Application of confined lanthanum modified carbon nanotube anode material in selective electrochemical degradation of wastewater containing organophosphorus
By using confined lanthanum-modified carbon nanotube anode materials, the interfacial adsorption and CP bond activation of glyphosate are enhanced, solving the problems of AMPA generation and phosphorus conversion in glyphosate degradation, and achieving efficient and environmentally friendly glyphosate wastewater treatment.
Patent Information
- Application Number
- CN202611569878.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-20
AI Technical Summary
Existing electrochemical oxidation technologies are insufficient to effectively inhibit the formation of AMPA during the degradation of glyphosate, and it is also difficult to convert the phosphorus in glyphosate into inorganic phosphates, posing a risk of secondary pollution.
By regulating the spatial distribution of lanthanum species within the channels of carbon nanotubes, confined lanthanum-modified carbon nanotube anode materials were prepared, enhancing the interfacial adsorption and CP bond activation capabilities of glyphosate and promoting the selective degradation of glyphosate and the release of inorganic phosphates.
It achieves efficient removal of glyphosate, inhibits AMPA formation, reduces the ecotoxicity of the treatment solution, and improves the conversion efficiency of phosphorus. The material has good stability and reduces the risk of lanthanum leaching.
Smart Images

Figure CN123130902A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of environmental functional materials and wastewater electrochemical treatment technology, and in particular to the application of a confined lanthanum-modified carbon nanotube anode material in the selective electrochemical degradation of glyphosate-containing wastewater. Specifically, it relates to a confined lanthanum-modified carbon nanotube anode material and its preparation method, as well as the application of this anode material in the selective electrochemical degradation of glyphosate-containing wastewater, inhibition of AMPA formation, and conversion of phosphorus-containing pollutants. Background Technology
[0002] Glyphosate is a widely used organophosphorus herbicide, used in large quantities in agricultural production, landscaping, and municipal environmental management. Due to its environmental persistence, glyphosate and its degradation products can enter surface water, groundwater, municipal sewage, and reclaimed water systems, posing potential risks to ecosystems and human health.
[0003] Existing methods for treating glyphosate include physical adsorption, biodegradation, chemical oxidation, and electrochemical oxidation. Among these, physical adsorption suffers from issues of pollutant transfer and adsorbent regeneration; biodegradation has a long reaction cycle and is greatly affected by environmental conditions; chemical oxidation usually requires the addition of an external oxidant, which may lead to secondary pollution; and while conventional electrochemical oxidation has advantages such as simple operation and controllable reaction, it lacks the ability to selectively recognize and activate specific chemical bonds in glyphosate molecules.
[0004] The degradation of glyphosate typically involves two main pathways: CN bond breaking and CP bond breaking. CN bond breaking often generates aminomethylphosphonic acid (AMPA), which is highly toxic and persistent. Existing electrochemical anode materials are ineffective in inhibiting AMPA formation and promoting the conversion of phosphorus in glyphosate to inorganic phosphates. Therefore, there is an urgent need to develop an electrochemical anode material that can achieve targeted degradation of glyphosate, inhibit AMPA formation, and reduce the ecotoxicity of the treatment solution. Summary of the Invention
[0005] To address the above technical problems, this invention provides an application of confined lanthanum-modified carbon nanotube anode material in the selective electrochemical degradation of glyphosate-containing wastewater. This invention enhances the glyphosate interfacial adsorption and CP bond activation capabilities by regulating the spatial distribution of lanthanum species within the internal channels of carbon nanotubes, thereby achieving efficient glyphosate removal, AMPA formation inhibition, and inorganic phosphate release.
[0006] The present invention aims to provide an application of confined lanthanum-modified carbon nanotube anode material in the selective electrochemical degradation of organophosphorus wastewater. The confined lanthanum-modified carbon nanotube anode material comprises a conductive substrate, confined lanthanum-modified carbon nanotubes loaded on the surface of the conductive substrate, and a binder. The confined lanthanum-modified carbon nanotubes are carbon nanotubes with open ports and internal channels as carriers, and the internal channels of the carrier are loaded with lanthanum active species. The lanthanum active species include La(OH)3.
