Highly impermeable prestressed concrete precast slab and method for manufacturing the same
By combining various auxiliary materials and improving the process, the problems of early cracking and insufficient impermeability of UHPC precast slabs under mass production conditions were solved, realizing the preparation of high impermeability prestressed concrete precast slabs and improving their compressive strength and impermeability performance.
Patent Information
- Application Number
- CN202611560827.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional UHPC precast panels suffer from early cracking, insufficient impermeability, and difficulty in meeting durability standards under mass production conditions. In particular, the weak bonding between steel fibers and the matrix, low water-cement ratio, and resulting self-shrinking microcracks and poor impermeability are due to these issues.
By employing a variety of auxiliary materials and process improvements, including phosphated modified steel fibers, pre-wetted shale ceramsite internal curing, fiber-powder pre-dispersion, pre-tensioning pre-stressing, and layered pouring with secondary vibration, high impermeability prestressed concrete precast slabs are formed.
It improves the bond strength between fibers and the matrix, suppresses interfacial microcracks, enhances the compressive strength and flexural toughness of concrete, and significantly improves the impermeability of precast slabs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of precast concrete slab technology, specifically a high impermeability prestressed concrete precast slab and its preparation method. Background Technology
[0002] In the standardized manufacturing system of prefabricated buildings and highway and municipal engineering, the manufacturing of reinforced concrete prefabricated frames and other concrete structural components with large demand, such as reinforced concrete prefabricated frames and bridge prefabricated decks, has long faced common industry problems such as early cracking under mass production conditions, insufficient impermeability stability, and difficulty in meeting later durability standards. Ultra-high performance concrete (UHPC) has been gradually promoted and applied due to its excellent mechanical strength, fracture toughness and matrix density. It can not only significantly reduce the structural cross-sectional size and total material usage, but also provide a feasible path for the comprehensive performance upgrade of prefabricated frame beams and columns, bridge prefabricated decks and other components.
[0003] As the core reinforcing component in the UHPC system that plays a bridging and crack-resistant role, steel fibers are conventionally used to optimize the impermeability of concrete by adding modifiers such as organic latex. However, the surface of steel fibers after being coated with an anti-rust layer lacks active groups, and the interfacial adhesion between organic latex and steel fibers is weak. It can only fill some of the pores in the matrix through physical filling. Under the long-term service of bridge dynamic loads and environmental temperature changes, organic latex is prone to peeling off from the surface of steel fibers and cement matrix. This not only completely loses the original impermeability effect, but also generates new pores and connecting gaps at the peeling interface, which greatly widens the chloride ion penetration channels.
[0004] Chinese invention patent application CN112430039A discloses an ultra-high performance concrete and its preparation method. The method involves modifying the surface of steel fibers. First, the surface of the steel fibers is wiped with acetone. Then, the steel fibers are immersed in a 3.5-4.5% zinc phosphate solution at room temperature for 2-3 hours to obtain modified steel fibers. This zinc phosphate modification technology coats the surface of the steel fibers with a phosphate film of several micrometers. The phosphate film improves the frictional properties of the steel fiber surface, increases the surface roughness of the steel fibers, and enhances the adhesion between the steel fibers and the ultra-high performance concrete, thereby improving its toughness in the ultra-high performance concrete and further enhancing the strength and crack resistance of the ultra-high performance concrete.
[0005] However, when the above-mentioned solutions are implemented in industrial production and manufacturing, the following shortcomings still exist: the room temperature phosphating treatment has a long cycle and low efficiency; the surface modification effect of steel fibers is unstable; the fiber-matrix interface bonding is weak; at the same time, the water-cement ratio of ultra-high performance concrete is low, and self-shrinkage stress is easily generated during hydration, which can lead to microcracks. As a result, the impermeability and mechanical properties of precast slabs are difficult to consistently meet the standards. Furthermore, the long-term soaking process is also difficult to meet the requirements for large-scale continuous production, which limits the engineering application of this process in the manufacture of reinforced concrete precast frames and other concrete structural components. Summary of the Invention
[0006] The purpose of this invention is to provide a high-permeability prestressed concrete slab and its preparation method. By compounding various auxiliary materials, phosphated modified steel fibers, internal curing with pre-wetted shale ceramsite sand and fiber-powder pre-dispersion, pre-tensioning pre-stressing, layered pouring and secondary vibration, and graded release, the problem of poor permeability of traditional UHPC precast slabs caused by numerous original pores in the matrix, weak fiber-matrix interface bonding, and self-shrinkage microcracks due to low water-cement ratio is solved.
