Sound-absorbing noise-reducing rubber asphalt mixture and preparation method and application thereof
By modifying asphalt with waste tire rubber powder and designing specific gradations, a sound-absorbing and noise-reducing rubber asphalt mixture was prepared. This solved the problem of synergistic effect between noise reduction and road performance in tunnel environments, improved the skid resistance and durability of tunnel pavements, and achieved comprehensive performance improvement through multi-objective optimization.
Patent Information
- Application Number
- CN202611535175.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-20
AI Technical Summary
Existing rubber-modified asphalt mixtures are difficult to achieve a synergy between noise reduction and road performance in tunnel environments. Their anti-skid performance deteriorates rapidly, they lack a comprehensive performance evaluation system, and they are prone to rutting, cracking, water damage, and other defects in tunnel environments.
Waste tire rubber powder is used to modify asphalt, which is combined with coarse aggregate, fine aggregate and mineral powder of specific gradation to form a highly elastic network structure and interconnected pores. Through shear swelling and gradation design, sound-absorbing and noise-reducing rubber asphalt mixture is prepared to enhance high-temperature rutting resistance, sound absorption and noise reduction, long-term skid resistance and water stability.
It achieves excellent sound absorption and noise reduction, long-term anti-slip effect, high temperature stability and water stability in tunnel environment, improves the overall performance of the material and extends its service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of road materials technology, specifically relating to a sound-absorbing and noise-reducing rubber asphalt mixture, its preparation method, and its application. Background Technology
[0002] Asphalt pavement is the main form of tunnel paving. The tunnel environment has significant unique characteristics: the semi-enclosed space causes vehicle noise to be constantly reflected by the tunnel walls and ceiling, creating a noticeable reverberation phenomenon, and noise pollution is more severe than in open road sections; at the same time, vehicles frequently brake and accelerate inside the tunnel, and the road surface is subjected to high temperatures and heavy traffic loads for a long time, making it prone to rutting, cracking and other defects; in addition, the tunnel environment is often accompanied by groundwater seepage, road surface washing and surface condensation due to poor ventilation. After moisture penetrates into the pavement, under the coupled effect of vehicle dynamic loads and temperature differences, it can easily cause water damage such as asphalt film peeling and loosening.
[0003] The existing technology has the following problems: Noise reduction and road performance are difficult to coordinate: The design of existing rubber-modified asphalt mixtures mainly focuses on mechanical properties, and the gradation design is mainly based on compactness and durability, resulting in low porosity and insufficient sound absorption and noise reduction performance; on the other hand, simply increasing the porosity to enhance the noise reduction effect may sacrifice water stability and durability.
[0004] Rapid decay of anti-skid performance: Frequent braking of vehicles in tunnels causes the surface texture of the road surface to decay rapidly under repeated wear from wheel loads. The fine aggregate suspension and dense structure of existing mixtures is difficult to maintain long-term anti-skid performance, and the surface is prone to "polishing" phenomenon.
[0005] There is a lack of a comprehensive performance evaluation system for tunnel environments: existing evaluation methods mostly examine single performance aspects separately, and there is a lack of a systematic approach that integrates noise reduction, anti-skid properties, high-temperature stability, low-temperature crack resistance, and water stability for multi-objective synergistic optimization. Summary of the Invention
[0006] In view of this, the purpose of the present invention is to provide a sound-absorbing and noise-reducing rubber asphalt mixture, its preparation method and application. The sound-absorbing and noise-reducing rubber asphalt mixture provided by the present invention has excellent sound absorption and noise reduction performance, long-term anti-skid performance, high temperature stability, low temperature crack resistance and water stability, and can be used for a long time.
[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a sound-absorbing and noise-reducing rubber asphalt mixture, the raw materials of which include base asphalt, waste tire rubber powder, coarse aggregate, fine aggregate and mineral powder; The mass of the base asphalt accounts for 4.0 to 6.5% of the total mass of the coarse and fine aggregates.
[0008] Preferably, the waste tire rubber powder is rubber powder obtained by crushing waste tires; the mass of the waste tire rubber powder is 15-25% of the mass of the base asphalt.
[0009] Preferably, the fineness of the waste tire rubber powder is 20-80 mesh.
[0010] Preferably, the coarse aggregate has a particle size ≥ 2.36 mm and ≤ 16.00 mm; the fine aggregate has a particle size > 0.075 mm and < 2.36 mm.
