Organic solid waste hydrothermal waste liquid modified geopolymer-based cementitious material and preparation method thereof
By using a commercially available chemical alkali-free activator combined with humic acid modification, the problems of high cost and hydration inhibition in sludge hydrothermal wastewater treatment and geopolymer preparation were solved, realizing the preparation of low-carbon and environmentally friendly cementitious materials and improving the compressive strength and engineering application potential of the materials.
Patent Information
- Application Number
- CN202611309563.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-20
AI Technical Summary
In existing technologies, the treatment cost of sludge hydrothermal waste liquid is high, traditional geopolymer preparation relies on commercial chemical alkalis, and direct incorporation of waste liquid can easily lead to hydration inhibition. Existing research has failed to effectively utilize the modification value of organic matter on the gel structure of geopolymers.
Using a method without commercial chemical alkalis, the alkaline environment provided by carbide slag and the sulfate activation effect of desulfurized gypsum are utilized, combined with a specific amount of humic acid or humic-like products as modifiers, to synergistically activate the inorganic framework and guide the densification of hydration products, thus preparing a geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid.
It achieves low-cost, low-carbon emission disposal of sludge hydrothermal waste liquid, improves the compressive strength and hydration performance of geopolymer-based cementitious materials, broadens the application path of waste liquid in the building materials field, and has good industrial adaptability and large-scale prospects.
Smart Images

Figure CN123131084A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid and its preparation method. Background Technology
[0002] With the acceleration of urbanization, there is an urgent need for the harmless and resource-based disposal of organic solid waste such as municipal sludge. While high-temperature and high-pressure hydrothermal treatment (such as hydrothermal carbonization and hydrothermal liquefaction) can effectively reduce sludge volume and recover high-value solid products, this process generates large amounts of high-concentration hydrothermal wastewater with extremely high COD and ammonia nitrogen content, and is rich in humic substances and other large-molecule organic matter, as well as Maillard reaction products, exhibiting strong biochemical inhibition. Currently, the industry typically recycles this wastewater to sewage treatment plants, but its high toxicity and heavy load severely impact the microbial system, and the high treatment costs have become a bottleneck for the engineering application of hydrothermal technology.
[0003] On the other hand, geopolymers, as a type of low-carbon cementitious material, are mostly produced by alkaline activation using industrial solid wastes such as slag and fly ash as precursors. However, traditional preparation processes are highly dependent on chemical alkaline activators such as water glass and sodium hydroxide, and consume a large amount of purified water, which not only increases costs but also weakens the green and low-carbon attributes of geopolymers due to carbon emissions during the production process.
[0004] Currently, existing technologies for the treatment of sludge and hydrothermal wastewater and the preparation of novel geopolymer materials have the following objective limitations:
[0005] (1) The biochemical treatment of hydrothermal waste liquid is costly and limited in scale. It requires dilution or pretreatment and is difficult to dispose of in situ at low cost.
[0006] (2) Geopolymer preparation relies excessively on chemical alkalis and water purification, which is not economical and environmentally friendly.
[0007] (3) When organic macromolecules in waste liquid directly replace mixing water, they will create steric hindrance on the surface of inorganic particles, interfering with the hydration reaction and causing sluggish coagulation or decreased strength.
[0008] (4) Existing studies mostly regard organic matter in waste liquid as harmful impurities and have not yet effectively utilized its potential modification value for geopolymer gel structure by its humic components. Summary of the Invention
[0009] To address the above technical problems, this invention discloses a geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid and its preparation method, which solves the problems of limited disposal of sludge hydrothermal waste liquid in the prior art, reliance on commercial chemical alkalis for traditional geopolymers, and easy hydration inhibition caused by direct incorporation of waste liquid.
[0010] The technical solution adopted by this invention is as follows:
[0011] A method for preparing a geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater includes the following steps:
[0012] Step S1: Dry, grind, and mix the inorganic solid waste raw materials evenly to obtain a dry precursor; the inorganic solid waste raw materials include slag, desulfurized gypsum, and carbide slag;
[0013] Step S2: Measure the liquid phase according to a liquid-to-solid ratio (mass percentage of liquid phase to solid phase) of 0.4~0.6. The liquid phase is the original state of sludge hydrothermal wastewater or an aqueous solution containing active organic matter. The liquid phase contains humic acid or humic-like products; and the mass of the humic acid or humic-like products accounts for 0.5%~2.0% of the mass of the dry precursor.
