Method for preparing negative electrode composite for zinc ion battery

By forming interconnected internal mesopores and external micropores in the zinc-ion battery anode material and enhancing interfacial bonding through CO-Zn covalent bonds, the problems of zinc dendrite formation and coating peeling in zinc-based anodes were solved, thus achieving a high-efficiency performance improvement in zinc-ion batteries.

CN123130833APending Publication Date: 2026-11-20FUJIAN XFH NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611412432.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing zinc-based anodes are prone to zinc dendrite formation, causing battery short circuits, low cycle life, and the coating cannot achieve hierarchical control of internal channels. The coating will fall off and fail after long cycles, resulting in low coulombic efficiency.

Method used

Zn(NO₃)₂, 2-methylimidazole and etching aids are mixed in a planetary dry ball mill, and then subjected to gradient heating in an inert atmosphere to form interconnected channels of internal mesopores and external micropores. The interfacial bonding is enhanced by CO-Zn covalent bonds, which avoids zinc dendrites and pulverization of active materials.

Benefits of technology

It effectively suppresses zinc dendrites, improves coulombic efficiency and cycle life, simplifies processes, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a method for preparing a negative electrode composite material for zinc-ion batteries, comprising the following steps: ball milling and mixing of raw materials, gradient heating carbonization, and post-treatment purification. Through the thermal decomposition of an etching aid to generate a gaseous state, the gaseous medium can penetrate into the interior of the ZIF crystal and be etched from the inside out in a gradient manner, forming continuous interconnected channels of inner mesopores and outer micropores; the outer micropores sieve molecule separation, and the inner mesopores shorten the diffusion path, synergistically suppressing zinc dendrites; furthermore, during the pyrolysis process, Zn²⁺… + The oxidation process generates nano-ZnO, which simultaneously forms C-O-Zn covalent bonds with the oxygen-containing active sites on the inner wall of the carbon cage. This process is not merely a physical encapsulation, but significantly enhances the interfacial bonding strength. As a result, the particles do not detach or pulverize during the volume expansion of charging and discharging. The gradient pores enable rapid ion sieving and mass transfer, while the covalent interface enhances the particle binding force. This dual synergistic effect inhibits the pulverization of zinc dendrites and active materials, suppresses side reactions, and significantly reduces the probability of direct contact between electrolyte moisture and active materials, thereby improving coulombic efficiency and cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of negative electrode materials, and in particular to a method for preparing a negative electrode composite material for zinc-ion batteries. Background Technology

[0002] Aqueous zinc-ion batteries possess advantages such as high safety, low cost, no explosion risk, abundant zinc resources, and environmental friendliness, making them a mainstream new energy storage system for wind and solar energy storage, low-speed electric vehicles, and backup power. Currently, commercial / laboratory zinc-based anodes are mainly divided into three categories: metallic zinc foil anodes, pure zinc oxide anodes, and ordinary MOF-derived carbon-zinc composite anodes.

[0003] All of the above-mentioned negative electrodes exhibit significant defects. Pure zinc metal negative electrodes show severe dendrite formation and hydrogen evolution, while the zinc foil surface lacks ion sieving channels. 2+ Randomly deposited sharp zinc dendrites easily pierce the separator, causing a battery short circuit. In aqueous electrolytes, hydrated zinc ions carrying coordinated water continuously contact metallic zinc, triggering the HER (hydrogen evolution reaction), leading to continuous electrolyte consumption, battery bulging, and a cycle life generally below 300 hours. Furthermore, existing MOF coatings only physically cover the zinc foil surface, failing to achieve hierarchical control of internal pores, resulting in coating detachment and failure during long cycles. Pure ZnO anodes exhibit extremely poor conductivity, are prone to structural collapse, have high electronic conduction resistance, and poor rate performance. During charge and discharge, the deintercalation and intercalation of zinc in ZnO... The volume expansion is as high as 40%, the particles are easily pulverized and detached, and the capacity retention rate after 500 cycles at 0.2 A / g is less than 65%, which cannot meet the requirements of long-term energy storage. In addition, conventional ZIF-8 derived carbon has no hierarchical pores and slow ion transport; the existing ZIF-8 direct high-temperature carbonization only generates a single microporous structure with narrow channels and high resistance to desolvation of hydrated zinc ions; there is no in-situ etching to regulate the mesoporous channels, the ion diffusion path is long, and polarization is severe at high current densities; moreover, ZnO particles have no spatial confinement, and they agglomerate and grow during pyrolysis, significantly reducing the number of active sites. Therefore, it is necessary to propose a new solution to address the above problems. Summary of the Invention