[0007] The objective of this invention can be achieved through the following technical solutions: A method for preparing a high-permeability prestressed concrete precast slab includes the following steps: Step 1: Phosphate and pre-wet the pre-treated and activated end-hook steel fibers and shale ceramic sand respectively to obtain phosphated modified steel fibers and pre-wetted shale ceramic sand; Step 2: Put silicate cement, fly ash, S95 grade mineral powder, mixed quartz sand and basalt crushed stone into a mixer and dry mix at a speed of 40-50 r / min for 1-2 min. First, add water-reducing agent solution accounting for 1 / 3 of the total volume of the water-reducing agent solution and stir at a speed of 40-60 r / min for 0.5-1 min. Then, sprinkle fiber-powder pre-dispersion through a vibrating feeder and stir for 1-1.5 min. Then, add the remaining water-reducing agent solution and pre-wetted shale ceramsite sand and continue stirring at a speed of 70-80 r / min for 2-2.5 min to obtain concrete mixture. Step 3: First, tension the concrete in stages on the tensioning platform, then pour the concrete mixture in layers and vibrate it to form the shape. After in-situ curing with moisture until the strength reaches the standard, release the tension in stages and then transfer it to the standard curing room for continued moisture curing to obtain a high-permeability prestressed concrete precast slab.
[0008] Furthermore, the specific preparation method of the phosphate-modified steel fiber in step one is as follows: The pretreated and activated end-hook steel fibers are placed into a porous PP mesh basket and immediately immersed in the phosphating solution. They are then soaked in a 75°C water bath for 20 minutes, during which the mesh basket is shaken for 10-15 seconds every 2-3 minutes. After removal, they are rinsed with deionized water 3-5 times and dried at 60-80°C for 10-20 minutes to obtain phosphated modified steel fibers.
[0009] The aperture of the above-mentioned porous PP mesh basket is 1-2mm.
[0010] Furthermore, the specific preparation method of the pre-wetted shale ceramic sand in step one is as follows: Completely immerse the shale ceramic sand in deionized water at room temperature for 72 hours, stirring occasionally. After soaking, pour off the excess water, place the wet ceramic sand on a non-absorbent steel tray, cover its surface with paper towels, and replace the paper towels with new ones after they are completely wet. Repeat this process until no water stains appear on the paper towels. At this point, the ceramic sand has reached a saturated surface-dry state with a saturated water absorption rate of 15-20%, thus obtaining pre-wetted shale ceramic sand.
[0011] The shale ceramic sand consists of 3-5mm continuously graded particles; the pre-wetted shale ceramic sand needs to be covered with a damp cloth for storage.
[0012] Furthermore, in step two, the mass ratio of silicate cement, fly ash, S95 grade mineral powder, mixed quartz sand, basalt crushed stone, and fiber-powder pre-dispersion is 410-430:50-60:150-180:560-640:560-640:175-205.
[0013] Furthermore, the specific preparation method of the fiber-powder pre-dispersion in step two is as follows: Phosphated modified steel fibers, silica fume, and Wernbinder are premixed in a mixer at a speed of 400-600 r / min for 30-40 s to prepare a fiber-powder predispersant.
[0014] The mass ratio of the above-mentioned phosphated modified steel fiber, silica fume and Wenlun rubber is 140-160:35-45:0.05-0.1.
[0015] Furthermore, the specific preparation method of the water-reducing agent solution in step two is as follows: A polycarboxylate superplasticizer with a solid content of 99% was dissolved in deionized water to obtain a superplasticizer solution.
[0016] The ratio of the above-mentioned polycarboxylate superplasticizer to deionized water is 22-26g: 125-150mL.
[0017] Furthermore, in step three, the tensile strength is increased to 0.70-0.75 times the standard tensile strength value in stages, with each stage held for 3-5 minutes.
[0018] Furthermore, the specific preparation method for layered pouring and vibration compaction of the concrete mixture in step three is as follows: The concrete mixture is poured in two layers. First, pour the mixture to half the height of the mold, turn on the vibrating table and vibrate for 15-20 seconds, then let it stand for 3-5 minutes. Then pour the remaining concrete mixture and vibrate it again for 8-10 seconds. After smoothing the surface, cover it with plastic film and let it stand at room temperature for 36-48 hours. After the compressive strength of the test blocks under the same conditions reaches 60% of the design strength, the mold is removed.
[0019] Furthermore, the in-situ moisturizing maintenance method in step three involves covering the surface with a water-retaining cloth, sprinkling water regularly to keep the surface moist, and controlling the ambient temperature at 18-22℃.
[0020] Furthermore, the specific preparation method for the graded release in step three is as follows: When the compressive strength of the test block cured under the same conditions reaches 90% of the design strength and the curing period reaches 7 days or more, the tension can be released. The tension is released slowly in stages using hydraulic jacks. The tension control stress is gradually reduced from 100% to 80%, 60%, 30%, and 0, with each stage held for 3-5 minutes to ensure that each steel strand is released symmetrically. After all steel strands have completely released the tension, the excess steel strands are cut off symmetrically and step by step using a grinding wheel.
[0021] Furthermore, in step three, the temperature of the standard curing room is 20±2℃, the humidity is ≥95%, and the curing time is 14-28 days.