[0011] Preferably, the mineral powder is finely ground limestone powder with a particle size ≤0.075mm.
[0012] Preferably, the coarse aggregate, fine aggregate and mineral powder adopt a continuous dense gradation AC-13 type, wherein the 4.75mm sieve aperture has a passing rate of 25~35%, the 2.36mm sieve aperture has a passing rate of 20~28%, and the 0.075mm sieve aperture has a passing rate of 4~7%.
[0013] Preferably, the mass ratio of the coarse aggregate, fine aggregate and mineral powder is 75~85:8~21:4~7.
[0014] This invention also provides a method for preparing the sound-absorbing and noise-reducing rubber asphalt mixture described in the above technical solution, comprising the following steps: After heating the base asphalt, waste tire rubber powder is added and shear swelling is performed to obtain rubber-modified asphalt. After mixing coarse and fine aggregates and heating them a second time, dry mixing is performed. The rubber-modified asphalt is added to the resulting dry mixture and then preheated mineral powder is added and mixed again. The resulting material is the sound-absorbing and noise-reducing rubber asphalt mixture.
[0015] Preferably, the shear rate of the shear swelling is 3000~5000 r / min, and the time is 30~90 min.
[0016] The present invention also provides the application of the sound-absorbing and noise-reducing rubber asphalt mixture described in the above technical solution or the sound-absorbing and noise-reducing rubber asphalt mixture prepared by the preparation method described in the above technical solution in tunnel pavement.
[0017] This invention provides a sound-absorbing and noise-reducing rubber asphalt mixture, the raw materials of which include base asphalt, waste tire rubber powder, coarse aggregate, fine aggregate and mineral powder; The mass of the base asphalt accounts for 4.0 to 6.5% of the total mass of the coarse and fine aggregates.
[0018] Beneficial effects: 1. Significantly improved high-temperature rutting resistance Waste tire rubber powder fully swells in the base asphalt to form a highly elastic three-dimensional network structure, significantly enhancing the high-temperature viscoelasticity and recovery ability of the base asphalt mastic; coarse aggregate forms a good skeleton support, providing greater internal friction.
[0019] 2. Excellent sound absorption and noise reduction performance The high porosity generated by the gradation of coarse aggregate, fine aggregate and mineral powder forms a connected pore structure, providing ample connecting channels and internal space for sound waves, so that sound energy is efficiently dissipated through friction and viscosity; the sound absorption coefficient in the mid-frequency range (160~800Hz) is stable at 0.15~0.18.
[0020] 3. Excellent long-lasting anti-slip performance The coarse aggregate, fine aggregate, and mineral powder gradation form a coarse skeleton structure. The coarse aggregate forms a strongly interlocked macro skeleton that can resist the loss of texture caused by load. The road surface forms a "deep valley-peak" synergistic micro texture with a high texture distribution density.
[0021] 4. Enhanced water stability Waste tire rubber powder increases the viscosity and interfacial adhesion of asphalt mastic. Waste tire rubber powder modifies asphalt to form a thicker asphalt film, effectively preventing water from penetrating to the aggregate surface. Waste tire rubber powder also improves the interfacial adhesion of asphalt to aggregate through shearing and swelling.
[0022] 5. Improved low-temperature crack resistance After the waste tire rubber powder particles swell, they form a highly elastic network structure inside the mixture, giving the material excellent stress relaxation ability, effectively inhibiting the generation and propagation of microcracks at low temperatures, increasing flexural strain by 42.4%, and reducing stiffness modulus. Detailed Implementation
[0023] This invention provides a sound-absorbing and noise-reducing rubber asphalt mixture, the raw materials of which include base asphalt, waste tire rubber powder, coarse aggregate, fine aggregate and mineral powder; The mass ratio of the base asphalt to the total mass of the coarse and fine aggregates (asphalt-aggregate ratio) is 4.0 to 6.5%.
[0024] Unless otherwise specified, the present invention does not have special requirements on the source of raw materials used, and commercially available products well known to those skilled in the art can be used.
[0025] In one embodiment, the base asphalt is road petroleum asphalt.
[0026] In one embodiment, the waste tire rubber powder is rubber powder obtained by crushing waste tires, and is used as a modifier; the mass of the waste tire rubber powder is 15-25% of the mass of the base asphalt, and in a specific embodiment it is 20%; the fineness of the waste tire rubber powder is 20-80 mesh, and in a specific embodiment it is 80 mesh.