[0004] In view of this, the present invention addresses the deficiencies of the existing technology, and its main objective is to provide a method for preparing a negative electrode composite material for zinc-ion batteries. This method can effectively solve the problems of existing zinc-based negative electrodes, such as easy formation of zinc dendrites, easy short circuits in batteries, low cycle life, coatings that only physically cover the surface of zinc foil and cannot achieve hierarchical control of internal channels, coating peeling and failure during long cycles, and low coulombic efficiency.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a negative electrode composite material for zinc-ion batteries includes the following steps: (1) Zn(NO3)26H2O, 2-methylimidazole and etching aid are put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O and 2-methylimidazole is 1:(3.8-4.2). The mass of the etching aid is 2.0-3.5wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling is carried out at room temperature at a speed of 300r / min for 3.5h and a ball-to-material ratio of 7:1 to obtain precursor powder. (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air, the flow rate of the inert gas is 70 mL / min, heat it to 240-280℃ at a heating rate of 2-3℃ / min, hold it for 90 min, then heat it to 480℃ at a heating rate of 2-3℃ / min, hold it for 60 min, then heat it to 650℃ at a heating rate of 2-3℃ / min, hold it for 120 min, and after cooling, obtain the coarse material; (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0006] As a preferred embodiment, the etching aid is ammonium oxalate.

[0007] As a preferred embodiment, the inert gas is nitrogen.

[0008] As a preferred embodiment, the grinding ball is made of zirconium oxide.

[0009] As a preferred embodiment, the size ratio of the grinding balls is 1:2.

[0010] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, as can be seen from the above technical solution: The etching aid decomposes upon heating to generate a gaseous state. This gaseous medium can penetrate into the ZIF crystal and be etched from the inside out in a gradient manner, forming continuous interconnected channels of internal mesopores and external micropores. The outer micropores sieve molecule separation, while the inner mesopores shorten the diffusion path, synergistically suppressing zinc dendrites. Furthermore, during pyrolysis, Zn²⁺… +The oxidation process generates nano-ZnO, which simultaneously forms CO-Zn covalent bonds with oxygen-containing active sites on the inner wall of the carbon cage. This is not simply a physical encapsulation, but rather a significant improvement in interfacial bonding strength. As a result, the particles do not detach or pulverize during the volume expansion of charging and discharging. The gradient pores enable rapid ion sieving and mass transfer, while the covalent interface enhances the particle binding force. This dual synergistic effect inhibits the pulverization of zinc dendrites and active materials, suppresses side reactions, and significantly reduces the probability of direct contact between electrolyte moisture and active materials, thereby improving coulombic efficiency and cycle life. Furthermore, the entire process is solvent-free, with etching, carbonization, and bonding formation completed in a single heating cycle within the same tube furnace. There is no water washing or organic waste liquid, simplifying the process and significantly reducing costs.

[0011] To more clearly illustrate the structural features and effects of the present invention, the present invention will be described in detail below with reference to specific embodiments. Detailed Implementation

[0012] This invention discloses a method for preparing a negative electrode composite material for zinc-ion batteries, which includes the following steps: (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid are put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O and 2-methylimidazole is 1:(3.8-4.2). The mass of the etching aid is 2.0-3.5wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. This effectively avoids damage to the carbon cage skeleton due to insufficient etching or excessive corrosion. Dry ball milling is carried out at room temperature at a speed of 300r / min for 3.5h. The ball-to-material ratio is 7:1 to obtain precursor powder. The etching aid is ammonium oxalate, the grinding balls are made of zirconium oxide, and the size ratio of the grinding balls is 1:2.

[0013] (2) Spread the precursor powder obtained in step (1) evenly on a corundum boat, introduce an inert gas to isolate it from air, the flow rate of the inert gas is 70 mL / min, heat to 240-280℃ at a heating rate of 2-3℃ / min, hold for 90 min, ammonium oxalate completely decomposes to generate gaseous oxalic acid, which penetrates and corrodes the interior of the ZIF crystal, pre-constructing mesoporous cavities, then heat to 480℃ at a heating rate of 2-3℃ / min, hold for 60 min, 2-methylimidazolium carbonizes to form a carbon cage framework, Zn² + Simultaneous oxidation generates ZnO, and the oxygen-containing sites on the carbon wall form CO-Zn covalent bonds with the ZnO surface. Then, the temperature is increased to 650℃ at a heating rate of 2-3℃ / min and held for 120min. The carbon skeleton is slightly graphitized, and the internal and external channels are completely connected, improving the overall conductivity. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0014] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0015] The following detailed description is based on multiple embodiments.

