A high-leakage self-healing component release concrete and a preparation method thereof
By preparing a composite repair agent and composite carrier that combine adhesion and flexibility, the problems of self-healing function decay and component compatibility of high-strength self-healing concrete under extreme conditions were solved, and the impermeability, erosion resistance and long-term durability of high-permeability self-healing component release concrete were realized.
Patent Information
- Application Number
- CN202611493085.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing high-strength self-healing concrete is prone to microbial activity decay under long-term alternating wet and dry conditions or extreme temperature conditions, and its self-healing function is unsustainable. In addition, the large number of micropores introduced by carbon dioxide foaming weakens the load-bearing capacity of the matrix, and the compatibility and dispersion uniformity between components are difficult to control, affecting the applicability of practical engineering.
A composite repair agent with adhesive properties, film-forming properties, and flexibility is prepared by using a composite repair agent and a composite carrier. A prepolymer is formed by ring-opening esterification and etherification of epoxy resin with components such as castor oil acid, and then graft copolymerized with methyl methacrylate. The polyurethane prepolymer reacts with isocyanate to form a composite carrier with both flexible segments and rigid hard segments, which is loaded into concrete to release the repair agent under crack stress and water flow.
It improves the self-healing efficiency, impermeability, and long-term durability of concrete cracks, reduces the premature release of repair agents, enhances adhesion and film density, mitigates the risk of crack propagation and brittle fracture, and improves erosion resistance and service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of concrete preparation technology, specifically relating to a high-permeability self-healing component-releasing concrete and its preparation method. Background Technology
[0002] Concrete is the most widely used structural material in construction engineering, but it is inherently brittle with extremely low tensile strength. Under the long-term effects of loads, temperature stress, drying shrinkage, and chemical corrosion, microcracks are almost inevitable. Once cracks form, they provide a channel for harmful media such as water, chloride ions, and sulfate to penetrate, leading to steel corrosion and structural deterioration, forming a vicious cycle of "cracking—penetration—re-cracking," seriously threatening the durability of the project. Traditional waterproofing relies on external waterproofing layers such as membranes and coatings, which are passive defense systems. Organic materials are prone to aging and failure, with a lifespan far shorter than the structural design life, and construction is complex with high maintenance costs. Against this backdrop, high-permeability self-healing component release concrete has become a research hotspot. This technology pre-embeds active chemical substances or microbial spores into the concrete to form self-healing components. When cracks form and water seeps in, the components are activated and release repair products, generating insoluble crystals that self-seal the cracks. This shifts the waterproofing concept from passive repair to active repair, providing a new path to solve the industry problem of building leakage.
[0003] Patent CN108793885B discloses a high-strength self-healing concrete. The raw materials of this concrete are grouped by weight as follows: 100-120 parts silicate cement, 30-50 parts water, 10-20 parts carbon dioxide foaming agent, 20-30 parts dispersant, 55-65 parts aggregate, 20-30 parts microbial composite, 20-30 parts modified fiber composite, 1-3 parts phenolic antioxidant, 1-3 parts stearic acid, and 4-8 parts modified isoprene petroleum resin. This patented high-strength self-healing concrete, through specific proportions and preparation methods, increases flexural and compressive strength to a certain extent, while also enhancing the concrete's self-healing ability, extending the repair time, and exhibiting stronger durability and density. The strength recovery rate of the repaired concrete is high. Through the examples and comparative examples of this patent, it can be seen that the components of this high-strength self-healing concrete have a synergistic effect. When a component is replaced, the flexural and compressive strength of the concrete decreases significantly, and the recovery rate also decreases significantly.
[0004] However, the high-strength self-healing concrete disclosed in this patent still has certain defects: First, the survival and activity of the microbial complex are highly dependent on the alkaline environment and sufficient moisture. Under long-term alternating wet and dry conditions or extreme temperature conditions, the activity of microorganisms is prone to decay, resulting in the unsustainability of the self-healing function. Second, although carbon dioxide foaming improves the density, the large number of micropores introduced weakens the load-bearing capacity of the matrix to a certain extent, and there is an inherent contradiction between strength and self-healing performance. Third, although the multi-component synergistic system has significant effects, the compatibility and dispersion uniformity between the components are difficult to control precisely in large-volume construction, which can easily cause uneven local performance and limit its practical engineering applicability. Summary of the Invention
[0005] The purpose of this invention is to provide a high-permeability, self-healing component-releasing concrete and its preparation method, which solves the technical problems of poor impermeability and self-healing properties of concrete in the prior art.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A high-permeability self-healing component-release concrete, comprising a composite repair agent and a composite carrier;
[0008] The preparation method of the composite repair agent includes the following steps:
[0009] Q1: Add epoxy resin, ricinoleic acid, 4-benzyloxyphenol, N,N-dimethylethanolamine and triphenylphosphine to a container, heat and stir, continue to increase the temperature to react, cool down after the reaction is completed, add dipropylene glycol methyl ether, stir and mix to obtain the prepolymer;
[0010] Q2: The prepolymer obtained in Q1 is heated, and then methyl methacrylate, N-hydroxymethylacrylamide and benzoyl peroxide are added in sequence. After the reaction is maintained at the temperature, benzoyl peroxide is added to continue the reaction, followed by the addition of triethanolamine. After stirring and mixing, the mixture is filtered to obtain the composite repair agent.