[0007] In some embodiments of the present invention, the confined lanthanum-modified carbon nanotube anode material is prepared by the following method; Raw carbon nanotubes were placed in a strong oxidizing acid solution, dispersed by ultrasound, and heated under reflux to obtain carbon nanotubes with open ports and internal channels. The lanthanum salt precursor was dissolved in a solvent, and the carbon nanotubes obtained above were added. After ultrasonic and stirring treatment, the lanthanum salt precursor entered the internal channels of the carbon nanotubes to obtain a mixed system. An alkaline solution was added to the resulting mixture to cause lanthanum species to hydrolyze and precipitate in situ and be confined and deposited in the internal channels of carbon nanotubes, thus obtaining a confined lanthanum-modified carbon nanotube composite material. The confined lanthanum-modified carbon nanotube composite material was mixed with a binder in an organic solvent to prepare an electrode slurry. The electrode slurry was then coated onto the surface of a conductive substrate and dried to obtain a confined lanthanum-modified carbon nanotube anode material.
[0008] In some embodiments of the present invention, the concentration of the strong oxidizing acid solution is 60-70 wt%; the strong oxidizing acid in the strong oxidizing acid solution is selected from one or more of nitric acid, concentrated sulfuric acid and hydrogen peroxide; The heating reflux temperature is 400-420K, and the reflux time is 10-18h; It also includes low-temperature freezing and freeze-drying; the low-temperature freezing time is 10-60 min, and the freeze-drying time is 24-72 h.
[0009] In some embodiments of the present invention, the lanthanum salt precursor is selected from one or more of lanthanum nitrate, lanthanum chloride, and lanthanum acetate.
[0010] In some embodiments of the present invention, the mass ratio of the lanthanum salt precursor to carbon nanotubes is 0.05:1 to 0.35:1.
[0011] In some embodiments of the present invention, the alkaline solution includes one or more of NaOH solution, KOH solution, or NH4OH solution, and the final concentration of the alkali in the system is [missing information]. .
[0012] In some embodiments of the present invention, the adhesive is one or more of PVDF, PTFE or Nafion.
[0013] The organic solvents include, but are not limited to, polar organic solvents capable of dissolving polyvinylidene fluoride adhesives, such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), and dimethyl sulfoxide (DMSO).
[0014] The conductive substrate is a titanium sheet, titanium mesh, carbon paper, graphite sheet, or conductive carbon cloth.
[0015] In some embodiments of the present invention, the solid content of the electrode slurry is 10-100 mg / mL; The thickness of the active layer in the confined lanthanum-modified carbon nanotube anode material is 10-200 μm.
[0016] In some embodiments of the present invention, the electrochemical degradation conditions are: a voltage of 0.8-3.0V, an electrolyte of one or more of NaCl, Na2SO4, or NaNO3; the confined lanthanum-modified carbon nanotube anode material is used as the anode, and graphite, titanium, carbon paper, or stainless steel is used as the cathode.
[0017] In some embodiments of the present invention, the concentration of organophosphorus in the wastewater is [missing information]. ; The organophosphorus is selected from one or more of glyphosate, glufosinate, dipropylphosphonic acid, and aminotrimethylenephosphonic acid. The technical solution of the present invention has the following advantages compared with the prior art: This invention exposes the internal channels of carbon nanotubes through strong acid opening and freeze-drying, allowing lanthanum species to enter the inner cavity and deposit in situ, forming confined lanthanum active sites. These confined lanthanum sites enhance the adsorption of glyphosate at the electrode interface, increasing the reaction residence time and interfacial reaction efficiency of glyphosate on the anode surface. The confined lanthanum sites promote selective CP bond cleavage in glyphosate and inhibit CN bond cleavage, thereby reducing AMPA formation. The anode can increase PO4 content. 3- The release efficiency allows for the conversion of more phosphorus in glyphosate into inorganic phosphate. The glyphosate solution treated with this anode exhibits significantly reduced inhibitory effects on seed germination and seedling growth. Confined lanthanum species have a lower risk of lanthanum leaching than lanthanum species loaded on the outer surface, resulting in better material stability. Attached Figure Description
[0018] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein... Figure 1This is a schematic diagram illustrating the preparation process and structural distribution of the confined lanthanum-modified carbon nanotube material of this invention; including the preparation of open-channel carbon nanotubes, the introduction of lanthanum salt precursors, alkaline in-situ precipitation, and the spatial distribution differences between La / CNT-in and La / CNT-out; wherein, a: schematic diagram of the preparation process of La / CNT-in and La / CNT-out; b: transmission electron microscopy image of La / CNT-in; c: elemental distribution map of La / CNT-in; d: O1s XPS spectra of La / CNT-in and La / CNT-out; e: transmission electron microscopy image of La / CNT-out; f: elemental distribution map of La / CNT-out; g: XRD patterns of CNT, La / CNT-in, and La / CNT-out.
