Phosphogypsum-based aggregate, method for preparing the same, and use thereof
By redesigning the composition and reaction pathway of modified phosphogypsum with alkaline solid waste and cement, and combining the carbonization-hydration synergistic hardening mode with moisture control of internal curing agent, the problems of low strength and poor stability of phosphogypsum-based aggregates were solved, achieving the effect of high early strength and low water absorption.
Patent Information
- Application Number
- CN202611607227.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-20
AI Technical Summary
Existing phosphogypsum-based aggregates have low strength, poor early stability, high water absorption, and cannot effectively solidify free phosphorus and fluoride ions in phosphogypsum.
Modified phosphogypsum was prepared by mixing and aging phosphogypsum with a calcium-based alkaline precipitant. After mixing with an internal curing agent, slag, alkaline solid waste and cement, it was carbonized under a CO₂ atmosphere to form a partitioned structure of a carbonized surface layer and a hydrated core. The carbonization-hydration synergistic hardening mode was utilized, and saturated surface-dried zeolite powder was used as an internal curing agent to regulate moisture release.
It improves the early strength and long-term stability of phosphogypsum-based aggregates, reduces water absorption, and enables the rapid establishment of the early load-bearing skeleton and the continuous densification of the later structure.
Abstract
Description
Technical Field
[0001] This invention relates to the field of building materials technology, specifically to a phosphogypsum-based aggregate, its preparation method, and its application. Background Technology
[0002] Phosphogypsum-based aggregate is a type of artificial aggregate made primarily from industrial waste phosphogypsum through a specific process. Existing phosphogypsum-based aggregates are mainly hydration-hardening types, typically composed of 45 wt.% phosphogypsum, 50 wt.% mineral powder, and 5 wt.% alkaline cementitious materials. The strength of this type of phosphogypsum-based aggregate primarily comes from ettringite. A highly alkaline environment, provided by cement or other alkaline cementing materials or solid waste, activates the silica-alumina components in the mineral powder, while the phosphogypsum provides SO4. 2- The mineral powder reacts with each other to form hydration products (mainly ettringite). However, the reaction degree of the mineral powder is limited, and the amount of hydration products generated is small, resulting in low aggregate strength. More importantly, ettringite is unstable under changes in temperature and humidity and is prone to phase transformation, leading to instability. Moreover, this type of phosphogypsum-based aggregate lacks calcium hydroxide, and ettringite is prone to react and decompose with CO2, resulting in low early strength, high water absorption, and poor long-term stability of the phosphogypsum-based aggregate. It also cannot effectively solidify the free phosphorus and fluoride ions in the phosphogypsum. Summary of the Invention
[0003] In view of this, the purpose of this invention is to provide a phosphogypsum-based aggregate, its preparation method, and its application. The phosphogypsum-based aggregate provided by this invention has high early strength, low water absorption, and good long-term stability.
[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing phosphogypsum-based aggregate, comprising the following steps: Phosphogypsum and calcium-based alkaline precipitant are mixed and aged to obtain modified phosphogypsum; By weight, 40-60 parts of the modified phosphogypsum, 5-15 parts of the internal curing agent, 15-25 parts of slag, 20-30 parts of alkaline solid waste and 5 parts of cement are mixed to obtain a mixed powder; the mixed powder is mixed with water and then subjected to disc granulation to obtain a green body; the internal curing agent is saturated surface-dry zeolite powder; The green body is carbonized under a CO2 atmosphere to obtain carbonized aggregate; The carbonized aggregate is cured to obtain phosphogypsum-based aggregate; The calcium-based alkaline precipitant comprises calcium oxide and / or calcium hydroxide; The alkaline solid waste is steel slag and / or magnesium slag.
[0005] Preferably, the volume concentration of CO2 in the CO2 atmosphere is 20-50%; The carbonization pressure is 0.1~0.5MPa, and the time is 10~36h.
[0006] Preferably, the calcium-based alkaline precipitant includes carbide slag and / or lime; The mass ratio of the phosphogypsum to the calcium-based alkaline precipitant is 100:2~5.
[0007] Preferably, the water-to-binder ratio of the water to the mixed powder is 0.15 to 0.23.