[0011] The working principle of the composite repair agent in this invention is as follows: epoxy resin first undergoes ring-opening esterification and etherification with ricinoleic acid and 4-benzyloxyphenol under the action of N,N-dimethylethanolamine and triphenylphosphine to form a prepolymer containing ester bonds, ether bonds, hydroxyl groups and flexible segments; then, under the initiation of benzoyl peroxide, it undergoes graft copolymerization with methyl methacrylate and N-hydroxymethylacrylamide to obtain a composite repair agent with adhesiveness, film-forming properties, flexibility and interfacial compatibility.
[0012] The method for preparing the composite carrier includes the following steps:
[0013] S1: Polytetrahydrofuran diol is added to a container, heated, dehydrated under vacuum, cooled, and under nitrogen atmosphere, isophorone diisocyanate is added to the container. Then xylene containing dibutyltin dilaurate is added dropwise, and the reaction is continued by stirring to obtain polyurethane prepolymer.
[0014] S2: Add xylene containing 2,5-tetrahydrofurandimethyl alcohol to the polyurethane prepolymer obtained in S1, stir and react under nitrogen atmosphere, then add xylene containing 4,4'-methylenebis(3-chloro-2,6-diethylaniline), continue stirring and react, and after the reaction is completed, obtain polyurethane liquid.
[0015] S3: Add the polyurethane liquid obtained in S2 into a polytetrafluoroethylene mold, dry it, add it into N,N-dimethylformamide for dissolution, dry it, and obtain a composite carrier.
[0016] The working principle of the composite carrier in this invention is as follows: Polytetrahydrofuran diol first undergoes an addition reaction with isophorone diisocyanate under the catalysis of dibutyltin dilaurate to form an isocyanate-terminated polyurethane prepolymer; subsequently, 2,5-tetrahydrofurandiethanol reacts with the terminal isocyanate groups of the prepolymer to achieve diol chain extension, and 4,4'-methylenebis(3-chloro-2,6-diethylaniline) further reacts with the remaining isocyanate groups to form urea bonds, thereby constructing a polyurethane-urea segmented structure containing urethane bonds and urea bonds; finally, after casting, drying and DMF dissolution and reconstruction, a composite carrier with flexible segments, rigid hard segments and good interfacial stability is obtained.
[0017] A high-permeability self-healing component-release concrete is composed of the following parts by weight: 80-90 parts cement, 10-20 parts fly ash, 15-25 parts mineral powder, 3-6 parts silica fume, 130-160 parts fine aggregate, 160-220 parts coarse aggregate, 30-45 parts water, 0.8-1.4 parts water-reducing agent, 0.5-1.2 parts fiber, 0.4-0.9 parts composite repair agent, and 8-15 parts composite carrier.
[0018] In step Q1, the ratio of epoxy resin, ricinoleic acid, 4-benzyloxyphenol, N,N-dimethylethanolamine, triphenylphosphine, and dipropylene glycol methyl ether is (70-75) g : (40-48) g : (20-30) g : (4-7) g : (0.25-0.35) g : (5-9) g; the heating and stirring temperature is 150-160℃, and the stirring time is 10-20 min; the reaction temperature is further increased to 220-225℃, and the reaction time is 4-6 h; after the reaction is completed, the temperature is lowered to 160±5℃, and the stirring and mixing time is 30-45 min.
[0019] In step Q2, the ratio of prepolymer, methyl methacrylate, N-hydroxymethylacrylamide, triethanolamine, and benzoyl peroxide is (88-95) g: (5-12) g: (3-6) g: (5-7.5) g: (1.2-1.8) g, where the amount of benzoyl peroxide is the sum of the initial addition and subsequent additions; the heat preservation reaction temperature is 120-130℃, and the heat preservation reaction time is 1-2 h; the addition of triethanolamine and stirring time is 1-3 h, and filtration is performed using an 80-100 mesh filter.
[0020] In step S1, the ratio of polytetrahydrofuran diol, isophorone diisocyanate, dibutyltin dilaurate, and xylene is (10-12) g: (8.12-8.94) g: (0.01-0.04) g: (18-22) g, and the average molecular weight of the polytetrahydrofuran diol is 900-1100. The temperature is raised to 115-120℃, vacuum dehydration is carried out for 1-2 hours, the temperature is lowered to 80-82℃, and the reaction is continued with stirring for 2-4 hours.
[0021] In step S2, the ratio of 2,5-tetrahydrofurandimethyl alcohol, polyurethane prepolymer, and 4,4'-methylenebis(3-chloro-2,6-diethylaniline) is (2.56-3.42) g : (12.53-14.69) g : (2.01-2.25) g. The stirring reaction temperature is 110-120℃, the time is 3-5 h, and the continued stirring reaction time is 2-4 h.
[0022] In step S3, the drying temperature before dissolution is 80-82℃ and the time is 20-24h. The drying process after dissolution is as follows: first, drying at 50-55℃ for 10-12h, and then drying at 80-84℃ for 20-24h.
[0023] A method for preparing high-permeability, self-healing component-releasing concrete includes the following steps:
[0024] Step 1: Add the composite repair agent to the composite carrier, stir and mix, and let stand to obtain the composite carrier loaded with the composite repair agent;
[0025] Step 2: Add cement, fly ash, mineral powder and silica fume to the mixer and mix once. Then add fine aggregate and mix. Add coarse aggregate and mix again. Then add water containing water-reducing agent and mix evenly to obtain slurry. Then add fiber and continue mixing. Finally, add composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0026] In step 1, the stirring speed is 400-500 rpm, the time is 10-30 min, and the settling time is 40-60 min.