[0019] Figure 2 This invention relates to the effects of different La precursor to CNT mass ratios on glyphosate removal rate and AMPA formation, and the effects of La / CNT-in, La / CNT-out, and CNT on glyphosate degradation, AMPA formation, and PO4. 3- Effects of release and phosphorus distribution; including: a) the effect of different La precursor to CNT mass ratios on glyphosate removal rate and AMPA generation; b) the change of glyphosate concentration with reaction time in La / CNT-in, La / CNT-out, and CNT anode systems; c) a comparison of glyphosate adsorption by La / CNT-in, La / CNT-out, and CNT under no applied voltage conditions; d) the change of AMPA concentration with reaction time in different anode systems; e) the PO4 concentration in different anode systems. 3- Concentration changes with reaction time; f: Phosphorus concentrations in glyphosate, AMPA, and PO4 after reaction in different anolyte systems. 3- The distribution ratio in.
[0020] Figure 3 This is a schematic diagram illustrating the mechanism of glyphosate adsorption and selective bond breaking pathway regulated by confined lanthanum sites in this invention; it shows that La / CNT-in enhances glyphosate adsorption, promotes CP bond breaking, and inhibits CN bond breaking. a: Comparison of glyphosate adsorption energies of La / CNT-in, La / CNT-out, and CNT; b: Relationship between AMPA formation ratio and glyphosate adsorption energy; c: Comparison of energy barriers for CP and CN bond breaking in the CNT system; d: Comparison of energy barriers for CP and CN bond breaking in the La / CNT-out system; e: Comparison of energy barriers for CP and CN bond breaking in the La / CNT-in system.
[0021] Figure 4This invention presents the lanthanum leaching behavior of La / CNT-in and La / CNT-out anodes and the results of the phytotoxicity evaluation of the treatment solutions. Specifically: a) Comparison of lanthanum leaching amounts at the La / CNT-in and La / CNT-out anodes after multiple cycles; b) Physical images showing the effects of water, glyphosate solution, AMPA solution, and solutions treated with La / CNT-in, La / CNT-out, and CNT systems on seed germination and seedling growth; c) Statistical results of seedling length under different treatment conditions. Detailed Implementation
[0022] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0023] Example 1:
[0024] This embodiment provides a method for preparing confined lanthanum-modified carbon nanotube materials, as detailed below: 1. Weigh 3.00 g of raw carbon nanotubes and add them to 200 mL of 68 wt% nitric acid. Disperse the mixture by sonication for 1 h, then reflux at 413.2 K for 14 h. After the reaction is complete, cool to room temperature, filter to collect the solid, and wash with deionized water until the filtrate is neutral. Dry the obtained solid under vacuum at 343.2 K for 8 h, then freeze it at low temperature for 30 min, and then freeze-dry it for 48 h to obtain open-channel carbon nanotubes.
[0025] 2. Weigh 0.9925 g of lanthanum nitrate hexahydrate, dissolve it in deionized water, add 3.97 g of the above-obtained open-channel carbon nanotubes, mix under probe sonication for 2 h, then magnetically stir for 4 h. Add dropwise to the system... The solution was prepared so that the final NaOH concentration was [value missing]. After the reaction was complete, the material was filtered, washed, and vacuum dried to obtain confined lanthanum-modified carbon nanotube material, denoted as La / CNT-in. The material preparation process and confined structure are as follows: Figure 1 As shown.
[0026] Example 2
[0027] This embodiment provides a method for preparing confined lanthanum-modified carbon nanotube materials, similar to Example 1, except that in step two, the mass ratio of lanthanum nitrate hexahydrate to open-channel carbon nanotubes is 0.05:1.
[0028] Example 3
[0029] This embodiment provides a method for preparing confined lanthanum-modified carbon nanotube materials, similar to Example 1, except that in step two, the mass ratio of lanthanum nitrate hexahydrate to open-channel carbon nanotubes is 0.13:1.
[0030] Example 4
[0031] This embodiment provides a method for preparing confined lanthanum-modified carbon nanotube materials, similar to Example 1, except that in step two, the mass ratio of lanthanum nitrate hexahydrate to open-channel carbon nanotubes is 0.25:1.
