A slump retaining and slow release type water reducing agent
By combining immediate dispersion mother liquor, intermediate-time slow-release mother liquor, late-time slow-release mother liquor, and competitive adsorption compensation liquid, the problem of unstable concrete flowability in existing technologies has been solved. This allows for dynamic adjustment of the water-reducing agent composition based on site conditions, thereby improving the controllability and stability of construction quality.
Patent Information
- Application Number
- CN202611200005.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-20
AI Technical Summary
Existing slump-retaining and water-reducing agents are difficult to maintain the flowability of concrete under different cement batches, sand sources, or ambient temperatures, and the on-site mixing process can easily lead to excessively high initial fluidity, prolonged setting time, and unstable quality.
A combination of immediate dispersion mother liquor, intermediate-time slow-release mother liquor, late-time slow-release mother liquor, and competitive adsorption compensation liquid is used to provide water reduction and dispersion in the initial, transportation, and waiting/pumping stages of concrete, respectively. The proportion of each mother liquor is adjusted through on-site testing to adapt to different materials and environmental conditions.
It enables dynamic adjustment of the water-reducing agent composition according to actual needs, improves the stability of concrete flowability, reduces the risk of excessive fluidity and abnormal setting, and ensures the controllability of construction quality.
Smart Images

Figure CN123131071A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of concrete admixtures, specifically to a slump-retaining, slow-release water-reducing agent. Background Technology
[0002] Polycarboxylate superplasticizers, characterized by high water reduction rate, low dosage, and adjustable molecular structure, have been widely used in ready-mixed concrete, pumped concrete, and high-performance concrete. For projects involving long-distance transportation, high-temperature construction, long pumping times, or continuous pouring in sections, simply ensuring the slump of the concrete upon discharge is often insufficient to meet construction requirements. The superplasticizer needs to continuously release and disperse during transportation, waiting, pumping, and pouring stages. Therefore, existing slump-retaining superplasticizers typically delay slump loss by increasing the proportion of slow-release polycarboxylate mother liquor, increasing the total superplasticizer dosage, or using a secondary addition method.
[0003] However, the slump retention performance of concrete on-site is not only determined by transportation time, but also influenced by factors such as cement mineral composition and specific surface area, mineral admixture ratio, mud content and methylene blue value of sand and gravel, material temperature, ambient temperature, water-cement ratio, and mixing state. The same fixed formula may exhibit insufficient initial dispersion, excessively rapid early release, insufficient release in the middle stage, insufficient release in the later stage, or delayed release under different cement batches, sand sources, or ambient temperatures. Especially when mud content and methylene blue value increase, polycarboxylate superplasticizer molecules are easily competitively adsorbed by clay and fine powders with high specific surface area. Although the slump loss detected on-site may show similarities to insufficient slow-release components, the actual cause is the premature and ineffective consumption of the effective components. If the two causes are not distinguished and the slow-release mother liquor or total admixture is directly increased, the newly added components may still be adsorbed by fine powders, failing to stably improve the slump retention effect and increasing material costs.
[0004] Current on-site mixing processes typically rely on the slump of a single test mix or the arrival of the transport truck, with operators adding water-reducing agents, slump-maintaining mother liquor, or water based on experience. This approach carries several risks: First, relying solely on the flowability at a single moment makes it difficult to determine whether insufficient total effective admixture, mismatched release timing, or competitive adsorption leading to effective component loss, potentially resulting in incorrect adjustments. Second, directly increasing the total admixture may cause excessively high flowability at the mixer, leading to segregation, bleeding, decreased cohesiveness, and abnormal pumping pressure, and may also prolong setting time. While adding water-reducing agents on-site can restore slump quickly, if the timing and proportion of addition do not match the subsequent construction time, rapid loss may occur again during pumping or pouring. Different mother liquors have varying solid content; if mixing is based solely on liquid mass or volume without converting to effective solid content, the actual functional component ratio will deviate from the set value. Repeated additions make it difficult to trace the cumulative amount of admixture added to the same truckload of concrete, increasing the risks of abnormal setting, strength fluctuations, and difficulty in determining quality responsibility.
[0005] Existing technologies typically match temperature, transportation time, or target slump with a pre-set formulation. However, these methods usually output the proportions directly from scenario parameters without verifying the early consumption state and delayed replenishment recovery capacity of the water-reducing agent using the same batch of actual raw materials. When raw material batches change, discrepancies may arise between the pre-set formulation and the actual adsorption state on-site. Furthermore, determining the proportion of slow-release components solely based on a single slump retention time index fails to address the conflicting needs of the initial, intermediate, and later construction stages. Summary of the Invention
[0006] The purpose of this invention is to provide a slump-retaining slow-release water-reducing agent to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: A slump-retaining slow-release water-reducing agent is composed of an immediate dispersion mother liquor, a mid-term slow-release mother liquor, a late-term slow-release mother liquor, and a competitive adsorption compensation liquid. The immediate dispersion mother liquor, the mid-term slow-release mother liquor, the late-term slow-release mother liquor, and the competitive adsorption compensation liquid are stored independently. Instant dispersion mother liquor is used to provide water reduction and dispersion in the initial stage of concrete mixing; intermediate slow-release mother liquor is used to provide water reduction and dispersion in the concrete transportation and holding stage; late slow-release mother liquor is used to provide water reduction and dispersion in the concrete waiting, pumping or pouring stage; competitive adsorption compensating liquid is used to reduce the competitive adsorption of effective components in instant dispersion mother liquor, intermediate slow-release mother liquor and late slow-release mother liquor by cementitious materials and fine aggregate powder. With the total effective solid mass of the immediate dispersion mother liquor, intermediate-time slow-release mother liquor, late-time slow-release mother liquor and competitive adsorption compensation liquid as 100 parts, the effective solid mass of the immediate dispersion mother liquor is 35-50 parts, the effective solid mass of the intermediate-time slow-release mother liquor is 20-35 parts, the effective solid mass of the late-time slow-release mother liquor is 15-30 parts, and the effective solid mass of the competitive adsorption compensation liquid is 3-10 parts. When the slump-preserving slow-release water-reducing agent is applied to concrete, the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor and the competitive adsorption compensation liquid are mixed into a uniform and stable liquid mixture according to the on-site mixing results of the concrete to be constructed. The mass of the added liquid mixture is 0.5 to 2.5 wt% of the total mass of cementitious materials in the concrete to be constructed.
[0008] Furthermore, the instant dispersion mother liquor comprises instant dispersion polycarboxylate superplasticizer and water, and the solid content of the instant dispersion mother liquor is 35-50 wt%. The instant-dispersible polycarboxylate superplasticizer has carboxyl structural units and polyether side chain structural units in an unprotected state. In an alkaline simulated pore liquid with a temperature of 20±2℃ and a pH of 12.3~12.7, the effective carboxyl release time of the instant-dispersible polycarboxylate superplasticizer does not exceed 15 minutes. The effective carboxyl group release half-time is the time when the effective carboxyl group release of the instant-dispersible polycarboxylate superplasticizer reaches 50% of the cumulative effective carboxyl group release in 120 minutes.