[0014] Step S3: Mix the dry precursor with the liquid phase. First, stir at a low speed of 120-160 r / min for 100-150s. After stopping the machine and scraping off the residue, stir at a high speed of 250-320 r / min to fully wet and complex the solid and liquid phases, and obtain a geopolymer-based cementitious material slurry modified from organic solid waste hydrothermal waste liquid that can be used for casting and curing.
[0015] This technical solution does not add commercially available chemical alkali activating agents (such as water glass, sodium hydroxide, etc.). The active organic matter is humic acid or a humic-like component from sludge hydrothermal wastewater.
[0016] Using this technical solution, in the inorganic solid waste raw material, the dissolution of carbide slag releases OH... - It provides an alkaline activating environment, promoting the breakage of silicon-aluminum-oxygen bonds in slag / red mud; desulfurization gypsum provides SO4. 2- The system provides a sulfate-inducing environment, triggering the formation of micro-expansion products such as ettringite. These two components work synergistically to complete the initial construction of the inorganic framework. The inorganic solid waste dry material as a whole provides the precursor for the hydration reaction and the synergistic alkali-sulfate induction environment. The humic acid contained in the liquid phase or the humic-like products in the waste liquid contain abundant oxygen-containing functional groups (such as carboxyl groups and phenolic hydroxyl groups). At specific concentrations, these functional groups can target and modify the hydration products, and can react with free Ca in the system. 2+ Al 3+ The appropriate coordination and complexation of polyvalent cations serve as "templates" for micro-assembly, guiding the densification and development of hydrated gels. This effectively resists and compensates for the steric hindrance inhibition effect caused by other complex impurities in hydrothermal waste liquid, thereby achieving low-cost disposal of hydrothermal waste liquid and regulation of material properties.
[0017] Furthermore, the liquid phase is the original state of sludge hydrothermal waste liquid, which directly utilizes the humic products inherent in the waste liquid for in-situ synergistic solidification.
[0018] Furthermore, the liquid phase is an aqueous solution doped with active organic matter, which is humic acid.
[0019] As a further improvement of the present invention, the inorganic solid waste raw material is composed of slag, desulfurized gypsum and carbide slag, with a mass ratio of 5-7:2-4:1. More preferably, the mass ratio of the three is 6:3:1.
[0020] As a further improvement of the present invention, the inorganic solid waste raw material is composed of red mud, slag, desulfurized gypsum and carbide slag, with a mass ratio of 5-7:1-3:1-3:1. More preferably, the mass ratio of the four components is 6:2:1:1.
[0021] As a further improvement of the present invention, the amount of liquid phase added is such that the mass of humic acid or humic-like products accounts for 1.0% to 2.0% of the mass of the dry precursor.
[0022] As a further improvement of the present invention, the amount of liquid phase added is such that the mass of humic acid accounts for 2.0% of the mass of the dry precursor.
[0023] As a further improvement of the present invention, the liquid-to-solid ratio is 0.5.
[0024] As a further improvement of the present invention, in step S3, the mixture is first stirred at a low speed of 140 r / min for 120 s, and after stopping the machine and scraping off the residue, it is then stirred at a high speed of 285 r / min for at least 120 s.
[0025] As a further improvement of the present invention, in step S1, the powder is ground to a specific surface area of 400~450 m². 2 / kg. Further, in step S1, the slag, desulfurized gypsum, and carbide slag are dried and ground in a forced-air drying oven, and each component is weighed according to the set formula. They are then put into a dry mixer and dry-mixed for 3-5 minutes to obtain a uniformly mixed dry material precursor; or, in step S1, the red mud, slag, desulfurized gypsum, and carbide slag are dried and ground in a forced-air drying oven, and each component is weighed according to the set formula. They are then put into a dry mixer and dry-mixed for 3-5 minutes to obtain a uniformly mixed dry material precursor.