[0027] In one embodiment, the coarse aggregate is diabase; the particle size of the coarse aggregate is ≥2.36mm and ≤16.00mm; the fine aggregate is diabase; the particle size of the fine aggregate is >0.075mm and <2.36mm; the mineral powder is finely ground limestone powder with a particle size ≤0.075mm; the mass ratio of the coarse aggregate, fine aggregate and mineral powder is 75~85:8~21:4~7, and in specific embodiments it is 77.2:17.8:5.0, 81.4:13.6:5, 80.3:14.2:5.5 or 76.8:16.8:6.4.
[0028] In one embodiment, the mass ratio of the base asphalt to the total mass of the coarse and fine aggregates (asphalt-aggregate ratio) is 4.0-6.5%, and in specific embodiments it is 5.2%, 5.4% or 5.6%.
[0029] In one implementation, the coarse aggregate, fine aggregate, and mineral powder adopt a continuous dense gradation type AC-13, wherein the passing rate of the 4.75mm sieve is 25-35%, specifically 29.5% in this embodiment; the passing rate of the 2.36mm sieve is 20-28%, specifically 22.8% in this embodiment; and the passing rate of the 0.075mm sieve is 4-7%, specifically 5.0% in this embodiment. The passing rates of the key sieves are shown in Table 1. Table 1. Gradation of coarse aggregate, fine aggregate, and mineral powder
[0030] Structural features: Compared with conventional AC-13 gradation, the gradation of the present invention significantly reduces the passing rate of 4.75mm and 2.36mm sieves, and controls the passing rate of 9.5mm sieves at a low level, forming a coarse aggregate skeleton interlocking structure.
[0031] This invention proposes a sound-absorbing and noise-reducing rubber asphalt mixture for tunnel environments and its preparation method. Through a systematic study of the effects of rubber powder modification parameters (dosage, fineness, swelling time) and gradation structure (AC13-1, AC13-2, AC13-3) on the multi-dimensional performance of the mixture, the optimal solution was selected, with AC13-1 gradation + 20% rubber powder dosage + 80-mesh rubber powder fineness as the core. This solution, while ensuring excellent road performance (high temperature, low temperature, water stability), achieves synergistic optimization of noise reduction and long-term skid resistance in tunnel environments, providing a material design basis for tunnel rubber asphalt pavement projects.
[0032] In one embodiment, the bulk density of the sound-absorbing and noise-reducing rubber asphalt mixture is 2.544~2.575 g / cm³. 3 In the specific embodiment, it is 2.570 g / cm³. 3The void ratio (VV) is 4.0~6.5%, with 5.18% in the specific embodiment; the aggregate void ratio (VMA) is 18.74~19.29%, with 18.74% in the specific embodiment; and the bitumen saturation (VFA) is 63.78~85.53%, with 74.35% in the specific embodiment.
[0033] This invention also provides a method for preparing the sound-absorbing and noise-reducing rubber asphalt mixture described in the above technical solution, comprising the following steps: After heating the base asphalt, waste tire rubber powder is added and shear swelling is performed to obtain rubber-modified asphalt. After mixing coarse and fine aggregates and heating them a second time, dry mixing is performed. The rubber-modified asphalt is added to the resulting dry mixture and then preheated mineral powder is added and mixed again. The resulting material is the sound-absorbing and noise-reducing rubber asphalt mixture.
[0034] This invention involves heating the base asphalt, adding waste tire rubber powder, and then shearing and swelling it to obtain rubber-modified asphalt.
[0035] In one embodiment, the first heating is to 160~180℃, specifically 165~175℃; the shear rate of the shear swelling is 3000~5000r / min, specifically 3500~4500r / min, and the time is 30~90min, specifically 60min.
[0036] In this invention, coarse aggregate and fine aggregate are mixed and heated, then dry-mixed. The resulting dry-mixed material is then mixed with the rubber-modified asphalt, and preheated mineral powder is added and mixed again. The final product is the sound-absorbing and noise-reducing rubber asphalt mixture.