[0009] Furthermore, the medium-time slow-release mother liquor includes a first-type slow-release polycarboxylate superplasticizer and water, and the solid content of the medium-time slow-release mother liquor is 35-50 wt%. The first slow-release polycarboxylate superplasticizer includes a first hydrolyzable protective structure that can hydrolyze to form carboxyl groups in an alkaline environment of concrete. In an alkaline simulated pore liquid at a temperature of 20±2℃ and a pH of 12.3 to 12.7, the effective carboxyl group release time of the first slow-release polycarboxylate superplasticizer is 30 to 60 minutes.
[0010] Furthermore, the delayed-release mother liquor comprises a second delayed-release polycarboxylate superplasticizer and water, and the solid content of the delayed-release mother liquor is 35–50 wt%. The second slow-release polycarboxylate superplasticizer includes a second hydrolyzable protective structure that can hydrolyze to form carboxyl groups in an alkaline environment of concrete. In an alkaline simulated pore liquid at a temperature of 20±2℃ and a pH of 12.3 to 12.7, the effective carboxyl group release time of the second slow-release polycarboxylate superplasticizer is 70 to 120 minutes. The hydrolysis rate of the second hydrolyzable protective structure is less than that of the first hydrolyzable protective structure.
[0011] 5. A slump-retaining slow-release water-reducing agent according to claim 1, characterized in that: the competitive adsorption compensation liquid comprises clay adsorption inhibitor, fine powder dispersant and water; The competitive adsorption compensation solution comprises, by weight: 15-40 parts of clay adsorption inhibitor; 5-20 parts of fine powder dispersant; 40-80 parts water; The clay adsorption inhibitor is at least one of the following: quaternary ammonium salt type clay inhibitor, cationic polymer type clay inhibitor, and amphoteric polymer type clay inhibitor. The fine powder dispersant is at least one of low molecular weight polycarboxylic acid dispersants, polyphosphate dispersants, and sulfonate dispersants.
[0012] A method for preparing a slump-retaining slow-release water-reducing agent, applicable to a slump-retaining slow-release water-reducing agent, the method comprising: Immediate dispersion mother liquor, intermediate sustained release mother liquor, and late sustained release mother liquor were obtained respectively, and the solid content of the three mother liquors was adjusted so that the difference in solid content among the three mother liquors did not exceed 5 percentage points. According to the weight proportions of each raw material in the competitive adsorption compensation liquid, clay adsorption inhibitor and fine powder dispersant are added to water and stirred at a stirring rate of 200-500 rpm for 20-60 minutes to obtain a uniform and stable competitive adsorption compensation liquid. The immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competitive adsorption compensation liquid are respectively placed into independent storage containers, and metering interfaces for outputting the corresponding mother liquor are set up to obtain the slump-preserving slow-release water-reducing agent.
[0013] Furthermore, the immediate dispersion mother liquor, intermediate-release mother liquor, late-release mother liquor, and competing adsorption compensation solution are obtained through on-site preparation methods, specifically including the following steps: S1. Obtain the actual cementitious materials, aggregates, and mixing water used in the concrete to be constructed, and obtain the specific surface area data of the cementitious materials, the mud content data and methylene blue value of the aggregates, the ambient temperature, the estimated transportation time, the estimated waiting time, and the target flow performance range corresponding to different construction times. S2. Mix the instant dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor and the competitive adsorption compensation liquid according to the preset basic mixing ratio to prepare a basic water-reducing agent sample; S3. Prepare one-time addition samples and segmented addition samples using the cementitious materials, aggregates and mixing water actually used in the concrete to be constructed, so that the total effective solid addition amount of the base water-reducing agent sample is the same in the one-time addition samples and segmented addition samples. Among them, for the single-addition sample, all the basic water-reducing agent sample is added at the beginning of mixing; for the segmented addition sample, 70% to 85% of the total effective solid mass of the basic water-reducing agent sample is added at the beginning of mixing, and the remaining 15% to 30% is added at the intermediate testing time. S4. Obtain the actual flow performance data of the single-addition sample and the segmented-addition sample at the initial detection time, intermediate detection time and the later detection time, respectively; S5. Determine the early adsorption consumption coefficient based on the specific surface area data of the cementitious material, the methylene blue value of the aggregate, and the actual flow performance changes of the single-addition sample at the initial and intermediate detection times. The delayed addition recovery coefficient is determined based on the difference in actual flow performance between a single-addition sample and a segmented-addition sample at the later testing time, as well as the gap in the target flow performance in the later stage. The release time migration coefficient is determined based on the direction and amount of deviation of a single sample from the corresponding target flow performance range at the initial and later detection times. S6. Determine the type of water-reducing agent mismatch based on the early adsorption consumption coefficient, delayed addition recovery coefficient, and release time migration coefficient; S7. Based on the type of water-reducing agent mismatch, under the condition that the total effective solid mass of the functional components of the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competing adsorption compensation liquid remains unchanged, transfer the effective solid content of at least one mother liquor to another mother liquor, or increase the effective solid content of the competing adsorption compensation liquid, and determine the on-site mixing ratio. S8. Prepare verification water-reducing agent samples according to the on-site mixing ratio, and use the verification water-reducing agent samples to prepare verification concrete. Obtain the actual flow performance data of the verification concrete at each test time. When the actual flow performance data at each test time meets the corresponding target flow performance range, output the on-site mixing ratio.
[0014] Furthermore, the initial testing time is 5 to 10 minutes after the concrete is mixed, the intermediate testing time is 30 to 60 minutes after the concrete is mixed, and the later testing time is 90 to 120 minutes after the concrete is mixed. Actual flow performance data includes at least one of collapse and spread; The early adsorption consumption coefficient was determined based on the following data: The relative flow performance loss of a single sample from the initial detection time to the intermediate detection time; The ratio of aggregate methylene blue value to the methylene blue baseline value; The ratio of the specific surface area of a cementitious material to its reference specific surface area; The delayed addition recovery coefficient is determined based on the proportion of the difference in actual flow performance between the segmented addition sample and the single addition sample at the later detection time to the gap in the target flow performance of the single addition sample in the later stage. The release time migration coefficient is determined based on the difference between the relative flow performance deviation of a single-added sample at the initial detection time and the relative flow performance deviation at subsequent detection times.