[0027] In step 2, the first mixing time is 1-3 minutes, the stirring and mixing time is 2-4 minutes, the second mixing time is 1-3 minutes, the second mixing time is the mixing time after adding coarse aggregate, and the continued stirring time is 2-4 minutes.
[0028] The beneficial effects of this invention are as follows:
[0029] 1. This invention uses a composite carrier to adsorb and protect the composite repair agent, reducing the premature release of the repair agent during mixing and early hydration stages. When cracks appear in the structure and leakage occurs, the carrier releases the repair agent under the stress of the cracks and the action of water flow, allowing it to enter the cracks and capillary channels and form a bonded sealing layer. The composite repair agent works synergistically with the secondary hydration products of the cement matrix to improve the self-healing efficiency of cracks, impermeability and erosion resistance, and long-term durability. At the same time, the fibers and flexible carrier help to mitigate crack propagation.
[0030] 2. The composite repair agent obtained in this invention is applied to concrete. It is released from the composite carrier under crack propagation and water seepage, and migrates and spreads along crack walls, capillaries, and aggregate interface transition zones, forming a continuous organic sealing layer. This improves the concrete's impermeability, erosion resistance, self-healing properties, and long-term durability. The epoxy resin structure provides strong adhesion, methyl methacrylate segments help improve film density and water resistance, and castor oil acid flexible segments buffer micro-deformation of cracks, reducing the risk of brittleness and debonding of the repair layer. Amide, hydroxyl, and amine groups enhance interfacial bonding with cement hydration products through wetting, hydrogen bonding, and polar adsorption.
[0031] 3. This invention applies the prepared composite carrier to concrete, which can improve the self-healing, impermeability, erosion resistance, and long-term durability of concrete cracks. The polar structure contained in the composite carrier can adsorb, embed, and stably store the composite repair agent, reducing premature leakage and deactivation of the composite repair agent in mixing, high-alkali, and hydration environments. The flexible segments of polytetrahydrofuran contained in the carrier give the carrier good elasticity and impact resistance, while the hard segments formed by isophorone diisocyanate and aromatic diamine improve structural strength and stirring resistance. When cracks expand and are accompanied by water seepage, the carrier can release the repair agent under crack stress, interface debonding, water displacement, and capillary action, allowing it to enter the crack and form a sealing layer; at the same time, the carrier itself can also alleviate stress concentration through elastic deformation, crack deflection, and interface energy dissipation, thereby improving the service life of concrete. Detailed Implementation
[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0033] Example 1: This example discloses a method for preparing a composite repair agent, including the following steps:
[0034] Q1: Add 72g epoxy resin, 44g castor oil acid, 25g 4-benzyloxyphenol, 5.5g N,N-dimethylethanolamine and 0.30g triphenylphosphine to a container, heat to 155℃ and stir for 15min, then continue to heat to 222℃ and react for 5h. After the reaction is completed, cool to 160℃, add 7g dipropylene glycol methyl ether, stir and mix for 40min to obtain the prepolymer;
[0035] Q2: Heat 92g of prepolymer to 125℃, then add 8g of methyl methacrylate, 4.5g of N-hydroxymethylacrylamide and 1.35g of benzoyl peroxide in sequence. After reacting at this temperature for 1.5h, add 0.075g of benzoyl peroxide in two separate additions, each adding for 15min and then maintaining the temperature for 1.5h. Then add 6.2g of triethanolamine, stir and mix for 2h, and filter through a 90-mesh filter to obtain the composite repair agent.
[0036] This embodiment discloses a method for preparing a composite carrier, including the following steps:
[0037] S1: 11g of polytetrahydrofuran diol with an average molecular weight of 1000 was added to a container, heated to 120℃, and vacuum dehydrated for 1.5h. Then, the temperature was lowered to 80℃. Under nitrogen atmosphere, 8.45g of isophorone diisocyanate was added to the container, and then 20g of xylene containing 0.02g of dibutyltin dilaurate was added dropwise. After stirring and reacting for 3h, a polyurethane prepolymer was obtained.
[0038] S2: Add 20g of xylene containing 2.96g of 2,5-tetrahydrofurandimethylethanol to 13.6g of polyurethane prepolymer, stir and react at 115℃ for 4h under nitrogen atmosphere, then add 15g of xylene containing 2.12g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and continue stirring and reacting for 3h. After the reaction is completed, polyurethane liquid is obtained.
[0039] S3: Add polyurethane liquid to a polytetrafluoroethylene mold, dry at 80°C for 24 hours, dissolve in N,N-dimethylformamide, and dry at 50°C for 12 hours and 82°C for 22 hours to obtain a composite carrier.
[0040] This embodiment discloses a high-permeability self-healing component-release concrete, which is composed of the following parts by weight: 85 parts cement, 15 parts fly ash, 20 parts mineral powder, 4.5 parts silica fume, 145 parts fine aggregate, 190 parts coarse aggregate, 38 parts water, 1.1 parts polycarboxylate superplasticizer, 0.8 parts polypropylene fiber, 0.65 parts composite repair agent and 12 parts composite carrier.
[0041] This embodiment discloses a method for preparing high-permeability, self-healing component-releasing concrete, including the following steps:
[0042] Step 1: Add the composite repair agent to the composite carrier (crushed and sieved, particle size 0.45-0.88mm), stir and mix at 450rpm for 20min, and let stand for 50min to obtain the composite carrier loaded with the composite repair agent.