[0037] In one embodiment, the second heating is to 160~190℃, specifically 165~175℃; the dry mixing time is 5~15s, specifically 5~10s; the mixing time is 45~90s, specifically 50~90s; the preheating temperature is 160~190℃, specifically 165~175℃; the continued mixing time is 45~90s, specifically 50~90s; and the discharge temperature is controlled at 160~175℃, specifically 170℃.
[0038] The present invention also provides the application of the sound-absorbing and noise-reducing rubber asphalt mixture described in the above technical solution or the sound-absorbing and noise-reducing rubber asphalt mixture prepared by the preparation method described in the above technical solution in tunnel pavement.
[0039] In one embodiment, the tunnel pavement is prepared by laying the sound-absorbing and noise-reducing rubber asphalt mixture on the pavement and then molding it; the molding method is wheel rolling or Marshall compaction; the molding temperature is not lower than 150°C, and in a specific embodiment it is 175°C.
[0040] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention, but they should not be construed as limiting the scope of protection of the present invention.
[0041] Example The preparation method of sound-absorbing and noise-reducing rubber asphalt mixture is as follows: Step 1: Preparation of Rubber-Modified Asphalt The base asphalt was heated to 180℃, and 20% of the waste tire rubber powder (20-80 mesh) was added. The mixture was then subjected to high-speed shearing and swelling at a shear rate of 5000 r / min for 60 min to prepare rubber-modified asphalt. Step 2: Material preparation Prepare coarse aggregate (diabase), fine aggregate (diabase) and mineral powder according to the gradation requirements, and heat the aggregates to 190℃ respectively; Step 3: Mixing the ingredients Add the heated coarse and fine aggregates to the mixing pot and dry mix for 5 seconds; then add the rubber-modified asphalt and mix for 90 seconds; then add the preheated mineral powder and continue mixing for 90 seconds; the discharge temperature is controlled at 175℃. Step 4: Molding Standard specimens (rutted plates or Marshall specimens) were obtained by using wheel rolling or Marshall compaction molding at a molding temperature of 165℃. Step 5: Performance Testing The following performance tests were performed on the molded specimens: ① Volume index testing (porosity, density, etc.) ② High-temperature stability test (60℃ rutting test) ③ Low-temperature crack resistance test ④ Water stability test (freeze-thaw splitting test) ⑤ Anti-skid performance test (wheel abrasion test + pendulum value + laser scanning) ⑥ Noise reduction performance test (tire drop method + standing wave tube sound absorption coefficient) The specific testing method is as follows: ① High-temperature stability test (60℃ rutting test) Test basis: "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) T0719 "Rutting Test of Asphalt Mixtures" Test conditions: Temperature controlled at 60℃; Test procedure: Prepare standard rut plate specimens; The cyclic action of vehicle wheel load was simulated under a constant temperature of 60℃. The deformation d1 and d2 of the specimen were measured at 45 min and 60 min. Calculate the dynamic stability DS=(t2-t1)×N / (d2-d1), where N is the test wheel's reciprocating rolling speed (usually 42 times / min), t1=45min, and t2=60min.
[0042] Test indicators: dynamic stability DS (times / mm), deformation amount in the 45~60min stage.
[0043] ② Low-temperature crack resistance test Test standard: "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011) T0715; Test procedure: Prepare standard small beam specimens (typically 250mm × 30mm × 35mm); Three-point bending loading was performed under low-temperature conditions; The tensile strength RB, maximum tensile strain εB, and stiffness modulus SB of the specimen were determined. Test parameters: flexural tensile strength RB (MPa), maximum flexural strain εB (με), stiffness modulus SB (KPa).
[0044] ③ Water stability test (freeze-thaw splitting test) Test standard: Test procedures for asphalt and asphalt mixtures in highway engineering (JTG E20-2011) T0729; Test steps: Unfrozen group: Prepare standard Marshall specimens; keep them in a constant temperature water bath at 25℃ for 2 hours; conduct splitting test and determine the splitting tensile strength RT1.
[0045] Freeze-thaw group: Prepare standard Marshall specimens; vacuum saturate with water (vacuum degree 97.3 kPa, hold for 15 min); freeze at -18℃ for 16 h; thaw in a constant temperature water bath at 60℃ for 24 h; keep warm in a constant temperature water bath at 25℃ for 2 h; conduct splitting test and determine splitting tensile strength RT2.
[0046] Calculation index: Freeze-thaw splitting strength ratio (TSR) = (RT2 / RT1) × 100%.