[0008] Preferably, the rotation speed of the disc granulator is 30~50 rpm, and the angle between the disc surface and the horizontal plane is 45°. Water is added via atomized spraying during the disc granulation process; The disc granulation time is 10-15 minutes; the particle size of the green body is 7-20 mm.
[0009] Preferably, the saturated surface-dried zeolite powder has a dry basis moisture content of 25-40%; The preparation method of the saturated surface-dried zeolite powder includes the following steps: Zeolite powder is soaked in water until it becomes saturated, thus obtaining water-saturated zeolite powder; The water-saturated zeolite powder was vacuum filtered to obtain saturated surface-dry zeolite powder. The zeolite powder is lithium-ion modified Y-type zeolite powder; The zeolite powder has a median particle size of 10~45μm and a pore size of 0.004~15μm.
[0010] Preferably, the aging temperature is 23~27℃, the humidity is 40~60%, and the time is 6~24h.
[0011] This invention provides a phosphogypsum-based aggregate prepared by the preparation method described above, comprising a hydrated core and a carbonized surface layer covering the surface of the hydrated core; The carbonized surface layer comprises calcium carbonate crystals and silica gel; the hydrated core comprises C-(A)-SH gel and ettringite.
[0012] Preferably, the phosphogypsum-based aggregate has a 7-day compressive strength of 30-50 MPa, a 28-day compressive strength of 50-80 MPa, and a water absorption rate of <1%.
[0013] This invention provides the application of the phosphogypsum-based aggregate described in the above technical solution in building materials.
[0014] Beneficial technical effects: This invention addresses the problem of limited actual reaction rates and insufficient cementitious effect of slag in traditional hydration-hardening phosphogypsum-based aggregates due to high slag content. It redesigns the composition and reaction pathways of modified phosphogypsum, slag, alkaline solid waste, and cement. In hydration-based phosphogypsum aggregates, the slag reaction rate is relatively low, with a large amount remaining unreacted. This invention appropriately reduces the slag content and increases the proportion of alkaline solid wastes such as steel slag and / or magnesium slag, transforming the traditional hardening mode, which primarily relies on hydration, into a "carbonation-hydration synergistic" hardening mode that prioritizes carbonation followed by hydration. Specifically, the active calcium component in the alkaline solid waste mainly participates in the early carbonation reaction, the modified phosphogypsum provides sulfate for the subsequent formation of ettringite, and the slag provides active aluminum and silicon components. These components, along with cement and unreacted alkaline solid waste, participate in subsequent hydration, allowing different raw materials to play their respective roles at different reaction stages and improving the effective utilization of each component.
[0015] After the green body is formed by disc granulation, certain pores are retained between the particles and inside the aggregate, providing channels for CO2 to be transported from the outside to the inside. Due to the obvious surface-to-inside characteristic of the carbonization reaction, the aggregate forms a partitioned structure of "carbonized surface layer - incompletely carbonized core". The carbonized surface layer can quickly establish the early load-bearing skeleton of the aggregate and improve early strength; on the other hand, it forms a relatively dense outer barrier, which is conducive to reducing the migration of subsequent moisture and corrosive media into the aggregate interior, providing a foundation for the later durability of the aggregate.
[0016] Meanwhile, the incompletely carbonized areas (core) within the aggregate still retain a certain amount of slag, cement, and some alkaline solid waste, providing a reaction reserve for subsequent curing stages. Compared to fully carbonized aggregate, this spatial partitioning reaction method reduces the premature and complete coating of active particles with carbonate products during the carbonation stage, thereby reducing the obstruction of the dense carbonization product layer to the subsequent hydration reaction interface. After carbonation, the slag, cement, and unreacted alkaline solid waste retained in the core continue to undergo hydration reactions, generating hydration products such as ettringite under the condition of sulfate provided by phosphogypsum, and simultaneously forming cementitious phases such as C-(A)-SH gel. These hydration products further fill the residual pores after carbonation, and together with the carbonate hardening structure formed by the outer carbonation layer, promote the continuous densification of the aggregate matrix, thereby achieving spatial synergy of "outer carbonation strengthening - core continuous hydration," improving later strength and reducing aggregate water absorption.