[0026] As a further improvement of the present invention, in step S2, if the liquid phase adopts in-situ waste liquid disposal, the corresponding mass of the original sludge hydrothermal waste liquid is directly weighed; if an aqueous solution containing active organic matter is adopted, 0.5% to 4.0% of humic acid, accounting for 0.5% to 4.0% of the total mass of dry material, is uniformly dispersed in the mixing water in advance.
[0027] As a further improvement of the present invention, the method for preparing the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater also includes:
[0028] Step S4: The slurry of the geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid is injected into the mold, compacted to remove air bubbles, the surface is smoothed, covered with a film and sealed, and cured for 24 hours at a temperature of 20±2℃ and a relative humidity of ≥95%. The material is then demolded and continued to be sealed and cured until the target age is reached. Further, the compaction is achieved by vibrating on a mortar vibrating table for 60 seconds to remove air bubbles.
[0029] This invention also discloses a geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid, which is obtained by the preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid as described in any one of the above.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0031] First, the technical solution of this invention breaks through the traditional perception that organic matter in hydrothermal wastewater is purely considered "harmful impurities." It is the first to discover and verify the targeted modification value of active organic matter (humification-like products) on geopolymer cementation systems within a specific dosage range. Experiments show that introducing 0.5%~2.0% pure humic acid as a modifying liquid phase into an inorganic solid waste raw material system can effectively guide the dense assembly of hydration products, achieving a 28-day compressive strength of 12.23 MPa, a 22.2% improvement compared to the pure water baseline (10.01 MPa). This discovery overcomes the technical challenge of strength degradation caused by organic impurities in traditional technologies, breaks through the "organic inhibition" bottleneck, and achieves a reverse leap in mechanical properties.
[0032] Secondly, the technical solution of this invention can directly utilize the original state of sludge hydrothermal wastewater as the mixing liquid phase for geopolymers, eliminating the need for costly pretreatment processes such as detoxification, dilution, decolorization, or separation and purification. Relying on an optimized anti-inhibition solid waste framework system, even under the interference of complex organic impurities in the hydrothermal wastewater, the 28-day compressive strength of the solidified body can still stably reach 10.88 MPa, fully meeting the strength requirements of low-grade engineering materials such as conventional roadbed fillers, mine backfills, and slope protection projects. This technical solution broadens the wastewater disposal pathway, opening up an engineering path for the large-scale, low-cost disposal of hydrothermal wastewater in the building materials field, and effectively solving the bottleneck in wastewater disposal that restricts the engineering application of hydrothermal treatment technology.
[0033] Third, the technical solution of this invention eliminates the reliance on high-energy-consuming and high-carbon-emission commercial chemical alkaline activators such as water glass and sodium hydroxide in traditional geopolymer preparation. By utilizing the strong alkaline environment provided by carbide slag itself and the synergistic activation effect of sulfate in desulfurized gypsum, it achieves 100% utilization of bulk industrial solid waste (granulated blast furnace slag / red mud, carbide slag, desulfurized gypsum) and municipal sludge hydrothermal wastewater for the preparation of cementitious materials. This method cuts off the carbon footprint introduced by traditional alkaline activators at the source, significantly reduces raw material costs, and has significant low-carbon, environmentally friendly, and economic advantages.
[0034] Fourth, the preparation method of this invention has a short process flow and is simple to operate. It does not require modification of existing geopolymer production equipment or the addition of complex waste liquid pretreatment devices; it can be achieved simply by replacing conventional mixing water with hydrothermal waste liquid. This method is easy to promote and implement in existing building material production lines and has good industrial adaptability and prospects for large-scale application. Attached Figure Description
[0035] Figure 1 This is a flowchart of a method for preparing geopolymer-based cementitious materials modified from organic solid waste hydrothermal waste liquid, according to an embodiment of the present invention. Detailed Implementation
[0036] The preferred embodiments of the present invention will be described in further detail below.
[0037] Example 1
[0038] A method for preparing geopolymer-based cementitious materials modified from organic solid waste hydrothermal wastewater, such as... Figure 1 As shown, the organic matter is treated with humic acid, and the process includes the following steps:
[0039] Step S1: Dry the slag, desulfurized gypsum, and carbide slag in a forced-air drying oven, grind them to a specific surface area of 400~450 m² / kg, mix them evenly, weigh each component precisely according to the set formula, put them into a dry mixer and dry mix for 5 minutes until uniform, and then set aside to obtain the dry material precursor; the mass ratio of the slag, desulfurized gypsum, and carbide slag is 6:3:1.