[0043] Step 2: Add cement (PO 42.5 ordinary Portland cement), fly ash (Grade II fly ash), mineral powder (S95 grade granulated blast furnace slag powder), and silica fume (SiO2 mass fraction not less than 90%) to the mixer. Mix for 2 minutes, then add fine aggregate (natural sand with a fineness modulus of 2.4-2.8) and mix for 3 minutes. Add coarse aggregate (5-20mm continuously graded crushed stone) and mix for another 2 minutes. Then add water containing polycarboxylate superplasticizer and mix evenly to obtain a slurry. Then add polypropylene fiber and continue mixing for 3 minutes. Finally, add the composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0044] Example 2: This example discloses a method for preparing a composite repair agent, including the following steps:
[0045] Q1: Add 75g epoxy resin, 48g castor oil acid, 30g 4-benzyloxyphenol, 7g N,N-dimethylethanolamine and 0.35g triphenylphosphine to a container, heat to 160℃ and stir for 20min, then continue to heat to 225℃ and react for 6h. After the reaction is completed, cool to 160℃, add 9g dipropylene glycol methyl ether, stir and mix for 45min to obtain the prepolymer;
[0046] Q2: Heat 95g of prepolymer to 130℃, then add 12g of methyl methacrylate, 6g of N-hydroxymethylacrylamide and 1.62g of benzoyl peroxide in sequence. After reacting at this temperature for 2 hours, add 0.09g of benzoyl peroxide in two separate additions, each adding for 20 minutes and then keeping the temperature for 2 hours. Then add 7.5g of triethanolamine, stir and mix for 3 hours, and filter through a 100-mesh filter to obtain the composite repair agent.
[0047] This embodiment discloses a method for preparing a composite carrier, including the following steps:
[0048] S1: Add 10g of polytetrahydrofuran diol with an average molecular weight of 1000 to a container, heat to 120℃, dehydrate under vacuum for 2h, then cool to 82℃. Under nitrogen atmosphere, add 8.94g of isophorone diisocyanate to the container, then add 22g of xylene containing 0.04g of dibutyltin dilaurate. Continue stirring and reacting for 4h to obtain polyurethane prepolymer.
[0049] S2: Add 20g of xylene containing 3.42g of 2,5-tetrahydrofurandimethylethanol to 14.69g of polyurethane prepolymer, stir and react at 120℃ for 5h under nitrogen atmosphere, then add 15g of xylene containing 2.25g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and continue stirring and reacting for 4h. After the reaction is completed, polyurethane liquid is obtained.
[0050] S3: Add polyurethane liquid into a polytetrafluoroethylene mold, dry at 82°C for 24 hours, dissolve in N,N-dimethylformamide, and dry at 55°C for 12 hours and 84°C for 24 hours respectively to obtain a composite carrier.
[0051] This embodiment discloses a high-permeability self-healing component-release concrete, which is composed of the following parts by weight: 90 parts cement, 10 parts fly ash, 25 parts mineral powder, 6 parts silica fume, 130 parts fine aggregate, 220 parts coarse aggregate, 35 parts water, 1.4 parts polycarboxylate superplasticizer, 1.2 parts PVA fiber, 0.9 parts composite repair agent and 8 parts composite carrier.
[0052] This embodiment discloses a method for preparing high-permeability, self-healing component-releasing concrete, including the following steps:
[0053] Step 1: Add the composite repair agent to the composite carrier (crushed and sieved, particle size 0.45-0.88mm), stir and mix at 500rpm for 30min, and let stand for 60min to obtain the composite carrier loaded with the composite repair agent.
[0054] Step 2: Add cement (PO 42.5 ordinary Portland cement), fly ash (Grade II fly ash), mineral powder (S95 grade granulated blast furnace slag powder), and silica fume (SiO2 mass fraction not less than 90%) to the mixer. Mix for 3 minutes at a time. Then add fine aggregate (natural sand with a fineness modulus of 2.4-2.8) and mix for 4 minutes. Add coarse aggregate (5-20mm continuously graded crushed stone) and mix again for 3 minutes. Then add water containing polycarboxylate superplasticizer and mix evenly to obtain a slurry. Then add PVA fiber and continue mixing for 4 minutes. Finally, add the composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0055] Example 3: This example discloses a method for preparing a composite repair agent, including the following steps:
[0056] Q1: Add 70g epoxy resin, 40g castor oil acid, 20g 4-benzyloxyphenol, 4g N,N-dimethylethanolamine and 0.25g triphenylphosphine to a container, heat to 150℃ and stir for 10min, then continue to heat to 220℃ and react for 4h. After the reaction is completed, cool to 160℃, add 5g dipropylene glycol methyl ether, stir and mix for 30min to obtain the prepolymer;
[0057] Q2: Heat 88g of prepolymer to 120℃, then add 5g of methyl methacrylate, 3g of N-hydroxymethylacrylamide and 1.08g of benzoyl peroxide in sequence. After reacting at this temperature for 1 hour, add 0.06g of benzoyl peroxide in two separate additions, each adding for 15 minutes and then keeping the temperature for 1 hour. Then add 5g of triethanolamine, stir and mix for 1 hour, and filter through an 80-mesh filter to obtain the composite repair agent.
[0058] This embodiment discloses a method for preparing a composite carrier, including the following steps:
[0059] S1: 12g of polytetrahydrofuran diol with an average molecular weight of 1000 was added to a container, heated to 115℃, and vacuum dehydrated for 1 hour. Then, the temperature was lowered to 80℃, and 8.12g of isophorone diisocyanate was added to the container under nitrogen atmosphere. Then, 18g of xylene containing 0.01g of dibutyltin dilaurate was added dropwise. After stirring and reacting for 2 hours, a polyurethane prepolymer was obtained.