[0022] The beneficial effects of this invention are: 1. This invention employs two methods in the formulation of ultra-high performance concrete: modification with a zinc phosphate conversion film on the surface of steel fibers and internal curing with pre-wetted shale ceramsite. The zinc phosphate conversion film on the steel fiber surface prevents premature deterioration of the fibers in a high-alkali environment, improves the bond strength between the fibers and cement paste, and makes the interfacial transition zone denser. The pre-wetted shale ceramsite compensates for the self-shrinkage of the low water-cement ratio system through the slow release of internal pore water, while avoiding the formation of continuous permeation channels, thus helping to refine the pore structure and reduce interconnected porosity. These two measures work synergistically to inhibit the generation and propagation of interfacial microcracks, effectively improving the impermeability of precast slabs while enhancing the compressive strength and flexural toughness of concrete.
[0023] 2. In the preparation process of ultra-high performance concrete mixture, this invention utilizes the synergistic effect of powder pre-dispersion and staged feeding and mixing. First, the functional modified components are pre-mixed with silica fume and Wernite at high speed to form a pre-dispersion. Then, through staged water addition and feeding, the uniform distribution of each component is ensured, preventing damage to the functional components due to premature contact with dry, hard aggregates. This process, combined with the aforementioned steel fiber phosphate modification and pre-wetted shale ceramsite internal curing methods, helps to achieve uniform and stable interfacial strengthening and internal curing effects within the matrix. While maintaining the high toughness brought by the 2% high-content hook-shaped steel fiber, it also preserves the original working performance and imparts high impermeability to the finished precast slabs. Detailed Implementation
[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0025] Example 1: A method for preparing a high-permeability prestressed concrete precast slab, comprising the following steps: S1: 140g of pretreated and activated end-hook steel fibers are placed into a porous PP mesh basket with a pore size of 1mm and immediately immersed in phosphating solution. The basket is then soaked in a 75℃ water bath for 20min, with the basket shaken for 10s every 2min during the soaking period to ensure that the phosphating solution fully contacts the fiber surface. After removal, the fibers are rinsed 3 times with deionized water and dried at 60℃ for 10min to obtain phosphated modified steel fibers.
[0026] S2: Select 180g of 3-5mm continuously graded shale ceramic sand, completely immerse it in deionized water at room temperature (20℃) for 72 hours, stirring appropriately during the soaking process. After soaking, pour off the excess water, place the wet ceramic sand on a non-absorbent steel tray, cover its surface with paper towels, and replace the paper towels with new ones after they are completely wet. Repeat this process until no water stains appear on the paper towels. At this point, the ceramic sand has reached a saturated surface-dry state, and the pre-wetted shale ceramic sand is obtained.
[0027] Pre-wetted shale clay sand, covered with a damp cloth, serves as the internal curing water source for concrete. During cement hydration, it slowly releases moisture, compensating for the self-shrinkage of the low water-cement ratio system and inhibiting the initiation of microcracks in the matrix. On the other hand, it continuously maintains a high-humidity environment at the fiber-matrix interface. In this high-humidity alkaline environment, calcium ions released during cement hydration react with the zinc phosphate conversion film on the surface of phosphate-modified steel fibers, generating hydroxyapatite whiskers in situ. These whiskers fill and densify the fiber-matrix interface transition zone. The internal curing's inhibition of microcracks and its interface reinforcement work synergistically to optimize the interface structure.
[0028] S3: 140g of the phosphated modified steel fiber obtained in step S1, 35g of silica fume and 0.05g of Wernbinder are premixed in a mixer at a speed of 400r / min for 30s to prepare a fiber-powder predispersant; 22g of polycarboxylate superplasticizer with a solid content of 99% is dissolved in 125mL of deionized water to obtain a superplasticizer solution; Add 410g of silicate cement, 50g of fly ash, 150g of S95 grade mineral powder, 560g of mixed quartz sand, and 560g of basalt crushed stone to a mixer and dry mix at 40r / min for 1min. First, add 47mL of water-reducing agent solution (accounting for 1 / 3 of the total volume of water-reducing agent solution) and mix at 40r / min for 0.5min. Then, evenly sprinkle 175g of fiber-powder pre-dispersion through a vibrating feeder and mix for 1min. Next, add 94mL of water-reducing agent solution (accounting for 2 / 3 of the total volume of water-reducing agent solution) and the pre-wetted shale ceramsite sand obtained in step S2 and mix at 70r / min for 2min to obtain the concrete mixture.
[0029] S4: Arrange ordinary steel strands at the designed spacing on the tensioning platform fixed to the ground, tension them in stages to 0.70 times the standard value of tensile strength, hold the load for 3 minutes at each stage, lock the anchor, set up the steel mold and apply water-based release agent, pour the concrete mixture obtained in step S3 in two layers, first pour to half the height of the mold, turn on the vibrating table to vibrate for 15 seconds, stop for 3 minutes, then pour the remaining concrete mixture and vibrate it again for 8 seconds. The second vibration helps to remove air bubbles and improve the density. After smoothing the surface, cover it with plastic film and let it stand at room temperature (20℃) for 36 hours. After the compressive strength of the test block under the same conditions reaches 60% of the design strength, remove the mold to obtain the prestressed concrete slab to be released.