[0017] Furthermore, this invention introduces saturated surface-dried zeolite as an internal curing agent, utilizing its fine pores to strongly constrain internally stored water, thereby regulating the timing of moisture release from the aggregate. Compared to porous materials with larger pore sizes, such as shale powder, the water stored inside zeolite is less likely to be released in large quantities in a short time under the exothermic effect of carbonization. Therefore, it can produce two beneficial effects during the carbonization stage: firstly, it avoids the rapid release of stored water, which would lead to excessively high local moisture content and relative humidity in the aggregate, reducing the occupation of gas transport channels by liquid water, thus maintaining a moisture state conducive to the transport of CO2 into the aggregate and the continuous carbonization reaction; secondly, it reduces the premature consumption of internally stored water during the carbonization stage, allowing more moisture to be retained for subsequent curing stages.
[0018] As slag, cement, and unreacted alkaline solid waste continue to hydrate after carbonization, consuming pore water, the relative humidity inside the aggregate gradually decreases, creating a water potential difference. This drives the gradual release of stored water within the zeolite, providing a continuous internal water source for subsequent hydration reactions. This achieves coordination between the CO2 transport requirements of the carbonization stage and the continuous water supply requirements of the subsequent hydration stage, further promoting later-stage aggregate hydration and structural densification. Detailed Implementation
[0019] This invention provides a method for preparing phosphogypsum-based aggregate, comprising the following steps: Phosphogypsum and calcium-based alkaline precipitant are mixed and aged to obtain modified phosphogypsum; By weight, 40-60 parts of the modified phosphogypsum, 5-15 parts of the internal curing agent, 15-25 parts of slag, 20-30 parts of alkaline solid waste and 5 parts of cement are mixed to obtain a mixed powder; the mixed powder is mixed with water and then subjected to disc granulation to obtain a green body; the internal curing agent is saturated surface-dry zeolite powder; The green body is carbonized under a CO2 atmosphere to obtain carbonized aggregate; The carbonized aggregate is cured to obtain phosphogypsum-based aggregate; The calcium-based alkaline precipitant comprises calcium oxide and / or calcium hydroxide; The alkaline solid waste is steel slag and / or magnesium slag.
[0020] Unless otherwise specified, the materials and equipment used in this invention are all commercially available products in the field.
[0021] This invention involves mixing phosphogypsum and a calcium-based alkaline precipitant, followed by aging, to obtain modified phosphogypsum.
[0022] In this invention, the calcium-based alkaline precipitant comprises calcium oxide and / or calcium hydroxide; the calcium-based alkaline precipitant may include carbide slag and / or lime; the mass ratio of phosphogypsum to calcium-based alkaline precipitant can be 100:2~5, specifically 100:3, 100:3.5, or 100:4. In this invention, the aging temperature can be 23~27℃, specifically 24℃, 25℃, or 26℃; the aging humidity can be 40~60%, specifically 45%, 50%, or 55%; the aging time can be 6~24h, specifically 12h, 15h, or 20h. This invention, through aging, allows the calcium-based alkaline precipitant and phosphogypsum to react, pre-precipitating some fluorine and phosphorus ions, thus reducing the inhibitory effect of soluble phosphorus and fluorine impurities in phosphogypsum on the hydration of alkaline cementitious materials.
[0023] After the aging process is completed, the present invention further includes drying, crushing, and sieving the aged material obtained from the aging process. In this invention, the drying temperature can be 100-110℃, specifically 102℃, 105℃, or 108℃. The present invention does not have a specific limitation on the drying time; the aged material only needs to be dried to a constant weight. In this invention, the particle size of the sieved material obtained from the sieving process can be >200 mesh.
[0024] After obtaining the modified phosphogypsum, 40-60 parts by weight of the modified phosphogypsum, 5-15 parts by weight of the internal curing agent, 15-25 parts by weight of the slag, 20-30 parts by weight of the alkaline solid waste, and 5 parts by weight of the cement are mixed to obtain a mixed powder. The mixed powder is then mixed with water and subjected to disc granulation to obtain a green body. The cement, alkaline solid waste, and slag used in this invention all have alkaline characteristics. Their alkalinity is utilized to catalyze an alkaline-initiated reaction, resulting in slow hydration. The entire hydration process is similar to the hydration of persulfate phosphogypsum slag cement.