[0040] Step S2: Measure the liquid phase according to the liquid-solid ratio of 0.5. The liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 0.5% of the mass of the dry precursor, and is ultrasonically dispersed evenly.
[0041] Step S3: Mix the dry precursor with the liquid phase, first stir at a low speed of 140 r / min for 100-150 s, stop the machine and scrape off the residue, then stir at a high speed of 285 r / min to fully wet and complex the solid and liquid phases, and obtain a geopolymer-based cementitious material slurry modified from organic solid waste hydrothermal waste liquid that can be used for casting and curing.
[0042] Step S4: Pour the mixed slurry into standard molds in layers and vibrate on a mortar vibrating table for 60 seconds to remove air bubbles. After smoothing the surface, cover with a film and seal. Place in a constant temperature and humidity curing chamber (temperature 20±2℃, relative humidity ≥95%) for 24 hours, then demold and continue to seal and cure until the target age.
[0043] Example 2
[0044] Based on Example 1, the difference in this example is that the liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 1.0% of the mass of the dry precursor.
[0045] Example 3
[0046] Based on Example 1, the difference in this example is that the liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 1.5% of the mass of the dry precursor.
[0047] Example 4
[0048] Based on Example 1, the difference in this example is that the liquid phase is an aqueous solution with added high-purity humic acid powder, and the amount of liquid phase added satisfies that the mass of humic acid accounts for 2.0% of the mass of the dry precursor.
[0049] Comparative Example 1
[0050] Comparative Example 1 uses pure water as the baseline. Based on Example 1, 100% deionized water was measured and mixed as the liquid phase. The mixture was then molded according to standard procedures, vibrated to remove air, and sealed and cured in an environment of 20±2℃ and relative humidity ≥95%.
[0051] Comparative Example 2
[0052] Based on Example 1, the mass of humic acid in this comparative example accounts for 2.5% of the mass of the dry precursor.
[0053] Comparative Example 3
[0054] Based on Example 1, the mass of humic acid in this comparative example accounts for 3.0% of the mass of the dry precursor.
[0055] Comparative Example 4
[0056] Based on Example 1, the mass of humic acid in this comparative example accounts for 3.5% of the mass of the dry precursor.
[0057] Comparative Example 5
[0058] Based on Example 1, the mass of humic acid in this comparative example accounts for 4.0% of the mass of the dry precursor.
[0059] Example 5 (Hydrothermal waste liquid group)
[0060] Based on Example 1, without adding any exogenous humic acid, the untreated, undiluted, or unpurified raw sludge hydrothermal waste liquid was directly measured as the liquid phase and mixed to form the mixture. The curing conditions were the same as in Example 1. That is, the dry precursor from Example 1 was mixed with the untreated, undiluted, or unpurified raw sludge hydrothermal waste liquid to form the mixture.
[0061] Example 6
[0062] Based on Example 1, in step S1 of this example, red mud, slag, desulfurized gypsum, and carbide slag are dried, ground, and mixed evenly. After accurately weighing each component according to the set formula, they are put into a dry mixer and mixed evenly for later use to obtain a dry material precursor. The mass ratio of the red mud, slag, desulfurized gypsum, and carbide slag is 6:2:1:1. Everything else is the same as in Example 1.
[0063] Example 7
[0064] Based on Example 6, the liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 1.0% of the mass of the dry precursor.
[0065] Example 8
[0066] Based on Example 6, the liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 1.5% of the mass of the dry precursor.
[0067] Example 9
[0068] Based on Example 6, the liquid phase is an aqueous solution with added high-purity humic acid powder, wherein the mass of humic acid accounts for 2.0% of the mass of the dry precursor.
[0069] Comparative Example 6 (Red mud-based pure water reference group)
[0070] In this example, the liquid phase was 100% deionized water. Based on Example 6, 100% deionized water was measured and mixed as the liquid phase. The mixture was then molded according to standard procedures, vibrated to remove air, and sealed and cured in an environment of 20±2℃ and relative humidity ≥95%.