[0030] S5: After demolding, the precast slab remains on the tensioning platform, and the steel strands are kept in a tensioned and locked state. They must not be moved or hoisted. Then, the precast slab and the test blocks cured under the same conditions are subjected to in-situ moisturizing curing: covered with water-retaining cloth, water is sprayed regularly to keep the surface moist, and the curing environment temperature is controlled at 18℃. When the compressive strength of the test blocks cured under the same conditions reaches 90% of the design strength and the curing age reaches 7 days or more, the tension can be released. The overall staged release is carried out slowly using hydraulic jacks. The tension control stress is reduced from 100% to 80%, 60%, 30%, and 0% in stages, with each stage held for 3 minutes to ensure that each steel strand is released symmetrically and to avoid local stress concentration. After confirming that all steel strands have completely released the tension, the excess steel strands are symmetrically and stepwise removed with a grinding wheel. After the removal is completed, the precast slab is transferred to a standard curing room (temperature 18℃, humidity ≥95%) for continued moisturizing curing for 14 days to obtain a high-permeability prestressed concrete precast slab.
[0031] Example 2: A method for preparing a high-permeability prestressed concrete precast slab, comprising the following steps: S1: 150g of pretreated and activated end-hook steel fibers are placed into a porous PP mesh basket with a pore size of 1.5mm and immediately immersed in the phosphating solution. The basket is then soaked in a 75℃ water bath for 20min, during which the basket is shaken for 12.5s every 2.5min to ensure that the phosphating solution fully contacts the fiber surface. After removal, the fiber is rinsed 4 times with deionized water and dried at 70℃ for 15min to obtain phosphated modified steel fibers.
[0032] S2: Select 200g of 3-5mm continuously graded shale ceramic sand, completely immerse it in deionized water at room temperature (22.5℃) for 72 hours, stirring appropriately during the soaking process. After soaking, pour off the excess water, place the wet ceramic sand on a non-absorbent steel tray, cover its surface with paper towels, and replace the paper towels with new ones after they are completely wet. Repeat this process until no water stains appear on the paper towels. At this point, the ceramic sand has reached a saturated surface-dry state, and the pre-wetted shale ceramic sand is obtained.
[0033] S3: 150g of the phosphated modified steel fiber obtained in step S1, 40g of silica fume and 0.075g of Wernite are premixed in a mixer at a speed of 500r / min for 35s to prepare a fiber-powder predispersant; 24g of polycarboxylate superplasticizer with a solid content of 99% is dissolved in 137.5mL of deionized water to obtain a superplasticizer solution; 420g of silicate cement, 55g of fly ash, 165g of S95 grade mineral powder, 600g of mixed quartz sand, and 600g of basalt crushed stone were put into a mixer and dry-mixed at 45r / min for 1.5min. First, 52mL of water-reducing agent solution (accounting for 1 / 3 of the volume of water-reducing agent solution) was added and stirred at 50r / min for 0.75min. Then, 190g of fiber-powder pre-dispersion was evenly sprinkled in through a vibrating feeder and stirred for 1.25min. Next, 105mL of water-reducing agent solution (accounting for 2 / 3 of the volume of water-reducing agent solution) and the pre-wetted shale ceramsite sand obtained in step S2 were added and stirred at 75r / min for 2.25min to obtain the concrete mixture.
[0034] S4: Arrange ordinary steel strands at the designed spacing on the tensioning platform fixed to the ground, tension them in stages to 0.725 times the standard value of tensile strength, hold the load for 4 minutes at each stage, lock the anchor, set up the steel mold and apply water-based release agent, pour the concrete mixture obtained in step S3 in two layers, first pour to half the height of the mold, turn on the vibrating table to vibrate for 17.5s, stop for 4 minutes, then pour the remaining concrete mixture and vibrate it again for 9s. The second vibration helps to remove air bubbles and improve the density. After smoothing the surface, cover it with plastic film and let it stand at room temperature (22.5℃) for 42 hours. After the compressive strength of the test block under the same conditions reaches 60% of the design strength, remove the mold to obtain the prestressed concrete slab to be released.
[0035] S5: After demolding, the precast slab remains on the tensioning platform, and the steel strands are kept in a tensioned and locked state. They must not be moved or hoisted. Then, the precast slab and the test blocks cured under the same conditions are subjected to in-situ moisturizing curing: covered with water-retaining cloth, water is sprayed regularly to keep the surface moist, and the curing environment temperature is controlled at 20℃. When the compressive strength of the test blocks cured under the same conditions reaches 90% of the design strength and the age reaches 7 days or more, the tension can be released. The overall staged release is carried out slowly using hydraulic jacks. The tension control stress is reduced from 100% to 80%, 60%, 30%, and 0% in stages, with each stage held for 4 minutes to ensure that each steel strand is released symmetrically and to avoid local stress concentration. After confirming that all steel strands have completely released the tension, the excess steel strands are symmetrically and stepwise removed with a grinding wheel. After the removal is completed, the precast slab is transferred to a standard curing room (temperature 20℃, humidity ≥95%) for continued moisturizing curing for 21 days to obtain a high-permeability prestressed concrete precast slab.
