamide aqueous solution is obtained by dissolving polyacrylamide in deionized water and stirring for 60-80 hours. This long pre-dissolution and stirring process ensures that the polyacrylamide macromolecules fully swell and expand, eliminating undissolved micelles and entanglements, forming a uniform, clear polymer protective liquid with optimal molecular chain state. When this solution comes into contact with the second mixture, the expanded polyacrylamide chains can quickly and uniformly complete multi-point adsorption and entanglement anchoring on the graphene surface, thereby constructing a large-area three-dimensional steric hindrance shielding network and giving the graphene slurry ultra-long-term dispersion stability.

[0040] Specifically, in step S3, the hydrogen peroxide and the third mixture are continuously stirred during the reaction for 60-80 hours. Under gentle and continuous stirring conditions, hydrogen peroxide can slowly decompose and release tiny oxygen bubbles. At the same time, it exerts a gentle oxidative etching effect, selectively eroding the active sites at the edges of incompletely peeled thick graphite or carbon black aggregates, weakening the remaining interlayer bonding forces. The slowly released oxygen nucleates, accumulates, and continuously expands in the expanded interlayer, pushing the graphite sheets apart layer by layer in a gas-assisted manner. The oxidation degree of the entire process is extremely low, which can completely preserve the intrinsic sp² lattice structure of graphene, ultimately obtaining few-layer graphene with few lattice defects and excellent electrical and thermal conductivity.

[0041] Specifically, in step S3, the volume of hydrogen peroxide is 15 mL to 25 mL. This dosage allows for precise control of the overall intensity of oxidative etching and the rate of oxygen generation in the system. This ensures that the hydrogen peroxide only performs limited weak oxidative modification on the edges of thick layers that are difficult to peel off, without excessively attacking the already peeled graphene substrate or causing lattice damage. At the same time, the amount of oxygen generated is sufficient to effectively perform layer-by-layer aerodynamic peeling of the expanded carbon layer. This achieves a balance between high peeling yield and excellent product quality without introducing strong acids or strong oxidants.

[0042] Specifically, in step S3, the settling time is 2 to 3 days. After the mixing system stops stirring, it is allowed to settle naturally for 2 to 3 days. The thick graphite layers, large carbon black particles, and a small amount of agglomerates that have not been fully exfoliated will slowly settle to the bottom under gravity. Meanwhile, the highly stable and dispersed few-layer graphene remains uniformly suspended in the supernatant, appearing as a black ink, due to the synergistic effect of the steric hindrance between the layers and the hydrophilic microgroups at the edges. Subsequently, only the supernatant needs to be aspirated and centrifuged to collect high-purity graphene powder. This classification method based on natural sedimentation can avoid mechanical damage to the graphene sheets caused by high centrifugal force and maintain the integrity of the few-layer graphene to the greatest extent.

[0043] Example 2 This embodiment provides a specific step-by-step method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system, including the following steps: Step W1: Accurately measure 0.8–1.2 g of graphite powder, 160–240 μL of tetramethylammonium hydroxide, 800–1200 μL of tetraethylammonium hydroxide, and 40–60 mL of water and mix them thoroughly in the high-pressure reactor. Transfer the mixture to the high-pressure reactor and seal it. Start the stirring program, maintaining the reaction temperature inside the reactor at a constant 120–150°C, and controlling the internal mechanical stirring shaft at a high speed of 1100–1300 rpm. Under these conditions of high temperature, high pressure, and high-speed flow shear, continue the reaction for 3900–4200 minutes. After the reaction is complete, turn off the heating system and allow the reactor to cool completely to room temperature before depressurizing. Transfer the primary exfoliated black mixed sample from the reactor intact to a receiving beaker.

[0044] Step W2: In-situ adsorption and anchoring of long-chain polymers, anti-agglomeration, and macromolecular intercalation. Separately, weigh 1.5–2.5 g of polyacrylamide and dissolve it thoroughly in 150–250 mL of deionized water to prepare a completely clear polymer protective solution. Then, pour the prepared polyacrylamide aqueous solution entirely into the graphite sample that underwent primary expansion in Step W1. Turn on a standard laboratory mechanical stirrer and maintain a steady medium-speed stirring for 70–80 hours at room temperature and atmospheric pressure. During this process, the long carbon chains of polyacrylamide, through van der Waals forces and hydrophobic interactions, densely network and spread on the surface of the primary graphene, forming a long-term stable molecular steric hindrance.