[0015] Furthermore, when the early adsorption consumption coefficient is not less than the second adsorption threshold and the delayed addition recovery coefficient is less than the recovery threshold, the water-reducing agent mismatch type is determined to be the early competitive adsorption type. When the delayed addition recovery coefficient is not less than the recovery threshold and the release time migration coefficient is not less than the positive migration threshold, the water-reducing agent mismatch type is determined to be the release time advance type. When the actual flow performance data at the initial detection time meets the corresponding target flow performance range, the actual flow performance data at the intermediate detection time is lower than the corresponding target flow performance range, and the release time migration coefficient is between the negative migration threshold and the positive migration threshold, the water-reducing agent mismatch type is determined to be the medium-time release insufficiency type. When the actual flow performance data at the initial and intermediate detection times meet the corresponding target flow performance range, the actual flow performance data at the later detection times are lower than the corresponding target flow performance range, and the delayed addition recovery coefficient is not less than the recovery threshold, the water-reducing agent mismatch type is determined to be the late release insufficient type. When the release time migration coefficient is not greater than the negative migration threshold, the actual flow performance data at the initial detection time is lower than the corresponding target flow performance range, and the actual flow performance data at the later detection time meets or exceeds the corresponding target flow performance range, the water-reducing agent mismatch type is determined to be the release time lag type. When the actual flow performance data at all three detection times are lower than the corresponding target flow performance range, and the early adsorption consumption coefficient is less than the first adsorption threshold, the water-reducing agent mismatch type is determined to be insufficient total effective dosage. The first adsorption threshold is less than the second adsorption threshold.
[0016] Furthermore, when the mismatch type of the water-reducing agent is early competitive adsorption type, the mass percentage of the competitive adsorption compensation liquid in the total effective solid mass of the four components is increased by 3 to 8 percentage points, the mass percentage of the immediate dispersion mother liquor in the total effective solid mass of the four components is increased by 2 to 5 percentage points, and the corresponding effective solid content is deducted from the intermediate and subsequent slow-release mother liquors according to the effective solid mass ratio of the intermediate and subsequent slow-release mother liquors before preparation. When the mismatch type of the water-reducing agent is the early release time type, 5 to 12 percent of the total effective solids of the four components are transferred out from the immediate dispersion mother liquor. 20% to 40% of the transferred effective solids are allocated to the intermediate slow-release mother liquor, and 60% to 80% of the transferred effective solids are allocated to the late slow-release mother liquor. When the water-reducing agent mismatch type is the medium-time release deficiency type, the mass percentage of the medium-time slow-release mother liquor in the total effective solid mass of the four components increases by 4 to 10 percentage points, and the corresponding effective solid content is preferentially deducted from the immediate dispersion mother liquor. When the mismatch type of the water-reducing agent is the insufficient release type, the mass percentage of the slow-release mother liquor in the total effective solids of the four components increases by 6 to 15 percentage points. Of the increased effective solids, 60% to 80% is transferred out by the immediate dispersion mother liquor, and the remaining effective solids are transferred out by the intermediate slow-release mother liquor. When the mismatch type of the water-reducing agent is the delayed release type, 4 to 10 percent of the total effective solids of the four components are transferred from the delayed-release mother liquor. 60% to 80% of the transferred effective solids are allocated to the immediate dispersion mother liquor, and the remaining transferred effective solids are allocated to the intermediate-release mother liquor. When the mismatch type of water-reducing agent is insufficient total effective dosage, the effective solid mass ratio among the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competing adsorption compensation liquid should be kept constant, so that the total effective solid addition of water-reducing agent relative to the total mass of cementitious material increases by 3% to 8%; After each transfer of effective solids or adjustment of total effective solids addition, a new water-reducing agent sample and a new concrete sample are prepared for verification. The number of times effective solids are transferred in a single on-site mixing process shall not exceed three.
[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention uses a single-addition sample and a segmented-addition sample with the same total effective solid addition amount for on-site differential testing. This allows the recovery effect produced by delayed addition to be distinguished from simply increasing the total dosage, thus providing direct experimental basis for on-site judgment.
[0018] This invention converts the competitive adsorption of raw materials, the recovery capacity of delayed addition, and the release time sequence shift into the early adsorption consumption coefficient, the delayed addition recovery coefficient, and the release time sequence migration coefficient, respectively, which can distinguish the causes of slump loss that are similar in appearance but have different adjustment directions.
[0019] This invention prioritizes transferring the effective solids component of the mother liquor during the immediate, intermediate, and final stages while maintaining a constant total effective solids mass. The total dosage is increased only when the total effective dosage is deemed insufficient, thus reducing the risks of excessively high initial fluidity, delayed condensation, bleeding segregation, and uncontrolled cumulative dosage. This invention converts the effective solids ratio into on-site liquid mass based on the solids content of each mother liquor, avoiding proportioning deviations caused by directly mixing mother liquors with different solids contents according to liquid mass ratios. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the components of a slump-retaining, slow-release water-reducing agent according to the present invention; Figure 2 This is a flowchart illustrating the steps involved in preparing a slump-retaining, slow-release water-reducing agent according to the present invention. Figure 3 This is a schematic diagram illustrating an application scenario for a slow-release water-reducing agent. Detailed Implementation
[0021] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0022] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0023] Please see Figures 1 to 3 This invention provides a slump-retaining slow-release water-reducing agent, which consists of an immediate dispersion mother liquor, a mid-term slow-release mother liquor, a late-term slow-release mother liquor, and a competitive adsorption compensating liquid. The four mother liquors are stored independently. The immediate dispersion mother liquor provides water-reducing dispersion in the initial stage of concrete mixing; the mid-term slow-release mother liquor provides water-reducing dispersion during the concrete transport and holding stage; the late-term slow-release mother liquor provides water-reducing dispersion during the concrete waiting, pumping, or pouring stage; and the competitive adsorption compensating liquid reduces the competitive adsorption of the effective components in the first three mother liquors by cementitious materials and fine aggregate powder.
[0024] Based on a total effective solids mass of 100 parts for the four mother liquors, the effective solids mass of the immediate-dispersing mother liquor is 35–50 parts, the effective solids mass of the intermediate-release mother liquor is 20–35 parts, the effective solids mass of the late-release mother liquor is 15–30 parts, and the effective solids mass of the competing adsorption compensation liquid is 3–10 parts. After on-site preparation, the four mother liquors are mixed into a homogeneous and stable liquid mixture. The added mass of the liquid mixture is 0.5–2.5 wt% of the total mass of the cementitious materials in the concrete to be constructed.
[0025] This invention also provides a method for preparing a slump-retaining, slow-release water-reducing agent. On-site, two samples are prepared using the actual raw materials of the concrete to be constructed: a single-addition sample and a segmented-addition sample. The total effective solids content of the water-reducing agent is the same in both samples. For the single-addition sample, all the base water-reducing agent is added at the initial mixing stage. For the segmented-addition sample, 70%–85% of the total effective solids is added at the initial mixing stage, with the remaining 15%–30% added at intermediate testing points. Based on the flow performance data of the two samples at the initial, intermediate, and later testing points, the early adsorption consumption coefficient, delayed addition recovery coefficient, and release time migration coefficient are determined. Then, based on each coefficient and the target flow performance at each stage, the water-reducing agent mismatch type is determined.