[0071] Comparative Example 7
[0072] Based on Example 6, the mass of humic acid in this comparative example accounts for 2.5% of the mass of the dry precursor.
[0073] Comparative Example 8
[0074] Based on Example 6, the mass of humic acid in this comparative example accounts for 3.0% of the mass of the dry precursor.
[0075] Comparative Example 9
[0076] Based on Example 6, the mass of humic acid in this comparative example accounts for 3.5% of the mass of the dry precursor.
[0077] Comparative Example 10
[0078] Based on Example 6, the mass of humic acid in this comparative example accounts for 4.0% of the mass of the dry precursor.
[0079] Example 10 (Red mud-based hydrothermal waste liquid group)
[0080] Based on Example 6, the liquid phase is 100% untreated raw sludge hydrothermal wastewater, and the mixing, molding, and curing are the same as in Example 1. That is, the dry precursor of Example 6 is mixed with 100% untreated raw sludge hydrothermal wastewater for molding.
[0081] All samples in the examples and comparative examples were subjected to compressive strength and setting time tests to comprehensively evaluate the effects of organic matter gradient and hydrothermal waste liquid on the macroscopic mechanical and working properties of the gelation system.
[0082] The unconfined compressive strength (UCS) of the specimens at different ages was tested. The compressive strength of each group of specimens was tested at 3d and 28d. The results are shown in Table 1 and Table 2.
[0083] Table 1. Test results of compressive strength of slag-based system at different ages.
[0084]
[0085] Table 2. Results of compressive strength tests on red mud-based systems at different ages.
[0086]
[0087] As can be seen from the comparison results in Tables 1 and 2, in the embodiment where the mass of humic acid accounts for 0.5% to 2.0% of the mass of the dry precursor, the 3-day and 28-day unconfined compressive strengths are higher when using the technical solution of the present invention.
[0088] The setting time of the slurry in each example and comparative example was tested in accordance with the "Test Methods for Standard Consistency Water Requirement, Setting Time and Soundness of Cement" (GB / T 1346).
[0089] Test results show that the amount of organic matter added has a significant regulatory effect on the setting time of the geopolymer system, and all meet the standards:
[0090] (1) Within the effective dosage range of 0.5% to 2.5% of the dry precursor by mass of humic acid (Examples 1-4 and Examples 6-9), due to the initial coordination complexation of active organic matter and metal ions, the initial setting time of the slurry shows a moderately delayed trend compared with the pure water reference group (Comparative Example 1 and Comparative Example 6). This feature provides more time for stirring and molding operations in engineering applications, avoiding the drawback of traditional geopolymers being prone to "flash setting".
[0091] (2) When the mass of humic acid exceeds the critical value of 2.0% of the dry precursor (as in Comparative Examples 2 and 7), the setting time is significantly prolonged; when the humic acid content reaches 4.0% (Comparative Examples 5 and 10), the slurry exhibits extreme slow setting, and may even fail to set within 48 hours, appearing as a thin mud. This proves that the overloaded organic micelles completely block the overlap of hydration products.
[0092] (3) Although the hydrothermal waste liquid group (Example 5 and Example 10) was affected by complex impurities and the initial setting time was significantly later than that of the pure water group, thanks to the hydration compensation effect of endogenous humic substances, the slurry was able to complete the final setting smoothly and establish a stable structural strength as the age increased.
[0093] Comparative Example 1 (pure water reference group) and Example 4 (optimal modification group) were selected for microscopic morphology and structural characterization. FTIR spectroscopy analysis showed that the characteristic peak of the carboxyl group of humic acid in Example 4 underwent a significant wavenumber shift, confirming that it had formed a deep coordination complex with the calcium and aluminum ions dissolved from the inorganic dry material.
[0094] Scanning electron microscopy (SEM) was performed on the examples and comparative examples. The morphology showed that an extremely dense network of hydrated calcium silicate and ettringite was formed inside the examples 1-4; while in the comparative example 5, obvious organic matter coating was visible, which hindered the continued progress of the hydration reaction.
[0095] Leaching tests were conducted on the solidified bodies from Examples 5 and 10 to evaluate the environmental safety of wastewater disposal. The results showed that the geopolymer three-dimensional network exhibited excellent sequestration effects on heavy metals (Pb, Cr, etc.) and high concentrations of COD in the wastewater. The leachate indicators were all far below the limits of the "Identification Standard for Hazardous Waste - Leaching Toxicity Identification", demonstrating good environmental safety.