[0025] In this invention, the mixed powder comprises 40 to 60 parts of the modified phosphogypsum by weight, specifically 45, 50 or 55 parts.
[0026] In this invention, the mixed powder comprises 5 to 15 parts of internal curing agent, specifically 8 parts, 10 parts or 12 parts, based on the mass fraction of the modified phosphogypsum.
[0027] In this invention, the internal curing agent is saturated surface-dried zeolite powder; the dry basis moisture content of the internal curing agent can be 25-40%, specifically 30% or 35%. Conventional porous materials such as shale ceramsite have large pores and are prone to premature water release during carbonization, failing to provide moisture for subsequent hydration. However, this invention uses specific zeolite as a porous material for water storage, with smaller pores. By storing water through fine pores, the premature release of water during the exothermic carbonization reaction is suppressed, thus retaining moisture and maintaining CO2 transport conditions while providing moisture for subsequent hydration.
[0028] In this invention, the preparation method of the saturated surface-dry zeolite powder may include the following steps: soaking zeolite powder in water to absorb water until saturation, to obtain water-saturated zeolite powder; and vacuum filtering the water-saturated zeolite powder to obtain saturated surface-dry zeolite powder.
[0029] In this invention, the zeolite powder can be lithium-ion modified Y-type zeolite powder (LiY-type zeolite powder); the median particle size (D) of the zeolite powder 50 The pore size can be 10~45μm, specifically 20μm, 30μm or 45μm; the pore size of the zeolite powder can be 0.004~15μm, specifically 0.01μm, 0.1μm, 1μm or 10μm. This invention does not have a specific limitation on the water absorption time, as long as the water absorption of the zeolite powder reaches equilibrium.
[0030] In this invention, the mixed powder comprises 15 to 25 parts of slag, specifically 18, 20 or 23 parts, based on the mass fraction of the modified phosphogypsum.
[0031] In this invention, the mixed powder comprises 20 to 30 parts of alkaline solid waste, specifically 22, 25 or 27 parts, based on the mass fraction of the modified phosphogypsum.
[0032] In this invention, the mixed powder comprises 5 parts of cement based on the mass fraction of the modified phosphogypsum; the cement may specifically be ordinary silicate cement.
[0033] In this invention, the water-to-binder ratio of the water and the mixed powder can be 0.15 to 0.23, specifically 0.18, 0.2, or 0.22. In this invention, the water-to-binder ratio is the ratio of the mass of water added during the mixing process to the mass of all powder materials in their dry state.
[0034] In this invention, the rotation speed of the disc granulator can be 30-50 rpm, specifically 35 rpm, 40 rpm, or 45 rpm; the angle between the disc surface and the horizontal plane (disc tilt angle) can be 45°; water is added during the disc granulation process via atomized spraying; the granulation time can be 10-15 minutes, specifically 11 minutes, 12 minutes, 13 minutes, or 14 minutes; the particle size of the green body can be 7-20 mm, specifically 10 mm, 12 mm, 15 mm, or 18 mm. This invention uses disc granulation to add uniformly mixed powder to a disc granulator. During disc rotation, externally added water is sprayed evenly onto the surface of the rolling material in stages via atomized spraying, gradually wetting the material and causing it to agglomerate into spheres. After granulation, green bodies with a particle size of 7-20 mm and intact shape are selected for subsequent carbonization and curing.
[0035] After obtaining the green body, the present invention carbonizes the green body under a CO2 atmosphere to obtain carbonized aggregate.
[0036] In this invention, the volume concentration of CO2 in the CO2 atmosphere can be 20-50%, specifically 25%, 30%, 35%, or 45%; the carbonation pressure can be 0.1-0.5 MPa, specifically 0.2 MPa, 0.3 MPa, or 0.4 MPa; and the carbonation time is 10-36 hours, specifically 15 hours, 20 hours, or 30 hours. During the carbonation process, CO2 and the active calcium source in the alkaline solid waste react rapidly to generate calcium carbonate crystals that adhere to the surface of phosphogypsum, slag, and alkaline solid waste, providing a foundation for the early strength development of phosphogypsum-based aggregates. Simultaneously, the exothermic carbonation reaction induces the initial release of water from the internal curing agent, preventing self-shrinkage of the matrix. This invention controls the carbonation pressure to 0.1-0.5 MPa to avoid excessive carbonation pressure (e.g., reaching 1 MPa) which would increase the carbonation depth, causing carbonation products to encapsulate hydrated components and affect subsequent hydration processes.