[0045] Step W3: Mild oxidative etching with hydrogen peroxide and gas-assisted exfoliation. Slowly add 15-30 mL of hydrogen peroxide solution dropwise to the continuously stirred stabilization system from Step W2. Keep the mechanical stirrer running and continue the mild reaction at room temperature for 70-80 hours. This step utilizes the weak oxidative etching effect of hydrogen peroxide to chemically erode the edges of any remaining micron-sized, incompletely exfoliated graphite flakes in the slurry, and the oxygen released from the slow decomposition of hydrogen peroxide drives further loosening and exfoliation between layers, introducing hydrophilic microfunctional groups at the graphene edges. After the reaction is complete, stop the mechanical stirrer, allow the mixture to stand for 2-3 days for fractionation, and then centrifuge and dry the supernatant to obtain graphene.

[0046] Specifically, such as Figure 2 The diagram shows the structural schematics of the graphite powder raw material in step W1 and the graphene prepared in step W3 under a scanning electron microscope. After the reaction, the graphite layer on the surface of the raw material is peeled off layer by layer to obtain graphene. Figure 3 The image shown is a transmission electron microscope (TEM) image of graphite powder raw material and graphene. Compared to the very thick longitudinal dimension of the raw material, the graphene sheets obtained after exfoliation show a thinner longitudinal dimension. Figure 4 As shown in the figure, the graphene prepared in this embodiment has an atomic force microscope data image. The thickness of the graphene obtained by exfoliation is about 4.401 nm, which is about 6 to 7 layers of few-layer graphene.

[0047] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the above-described division of functional units and modules is merely an example. In practical applications, the above functions can be assigned to different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit. Furthermore, the specific names of the functional units and modules are only for easy differentiation and are not intended to limit the scope of protection of this application. The specific working process of the units and modules in the above system can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here.

[0048] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can occur depending on design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system, characterized in that, Includes the following steps: Step S1: Add the two prepared quaternary ammonium salts and the carbon source to be stripped to water and mix them evenly to obtain a first mixture. Then, perform intercalation and stripping of the first mixture under closed high pressure and shear conditions to obtain a second mixture. Step S2: Add an aqueous solution of polyacrylamide to the second mixture and stir to obtain a third mixture; Step S3: Add hydrogen peroxide to the third mixture. After the hydrogen peroxide reacts with the third mixture, allow it to stand and separate into layers. Take the supernatant and centrifuge it to obtain graphene powder.

2. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, The two quaternary ammonium salts are tetramethylammonium hydroxide and tetraethylammonium hydroxide, respectively.

3. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 2, characterized in that, In step S1, the mass of the carbon source to be stripped is 0.8g~1.2g, the volume of the tetramethylammonium hydroxide is 160μL~240μL, the volume of the tetramethylammonium hydroxide is 800μL~1200μL, and the volume of the water is 40mL~60mL.

4. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S1, during the process of intercalation and exfoliation of the mixture under closed high pressure and shear conditions to obtain the second mixture, the reaction temperature is maintained at 120℃~150℃ and the reaction time is 3500min~4200min.

5. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S1, the closed high pressure and shear conditions are achieved by adding the first mixture into a reaction vessel, the pressure inside the reaction vessel being 0.2 MPa to 0.35 MPa, and the first mixture being continuously mechanically stirred inside the reaction vessel at a speed of 1000 r / min to 1500 r / min.

6. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S2, a polyacrylamide aqueous solution with a mass fraction of 1% to 5% is added to the second mixture.

7. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S2, the polyacrylamide aqueous solution is obtained by dissolving polyacrylamide in deionized water and stirring for 60-80 hours.

8. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S3, the hydrogen peroxide and the third mixture are continuously stirred during the reaction process for 60-80 hours.

9. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S3, the volume of hydrogen peroxide is 15 mL to 25 mL.

10. The method for preparing few-layer graphene by exfoliating graphite and carbon black in an aqueous system according to claim 1, characterized in that, In step S3, the settling time is 2 to 3 days.