[0026] For early competitive adsorption type, increase the effective solids content of competitive adsorption compensation liquid and immediate dispersion mother liquor while keeping the total effective solids mass unchanged, and deduct the corresponding content from the intermediate and late-time slow-release mother liquor; for early release type, transfer part of the effective solids content in the immediate dispersion mother liquor to the intermediate and late-time slow-release mother liquor; for insufficient intermediate release type, increase the content of the intermediate slow-release mother liquor; for insufficient late-time release type, increase the content of the late-time slow-release mother liquor; for delayed release type, transfer part of the late-time slow-release mother liquor to the immediate dispersion mother liquor and intermediate slow-release mother liquor; increase the total effective dosage of water-reducing agent only when all three detection times are below the target and the early adsorption consumption coefficient is less than the first adsorption threshold.
[0027] Example 1 In this embodiment, an immediate dispersion mother liquor, a mid-term sustained-release mother liquor, a late-term sustained-release mother liquor, and a competitive adsorption compensation liquid are prepared, and each is provided with an independent storage container and metering interface.
[0028] The instant dispersion mother liquor uses a highly water-reducing polycarboxylic acid mother liquor with unprotected carboxyl structural units and polyether side chain structural units. 360 parts by weight of isopentenyl alcohol polyoxyethylene ether with a molecular weight of 2400 and 300 parts by weight of deionized water are added to a reaction vessel and stirred to dissolve at 20–30°C. 42 parts by weight of acrylic acid and 80 parts by weight of deionized water are prepared as the first dropping solution, and 1.2 parts by weight of ascorbic acid, 1.0 part by weight of mercaptopropionic acid, and 80 parts by weight of deionized water are prepared as the second dropping solution. 3.0 parts by weight of a 27.5% hydrogen peroxide aqueous solution are added to the reaction vessel, simultaneously adding the first and second dropping solutions. The first dropping solution is added over 2.5 hours, and the second dropping solution is added over 3 hours. After the addition is complete, the reaction continues for 1 hour. The pH is adjusted to 6.0–7.0 using a 30% sodium hydroxide aqueous solution, and water is added to adjust the solid content to 40 wt%, yielding the instant dispersion mother liquor.
[0029] The medium-time sustained-release mother liquor uses an ester-based polycarboxylic acid mother liquor containing a first hydrolyzable protective structure. 360 parts by weight of methyl allyl alcohol polyoxyethylene ether with a molecular weight of 2400 and 300 parts by weight of deionized water are added to the reactor. 25 parts by weight of acrylic acid, 20 parts by weight of hydroxyethyl acrylate, and 90 parts by weight of deionized water are prepared as the first dropping solution. 1.2 parts by weight of ascorbic acid, 1.1 parts by weight of mercaptopropionic acid, and 80 parts by weight of deionized water are prepared as the second dropping solution. The remaining initiation, dropping, heat preservation, and neutralization processes are the same as for the instantaneous dispersion mother liquor. Water is added to adjust the solid content to 40 wt%, thus obtaining the medium-time sustained-release mother liquor.
[0030] The subsequent sustained-release mother liquor was an ester-based polycarboxylic acid mother liquor containing a second hydrolyzable protective structure. 360 parts by weight of methyl allyl alcohol polyoxyethylene ether with a molecular weight of 2400 and 300 parts by weight of deionized water were added to the reactor. The first drop solution was prepared by adding 18 parts by weight of acrylic acid, 32 parts by weight of hydroxyethyl acrylate, 8 parts by weight of hydroxypropyl acrylate, and 100 parts by weight of deionized water. The second drop solution was prepared by adding 1.2 parts by weight of ascorbic acid, 1.0 part by weight of mercaptopropionic acid, and 80 parts by weight of deionized water. The first drop solution was added over 3 hours, and the second drop solution was added over 3.5 hours. After the addition was complete, the reaction continued for 1.5 hours. After neutralization, water was added to adjust the solid content to 40 wt%, yielding the subsequent sustained-release mother liquor. By increasing the proportion of hydrolyzable ester structural units and adjusting the composition of the comonomers, the overall hydrolysis rate of the second hydrolyzable protective structure was made lower than that of the first hydrolyzable protective structure.
[0031] The competitive adsorption compensation solution comprises, by weight, 25 parts of quaternary ammonium salt-type clay adsorption inhibitor, 10 parts of low molecular weight sodium polyacrylate fine powder dispersant with a number average molecular weight of 3000-5000, and 65 parts of water. Water is added to a stirring vessel, and the quaternary ammonium salt-type clay adsorption inhibitor and low molecular weight sodium polyacrylate are added sequentially at 300 rpm. Stirring continues for 40 minutes to obtain a homogeneous and stable competitive adsorption compensation solution.
[0032] Effective carboxyl group release was determined at half-time for the immediate-release mother liquor, intermediate-release mother liquor, and late-release mother liquor. Each mother liquor was added to an alkaline simulated pore liquid at 20±2℃ and pH 12.5, and the cumulative effective carboxyl group release per unit effective solid mass was measured at preset detection times. The corresponding cumulative effective carboxyl group release is denoted as The unit is millimoles per gram; the cumulative effective carboxyl group release over 120 minutes is recorded as... The unit is millimoles per gram; the half-time for the effective release of carboxyl groups is denoted as... The method for determining it is as follows: Table 1 lists the preparation and calibration results of the four mother liquors.
[0033] Table 1: Composition and Calibration Parameters of Four Mother Solutions As shown in Table 1, the solid content difference of the three polycarboxylate mother liquors is 0 percentage points and does not exceed 5 percentage points; the effective carboxyl group release half time of the immediate dispersion mother liquor does not exceed 15 minutes, the effective carboxyl group release half time of the intermediate slow-release mother liquor is between 30 and 60 minutes, and the effective carboxyl group release half time of the late slow-release mother liquor is between 70 and 120 minutes, respectively corresponding to the initial mixing stage, intermediate holding stage, and late construction stage as defined in the claims.
[0034] The four mother liquors were each stored in separate containers equipped with mass measuring devices. To avoid the on-site liquid weighing ratio deviating from the effective solid ratio due to different solid contents, the fourth... The target proportion of the mother liquor in the total effective solid mass of the functional components is denoted as: The total effective solid mass of the functional components planned to be added in this batch is recorded as follows: The unit is kilogram; the first The solid content of the mother liquor is denoted as ; will the first The mass of the mother liquor measured on-site is recorded as follows: If the unit is kilogram, then: Based on the above conversion results, the field controller controls the four metering interfaces to output the mother liquor. After the output is completed, the mixture is stirred at 200-400 rpm for 5-10 minutes to form a homogeneous and stable liquid mixture.
[0035] Example 2 This embodiment is used for on-site data acquisition and dual-sample differential testing. Specifically, six example scenarios with different raw material states and construction conditions are selected, denoted as samples Q1 to Q6. Each sample uses cement, fly ash, mineral powder, sand, stone, and mixing water actually used in the corresponding project to prepare both single-addition and segmented-addition samples. The amount of cementitious material used in each sample is 480 kg / m³, the water-cement ratio is 0.36, the liquid addition mass of the base water-reducing agent is 1.20 wt% of the cementitious material mass, and the effective solid mass ratio of the four mother liquors is 45:28:22:5.