[0047] ④ Anti-skid performance test (wheel abrasion test + pendulum value + laser scanning) 1. Wheel wear test Test conditions: Tire ground contact pressure: 0.7 MPa; Rotational speed: 75 r / min; Wear cycles: 0, 200, 500, 1000, 3000, 5000, 7000, 10000 cycles; Abrasion method: Abrasion with sand. Before each abrasion, divide 20g of sand into 8 equal parts and spread them evenly with a brush with a width of 5cm. Abrasive specifications: 0.25mm diameter corundum; Test procedure: Prepare standard rutted plate specimens; wear the surface of the specimens at different wear cycles (0~10000 cycles); take samples for testing at 0, 200, 500, 1000, 3000, 5000, 7000, and 10000 cycles respectively.
[0048] 2. Depth Testing (Sand Laying Method) Test method: The structural depth of the wheel track area was measured using simple tools such as a push plate, tracing paper and pencil; Test procedure: Weigh four portions of special sand material with the same mass and a particle size of 0.15~0.30mm; place the sand in the middle of the four sides of the wheel track; spread it evenly with a pusher to completely cover the wheel track; place tracing paper on the surface and trace the outline of the sand layer with a pencil; scan the sand layer outline image at a resolution of 300ppi for different wear cycles; use Photoshop's quick selection tool to delineate the sand layer area and read the pixel area through the histogram; complete the test in the four test areas (upper, lower, left, and right) of the wheel track in sequence, and take the average of the four results.
[0049] Calculation formula: TD = ρ · Sm Where: TD - structural depth, mm; m - mass of sand used in each test, g; ρ - bulk density of sand used for structural depth, g / cm³ 3 Take 1.63 g / cm 3 ; S-pixel area of the contour after the sand sample is flattened, in ppi 2 300ppi is 1 inch, or 2.54cm.
[0050] 3. Pendulum test Testing equipment: pendulum friction tester; Test steps: A shortened rubber sheet with dimensions of 6.35mm × 25.4mm × 31.75mm (standard dimensions are 6.35mm × 25.4mm × 76.2mm) was used. Pendulum values were measured at four locations to determine the structural depth, and the average of the four results was taken. The pavement temperature at the time of the test was t (°C), and the obtained pendulum value was... BPN t The pendulum value can be converted to the standard temperature of 20℃ using the following formula. BPN20 : BPN 20 = BPN t +Δ BPN: In the formula: ΔBPN is the temperature correction value, selected according to Table 2: Table 2 ΔBPN Values
[0051] 4. Texture Laser Scanning (PATT-II) Testing equipment: PATT-II road surface anti-skid texture tester; Test procedure: Laser scanning was performed using PATT-II equipment; the surface contour data of the specimen was processed using the texture data processing software provided with the equipment; nine indicators were calculated for the entire plate: mean texture depth (MTD), mean section depth (MPD), arithmetic mean deviation of the contour (Ra), root mean square deviation of the contour (Rq), root mean square slope of the contour (Δq), skewness (Rsk), steepness (Rku), macroscopic texture distribution density, and microscopic texture distribution density. This invention selects eight indicators, excluding Δq, for analysis.
[0052] Formulas for calculating each parameter: (1) Mean Tectonic Depth (MTD): MTD=(1 / N)×ΣH(x i ) In the formula: N - Total number of sampling points for cross-sectional profile; H(x i ) - Distance from each point on the contour to the peak line of the contour, mm.
[0053] (2) Mean section depth (MPD): MPD=(Max 1 +Max 2 ) / 2−Z(x i ) In the formula: Monkey 1 - Peak value 1; Monkey 2 - Peak value 2; Z(xi) - Average elevation of cross section, mm.
[0054] (3) Profile arithmetic mean deviation (Ra): Ra=(1 / N)×Σ|Z(x i )-Z̄| In the formula: Z(xi) - Elevation of sampling point, mm; Z̄ - Average elevation of cross section, mm.