[0037] After obtaining carbonized aggregate, the present invention cures the carbonized aggregate to obtain phosphogypsum-based aggregate.
[0038] In this invention, the curing time can be 21-28 days, specifically 23, 25, or 27 days; the curing temperature can be 23-27°C, specifically 24, 25, or 26°C; and the curing humidity can be 40-60%, specifically 45%, 50%, or 55%. During carbonization and subsequent curing, the internal curing agent plays a phased role in supplying internal moisture. During the carbonization stage, as the carbonization reaction continues and moisture migrates and is lost from the aggregate under a CO2 atmosphere, the pre-stored moisture in the internal curing agent is gradually released, compensating for localized moisture deficiencies during carbonization, maintaining the appropriate moisture content required for the carbonization reaction, promoting CO2 transport within the aggregate, and ensuring the continued carbonization reaction. After carbonation, unreacted slag, alkaline solid waste, and cement continue to undergo hydration reactions, constantly consuming pore water. This reduces the relative humidity inside the aggregate and creates a water potential difference (i.e., a humidity gradient exists within the aggregate). This further drives the slow release of stored water in the internal curing agent, providing continuous internal compensation water for subsequent hydration. This forms a synergistic internal curing process of "water replenishment during carbonation - continuous water supply during subsequent hydration," promoting the generation of later hydration products and filling the micropores remaining after carbonation, increasing the density of the aggregate's internal structure, and reducing water absorption.
[0039] This invention provides a phosphogypsum-based aggregate prepared by the preparation method described above, comprising a hydrated core and a carbonized surface layer covering the surface of the hydrated core; The carbonized surface layer comprises calcium carbonate crystals and silica gel; the hydrated core comprises C-(A)-SH gel and ettringite.
[0040] In this invention, the 7-day compressive strength of the phosphogypsum-based aggregate can be 30-50 MPa, specifically 35 MPa, 40 MPa, or 45 MPa; the 28-day compressive strength of the phosphogypsum-based aggregate can be 50-80 MPa, specifically 55 MPa, 60 MPa, 70 MPa, or 75 MPa; and the water absorption rate of the phosphogypsum-based aggregate can be <1%, specifically 0.2%, 0.5%, 0.7%, or 0.9%.
[0041] This invention provides the application of the phosphogypsum-based aggregate described in the above-mentioned technical solution in building materials. In this invention, the building materials may specifically include building aggregates, concrete blocks, or road base materials; the phosphogypsum-based aggregate may be specifically applied to concrete aggregates.
[0042] To further illustrate the present invention, the solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0043] In all embodiments of the present invention and comparative examples 1 to 4, the phosphogypsum was sourced from a phosphate chemical plant in Yunnan Province; the slag was sourced from a steel smelting plant in Yunnan Province; and the steel slag was sourced from a branch of Wuhan Iron and Steel Group. The natural environment for aging or the standard environment for maintenance are: temperature 25±2℃ and humidity 50±10%.
[0044] Example 1 Unprocessed phosphogypsum and carbide slag were mixed at a mass ratio of 100:5 and aged under natural conditions for 12 hours to obtain aged material. The aged material was then placed in a forced-air drying oven and dried at 105℃ to constant weight. After cooling, it was mechanically crushed and passed through a 200-mesh standard sieve. The material passing through the sieve was modified phosphogypsum.
[0045] D 50 Zeolite powder with a thickness of 45 μm was completely immersed in deionized water and statically absorbed water for 24 hours. After the water absorption reached equilibrium, the saturated zeolite powder was vacuum filtered using a vacuum filter to obtain saturated surface-dry zeolite powder (internal curing agent) with a saturated water absorption rate of 25%.
[0046] By weight percentage, 50% modified phosphogypsum, 20% slag powder, 25% steel slag, and 5% ordinary Portland cement are dry-mixed to obtain a dry mix. An internal curing agent, accounting for 10% of the total mass of the dry mix, is then added to the dry mix and mixed evenly in a forced mixer to obtain a mixed powder. The obtained mixed powder is mixed with water at a water-cement ratio of 0.18 and granulated using a disc granulator at 40 rpm to obtain a green body.