[0036] Example 3: A method for preparing a high-permeability prestressed concrete precast slab, comprising the following steps: S1: 160g of pretreated and activated end-hook steel fibers are placed into a porous PP mesh basket with a pore size of 2mm and immediately immersed in the phosphating solution. The basket is then soaked in a 75℃ water bath for 20min, with the basket shaken for 15s every 3min during the soaking process to ensure that the phosphating solution fully contacts the fiber surface. After removal, the fibers are rinsed 5 times with deionized water and dried at 80℃ for 20min to obtain phosphated modified steel fibers.
[0037] S2: Select 220g of 3-5mm continuously graded shale ceramic sand, completely immerse it in deionized water at room temperature (25℃) for 72h, stirring appropriately during the soaking process. After soaking, pour off the excess water, place the wet ceramic sand on a non-absorbent steel tray, cover its surface with paper towels, and replace the paper towels with new ones after they are completely wet. Repeat this process until no water stains appear on the paper towels. At this point, the ceramic sand has reached a saturated surface-dry state, and the pre-wetted shale ceramic sand is obtained.
[0038] S3: 160g of phosphated modified steel fiber obtained in step S1, 45g of silica fume and 0.1g of Wernbinder are premixed in a mixer at a speed of 600r / min for 40s to prepare fiber-powder predispersant; 26g of polycarboxylate superplasticizer with a solid content of 99% is dissolved in 150mL of deionized water to obtain superplasticizer solution. 430g of silicate cement, 60g of fly ash, 180g of S95 grade mineral powder, 640g of mixed quartz sand and 640g of basalt crushed stone were put into a mixer and dry-mixed at 50r / min for 2min. First, 57mL of water-reducing agent solution (accounting for 1 / 3 of the volume of water-reducing agent solution) was added and stirred at 60r / min for 1min. Then, 205g of fiber-powder pre-dispersion was evenly sprinkled in through a vibrating feeder and stirred for 1.5min. Then, 114mL of water-reducing agent solution (accounting for 2 / 3 of the volume of water-reducing agent solution) and the pre-wetted shale ceramsite sand obtained in step S2 were added and stirred at 80r / min for 2.5min to obtain concrete mixture.
[0039] S4: Arrange ordinary steel strands at the designed spacing on the tensioning platform fixed to the ground, tension them in stages to 0.75 times the standard value of tensile strength, hold the load for 5 minutes at each stage, lock the anchor, set up the steel mold and apply water-based release agent, pour the concrete mixture obtained in step S3 in two layers, first pour to half the height of the mold, turn on the vibrating table to vibrate for 20 seconds, stop for 5 minutes, then pour the remaining concrete mixture and vibrate it again for 10 seconds. The second vibration helps to remove air bubbles and improve the density. After smoothing the surface, cover it with plastic film and let it stand at room temperature (25℃) for 48 hours. After the compressive strength of the test block under the same conditions reaches 60% of the design strength, remove the mold to obtain the prestressed concrete slab to be released.
[0040] S5: After demolding, the precast slab remains on the tensioning platform, and the steel strands are kept in a tensioned and locked state. They must not be moved or hoisted. Then, the precast slab and the test blocks cured under the same conditions are subjected to in-situ moisturizing curing: covered with water-retaining cloth, water is sprayed regularly to keep the surface moist, and the curing environment temperature is controlled at 22℃. When the compressive strength of the test blocks cured under the same conditions reaches 90% of the design strength and the age reaches 7 days or more, the tension can be released. The overall staged release is carried out slowly using hydraulic jacks. The tension control stress is reduced from 100% to 80%, 60%, 30%, and 0% in stages, with each stage held for 5 minutes to ensure that each steel strand is released symmetrically and to avoid local stress concentration. After confirming that all steel strands have completely released the tension, the excess steel strands are symmetrically and stepwise removed with a grinding wheel. After the removal is completed, the precast slab is transferred to a standard curing room (temperature 22℃, humidity ≥95%) for continued moisturizing curing for 28 days to obtain a high-permeability prestressed concrete precast slab.
[0041] In Examples 1-3, the phosphated modified steel fibers obtained in step S1 all formed a uniform gray-black phosphate film on their surface, without rust spots, exposed substrate, or powdering; the phosphate film weight was 2.1 g / m³. 2 2.3g / m 2 3.1g / m 2 All are between 2-5 g / m 2Within the specified range, the above-mentioned steel fibers were immersed in a simulated concrete pore solution with a pH value of 12.6-13.0 for 24-72 hours. It was observed that the phosphated film did not show obvious dissolution or peeling, indicating that the phosphated modified steel fibers prepared in Examples 1-3 had qualified alkali resistance.