[0036] The specific surface area of the cementitious materials was obtained by measuring the Blaine surface area; the mud content of the aggregates was obtained based on the results of water washing and screening; the methylene blue value was obtained by testing the sand and gravel upon arrival; the ambient temperature was obtained by a temperature sensor in the test area; and the estimated transportation time and estimated waiting time were obtained from vehicle dispatch records and construction plans. Example samples from Example 2 are shown in Table 2 below.
[0037] Table 2: On-site Scene and Raw Material Parameters According to construction requirements, the initial testing time is set at 5-10 minutes after mixing, the intermediate testing time is set at 45 minutes after mixing, and the final testing time is set at 105 minutes after mixing. The target expansion at the three testing times are 650mm, 600mm, and 520mm, respectively. When the engineering technical requirements specify a target range, the first... The target lower limit at each detection time is denoted as... The unit is millimeters, and the upper limit of the target is denoted as... The unit is millimeters, and the representative value of the target used for calculation is denoted as... If the unit is millimeters, then: For the single-addition sample, all the base water-reducing agent was added at the initial mixing stage. For the segmented-addition sample, 80% of the total effective solid mass of the base water-reducing agent was added at the initial mixing stage, and the remaining 20% was added after testing was completed at the intermediate testing stage. The total effective solid mass of the water-reducing agent added was the same for both types of samples. The actual spread of the single-addition sample at the initial, intermediate, and final testing stages was recorded as follows: , and All units are millimeters; the actual spread of the segmented sample at the later testing time is recorded as . The units are millimeters. The test results are shown in Table 3 below.
[0038] Table 3: Spread data of single-powder and segmented-powder samples Example 3 To enable data from different units to participate in the early competitive adsorption evaluation, the initial relative flow performance loss, methylene blue normalized value, and specific surface area normalized value of the single-addition sample were determined separately.
[0039] The initial relative flow performance loss of a single sample is denoted as . The methylene blue value of the aggregate is recorded as... The unit is grams per kilogram. The baseline value for methylene blue is denoted as... The unit is grams per kilogram; in this example, it is 2.5 g / kg. The specific surface area of the cementitious material is denoted as... The unit is square meters per kilogram, and the benchmark value for specific surface area is denoted as... The unit is per square meter per kilogram; in this example, it is taken as 500 m² / kg. The normalized value of methylene blue is denoted as... The normalized value of the specific surface area is denoted as .in, Used to take the larger of the two values within the parentheses. Used to take the smaller of the two values within the parentheses: The early adsorption consumption coefficient is denoted as . The weighted average is determined by weighting the previous relative flow performance loss, the normalized value of methylene blue, and the normalized value of specific surface area. In this embodiment, the three weights are 0.50, 0.30, and 0.20, respectively, and the sum of the three weights is 1. The weights are set based on the following criteria: the actual flow performance loss in the early stage directly reflects the attenuation of the effective effect of the water-reducing agent in the current material system, and is given the highest weight; the methylene blue value directly reflects the adsorption capacity of the active clay in the fine aggregate for polycarboxylate molecules, and is given the second highest weight; the specific surface area of the cementitious materials reflects the total adsorption surface area provided by cement and mineral admixtures, and is used for supplementary evaluation. In practical applications, no less than 30 sets of historical mix design data of the same material system can be used, and the weights can be checked using the manual verification results of the mismatch type as labels, but the three input quantities and their physical meanings remain unchanged.
[0040] The delayed application recovery coefficient is denoted as... When the later-stage expansion of a single-stage sample is lower than the later-stage target expansion, the later-stage recovery of segmented-stage samples relative to the single-stage sample is used to determine the later-stage target notch of the single-stage sample. To avoid the denominator being zero, the preset correction amount is denoted as... The unit is millimeters; in this embodiment, 1 mm is used. and Limit the results to the range of 0 to 1: when Not less than When this occurs, it indicates that there is no later-stage target gap that needs to be recovered in a single sample application. This embodiment will... Set to 0 to prevent triggering mid-to-late game strategy additions.
[0041] Let the release time-series migration coefficient be denoted as This is used to compare the deviations of the initial and later stages from their respective target values. The initial target expansion is denoted as... The unit is millimeters, and the later target expansion is denoted as... If the unit is millimeters, then: when When the value is positive, it indicates that the water reduction and dispersion effect is concentrated in the earlier stage relative to the target; when... When the value is negative, it indicates that the water reduction and dispersion effect is concentrated in the later stage relative to the target. In order to avoid frequent replacements caused by small-scale detection fluctuations, this embodiment sets the positive migration threshold to 0.10 and the negative migration threshold to -0.10; the timing migration judgment is triggered only when the relative deviation difference between the initial stage and the later stage reaches 10 percentage points.
[0042] In this embodiment, the first adsorption threshold is set to 0.35, the second adsorption threshold is set to 0.55, and the recovery threshold is set to 0.40. The first adsorption threshold is used to exclude samples that obviously do not have competitive adsorption, the second adsorption threshold is used to identify samples that need to have competitive adsorption compensation solution added preferentially, and the recovery threshold means that only when the effective solids component is shifted back after at least 40% of the target gap in the later stage of the sample addition is it considered to be practically meaningful.
[0043] Each mismatch type is determined in the following order to avoid the same sample simultaneously meeting multiple conditions: first, early competitive adsorption type; then, pre-release type; next, mid-release insufficiency type, late-release insufficiency type, and delayed release type; finally, total effective dopant insufficiency type. Among these, the pre-release type, in addition to meeting the following conditions... and In addition, it requires that the initial actual expansion degree is higher than the initial target expansion degree; the subsequent insufficient release type requires that the initial and intermediate detection results meet the target range, and the later detection results are lower than the target range. .
[0044] Taking sample Q1 as an example, , , ,therefore ; .because Not less than the second adsorption threshold and If the value is less than the recovery threshold, Q1 is classified as an early competitive adsorption type.
[0045] Taking sample Q2 as an example, , , Since segmented deployment can compensate for most of the later target gaps, and the initial expansion is higher than the target, and the release timing migration coefficient is not less than the positive migration threshold, Q2 is determined to be a release timing forward shift type.
[0046] Taking sample Q5 as an example, the initial scaling factor was lower than the target, but the later scaling factor was higher than the target. If the value is not greater than the negative migration threshold, Q5 is classified as a release-time lag type. The calculation results for the six samples are shown in Table 4.