[0047] The obtained green body was transferred to a high-pressure carbonization reactor. After vacuuming and exhausting the gas, CO2 with a volume concentration of 50% was introduced and carbonized for 12 hours at a pressure of 0.2 MPa to obtain carbonized aggregate.
[0048] The carbonized aggregate was naturally cured under standard conditions for 28 days to obtain phosphogypsum-based aggregate.
[0049] The compressive strength, water absorption and apparent density of the prepared phosphogypsum-based aggregate were tested. The test methods were as follows: compressive strength, apparent density and water absorption: GB / T 17431.2-2010 "Lightweight aggregates and their test methods Part 2: Lightweight aggregates test methods".
[0050] Testing showed that the phosphogypsum-based aggregate prepared in Example 1 had a 7-day compressive strength of 40.2 MPa, a 28-day compressive strength of 68.6 MPa, a water absorption rate of 0.6%, and an apparent density of 1.63 g / cm³. 3 .
[0051] Example 2 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that, by mass percentage, 60% of the obtained modified phosphogypsum, 15% of slag powder, 20% of steel slag, and 5% of ordinary silicate cement were dry-mixed.
[0052] Testing revealed that the phosphogypsum-based aggregate prepared in Example 2 had a 7-day compressive strength of 36.2 MPa, a 28-day compressive strength of 61.6 MPa, a water absorption rate of 0.9%, and an apparent density of 1.47 g / cm³. 3 .
[0053] Example 3 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 was that the carbonization time was 10 hours.
[0054] Testing showed that the phosphogypsum-based aggregate prepared in Example 3 had a 7-day compressive strength of 38.2 MPa, a 28-day compressive strength of 66.2 MPa, a water absorption rate of 0.7%, and an apparent density of 1.58 g / cm³. 3 .
[0055] Example 4 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that the water-cement ratio of water to the mixed powder is 0.23.
[0056] Testing revealed that the phosphogypsum-based aggregate prepared in Example 4 had a 7-day compressive strength of 36.4 MPa, a 28-day compressive strength of 71.6 MPa, a water absorption rate of 0.7%, and an apparent density of 1.84 g / cm³. 3.
[0057] Example 5 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that the saturated water absorption rate of the zeolite powder with saturated surface dryness of the internal curing agent is 30%.
[0058] Testing showed that the phosphogypsum-based aggregate prepared in Example 5 had a 7-day compressive strength of 38.9 MPa, a 28-day compressive strength of 66.2 MPa, a water absorption rate of 0.6%, and an apparent density of 1.59 g / cm³. 3 .
[0059] As can be seen from Examples 1 to 5, the phosphogypsum-based aggregate prepared by the preparation method provided by the present invention has a 7-day compressive strength of 30-50 MPa, a 28-day compressive strength of 50-80 MPa, a water absorption rate of <1%, high early strength, low water absorption rate, and excellent performance.
[0060] Comparative Example 1 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that no internal curing agent was added.
[0061] Testing showed that the phosphogypsum-based aggregate prepared in Comparative Example 1 had a 7-day compressive strength of 30.27 MPa, a 28-day compressive strength of 39.5 MPa, a water absorption rate of 6.41%, and an apparent density of 1.53 g / cm³. 3 .
[0062] Comparative Example 2 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that the resulting green body was directly cured naturally under standard conditions for 28 days to obtain the phosphogypsum-based aggregate (i.e., without carbonization).
[0063] Testing revealed that the phosphogypsum-based aggregate prepared in Comparative Example 2 had a 7-day compressive strength of 7.2 MPa, a 28-day compressive strength of 25.7 MPa, a water absorption rate of 10.1%, and an apparent density of 1.23 g / cm³. 3 .
[0064] Comparative Example 3 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that the saturated surface-dried zeolite powder used as the internal curing agent was replaced with shale powder.