[0032] Example 5
[0033] This embodiment provides a method for preparing confined lanthanum-modified carbon nanotube materials, similar to Example 1, except that in step two, the mass ratio of lanthanum nitrate hexahydrate to open-channel carbon nanotubes is 0.35:1.
[0034] Comparative Example 1: This comparative example provides a method for preparing a lanthanum-modified carbon nanotube material with an external surface loaded, as detailed below: 3.00 g of raw carbon nanotubes were weighed and added to 200 mL of 38 wt% nitric acid. The mixture was ultrasonically dispersed for 1 h, followed by reflux at 382.2 K for 14 h. After filtration, washing until neutral, and vacuum drying, purified carbon nanotubes were obtained. Following the lanthanum salt introduction and alkaline precipitation steps in Example 1, the purified carbon nanotubes were used to replace the open-channel carbon nanotubes to prepare a lanthanum-modified carbon nanotube material with an outer surface loaded with lanthanum, denoted as La / CNT-out. This material was used as a comparative example to illustrate the effect of the spatial distribution of lanthanum species on performance.
[0035] Comparative Example 2 A purified carbon nanotube (CNT) is provided.
[0036] Application Example 1: I. Anode Preparation 1. Cut the titanium plate into 10mm×10mm square bases. Use silicon carbide sandpaper to grind and polish the surface of the titanium base to remove the dense oxide film on the titanium surface and improve the surface roughness of the base, thereby improving the adhesion performance of the catalytic coating. After grinding, place the titanium sheet in acetone, anhydrous ethanol and deionized water for ultrasonic cleaning for 10 minutes each to remove surface oil and grinding debris. After cleaning, dry the titanium sheet and set it aside for use.
[0037] 2. La / CNT-in and PVDF were mixed and ground at a mass ratio of 9:1. 1 mL of N-methylpyrrolidone was added to prepare a homogeneous slurry with a solid content of 20 mg / mL. The slurry was coated onto both sides of a pretreated titanium sheet, and the solvent was removed by drying to obtain a La / CNT-in anode with a thickness of 10-60 μm. La / CNT-out anodes and CNT anodes were prepared using the same method.
[0038] II. Electrochemical Treatment of Glyphosate Wastewater The prepared La / CNT-in anode was used as the anode, and a graphite plate as the cathode, placed in a diaphragm-free electrolytic cell. The electrode spacing was 1 cm, and the electrolyte volume was 30 mL. Glyphosate and 50 mM NaCl were used. An electrolytic reaction was initiated under a constant voltage of 1.6 V. Samples were taken periodically during the reaction, residual oxides were quenched with sodium thiosulfate, and glyphosate, AMPA, and PO4 were measured. 3- concentration.
[0039] like Figure 2 As shown, when the mass ratio of La precursor to CNT is 0.25:1, the glyphosate removal rate is high and the AMPA formation is lowest. The La / CNT-in anode can achieve near-complete glyphosate removal within 5 hours, while significantly inhibiting AMPA accumulation and promoting PO42-. 3- Release. Compared to La / CNT-out and CNT, more phosphorus is converted to PO4 in the La / CNT-in system. 3- -P, while the proportion of AMPA-P decreased significantly, indicating that the confined lanthanum sites can regulate the glyphosate degradation pathway.
[0040] Selective bond breaking mechanism verification To illustrate the regulatory role of confined lanthanum sites on the glyphosate degradation pathway, the reaction mechanism was verified using adsorption energy calculations, P2p electronic structure analysis, and energy barrier comparisons of the reaction pathway. The results are as follows: Figure 3 As shown, La / CNT-in exhibits stronger adsorption of glyphosate than La / CNT-out and CNT, and the AMPA formation ratio decreases with increasing adsorption. Further reaction pathway analysis indicates that La / CNT-in facilitates the reduction of the CP bond breaking energy barrier and increases the difficulty of CN bond breaking, thereby shifting glyphosate degradation from the AMPA formation pathway to the CP bond breaking and phosphate release pathway.
[0041] Lanthanum leaching and treatment solution toxicity evaluation The lanthanum leaching amount was measured in the solutions after the La / CNT-in and La / CNT-out anodic reactions. The results are as follows: Figure 4 As shown, La / CNT-in maintains a lower lanthanum leaching rate than La / CNT-out during long-term operation.