[0055] (4) Root mean square deviation of profile (Rq): Rq=√[(1 / N)×Σ(Z(x i )-Z̄) 2 ] (5) Skewness (Rsk): Rsk=[1 / (Rq) 3 ]×(1 / N)×Σ(Z(x i )-Z̄) 3 (6) Steepness (Rku): Rku=[1 / (Rq) 4 ]×(1 / N)×Σ(Z(x i )-Z̄) 4 ⑤ Noise reduction performance test (tire drop method + standing wave tube sound absorption coefficient) 1. Tire drop test for noise Test principle: To simulate the excitation mechanism of road noise during actual driving in an indoor environment and evaluate the acoustic performance of materials. Experimental setup: Slope angle: 30°; Slope length: 100cm; Top elevation: 60cm; Height of the bottom of the slope from the ground: 10cm; Simulated impact source: a standard small passenger car tire weighing approximately 28 kg, with a tire pressure of 0.2 MPa; Measurement point layout: Equivalent near wheel position: 1m from the point of impact; At a point equivalent to half the width of a lane: 1.9m from the point of impact; At the equivalent single-lane width: 3.75m from the point of impact; Specimen Requirements: Standard rutting slabs must be prepared strictly in accordance with the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011); when testing 4cm thick single-layer rutting slabs, a wooden board must be placed underneath to ensure that the specimen surface is completely flush with the bottom of the slope. Test procedure: Roll the tire down the slope and impact the surface of the test specimen; set up sound level meters at each measuring point to collect sound pressure data; Record the peak sound level at each measuring point 2. Standing wave tube sound absorption coefficient test Test criteria: Relevant acoustic standards; Test equipment: Impedance tube test system, mainly including computer, data acquisition module, power amplifier, impedance tube and microphone; Test frequencies: 11 center frequencies of 1 / 3 octave band were selected, namely 160Hz, 200Hz, 250Hz, 315Hz, 400Hz, 500Hz, 630Hz, 800Hz, 1000Hz, 1250Hz and 1600Hz. Test steps: Prepare a standard sample and install it at the end of the impedance tube; By acquiring the signal transfer function of the microphone inside the impedance tube; The sound absorption coefficients of each asphalt mixture sample were calculated.
[0056] Table 3. Gradation of aggregates and mineral powder in each embodiment
[0057] Example 1: AC13-1 graded sound-absorbing and noise-reducing rubber asphalt mixture (optimal solution) Mixing ratio parameters: Waste tire rubber powder content: 20% (as a percentage of the base asphalt mass); Waste tire rubber powder fineness: 80 mesh; High-temperature shear swelling time: 60 min; Oil-stone ratio: 5.4%; Grading: AC13-1 (see Table 3 for the passing rate of each sieve aperture).
[0058] The experimental results are shown in Table 4: Table 4. Performance of the sound-absorbing and noise-reducing rubber asphalt mixture prepared in Example 1
[0059] The product physical properties are shown in Tables 5-8.
[0060] Table 5 Volumetric Parameters
[0061] Table 6 Mechanical and Durability Performance Indicators
[0062] Table 7 Anti-skid performance indicators (initial and after 10,000 cycles of wear)
[0063] Table 8 Noise Reduction Performance Indicators
[0064] Example 2: AC13-2 graded sound-absorbing and noise-reducing rubber asphalt mixture Mixing ratio parameters: Rubber powder content: 20%; Powder fineness: 80 mesh; High-temperature shear swelling time: 60 min; Oil-stone ratio: 5.6%; Gradation: AC13-2 (see Table 3 for gradation, 4.75mm passing rate 38.1%, 2.36mm passing rate 26.8%, fine aggregate content is higher than AC13-1).
[0065] The experimental results are shown in Table 9: Table 9. Performance of the sound-absorbing and noise-reducing rubber asphalt mixture prepared in Example 2
[0066] Example 3: AC13-3 graded sound-absorbing and noise-reducing rubber asphalt mixture Mixing ratio parameters: Rubber powder content: 20%; Powder fineness: 80 mesh; High-temperature shear swelling time: 60 min; Oil-stone ratio: 5.2%; Grading: AC13-3 (see Table 3).
[0067] The experimental results are shown in Table 10: Table 10 Performance of the sound-absorbing and noise-reducing rubber asphalt mixture prepared in Example 3
[0068] Comparative Example 1: Base Asphalt Mixture (Contrast with Existing Technology) Scheme: AC13-1 gradation, base asphalt (without rubber powder), asphalt-aggregate ratio 4.73%.