[0042] The pre-wetted shale ceramsite prepared in step S2 of Examples 1-3 was subjected to a saturated water absorption test according to the method for measuring the water absorption rate of lightweight aggregates for internal curing in ASTM C1761 "Standard Specification for Lightweight Aggregates for Internal Curing of Concrete". The mass of the saturated surface-dry sample M1 was weighed, and then it was placed in an oven at 110±5℃ for 24 hours to dry. After cooling, the dry mass M3 was weighed. The saturated water absorption rate was calculated as: saturated water absorption rate = (M1-M3) / M3×100%. The calculated 72-hour saturated water absorption rates of the pre-wetted shale ceramsite used in Examples 1, 2, and 3 were 18.2%, 19.5%, and 18.8%, respectively, all within the range of 15-20%. This indicates that the shale ceramsite used in the examples has a stable and sufficient water absorption capacity. After pre-wetting, it can play a role in water retention and curing inside the concrete, which is beneficial for compensating for autogenous shrinkage and improving impermeability.
[0043] In Examples 1-3, the hook-shaped steel fibers were purchased from Hebei Anyin Construction Engineering Group Co., Ltd.; shale ceramsite sand was purchased from Chongqing Pinhetai Building Materials Co., Ltd., with a specification of 3-5mm; polycarboxylate superplasticizer was purchased from Jinan Ruihongde Chemical Technology Co., Ltd., with a solid content of 99%; silicate cement was purchased from Guangzhou Yaowei Building Materials Co., Ltd., model P.Ⅱ52.5R; fly ash was purchased from Lingshou County Erping Mineral Products Processing Plant; silica fume was purchased from Lingshou County Yongshun Mineral Products Processing Plant; S95 grade mineral powder was purchased from Lingshou County Erping Mineral Products Processing Plant; basalt crushed stone was purchased from Lingshou County Chengwang Mineral Products Co., Ltd., with a specification of 10mm; water-based release agent was purchased from Handan Shengaochang Metal Products Co., Ltd.; the rest were commercially available raw materials.
[0044] The specific preparation steps of the end-hook type steel fiber pretreatment in Examples 1-3 are as follows: After grinding and polishing, the end-hook steel fibers are sequentially subjected to alkaline washing and degreasing in a 10% NaOH solution at 50°C for 10 minutes, acid washing and rust removal in a 25% H2SO4 solution at 60°C for 5 minutes, and surface activation treatment in a 25% H3PO4 solution at room temperature for 5 minutes. The fibers are rinsed with deionized water between each step to obtain pre-treated and activated end-hook steel fibers.
[0045] The specific preparation steps of the phosphating solution in Examples 1-3 are as follows: Weigh 8.0g of ZnO powder and add distilled water, stirring until a paste is formed. Add 20.0mL of 85% H3PO4 solution, then add 1.0g of citric acid, 0.5g of Ca(NO3)2, and 0.5g of Zn(NO3)2 in sequence. Finally, add distilled water to a final volume of 1L to obtain the phosphating solution.
[0046] In Examples 1-3, the mixed quartz sand was composed of 40-70 mesh and 20-40 mesh quartz sand in a mass ratio of 1:1; the 40-70 mesh and 20-40 mesh quartz sand were purchased from Lingshou County Chuanqing Mineral Products Co., Ltd.
[0047] Comparative Example 1: The difference from Example 1 is that in step S1, the steel fibers were not phosphated, and the pre-treated and activated end-hook type steel fibers (i.e., not immersed in phosphate solution) were used directly. The remaining steps remained unchanged, and a high-permeability prestressed concrete precast slab was obtained.
[0048] Comparative Example 2: The difference from Example 1 is that in step S2, non-porous ordinary crushed stone of equal mass and particle size is used to replace the pre-wetted shale ceramsite sand, while the other steps remain unchanged, resulting in a high-permeability prestressed concrete precast slab.
[0049] Comparative Example 3: The difference from Example 1 is that in step S3, fiber-powder pre-dispersion and staged feeding and mixing are not performed. Instead, equal masses of phosphated modified steel fiber, silica fume, and Wenlun adhesive are dry-mixed with equal masses of cement, fly ash, mineral powder, quartz sand, and basalt crushed stone for 1-2 minutes. Then, an equal volume of the entire water-reducing agent solution is added at once and stirred for 3-4 minutes. Finally, pre-wetted shale ceramsite sand is added and stirred for another 1-2 minutes. The remaining steps remain unchanged to obtain a high-permeability prestressed concrete precast slab.
[0050] The compressive strength, flexural strength, and chloride ion penetration resistance of the high-permeability prestressed concrete precast slabs prepared in Examples 1-3 and Comparative Examples 1-3 were tested. The autogenous shrinkage rate and workability of the concrete mixtures obtained in step S3 of Examples 1-3 and Comparative Examples 1-3 were tested, as follows: (1) Compressive strength: Referring to T / CECS 864-2021 "Standard for Test Methods of Ultra-High Performance Concrete", 100mm×100mm×100mm cubic specimens were used and cured to the specified age. Six specimens were prepared for each group of Examples 1-3 and Comparative Examples 1-3. After checking that the specimen size, the pressure plate of the press and the steel pad meet the specifications, the specimens were loaded at a rate of 1.2MPa / s on a 2000kN pressure testing machine until failure. The failure load P was recorded. cu =P / A is used to calculate the compressive strength of a cube, where A is the area of the specimen subjected to compression (mm²). 2 ).