[0042] The treated solutions were used in seed germination experiments. The results showed that untreated glyphosate and AMPA solutions significantly inhibited seed germination and seedling growth, while the La / CNT-in treatment solution significantly reduced the inhibitory effect on seedling growth, indicating that the anode material can effectively reduce the residual phytotoxicity of glyphosate treatment solutions.
[0043] in conclusion This invention achieves highly efficient and selective electrochemical degradation of glyphosate wastewater by constructing a confined lanthanum-modified carbon nanotube anode. This material utilizes the internal channels of the carbon nanotubes to spatially confine lanthanum species, enhancing glyphosate interfacial adsorption and promoting selective CP bond breaking, thereby inhibiting AMPA formation, promoting inorganic phosphate release, and reducing the phytotoxicity of the treated solution. This technology features feasible preparation methods, mild reaction conditions, low reagent dosage, and good environmental safety, making it suitable for treating glyphosate and other organophosphorus pollutants in wastewater.
[0044] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. The application of a confined lanthanum-modified carbon nanotube anode material in the selective electrochemical degradation of organophosphorus wastewater; the confined lanthanum-modified carbon nanotube anode material comprises a conductive substrate, confined lanthanum-modified carbon nanotubes and a binder loaded on the surface of the conductive substrate, wherein the confined lanthanum-modified carbon nanotubes are carbon nanotubes with open ports and internal channels as carriers, and the internal channels of the carriers are loaded with lanthanum active species.
2. The application according to claim 1, characterized in that, The confined lanthanum-modified carbon nanotube anode material was prepared by the following method; Raw carbon nanotubes were placed in a strong oxidizing acid solution, dispersed by ultrasound, and heated under reflux to obtain carbon nanotubes with open ports and internal channels. The lanthanum salt precursor was dissolved in a solvent, and the carbon nanotubes obtained above were added. After ultrasonic and stirring treatment, the lanthanum salt precursor entered the internal channels of the carbon nanotubes to obtain a mixed system. An alkaline solution was added to the resulting mixture to cause the lanthanum species to hydrolyze and precipitate in situ and be confined and deposited in the internal channels of the carbon nanotubes, thus obtaining a confined lanthanum-modified carbon nanotube composite material. The confined lanthanum-modified carbon nanotube composite material was mixed with a binder to prepare an electrode slurry, which was then coated onto the surface of a conductive substrate and dried to obtain a confined lanthanum-modified carbon nanotube anode material.
3. The application according to claim 2, characterized in that, The concentration of the strong oxidizing acid solution is 60-70 wt%; the strong oxidizing acid in the strong oxidizing acid solution is selected from one or more of nitric acid, concentrated sulfuric acid, and hydrogen peroxide; The heating reflux temperature is 400-420K, and the reflux time is 10-18h; It also includes low-temperature freezing and freeze-drying; the low-temperature freezing time is 10-60 min, and the freeze-drying time is 24-72 h.
4. The application according to claim 2, characterized in that, The lanthanum salt precursor is selected from one or more of lanthanum nitrate, lanthanum chloride, and lanthanum acetate.
5. The application according to claim 2, characterized in that, The mass ratio of the lanthanum salt precursor to carbon nanotubes is 0.05:1 to 0.35:
1.
6. The application according to claim 2, characterized in that, The alkaline solution includes one or more of NaOH solution, KOH solution, or NH4OH solution, and the final concentration of the alkali in the system is [missing information]. .
7. The application according to claim 2, characterized in that, The adhesive is one or more of PVDF, PTFE or Nafion; the conductive substrate is a titanium sheet, titanium mesh, carbon paper, graphite sheet or conductive carbon cloth.
8. The application according to claim 2, characterized in that, The solid content of the electrode slurry is 10-100 mg / mL; The thickness of the active layer in the confined lanthanum-modified carbon nanotube anode material is 0.1-0.15 mm.
9. The application according to claim 1, characterized in that, Electrochemical degradation conditions: voltage 0.8-3.0V, electrolyte one or more of NaCl, Na2SO4 or NaNO3; the confined lanthanum modified carbon nanotube anode material is used as the anode, and graphite, titanium, carbon paper or stainless steel is used as the cathode.
10. The application according to claim 1, characterized in that, The concentration of glyphosate in the wastewater was ; The organophosphorus is selected from one or more of glyphosate, glufosinate, dipropylphosphonic acid, or aminotrimethylenephosphonic acid.