[0047] Table 4: Coefficient Calculation Results and Mismatch Types Example 4 This embodiment is used to determine the on-site mixing ratio based on the mismatch type. According to the mismatch types in Table 4, the on-site mixing ratio is determined based on the basic effective solid mass ratio of 45:28:22:5. To ensure that the adjustment range varies with the target gap, while guaranteeing that the adjustment result is within the range defined in the claims, the [specific method / mechanism] will be [further specified]. The relative performance gap of each detection stage is denoted as The minimum allowable adjustment percentage for this mismatch type is denoted as The maximum allowable adjustment percentage is denoted as The reference gap used to achieve the maximum adjustment amount is denoted as In this embodiment, 0.20 is used; the percentage point of this adjustment is recorded as... : In the formula, the actual expansion degree of the detection stage corresponding to the adjustment object is denoted as... The unit is millimeters. During on-site execution, [the following will be used]. Round to 1 percentage point, and verify that the effective solid ratios of the immediate dispersion mother liquor, intermediate slow-release mother liquor, late slow-release mother liquor, and competitive adsorption compensation liquid are within the ranges of 35–50 parts, 20–35 parts, 15–30 parts, and 3–10 parts, respectively. If the calculated value is transferred and exceeds the range, the mother liquor is limited to the corresponding boundary, and the uncompleted transfer amount is allocated to another mother liquor in the same adjustment direction.
[0048] For sample Q1, the early adsorption consumption coefficient reached 0.6843 and the delayed addition recovery coefficient was only 0.2000. Therefore, the competitive adsorption compensation liquid was increased by 5 percentage points, and the immediate dispersion mother liquor was increased by 3 percentage points. A total of 8 percentage points were deducted from the intermediate and late-term slow-release mother liquors. The deduction amount was allocated according to the original ratio of 28:22, and after integerization, it was obtained as 48:24:18:10.
[0049] For sample Q2, 10 percentage points were transferred from the immediate dispersion stock solution, with 30% allocated to the intermediate-release stock solution and 70% allocated to the late-release stock solution, resulting in a ratio of 35:31:29:5.
[0050] For sample Q3, the target gap in the intermediate stage is: The medium-time slow-release mother liquor increased by 7 percentage points, and the increase was entirely transferred from the instantaneous dispersion mother liquor, resulting in a ratio of 38:35:22:5.
[0051] For sample Q4, the target gap in the later stage is The proportion of the slow-release mother liquor increased by 8 percentage points, of which 75% was transferred from the immediate dispersion mother liquor and 25% was transferred from the intermediate slow-release mother liquor, resulting in a ratio of 39:26:30:5.
[0052] For sample Q5, 7 percentage points were transferred from the delayed-release mother liquor, of which approximately 71% was allocated to the immediate dispersion mother liquor and the remainder to the intermediate-release mother liquor, resulting in a ratio of 50:30:15:5.
[0053] For sample Q6, keeping the relative ratio of the four mother liquors constant at 45:28:22:5, the amount of water-reducing agent liquid added was increased by 5% from 1.20wt% of the cementitious material mass to obtain 1.26wt%. The adjustment results for each sample are shown in Table 5 below.
[0054] Table 5: Effective Solid Proportion and Total Dosage Corresponding to Mismatch Types Taking sample Q1 as an example, when the mass of cementitious material in each cubic meter of concrete is 480 kg, and the mass of liquid water-reducing agent added is 1.20 wt% of the mass of cementitious material, the planned total mass of liquid water-reducing agent to be added is 5.76 kg. Considering that the solid content of A, B, and C is 40 wt%, and the solid content of D is 35 wt%, the liquid mass ratio of 48:24:18:10 is not directly used for weighing on-site. Instead, the liquid mass is first calculated based on the target effective solid ratio and the solid content of each mother liquor, and then the output of the four metering interfaces is normalized so that the actual effective solid ratio of the four mother liquors meets the 48:24:18:10 ratio. This avoids the situation where the solid content of mother liquor D is lower than that of other mother liquors, resulting in insufficient effective solids due to competitive adsorption compensation when directly proportioned by liquid mass.
[0055] Example 5 The purpose of this embodiment is to conduct verification. Verification water-reducing agent samples are prepared according to the on-site mixing ratios in Table 5, and verification concrete is prepared using the same actual raw materials, mix proportions, mixing procedures, and testing times as in Example 2. During the verification phase, the initial, intermediate, and later spread are recorded, and bleeding, segregation, and setting anomalies are observed. When the spread at all three testing times is within the corresponding target range, and no visible bleeding bands, coarse aggregate accumulation, or obvious segregation appear in the concrete, the current on-site mixing ratio is output; otherwise, the mismatch type is re-determined based on the verification results, and the next effective solids component transfer is performed.
[0056] In this embodiment, the initial target range was set to 630–670 mm, the intermediate target range to 580–620 mm, and the final target range to 500–540 mm. The verification results after adjustment of six samples are shown in Table 6 below.
[0057] Table 6: Verification of the flow properties of concrete after conditioning Table 6 shows that Q1, without increasing the total liquid content, achieved the target expansion range in the initial, intermediate, and later stages by increasing the proportion of competitive adsorption compensation liquid and instantaneous dispersion mother liquor, indicating that this sample does not require further increase in the sustained-release mother liquor or total content. Q2, by shifting some of the effective solids component of the instantaneous dispersion mother liquor later, reduced the initial excess and improved the later expansion. Q3 and Q4 improved the performance of the corresponding stages by increasing the intermediate and late-stage sustained-release mother liquors, respectively. Q5, by shifting some components of the late-stage sustained-release mother liquor earlier, improved the initial deficiency and prevented the later expansion from continuing to increase. Q6, only after confirming that all three detection times were insufficient and early competitive adsorption was not significant, increased the total content to avoid treating all slump losses by increasing the total amount.
[0058] To limit the risks of repeated on-site mixing, the effective solids content should not be transferred more than three times in a single on-site mixing. After each transfer, the cumulative effective solids mass of the four mother liquors and the cumulative amount of water-reducing agent added relative to the cementitious material should be recalculated. Automatic mixing should be stopped and manual verification should be initiated when the proportion of any mother liquor exceeds the range defined in the claims, the total liquid added mass exceeds 2.5 wt% of the cementitious material mass, obvious bleeding and segregation of the concrete is verified, or the target range cannot be met simultaneously at the three testing times after three consecutive adjustments. This is to check for incorrect addition of raw materials, abnormal moisture content, weighing device deviation, or abnormal compatibility between the water-reducing agent and the cementitious material.
[0059] In short-term construction scenarios where the estimated transport time does not exceed 30 minutes and there is no long waiting time for pumping, the initial detection time is preferably 5 minutes after mixing is completed, the intermediate detection time is preferably 30 minutes, and the final detection time is preferably 90 minutes. In conventional pumping scenarios where the estimated transport time is 30-75 minutes, the initial detection time is preferably 8 minutes after mixing is completed, the intermediate detection time is preferably 45 minutes, and the final detection time is preferably 105 minutes. In long-term construction scenarios where the estimated transport time exceeds 75 minutes or the estimated waiting time exceeds 30 minutes, the initial detection time is preferably 10 minutes after mixing is completed, the intermediate detection time is preferably 60 minutes, and the final detection time is preferably 120 minutes. All of the above detection times fall within the ranges of 5-10 minutes, 30-60 minutes, and 90-120 minutes as defined in the claims.
[0060] After the testing time is selected based on the estimated transportation and waiting time, the three target flow performance ranges are determined by the construction mix design notification and pumping requirements. On-site mixing only changes the effective solid distribution of the four mother liquors or adjusts the total admixture if the total effective admixture is insufficient, without restoring flow performance by adding additional water, thereby avoiding the impact of water-cement ratio changes on concrete strength and durability.