[0060] S2: Add 20g of xylene containing 2.56g of 2,5-tetrahydrofurandimethylethanol to 12.53g of polyurethane prepolymer, stir and react at 110℃ for 3h under nitrogen atmosphere, then add 15g of xylene containing 2.01g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and continue stirring and reacting for 2h. After the reaction is completed, polyurethane liquid is obtained.
[0061] S3: Add polyurethane liquid to a polytetrafluoroethylene mold, dry at 80°C for 20 hours, dissolve in N,N-dimethylformamide, and dry at 50°C for 10 hours and 80°C for 20 hours respectively to obtain a composite carrier.
[0062] This embodiment discloses a high-permeability self-healing component-release concrete, which is composed of the following parts by weight: 80 parts cement, 20 parts fly ash, 15 parts mineral powder, 3 parts silica fume, 160 parts fine aggregate, 160 parts coarse aggregate, 45 parts water, 0.8 parts polycarboxylate superplasticizer, 0.5 parts polypropylene fiber, 0.4 parts composite repair agent and 15 parts composite carrier.
[0063] This embodiment discloses a method for preparing high-permeability, self-healing component-releasing concrete, including the following steps:
[0064] Step 1: Add the composite repair agent to the composite carrier (crushed and sieved, particle size 0.45-0.88mm), stir and mix at 400rpm for 10min, and let stand for 40min to obtain the composite carrier loaded with the composite repair agent.
[0065] Step 2: Add cement (PO 42.5 ordinary Portland cement), fly ash (Grade II fly ash), mineral powder (S95 grade granulated blast furnace slag powder), and silica fume (SiO2 mass fraction not less than 90%) to the mixer. Mix for 1 minute, then add fine aggregate (natural sand with a fineness modulus of 2.4-2.8) and mix for 2 minutes. Add coarse aggregate (5-20mm continuously graded crushed stone) and mix for another 1 minute. Then add water containing polycarboxylate superplasticizer and mix evenly to obtain a slurry. Then add polypropylene fiber and continue mixing for 2 minutes. Finally, add the composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0066] Example 4: This example discloses a method for preparing a composite repair agent, including the following steps:
[0067] Q1: Add 74g epoxy resin, 42g castor oil acid, 28g 4-benzyloxyphenol, 6g N,N-dimethylethanolamine and 0.32g triphenylphosphine to a container, heat to 158℃ and stir for 18min, then continue to heat to 224℃ and react for 5.5h. After the reaction is completed, cool to 160℃, add 8g dipropylene glycol methyl ether, stir and mix for 40min to obtain the prepolymer;
[0068] Q2: Heat 90g of prepolymer to 128℃, then add 10g of methyl methacrylate, 5g of N-hydroxymethylacrylamide and 1.44g of benzoyl peroxide in sequence. After reacting at this temperature for 2 hours, add 0.08g of benzoyl peroxide in two separate additions, each adding for 20 minutes and maintaining the temperature for 1.5 hours. Then add 6.8g of triethanolamine and stir to mix for 2.5 hours. Filter through a 100-mesh filter to obtain the composite repair agent.
[0069] This embodiment discloses a method for preparing a composite carrier, including the following steps:
[0070] S1: Add 10.5g of polytetrahydrofuran diol with an average molecular weight of 1000 to a container, heat to 118℃, dehydrate under vacuum for 1.5h, then cool to 81℃. Under nitrogen atmosphere, add 8.60g of isophorone diisocyanate to the container, then add 21g of xylene containing 0.03g of dibutyltin dilaurate. Continue stirring and reacting for 3h to obtain polyurethane prepolymer.
[0071] S2: Add 20g of xylene containing 3.20g of 2,5-tetrahydrofurandimethylethanol to 14.0g of polyurethane prepolymer, stir and react at 118℃ for 4h under nitrogen atmosphere, then add 15g of xylene containing 2.20g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and continue stirring and reacting for 3h. After the reaction is completed, polyurethane liquid is obtained.
[0072] S3: Add polyurethane liquid to a polytetrafluoroethylene mold, dry at 82°C for 22 hours, dissolve in N,N-dimethylformamide, and dry at 55°C for 11 hours and 82°C for 22 hours respectively to obtain a composite carrier.
[0073] This embodiment discloses a high-permeability self-healing component-release concrete, which is composed of the following parts by weight: 88 parts cement, 12 parts fly ash, 22 parts mineral powder, 5 parts silica fume, 150 parts fine aggregate, 200 parts coarse aggregate, 40 parts water, 1.2 parts polycarboxylate superplasticizer, 1.0 part basalt fiber, 0.75 parts composite repair agent and 13 parts composite carrier.
[0074] This embodiment discloses a method for preparing high-permeability, self-healing component-releasing concrete, including the following steps:
[0075] Step 1: Add the composite repair agent to the composite carrier (crushed and sieved, particle size 0.45-0.88mm), stir and mix at 480rpm for 25min, and let stand for 55min to obtain the composite carrier loaded with the composite repair agent.