[0051] (2) Flexural strength: The test was conducted in accordance with T / CECS 864-2021 "Standard for Test Methods of Ultra-High Performance Concrete". Three prism specimens with dimensions of 100mm×100mm×400mm were used in each group of Examples 1-3 and Comparative Examples 1-3 for four-point flexural strength tests. The loading rate was 0.1MPa / s. The tests were conducted in a 30-ton universal testing machine (WDW-300 type). The flexural strength was calculated by recording the data through the testing machine. ƒ=FL / (bh 2 ), where: ƒ is the flexural strength of the prism (MPa), F is the failure load of the prism (N); L is the spacing of the bottom supports (mm); b is the width of the prism cross section (mm); h is the height of the prism cross section (mm).
[0052] (3) Chloride ion penetration resistance: The chloride ion penetration resistance of specimens in Examples 1-3 and Comparative Examples 1-3 was tested according to the Rapid Chloride Ion Migration Coefficient Method (RCM Method) in GB / T 50082-2024 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" for 56 days. The specimens were 100mm×100mm×50mm in size, and their chloride ion migration coefficient was tested.
[0053] (4) Autogenous shrinkage rate: The test was conducted according to the non-contact method in GB / T 50082—2024 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". Equal amounts of concrete mixtures obtained in step S3 of Examples 1-3 and Comparative Examples 1-3 were cast into prism specimens of 100mm×100mm×515mm for testing. The test section length was 450mm. The mold was lined with PVC film and coated with lubricant to eliminate friction. The surface of the specimen was covered with plastic film to prevent moisture evaporation. The final setting time was taken as zero point. The specimens were cured at a constant temperature of 20±2℃ for 56 days and then tested. The autogenous shrinkage rate was calculated by the ratio of displacement change to test section length.
[0054] (5) Workability (spreadability): Spreadability test was conducted in accordance with T / CECS 864-2021 "Standard for Test Methods of Ultra-High Performance Concrete". Ensure that the inner wall of the slump test tube is wet but without water accumulation. Place it in the center of the spreadability plate and pour equal amounts of concrete mixtures obtained in step S3 of Examples 1-3 and Comparative Examples 1-3 into the tube. Smooth the excess mortar on the surface with a trowel. Lift the tube at a uniform speed within 3-7 seconds. When the slurry stops flowing, measure the maximum spread diameter. The standard qualified spreadability range is 550-750 mm.
[0055] The results are shown in Table 1: Table 1 Performance test results of concrete specimens and concrete mixtures in each example / comparative example As can be seen from Table 1, compared with the comparative examples, the high impermeability prestressed concrete precast slabs prepared in Examples 1-3 and the concrete mixture prepared in step S3 have higher compressive strength and flexural strength, lower chloride ion migration coefficient and self-shrinkage rate, while ensuring that the workability meets the construction requirements. Phosphating modification reduces the friction between fibers, and the pre-dispersion process improves the fiber distribution, thereby mitigating the negative impact of end-hooked fibers on flowability, and the spread is qualified.
[0056] The flexural strength and chloride ion penetration resistance of Comparative Example 1 were significantly worse than those of the Example. This is because omitting the phosphating process of the steel fibers resulted in the lack of protection and interfacial strengthening effect of the zinc phosphate conversion film on the surface of the steel fibers. This led to increased porosity and reduced bond strength in the fiber-matrix interface transition zone. As a weak link in concrete, this interface zone is prone to microcracks under load and self-shrinkage stress, which are interconnected with the capillaries inside the matrix, forming continuous chloride ion penetration channels. This resulted in an increased chloride ion migration coefficient and poor impermeability. At the same time, the steel fibers were directly exposed to the highly alkaline pore solution of the concrete, further weakening the long-term reinforcing effect of the fibers and the density of the matrix.
[0057] The self-shrinkage rate and chloride ion migration coefficient of Comparative Example 2 were significantly higher than those of Example 2. This is because without the introduction of pre-wetted shale ceramsite, the ultra-low water-cement ratio system lacked internal moisture replenishment in the later stages of cement hydration, which intensified the self-drying of capillaries. The resulting self-shrinkage stress formed a microcrack network in the matrix. At the same time, due to the lack of internal curing water, the degree to which hydration products filled the capillaries decreased, and the interconnected porosity of the matrix increased, thus affecting the impermeability.
[0058] The compressive strength, flexural strength, and spread of Comparative Example 3 were significantly lower than those of the Example. This is because after eliminating the pre-dispersion of powder and the staged feeding and mixing, the functional modified components came into intense mechanical contact with the coarse aggregate during the dry mixing stage, resulting in damage to some of the zinc phosphate conversion film. At the same time, the uniformity of the components in the ultra-low water-binder ratio slurry decreased, and local agglomeration increased, leading to unqualified spread and difficulty in fully realizing the fiber toughening effect. Ultimately, this resulted in the simultaneous deterioration of mechanical properties and impermeability, and a decline in the workability of the slurry.