[0061] The above embodiments are used to illustrate the technical solutions of the present invention, and are not intended to limit the scope of protection of the present invention. Those skilled in the art can adapt and adjust the specific polycarboxylic acid structure, clay adsorption inhibitor type, detection time, weight, and threshold of each mother liquor without departing from the core concept of the present invention, but the technical relationship of independent storage of the four functional mother liquors, differential detection of dual samples with the same total effective solids, determination of three coefficients, and directional transfer of effective solids components according to mismatch type should still be maintained.
Claims
1. A slump-retaining slow-release water-reducing agent, characterized in that: The slump-preserving slow-release water-reducing agent is composed of an immediate dispersion mother liquor, a mid-term slow-release mother liquor, a late-term slow-release mother liquor, and a competitive adsorption compensation liquid. The immediate dispersion mother liquor, the mid-term slow-release mother liquor, the late-term slow-release mother liquor, and the competitive adsorption compensation liquid are stored independently. The instant dispersion mother liquor is used to provide water reduction and dispersion in the initial stage of concrete mixing, the intermediate-time slow-release mother liquor is used to provide water reduction and dispersion in the concrete transportation and holding stage, and the late-time slow-release mother liquor is used to provide water reduction and dispersion in the concrete waiting, pumping or pouring stage. The competitive adsorption compensating liquid is used to reduce the competitive adsorption of effective components in the instant dispersion mother liquor, intermediate-time slow-release mother liquor and late-time slow-release mother liquor by cementitious materials and fine aggregate powder. With a total effective solid mass of 100 parts in the immediate dispersion mother liquor, intermediate-time slow-release mother liquor, late-time slow-release mother liquor, and competitive adsorption compensation liquid, the effective solid mass of the immediate dispersion mother liquor is 35-50 parts, the effective solid mass of the intermediate-time slow-release mother liquor is 20-35 parts, the effective solid mass of the late-time slow-release mother liquor is 15-30 parts, and the effective solid mass of the competitive adsorption compensation liquid is 3-10 parts. When the slump-retaining slow-release water-reducing agent is applied to concrete, the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor and the competitive adsorption compensation liquid are mixed into a uniform and stable liquid mixture according to the on-site mixing results of the concrete to be constructed. The added mass of the liquid mixture is 0.5 to 2.5 wt% of the total mass of cementitious materials in the concrete to be constructed.
2. The slump-retaining slow-release water-reducing agent according to claim 1, characterized in that: The instant dispersion mother liquor comprises an instant dispersion polycarboxylate superplasticizer and water, and the solid content of the instant dispersion mother liquor is 35-50 wt%. The instant-dispersible polycarboxylate superplasticizer has carboxyl structural units and polyether side chain structural units in an unprotected state. In an alkaline simulated pore liquid with a temperature of 20±2℃ and a pH of 12.3~12.7, the effective carboxyl release time of the instant-dispersible polycarboxylate superplasticizer does not exceed 15 minutes. The effective carboxyl group release half-time refers to the time when the effective carboxyl group release of the instant-dispersible polycarboxylate superplasticizer reaches 50% of the cumulative effective carboxyl group release over 120 minutes.
3. The slump-retaining slow-release water-reducing agent according to claim 1, characterized in that: The medium-time slow-release mother liquor comprises a first slow-release polycarboxylate superplasticizer and water, and the solid content of the medium-time slow-release mother liquor is 35-50 wt%. The first slow-release polycarboxylate superplasticizer includes a first hydrolyzable protective structure that can hydrolyze to form carboxyl groups in an alkaline environment of concrete. In an alkaline simulated pore liquid at a temperature of 20±2℃ and a pH of 12.3 to 12.7, the effective carboxyl group release time of the first slow-release polycarboxylate superplasticizer is 30 to 60 minutes.
4. The slump-retaining slow-release water-reducing agent according to claim 3, characterized in that: The post-release mother liquor comprises a second-release polycarboxylate superplasticizer and water, and the solid content of the post-release mother liquor is 35-50 wt%. The second slow-release polycarboxylate superplasticizer includes a second hydrolyzable protective structure that can hydrolyze to form carboxyl groups in an alkaline environment of concrete. In an alkaline simulated pore liquid at a temperature of 20±2℃ and a pH of 12.3 to 12.7, the effective carboxyl group release time of the second slow-release polycarboxylate superplasticizer is 70 to 120 minutes. The hydrolysis rate of the second hydrolyzable protective structure is less than that of the hydrolyzable protective structure.
5. The slump-retaining slow-release water-reducing agent according to claim 1, characterized in that: The competitive adsorption compensating liquid comprises clay adsorption inhibitor, fine powder dispersant and water; The competitive adsorption compensation solution comprises, by weight: 15-40 parts of clay adsorption inhibitor; 5-20 parts of fine powder dispersant; 40-80 parts water; The clay adsorption inhibitor is at least one of quaternary ammonium salt type clay inhibitor, cationic polymer type clay inhibitor, and amphoteric polymer type clay inhibitor. The fine powder dispersant is at least one of low molecular weight polycarboxylic acid dispersant, polyphosphate dispersant, and sulfonate dispersant.
6. A method for preparing a slump-retaining slow-release water-reducing agent, applied to the slump-retaining slow-release water-reducing agent according to claim 1, characterized in that: The preparation method of the slump-retaining slow-release water-reducing agent includes: The immediate dispersion mother liquor, the intermediate sustained-release mother liquor, and the late sustained-release mother liquor were obtained respectively, and the solid content of the three mother liquors was adjusted so that the difference in solid content among the three mother liquors did not exceed 5 percentage points. According to the weight parts of each raw material in the competitive adsorption compensation liquid, clay adsorption inhibitor and fine powder dispersant are added to water and stirred at a stirring rate of 200-500 rpm for 20-60 minutes to obtain a uniform and stable competitive adsorption compensation liquid. The immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competitive adsorption compensation liquid are respectively placed into independent storage containers, and metering interfaces for outputting the corresponding mother liquor are set up to obtain the slump-preserving slow-release water-reducing agent.