[0076] Step 2: Add cement (PO 42.5 ordinary Portland cement), fly ash (Grade II fly ash), mineral powder (S95 grade granulated blast furnace slag powder), and silica fume (SiO2 mass fraction not less than 90%) to the mixer. Mix for 2 minutes, then add fine aggregate (natural sand with a fineness modulus of 2.4-2.8) and mix for 3 minutes. Add coarse aggregate (5-20mm continuously graded crushed stone) and mix for another 2 minutes. Then add water containing polycarboxylate superplasticizer and mix evenly to obtain a slurry. Then add basalt fiber and continue mixing for 3 minutes. Finally, add the composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0077] Example 5: This example discloses a method for preparing a composite repair agent, including the following steps:
[0078] Q1: Add 71g epoxy resin, 46g castor oil acid, 23g 4-benzyloxyphenol, 5g N,N-dimethylethanolamine and 0.28g triphenylphosphine to a container, heat to 152℃ and stir for 12min, then continue to heat to 221℃ and react for 4.5h. After the reaction is completed, cool to 160℃, add 6g dipropylene glycol methyl ether, stir and mix for 35min to obtain the prepolymer;
[0079] Q2: Heat 94g of prepolymer to 123℃, then add 7g of methyl methacrylate, 4g of N-hydroxymethylacrylamide and 1.26g of benzoyl peroxide in sequence. After reacting at this temperature for 1.5h, add 0.07g of benzoyl peroxide in two separate additions, each adding for 15min and then maintaining the temperature for 1.5h. Then add 5.8g of triethanolamine, stir and mix for 2h, and filter through a 90-mesh filter to obtain the composite repair agent.
[0080] This embodiment discloses a method for preparing a composite carrier, including the following steps:
[0081] S1: 11.5g of polytetrahydrofuran diol with an average molecular weight of 1000 was added to a container, heated to 116℃, and vacuum dehydrated for 1.5h. Then, the temperature was lowered to 80℃, and 8.30g of isophorone diisocyanate was added to the container under nitrogen atmosphere. Then, 19g of xylene containing 0.02g of dibutyltin dilaurate was added dropwise. After stirring and reacting for 3h, a polyurethane prepolymer was obtained.
[0082] S2: Add 20g of xylene containing 2.80g of 2,5-tetrahydrofurandimethylethanol to 13.0g of polyurethane prepolymer, stir and react at 112℃ for 3.5h under nitrogen atmosphere, then add 15g of xylene containing 2.08g of 4,4'-methylenebis(3-chloro-2,6-diethylaniline), and continue stirring and reacting for 3h. After the reaction is completed, polyurethane liquid is obtained.
[0083] S3: Add polyurethane liquid into a polytetrafluoroethylene mold, dry at 80°C for 22 hours, dissolve in N,N-dimethylformamide, and dry at 52°C for 10 hours and 81°C for 21 hours to obtain a composite carrier.
[0084] This embodiment discloses a high-permeability self-healing component-release concrete, which is composed of the following parts by weight: 83 parts cement, 18 parts fly ash, 18 parts mineral powder, 4 parts silica fume, 155 parts fine aggregate, 180 parts coarse aggregate, 42 parts water, 1.0 part polycarboxylate superplasticizer, 0.7 parts basalt fiber, 0.55 parts composite repair agent and 10 parts composite carrier.
[0085] This embodiment discloses a method for preparing high-permeability, self-healing component-releasing concrete, including the following steps:
[0086] Step 1: Add the composite repair agent to the composite carrier (crushed and sieved, particle size 0.45-0.88mm), stir and mix at 430rpm for 18min, and let stand for 45min to obtain the composite carrier loaded with the composite repair agent.
[0087] Step 2: Add cement (PO 42.5 ordinary Portland cement), fly ash (Grade II fly ash), mineral powder (S95 grade granulated blast furnace slag powder), and silica fume (SiO2 mass fraction not less than 90%) to the mixer. Mix for 2 minutes at a time. Then add fine aggregate (natural sand with a fineness modulus of 2.4-2.8) and mix for 2 minutes. Next, add coarse aggregate (5-20mm continuously graded crushed stone) and mix for another 2 minutes. Then add water containing polycarboxylate superplasticizer and mix evenly to obtain a slurry. Then add basalt fiber and continue mixing for 2 minutes. Finally, add the composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
[0088] Comparative Example 1: Compared with Example 1, Comparative Example 1 did not add composite repair agent and composite carrier during the preparation of concrete, and all other conditions remained unchanged.
[0089] Comparative Example 2: Compared with Example 1, Comparative Example 2 directly incorporated the composite repair agent during the concrete preparation process without adding a composite carrier, while keeping all other conditions unchanged.
[0090] Comparative Example 3: Compared with Example 1, Comparative Example 3 directly added a composite carrier during the concrete preparation process without loading a composite repair agent, while keeping other conditions unchanged.
[0091] Comparative Example 4: Compared with Example 1, Comparative Example 4 uses the prepolymer in Q1 instead of the composite repair agent in the concrete preparation process, while keeping other conditions unchanged.
[0092] Comparative Example 5: Compared with Example 1, Comparative Example 5 uses zeolite instead of composite carrier in the process of preparing concrete, while other conditions remain unchanged.
[0093] Comparative Example 6: Compared with Example 1, Comparative Example 6 did not add fibers during the preparation of concrete, while all other conditions remained unchanged.