[0065] Testing showed that the phosphogypsum-based aggregate prepared in Comparative Example 3 had a 7-day compressive strength of 28.2 MPa, a 28-day compressive strength of 55.3 MPa, a water absorption rate of 7.3%, and an apparent density of 1.47 g / cm³. 3Using shale powder as an internal curing agent results in premature water release during the exothermic carbonization stage, which fails to provide moisture for subsequent hydration and affects the hydration process. Consequently, the prepared phosphogypsum-based aggregate has low strength and high water absorption.
[0066] Comparative Example 4 The phosphogypsum-based aggregate was prepared using the preparation method provided in Example 1. The only difference from Example 1 is that the internal curing agent was replaced with dried zeolite powder, and the aggregate was prepared according to a water-cement ratio of 0.18.
[0067] Testing showed that the phosphogypsum-based aggregate prepared in Comparative Example 4 had a 7-day compressive strength of 35.9 MPa, a 28-day compressive strength of 45.7 MPa, a water absorption rate of 6.48%, and an apparent density of 1.59 g / cm³. 3 Although dried zeolite can promote carbon dioxide transfer and increase carbonization strength, it cannot provide a continuous water transport channel for subsequent hydration. As a result, the degree of subsequent hydration reaction remains low, leading to low strength and high water absorption of the prepared phosphogypsum-based aggregate.
[0068] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a phosphogypsum-based aggregate, characterized in that, Includes the following steps: Phosphogypsum and calcium-based alkaline precipitant are mixed and aged to obtain modified phosphogypsum; By weight, 40-60 parts of the modified phosphogypsum, 5-15 parts of the internal curing agent, 15-25 parts of slag, 20-30 parts of alkaline solid waste and 5 parts of cement are mixed to obtain a mixed powder; the mixed powder is mixed with water and then subjected to disc granulation to obtain a green body; the internal curing agent is saturated surface-dry zeolite powder; The green body is carbonized under a CO2 atmosphere to obtain carbonized aggregate; The carbonized aggregate is cured to obtain phosphogypsum-based aggregate; The calcium-based alkaline precipitant comprises calcium oxide and / or calcium hydroxide; The alkaline solid waste is steel slag and / or magnesium slag.
2. The production method according to claim 1, characterized by, The volume concentration of CO2 in the CO2 atmosphere is 20-50%. The carbonization pressure is 0.1~0.5MPa, and the time is 10~36h.
3. The preparation method according to claim 1, characterized in that, The calcium-based alkaline precipitant includes carbide slag and / or lime; The mass ratio of the phosphogypsum to the calcium-based alkaline precipitant is 100:2~5.
4. The preparation method according to claim 1, characterized in that, The water-cement ratio of the water and the mixed powder is 0.15~0.
23.
5. The preparation method according to claim 1, characterized in that, The rotation speed of the disc granulator is 30~50 rpm, and the angle between the disc surface and the horizontal plane is 45°. Water is added via atomized spraying during the disc granulation process; The disc granulation time is 10-15 minutes; the particle size of the green body is 7-20 mm.
6. The preparation method according to claim 1, characterized in that, The saturated surface-dried zeolite powder has a dry basis moisture content of 25-40%; The preparation method of the saturated surface-dried zeolite powder includes the following steps: Zeolite powder is soaked in water until it becomes saturated, thus obtaining water-saturated zeolite powder; The water-saturated zeolite powder was vacuum filtered to obtain saturated surface-dry zeolite powder. The zeolite powder is lithium-ion modified Y-type zeolite powder; The zeolite powder has a median particle size of 10~45μm and a pore size of 0.004~15μm.
7. The preparation method according to claim 1 or 3, characterized in that, The aging process is carried out at a temperature of 23-27°C, a humidity of 40-60%, and a time of 6-24 hours.
8. The phosphogypsum-based aggregate prepared by the preparation method according to any one of claims 1 to 7, characterized in that, The phosphogypsum-based aggregate includes a hydrated core and a carbonized surface layer covering the surface of the hydrated core; The carbonized surface layer comprises calcium carbonate crystals and silica gel; the hydrated core comprises C-(A)-SH gel and ettringite.
9. The phosphogypsum-based aggregate according to claim 8, characterized in that, The phosphogypsum-based aggregate has a 7-day compressive strength of 30-50 MPa, a 28-day compressive strength of 50-80 MPa, and a water absorption rate of <1%.
10. The use of the phosphogypsum-based aggregate according to claim 8 or 9 in building materials.