7. The method for preparing a slump-retaining slow-release water-reducing agent according to claim 6, characterized in that: The immediate dispersion mother liquor, intermediate-time sustained-release mother liquor, late-time sustained-release mother liquor, and competitive adsorption compensation solution are obtained through on-site preparation methods, specifically including the following steps: S1. Obtain the actual cementitious materials, aggregates, and mixing water used in the concrete to be constructed, and obtain the specific surface area data of the cementitious materials, the mud content data and methylene blue value of the aggregates, the ambient temperature, the estimated transportation time, the estimated waiting time, and the target flow performance range corresponding to different construction times. S2. Mix the instantaneous dispersion mother liquor, intermediate slow-release mother liquor, late slow-release mother liquor and competitive adsorption compensation liquid according to the preset basic mixing ratio to prepare a basic water-reducing agent sample; S3. Prepare a single-addition sample and a segmented-addition sample using the cementitious materials, aggregates and mixing water actually used in the concrete to be constructed, so that the total effective solid content of the base water-reducing agent sample in the single-addition sample and the segmented-addition sample is the same. Wherein, the single-addition sample is the addition of all the basic water-reducing agent sample at the initial stage of mixing, and the segmented addition sample is the addition of 70% to 85% of the total effective solid mass of the basic water-reducing agent sample at the initial stage of mixing, with the remaining 15% to 30% added at intermediate testing points; S4. Obtain the actual flow performance data of the single-addition sample and the segmented-addition sample at the initial detection time, intermediate detection time and later detection time, respectively; S5. Determine the early adsorption consumption coefficient based on the specific surface area data of the cementitious material, the methylene blue value of the aggregate, and the actual flow performance changes of the single-addition sample at the initial and intermediate detection times. The delayed addition recovery coefficient is determined based on the difference in actual flow performance between the single-addition sample and the segmented-addition sample at the later detection time and the gap in the later target flow performance. The release timing migration coefficient is determined based on the direction and amount of deviation of the single-added sample from the corresponding target flow performance range at the initial and later detection times. S6. Determine the water-reducing agent mismatch type based on the early adsorption consumption coefficient, delayed addition recovery coefficient, and release time migration coefficient. S7. Based on the type of water-reducing agent mismatch, under the condition that the total effective solid mass of the functional components of the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competing adsorption compensation liquid remains unchanged, transfer the effective solid content of at least one mother liquor to another mother liquor, or increase the effective solid content of the competing adsorption compensation liquid, and determine the on-site mixing ratio. S8. Prepare verification water-reducing agent samples according to the on-site mixing ratio, and use the verification water-reducing agent samples to prepare verification concrete. Obtain the actual flow performance data of the verification concrete at each test time. When the actual flow performance data at each test time meets the corresponding target flow performance range, output the on-site mixing ratio.
8. The method for preparing a slump-retaining slow-release water-reducing agent according to claim 7, characterized in that: The initial testing time is 5 to 10 minutes after the concrete is mixed; the intermediate testing time is 30 to 60 minutes after the concrete is mixed; and the later testing time is 90 to 120 minutes after the concrete is mixed. Actual flow performance data includes at least one of collapse and spread; The early adsorption consumption coefficient was determined based on the following data: The relative flow performance loss of a single sample from the initial detection time to the intermediate detection time; The ratio of aggregate methylene blue value to the methylene blue baseline value; The ratio of the specific surface area of a cementitious material to its reference specific surface area; The delayed addition recovery coefficient is determined based on the proportion of the difference in actual flow performance between the segmented addition sample and the single addition sample at the later detection time to the gap in the target flow performance of the single addition sample in the later stage. The release time migration coefficient is determined based on the difference between the relative flow performance deviation of a single-added sample at the initial detection time and the relative flow performance deviation at subsequent detection times.
9. A method for preparing a slump-retaining slow-release water-reducing agent according to claim 7, characterized in that: When the early adsorption consumption coefficient is not less than the second adsorption threshold and the delayed addition recovery coefficient is less than the recovery threshold, the water-reducing agent mismatch type is determined to be the early competitive adsorption type. When the delayed addition recovery coefficient is not less than the recovery threshold and the release time migration coefficient is not less than the positive migration threshold, the water-reducing agent mismatch type is determined to be the release time advance type. When the actual flow performance data at the initial detection time meets the corresponding target flow performance range, the actual flow performance data at the intermediate detection time is lower than the corresponding target flow performance range, and the release time migration coefficient is between the negative migration threshold and the positive migration threshold, the water-reducing agent mismatch type is determined to be the medium-time release insufficiency type. When the actual flow performance data at the initial and intermediate detection times meet the corresponding target flow performance range, the actual flow performance data at the later detection times are lower than the corresponding target flow performance range, and the delayed addition recovery coefficient is not less than the recovery threshold, the water-reducing agent mismatch type is determined to be the late release insufficient type. When the release time migration coefficient is not greater than the negative migration threshold, the actual flow performance data at the initial detection time is lower than the corresponding target flow performance range, and the actual flow performance data at the later detection time meets or exceeds the corresponding target flow performance range, the water-reducing agent mismatch type is determined to be the release time lag type. When the actual flow performance data at all three detection times are lower than the corresponding target flow performance range, and the early adsorption consumption coefficient is less than the first adsorption threshold, the water-reducing agent mismatch type is determined to be insufficient total effective dosage. The first adsorption threshold is less than the second adsorption threshold.
10. The method for preparing a slump-retaining slow-release water-reducing agent according to claim 9, characterized in that: When the mismatch type of the water-reducing agent is early competitive adsorption type, the mass percentage of the competitive adsorption compensation liquid in the total effective solid mass of the four components is increased by 3 to 8 percentage points, the mass percentage of the immediate dispersion mother liquor in the total effective solid mass of the four components is increased by 2 to 5 percentage points, and the corresponding effective solid content is deducted from the intermediate and late slow-release mother liquors according to the effective solid mass ratio of the intermediate and late slow-release mother liquors before preparation. When the mismatch type of the water-reducing agent is the early release time type, 5 to 12 percent of the total effective solids of the four components are transferred out from the immediate dispersion mother liquor. 20% to 40% of the transferred effective solids are allocated to the intermediate slow-release mother liquor, and 60% to 80% of the transferred effective solids are allocated to the late slow-release mother liquor. When the water-reducing agent mismatch type is the medium-time release deficiency type, the mass percentage of the medium-time slow-release mother liquor in the total effective solid mass of the four components increases by 4 to 10 percentage points, and the corresponding effective solid content is preferentially deducted from the immediate dispersion mother liquor. When the mismatch type of the water-reducing agent is the insufficient release type, the mass percentage of the slow-release mother liquor in the total effective solids of the four components increases by 6 to 15 percentage points. Of the increased effective solids, 60% to 80% is transferred out by the immediate dispersion mother liquor, and the remaining effective solids are transferred out by the intermediate slow-release mother liquor. When the mismatch type of the water-reducing agent is the delayed release type, 4 to 10 percent of the total effective solids of the four components are transferred from the delayed-release mother liquor. 60% to 80% of the transferred effective solids are allocated to the immediate dispersion mother liquor, and the remaining transferred effective solids are allocated to the intermediate-release mother liquor. When the mismatch type of water-reducing agent is insufficient total effective dosage, the effective solid mass ratio among the immediate dispersion mother liquor, the intermediate slow-release mother liquor, the late slow-release mother liquor, and the competing adsorption compensation liquid should be kept constant, so that the total effective solid addition of water-reducing agent relative to the total mass of cementitious material increases by 3% to 8%; After each transfer of effective solids or adjustment of total effective solids addition, a new water-reducing agent sample and a new concrete sample are prepared for verification. The number of times effective solids are transferred in a single on-site mixing process shall not exceed three.