[0094] Performance testing:
[0095] The concretes prepared in Examples 1-5 and Comparative Examples 1-6 were subjected to performance tests. The performance of the mixtures was tested according to GB / T 50080-2016 "Standard for Test Methods of Performance of Ordinary Concrete Mixtures", including slump, slump loss over time, apparent density, air content, bleeding rate, and segregation resistance, to evaluate the effects of the composite repair agent, composite carrier, and fiber incorporation on the workability, plasticity retention, and mixing stability of the concrete. The physical and mechanical properties of the samples were tested according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete", mainly including compressive strength, splitting tensile strength, flexural strength, static compressive modulus of elasticity, water absorption, hardened concrete density, and abrasion resistance. The long-term performance and durability of the samples were tested according to GB / T The tests were conducted according to GB / T 50082-2024, "Standard for Test Methods of Long-Term Performance and Durability of Concrete," mainly including resistance to water penetration, resistance to chloride ion penetration, shrinkage performance, early cracking performance, carbonation performance, resistance to sulfate attack, frost resistance, and resistance to gas penetration. After standard curing for 28 days, external force was applied to some specimens to form pre-existing cracks, and the crack width was controlled. The specimens were then placed in water immersion, seepage, or wet-dry cycle environments for healing curing. After healing, the water penetration resistance was retested according to GB / T 50082-2024, and the flexural strength or splitting tensile strength was retested according to GB / T 50081-2019. The crack closure rate (crack closure rate = (average crack width before healing - average crack width after healing) / average crack width before healing × 100%), the impermeability recovery rate, and the strength recovery rate were used as evaluation indicators for self-healing repair effect. The test results are shown in Table 1.
[0096] Table 1. Test results of the properties and compressive strength of each group of concrete mixtures
[0097]
[0098] Table 2. Test results of mechanical properties and some durability properties of concrete in each group.
[0099]
[0100] Table 3. Test results of long-term durability and post-cracking self-healing recovery performance of concrete in each group.
[0101]
[0102] As shown in Tables 1-3, the high-permeability self-healing component-release concretes obtained in Examples 1-5 are superior to those in Comparative Examples 1-6 in terms of mixture properties, mechanical properties, impermeability, self-healing performance, and long-term durability. This invention uses a composite carrier to load and protect the composite repair agent, reducing premature release of the repair agent during mixing and early hydration stages, and achieving directional release under crack propagation and seepage. This allows the repair agent to migrate and spread along the crack walls and capillary channels, forming a continuous and dense sealing layer.
[0103] From the perspective of the mixture properties, Examples 1-5 all exhibited good workability, low bleeding rate, and low segregation resistance index, indicating that the introduction of the composite carrier and composite repair agent did not significantly damage the stability of the concrete mixture. In particular, Examples 2 and 4, while maintaining high mechanical properties, still showed good mixing uniformity and low bleeding tendency.
[0104] From the perspective of mechanical properties, Examples 2 and 4 showed the best overall performance, indicating that the synergistic effect of a better water-cement ratio, higher active components of mineral admixtures, more suitable fiber content, and a better repair agent / carrier ratio can significantly improve the compressive strength, splitting tensile strength, and flexural strength of concrete. Example 3, due to its higher water content, lower composite repair agent content, and larger carrier content, had a lower strength level than the other examples, but it was still superior to most comparative examples, demonstrating that the system of the present invention has good comprehensive performance across a wide range of proportions.
[0105] In terms of durability, the maximum water penetration height, chloride ion migration coefficient, water absorption rate, carbonation depth, and gas permeability coefficient of Examples 1-5 were significantly lower than those of the comparative examples, indicating that the internal pore structure of the concrete obtained by the present invention is more compact and the medium transmission channels are effectively blocked. Meanwhile, the example group exhibited higher strength retention and relative dynamic modulus of elasticity in sulfate attack and freeze-thaw cycle tests, indicating better long-term service stability.
[0106] In terms of post-crack self-healing and recovery performance, the crack closure rate, impermeability recovery rate, and flexural strength recovery rate of Examples 1-5 were significantly higher than those of the comparative examples, with Examples 2 and 4 showing the best performance. Although Comparative Example 2 directly added a composite repair agent, which could improve the post-crack repair effect to some extent, its recovery effect was significantly lower than that of the Example group due to the lack of adsorption, storage, and controlled release of the repair agent by the composite carrier. Comparative Example 3 only added a composite carrier without loading the composite repair agent, and its self-healing and repair ability was only slightly improved. After replacing the composite carrier with zeolite, Comparative Example 5 had a certain adsorption effect, but due to the lack of a flexible organic structure and interfacial energy dissipation capacity, its impermeability recovery rate and strength recovery rate were still significantly lower than those of the Example group. When no fiber was added, Comparative Example 6 still had a certain post-crack repair ability, but due to the decreased crack control ability, the crack width was more easily expanded, so its self-healing and recovery effect was significantly worse than that of Example 1.
[0107] In summary, this invention, through the synergistic effect of composite repair agent, composite carrier and fiber, can not only improve the impermeability, erosion resistance and long-term durability of concrete, but also achieve more efficient self-healing repair under crack and leakage conditions, thereby significantly improving the service reliability and service life of concrete.
[0108] The above embodiments describe in detail the structure, features, and effects of the present invention. The above description is only a preferred embodiment of the present invention. Any changes made in accordance with the concept of the present invention, or equivalent embodiments modified to have equivalent changes, shall still fall within the scope of protection of the present invention if they do not exceed the scope covered by the specification.
[0109] Although embodiments of the invention have been disclosed for illustrative purposes, those skilled in the art will understand that various substitutions, variations, and modifications are possible without departing from the spirit and scope of the invention and the appended claims. Therefore, the scope of the invention is not limited to the contents disclosed in the embodiments.