[0069] The experimental results are shown in Table 11: Table 11 Performance of the base asphalt mixture prepared in Comparative Example 1
[0070] This comparative example demonstrates that, without the addition of rubber powder, the high-temperature stability, low-temperature crack resistance, and water stability of the base asphalt mixture are significantly inferior to those of the rubber-modified asphalt mixture, and its low-temperature performance does not meet the specifications for polymer-modified asphalt mixtures in cold winter regions (εB < 2500 με).
[0071] Comparative Example 2: Control Test with Different Rubber Powder Content Solution: Using a fixed AC13-1 gradation and 80-mesh adhesive powder, compare the sound absorption performance at three dosages: 15%, 20%, and 25%. The experimental results (standing wave tube method, 630~800Hz mid-frequency band) are shown in Table 12: Table 12 Properties of matrix asphalt mixtures prepared with different rubber powder contents
[0072] This comparative example demonstrates that although the 15% dosage has the highest sound absorption coefficient, the 20% dosage provides better interfacial adhesion and overall damping and vibration reduction effect while maintaining good sound absorption capacity, and is therefore determined to be the optimal dosage of adhesive powder.
[0073] Comparative Example 3: Comparison Test of Different Powder Fineness Scheme: Fixed AC13-1 gradation, 20% rubber powder content, and comparison of four finenesses: 20 mesh, 40 mesh, 60 mesh, and 80 mesh; The experimental results (standing wave tube method, average sound absorption coefficient in the high-frequency range above 800Hz) are shown in Table 13: Table 13 Properties of matrix asphalt mixtures prepared with different rubber powder fineness
[0074] As shown in Table 13, 80-mesh adhesive powder, due to its extremely large specific surface area, can form a denser and more elastic damping network in the gaps between aggregates, increasing the tortuosity of the sound wave propagation path and causing high-frequency sound waves to generate stronger viscosity and heat loss on the pore wall.
[0075] This invention has been described in detail, but it is only a part of the embodiments of this invention and not all of the embodiments. People can obtain other embodiments based on this embodiment without creative intent, and these embodiments all fall within the protection scope of this invention.
Claims
1. A sound-absorbing and noise-reducing rubber asphalt mixture, characterized in that, The raw materials include base asphalt, waste tire rubber powder, coarse aggregate, fine aggregate, and mineral powder; The mass of the base asphalt accounts for 4.0 to 6.5% of the total mass of the coarse and fine aggregates.
2. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1, characterized in that, The waste tire rubber powder is rubber powder obtained by crushing waste tires; the mass of the waste tire rubber powder is 15-25% of the mass of the base asphalt.
3. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1 or 2, characterized in that, The fineness of the waste tire rubber powder is 20-80 mesh.
4. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1, characterized in that, The coarse aggregate has a particle size ≥ 2.36 mm and ≤ 16.00 mm; the fine aggregate has a particle size > 0.075 mm and < 2.36 mm.
5. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1, characterized in that, The mineral powder is finely ground limestone powder with a particle size ≤0.075mm.
6. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1, 4, or 5, characterized in that, The coarse aggregate, fine aggregate, and mineral powder adopt a continuous dense gradation AC-13 type, wherein the passing rate of the 4.75mm sieve is 25~35%, the passing rate of the 2.36mm sieve is 20~28%, and the passing rate of the 0.075mm sieve is 4~7%.
7. The sound-absorbing and noise-reducing rubber asphalt mixture according to claim 1, characterized in that, The mass ratio of coarse aggregate, fine aggregate and mineral powder is 75~85:8~21:4~7.
8. The method for preparing the sound-absorbing and noise-reducing rubber asphalt mixture according to any one of claims 1 to 7, characterized in that, Includes the following steps: After heating the base asphalt, waste tire rubber powder is added and shear swelling is performed to obtain rubber-modified asphalt. After mixing coarse and fine aggregates and heating them a second time, dry mixing is performed. The rubber-modified asphalt is added to the resulting dry mixture and then preheated mineral powder is added and mixed again. The resulting material is the sound-absorbing and noise-reducing rubber asphalt mixture.
9. The preparation method according to claim 8, characterized in that, The shear rate of the shear swelling is 3000~5000 r / min, and the time is 30~90 min.
10. The application of the sound-absorbing and noise-reducing rubber asphalt mixture according to any one of claims 1 to 7 or the sound-absorbing and noise-reducing rubber asphalt mixture prepared by the preparation method according to any one of claims 8 to 9 in tunnel pavement.