[0016] Example 1 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:4. The mass of the etching aid was 3.0 wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300 r / min for 3.5 h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0017] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the gas to 260°C at a heating rate of 2.5°C / min and hold for 90 min. Then heat the gas to 480°C at a heating rate of 2.5°C / min and hold for 60 min. Then heat the gas to 650°C at a heating rate of 2.5°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0018] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0019] Example 2 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:3.8. The mass of the etching aid was 2.2wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300 r / min for 3.5 h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0020] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the gas to 270°C at a heating rate of 2°C / min and hold for 90 min. Then heat the gas to 480°C at a heating rate of 3°C / min and hold for 60 min. Then heat the gas to 650°C at a heating rate of 2°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0021] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0022] Example 3 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:4.1. The mass of the etching aid was 3.0 wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300 r / min for 3.5 h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0023] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the gas to 255°C at a heating rate of 3°C / min and hold for 90 min. Then heat the gas to 480°C at a heating rate of 2°C / min and hold for 60 min. Finally, heat the gas to 650°C at a heating rate of 3°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0024] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0025] Example 4 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:4.2. The mass of the etching aid was 2.0 wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300 r / min for 3.5 h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0026] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the material to 240°C at a heating rate of 2.5°C / min and hold for 90 min. Then heat the material to 480°C at a heating rate of 3°C / min and hold for 60 min. Finally, heat the material to 650°C at a heating rate of 3°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0027] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0028] Example 5 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:4.1. The mass of the etching aid was 2.8wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300 r / min for 3.5 h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0029] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the gas to 280°C at a heating rate of 2.5°C / min and hold for 90 min. Then heat the gas to 480°C at a heating rate of 2.5°C / min and hold for 60 min. Then heat the gas to 650°C at a heating rate of 2.5°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0030] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0031] Example 6 (1) Zn(NO3)26H2O, 2-methylimidazole, and etching aid were put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O to 2-methylimidazole was 1:4. The mass of the etching aid was 3.5wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling was carried out at room temperature at a speed of 300r / min for 3.5h. The ball-to-material ratio was 7:1 to obtain precursor powder. The etching aid was ammonium oxalate, the grinding balls were made of zirconium oxide, and the size ratio of the grinding balls was 1:2.

[0032] (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air. The flow rate of the inert gas is 70 mL / min. Heat the gas to 270°C at a heating rate of 3°C / min and hold for 90 min. Then heat the gas to 480°C at a heating rate of 3°C / min and hold for 60 min. Then heat the gas to 650°C at a heating rate of 3°C / min and hold for 120 min. After cooling, the coarse material is obtained. The inert gas is nitrogen.

[0033] (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

[0034] Performance tests were conducted on the above-mentioned multiple sets of embodiments. Among them, the electrochemical performance test was conducted using the standard test at 25°C, the voltage range of the symmetrical cell was ±0.5V, and the voltage window of the full cell was 0.2~1.8V. The test results are shown in Table 1 and Table 2.

[0035]

[0036] Table 1

[0037] Table 2 The performance test results of the above-mentioned multiple embodiments are shown in Tables 1 and 2. Among them, Example 1 has the best overall performance, with the best pore structure, a mesopore ratio of 62%, a total pore volume of 0.58 cm³ / g, and a specific surface area of ​​280 m² / g. At the same time, it has the highest ZnO loading and carbon cage nitrogen doping, which greatly improves the zinc ion intercalation and deintercalation ability. Moreover, the CO-Zn interface bonding strength is as high as 86 MPa, which makes its modified layer less prone to falling off and extends its service life. This can be clearly seen in the electrochemical performance. The symmetric cells assembled in Examples 1-6 can all be stably cycled for 1200h under a current density of 1 mA / cm², and there is no short circuit or zinc dendrite formation during the cycling process. The initial discharge specific capacity at a low current of 0.1 A / g can reach 330 mAh / g, the high rate capacity at 1 A / g is 276 mAh / g, and the capacity retention rate after 1500 cycles of the full cell is 93% under the condition of 0.5 A / g.

[0038] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the technical scope of the present invention. Therefore, any minor modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a negative electrode composite material for zinc-ion batteries, characterized in that: It includes the following steps: (1) Zn(NO3)26H2O, 2-methylimidazole and etching aid are put into a planetary dry ball mill. The molar ratio of Zn(NO3)26H2O and 2-methylimidazole is 1:(3.8-4.2). The mass of the etching aid is 2.0-3.5wt% of the total mass of Zn(NO3)26H2O and 2-methylimidazole. Dry ball milling is carried out at room temperature at a speed of 300r / min for 3.5h and a ball-to-material ratio of 7:1 to obtain precursor powder. (2) Spread the precursor powder obtained in step (1) on a corundum boat, introduce an inert gas to isolate it from the air, the flow rate of the inert gas is 70 mL / min, heat it to 240-280℃ at a heating rate of 2-3℃ / min, hold it for 90 min, then heat it to 480℃ at a heating rate of 2-3℃ / min, hold it for 60 min, then heat it to 650℃ at a heating rate of 2-3℃ / min, hold it for 120 min, and after cooling, obtain the coarse material; (3) Pass the coarse material obtained in step (2) through a 300-mesh sieve and use a weak airflow to remove trace amounts of free carbon impurities. The negative electrode composite material for zinc-ion batteries can be obtained without washing.

2. The method for preparing the negative electrode composite material for zinc-ion batteries according to claim 1, characterized in that: The etching aid is ammonium oxalate.

3. The method for preparing the negative electrode composite material for zinc-ion batteries according to claim 1, characterized in that: The inert gas is nitrogen.

4. The method for preparing the negative electrode composite material for zinc-ion batteries according to claim 1, characterized in that: The grinding balls are made of zirconium oxide.

5. The method for preparing the negative electrode composite material for zinc-ion batteries according to claim 1, characterized in that: The size ratio of the grinding balls is 1:2.