Claims
1. A high-permeability, self-healing, component-releasing concrete, characterized in that: Includes composite repair agents and composite carriers; The preparation method of the composite repair agent includes the following steps: Q1: Add epoxy resin, ricinoleic acid, 4-benzyloxyphenol, N,N-dimethylethanolamine and triphenylphosphine to a container, heat and stir, continue to increase the temperature to react, cool down after the reaction is completed, add dipropylene glycol methyl ether, stir and mix to obtain the prepolymer; Q2: The prepolymer obtained in Q1 is heated, and then methyl methacrylate, N-hydroxymethylacrylamide and benzoyl peroxide are added in sequence. After the reaction is kept at the temperature, benzoyl peroxide is added and reacted. Then triethanolamine is added, stirred and mixed, and filtered to obtain the composite repair agent. The method for preparing the composite carrier includes the following steps: S1: Polytetrahydrofuran diol is added to a container, heated, dehydrated under vacuum, cooled, and under nitrogen atmosphere, isophorone diisocyanate is added to the container. Then xylene containing dibutyltin dilaurate is added dropwise, and the reaction is continued by stirring to obtain polyurethane prepolymer. S2: Add xylene containing 2,5-tetrahydrofurandimethyl alcohol to the polyurethane prepolymer obtained in S1, stir and react under nitrogen atmosphere, then add xylene containing 4,4'-methylenebis(3-chloro-2,6-diethylaniline), continue stirring and react, and after the reaction is completed, obtain polyurethane liquid. S3: Add the polyurethane liquid obtained in S2 into a polytetrafluoroethylene mold, dry it, add it into N,N-dimethylformamide for dissolution, dry it, and obtain a composite carrier.
2. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that, It is composed of the following components by weight: 80-90 parts cement, 10-20 parts fly ash, 15-25 parts mineral powder, 3-6 parts silica fume, 130-160 parts fine aggregate, 160-220 parts coarse aggregate, 30-45 parts water, 0.8-1.4 parts water-reducing agent, 0.5-1.2 parts fiber, 0.4-0.9 parts composite repair agent, and 8-15 parts composite carrier.
3. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that: In step Q1, the ratio of epoxy resin, ricinoleic acid, 4-benzyloxyphenol, N,N-dimethylethanolamine, triphenylphosphine, and dipropylene glycol methyl ether is (70-75) g : (40-48) g : (20-30) g : (4-7) g : (0.25-0.35) g : (5-9) g; the heating and stirring temperature is 150-160℃, and the stirring time is 10-20 min; the reaction temperature is further increased to 220-225℃, and the reaction time is 4-6 h; after the reaction is completed, the temperature is lowered to 160±5℃, and the stirring and mixing time is 30-45 min.
4. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that: In step Q2, the ratio of prepolymer, methyl methacrylate, N-hydroxymethylacrylamide, triethanolamine, and benzoyl peroxide is (88-95) g: (5-12) g: (3-6) g: (5-7.5) g: (1.2-1.8) g, where the amount of benzoyl peroxide is the sum of the initial addition and subsequent additions; the heat preservation reaction temperature is 120-130℃, and the heat preservation reaction time is 1-2 h; the addition of triethanolamine and stirring time is 1-3 h, and filtration is performed using an 80-100 mesh filter.
5. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that: In step S1, the ratio of polytetrahydrofuran diol, isophorone diisocyanate, dibutyltin dilaurate, and xylene is (10-12) g: (8.12-8.94) g: (0.01-0.04) g: (18-22) g, and the average molecular weight of the polytetrahydrofuran diol is 900-1100. The temperature is raised to 115-120℃, vacuum dehydration is carried out for 1-2 hours, the temperature is lowered to 80-82℃, and the reaction is continued with stirring for 2-4 hours.
6. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that: In step S2, the ratio of 2,5-tetrahydrofurandimethyl alcohol, polyurethane prepolymer, and 4,4'-methylenebis(3-chloro-2,6-diethylaniline) is (2.56-3.42) g : (12.53-14.69) g : (2.01-2.25) g. The stirring reaction temperature is 110-120℃, the time is 3-5 h, and the continued stirring reaction time is 2-4 h.
7. The high-permeability self-healing component-releasing concrete according to claim 1, characterized in that: In step S3, the drying temperature before dissolution is 80-82℃ and the time is 20-24h. The drying process after dissolution is as follows: first, drying at 50-55℃ for 10-12h, and then drying at 80-84℃ for 20-24h.
8. A method for preparing high-permeability self-healing component-releasing concrete according to claim 1, characterized in that, Includes the following steps: Step 1: Add the composite repair agent to the composite carrier, stir and mix, and let stand to obtain the composite carrier loaded with the composite repair agent; Step 2: Add cement, fly ash, mineral powder and silica fume to the mixer and mix once. Then add fine aggregate and mix. Add coarse aggregate and mix again. Then add water containing water-reducing agent and mix evenly to obtain slurry. Then add fiber and continue mixing. Finally, add composite carrier loaded with composite repair agent and mix evenly to obtain high-permeability self-healing component release concrete.
9. The method for preparing high-permeability self-healing component-releasing concrete according to claim 8, characterized in that: In step 1, the stirring speed is 400-500 rpm, the time is 10-30 min, and the settling time is 40-60 min.
10. The method for preparing high-permeability self-healing component-releasing concrete according to claim 8, characterized in that: In step 2, the first mixing time is 1-3 minutes, the stirring and mixing time is 2-4 minutes, the second mixing time is 1-3 minutes, the second mixing time is the mixing time after adding coarse aggregate, and the continued stirring time is 2-4 minutes.