[0059] It should be noted that, in this document, terms such as “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0060] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.
Claims
1. A method for preparing a high-permeability prestressed concrete precast slab, characterized in that, Includes the following steps: Step 1: Phosphate and pre-wet the pre-treated and activated end-hook steel fibers and shale ceramic sand respectively to obtain phosphated modified steel fibers and pre-wetted shale ceramic sand; Step 2: Put silicate cement, fly ash, S95 grade mineral powder, mixed quartz sand and basalt crushed stone into a mixer and dry mix at a speed of 40-50 r / min for 1-2 min. First, add water-reducing agent solution accounting for 1 / 3 of the total volume of the water-reducing agent solution and stir at a speed of 40-60 r / min for 0.5-1 min. Then, sprinkle fiber-powder pre-dispersion through a vibrating feeder and stir for 1-1.5 min. Then, add the remaining water-reducing agent solution and pre-wetted shale ceramsite sand and continue stirring at a speed of 70-80 r / min for 2-2.5 min to obtain concrete mixture. Step 3: First, tension the concrete in stages on the tensioning platform, then pour the concrete mixture in layers and vibrate it to form the shape. After in-situ curing with moisture until the strength reaches the standard, release the tension in stages and then transfer it to the standard curing room for continued moisture curing to obtain a high-permeability prestressed concrete precast slab.
2. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method of the phosphate-modified steel fiber mentioned in step one is as follows: The pretreated and activated end-hook steel fibers are placed into a porous PP mesh basket and immediately immersed in the phosphating solution. They are then soaked in a 75°C water bath for 20 minutes, during which the mesh basket is shaken for 10-15 seconds every 2-3 minutes. After removal, they are rinsed with deionized water 3-5 times and dried at 60-80°C for 10-20 minutes to obtain phosphated modified steel fibers. The porous PP mesh basket has a mesh size of 1-2mm.
3. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method of the pre-wetted shale ceramic sand mentioned in step one is as follows: Completely immerse the shale ceramic sand in deionized water at room temperature for 72 hours, stirring occasionally. After soaking, pour off the excess water and place the wet ceramic sand on a non-absorbent steel tray. Cover its surface with paper towels and replace them with new ones when the paper towels are completely wet. Repeat this process until no water stains appear on the paper towels. At this point, the ceramic sand has reached a saturated surface-dry state with a saturated water absorption rate of 15-20%, thus obtaining pre-wetted shale ceramic sand. The shale ceramic sand consists of 180-220g of sieved 3-5mm continuously graded particles; the pre-wetted shale ceramic sand needs to be covered with a damp cloth for storage.
4. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The mass ratio of silicate cement, fly ash, S95 grade mineral powder, mixed quartz sand, basalt crushed stone and fiber-powder pre-dispersion in step two is 410-430: 50-60: 150-180: 560-640: 560-640: 175-205.
5. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method of the fiber-powder pre-dispersion described in step two is as follows: Phosphated modified steel fibers, silica fume, and Wernite are premixed in a mixer at a speed of 400-600 r / min for 30-40 s to prepare a fiber-powder predispersion. The mass ratio of the phosphated modified steel fiber, silica fume and Wenlun rubber is 140-160:35-45:0.05-0.
1.
6. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method of the water-reducing agent solution in step two is as follows: A polycarboxylate superplasticizer with a solid content of 99% was dissolved in deionized water to obtain a superplasticizer solution. The ratio of the polycarboxylate superplasticizer to deionized water is 22-26g: 125-150mL.
7. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, In step three, the tension is increased to 0.70-0.75 times the standard tensile strength value, and each stage is held for 3-5 minutes.
8. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method for layered pouring and vibration compaction of the concrete mixture in step three is as follows: The concrete mixture is poured in two layers. First, pour the mixture to half the height of the mold, turn on the vibrating table and vibrate for 15-20 seconds, then let it stand for 3-5 minutes. Then pour the remaining concrete mixture and vibrate it again for 8-10 seconds. After smoothing the surface, cover it with plastic film and let it stand at room temperature for 36-48 hours. After the compressive strength of the test blocks under the same conditions reaches 60% of the design strength, the mold is removed.
9. The method for preparing a high-permeability prestressed concrete precast slab according to claim 1, characterized in that, The specific preparation method for the graded release described in step three is as follows: When the compressive strength of the test block cured under the same conditions reaches 90% of the design strength and the curing period reaches 7 days or more, the tension can be released. The tension is released slowly in stages using hydraulic jacks. The tension control stress is gradually reduced from 100% to 80%, 60%, 30%, and 0, with each stage held for 3-5 minutes to ensure that each steel strand is released symmetrically. After all steel strands have completely released the tension, the excess steel strands are cut off symmetrically and step by step using a grinding wheel.
10. A high-permeability prestressed concrete precast slab, characterized in that, The high-permeability prestressed concrete precast slab is prepared by any one of claims 1-9.
Citation Information
Patent Citations
Ultra-high performance concrete and preparation method thereof
CN112430039A