[0096] Based on the above test results for compressive strength, setting time, microstructure, and environmental safety, it can be seen that:
[0097] (1) "Template-guided" modification mechanism of active organic matter: Experiments have shown that within the effective dose window of 0.5% to 2.0% of the mass of humic acid as a percentage of the mass of the dry precursor, organic matter acts as a "microscopic template" for the assembly of hydration products through coordination complexation, which significantly improves the density and macroscopic strength of the solidified body, especially overcoming the problem of slow early hydration kinetics of the red mud-based system.
[0098] (2) The failure law of "steric inhibition" of organic overload: When the mass of humic acid accounts for more than 2.0% of the mass of the dry precursor, the technical effect is reversed. The steric hindrance effect generated by the excess organic molecules blocks the diffusion and nucleation of ions, which is macroscopically manifested as a sharp decrease in strength and an extreme delay in condensation time.
[0099] (3) The "endogenous compensation" and "performance retention" effects of direct co-mixing of waste liquid: Although the impurities in the waste liquid are suppressed in the early stage, the humic substances it contains play a strong compensating role in the later stage of hydration. The 28-day compressive strength of Examples 5 and 10 reached the strength level comparable to that of the pure water reference group, realizing the high-value utilization and low-cost in-situ non-destructive disposal of sludge hydrothermal waste liquid.
[0100] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater, characterized in that: Includes the following steps: Step S1: Dry, grind, and mix the inorganic solid waste raw materials evenly to obtain a dry precursor; the inorganic solid waste raw materials include slag, desulfurized gypsum, and carbide slag; Step S2: Measure the liquid phase according to a liquid-to-solid ratio of 0.4~0.
6. The liquid phase is the original state sludge hydrothermal waste liquid or an aqueous solution containing active organic matter. The liquid phase contains humic acid or humic-like products; and the mass of the humic acid or humic-like products accounts for 0.5%~2.0% of the mass of the dry precursor. Step S3: Mix the dry precursor with the liquid phase. First, stir at a low speed of 120-160 r / min for 100-150s. After stopping the machine and scraping off the residue, stir at a high speed of 250-320 r / min to fully wet and complex the solid and liquid phases, and obtain a geopolymer-based cementitious material slurry modified from organic solid waste hydrothermal waste liquid that can be used for casting and curing.
2. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 1, characterized in that: The inorganic solid waste raw material consists of slag, desulfurized gypsum and carbide slag, with a mass ratio of 6:3:
1.
3. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 1, characterized in that: The inorganic solid waste raw material consists of red mud, slag, desulfurized gypsum and carbide slag, with a mass ratio of 6:2:1:
1.
4. The preparation method of geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 2 or 3, characterized in that: The amount of liquid phase added is such that the mass of humic acid or humic-like products accounts for 1.0% to 2.0% of the mass of the dry precursor.
5. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 4, characterized in that: The amount of liquid phase added is such that the mass of humic acid accounts for 2.0% of the mass of the dry precursor.
6. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 4, characterized in that: The liquid-to-solid ratio is 0.
5.
7. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 4, characterized in that: In step S3, the mixture is first stirred at a low speed of 140 r / min for 120 s, and after stopping the machine and scraping off the residue, it is then stirred at a high speed of 285 r / min for at least 120 s.
8. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 4, characterized in that: In step S1, the powder is ground to a specific surface area of 400~450 m². 2 / kg.
9. The preparation method of the geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater according to claim 1, characterized in that, Also includes: Step S4: Inject the slurry of the geopolymer-based cementitious material modified from organic solid waste hydrothermal waste liquid into the mold, vibrate to remove air bubbles, scrape the surface smooth, cover with a film and seal, and cure for 24 hours at a temperature of 20±2℃ and relative humidity ≥95% before demolding. Continue to seal and cure until the target age.
10. A geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater, characterized in that: The material was prepared using the method described in any one of claims 1 to 9, which is based on the preparation of a geopolymer-based cementitious material modified from organic solid waste hydrothermal wastewater.