Solid waste synergic utilization low-carbon concrete brick and preparation method thereof

By combining pretreated lightweight aggregates with polycarboxylate superplasticizers and using a high-density polyethylene film-wrapped curing process, the problems of gas release expansion deformation and drying shrinkage cracking in solid waste-based concrete products were solved, achieving high-quality preparation and early strength development of low-carbon concrete bricks.

CN123131104APending Publication Date: 2026-11-20BAODING XINGSHENGHUA NEW BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611583405.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing solid waste-based concrete products contain porous slag and other components that cause gas release, expansion and deformation, as well as drying shrinkage and cracking, making it difficult to guarantee molding quality and later performance.

Method used

The combination of pretreated lightweight aggregates and polycarboxylate superplasticizers improves molding workability through steric hindrance and alleviates volume shrinkage deformation through internal curing water release mechanism. At the same time, a high-density polyethylene film is used for closed wrapping and curing to maintain a humidity environment and promote hydration reaction.

Benefits of technology

It improves the molding and workability of plastic mixtures, reduces the cracking rate of products, enhances structural stability and early strength development, and achieves high-quality preparation of low-carbon concrete bricks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131104A_ABST
    Figure CN123131104A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of building materials, and discloses a kind of solid waste synergic utilization low-carbon concrete brick and preparation method, and the concrete brick is made of waste concrete pavement broken material, natural broken stone, stone powder, natural river sand, pretreated light fine aggregate, polycarboxylate superplasticizer, ordinary Portland cement, fly ash and mixing water, the pretreated light fine aggregate is the household garbage incinerator slag that is aged and degassed and is in the internal moisture saturated state, and the preparation method comprises the following steps: crushing and screening the waste concrete; the raw materials are segmented to carry out anhydrous dry mixing and forced wet mixing to prepare plastic mixture; low-frequency vibration and top pressure forming are carried out to obtain wet-state brick blank; finally, high-density polyethylene film is used to seal the brick stack and wrap for static curing. The application utilizes the slow water release internal curing of light fine aggregate and cooperates with the film moisturizing environment, relieves the drying shrinkage of the matrix; in combination with the pre-degassing treatment of the slag, the risk of product gas evolution expansion is reduced, and the overall volume stability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, specifically to a low-carbon concrete brick made from co-utilized solid waste and its preparation method. Background Technology

[0002] With the continuous advancement of urbanization, the emissions of construction waste and municipal solid waste incineration slag are constantly increasing. Using waste concrete blocks, incineration slag and other bulk solid wastes as the main raw materials to prepare building materials such as concrete bricks is an effective way to achieve resource recycling.

[0003] In the current process of preparing solid waste-based concrete, due to the limitations of raw material characteristics, the molding quality and later performance of the product are often difficult to guarantee. The composition of municipal solid waste incineration slag is relatively complex, containing a small amount of incompletely burned or residual active metals. When the raw slag is directly mixed with cement and water, the active metals will react in the alkaline hydration environment and release free gas. The gas evolution phenomenon will cause expansion stress in the matrix after the concrete is formed, which will lead to volume expansion and structural cracking of the product in the later stage.

[0004] Meanwhile, incinerator slag and waste concrete crushed materials generally have physical characteristics such as rough surface, high internal porosity and strong water absorption. During the dry and wet material mixing stage, porous aggregates will absorb a large amount of free mixing water in the system, resulting in a rapid reduction of free water in the plastic mixture. The rapid water absorption phenomenon will reduce the fluidity and workability of the mixture, increase physical friction resistance, and bring difficulties to the subsequent demolding and molding process, resulting in insufficient matrix packing density.

[0005] Furthermore, due to the excessive absorption of moisture by porous aggregates in the early stages of the system, coupled with the evaporation of moisture under traditional open or conventional watering curing conditions, the relative humidity of the matrix will decrease in the later stages of hydration. The lack of internal humidity will not only hinder the continuous hydration reaction of silicate minerals and affect the normal development of the mechanical strength of the product, but also cause drying shrinkage deformation. Existing conventional processes are difficult to form a long-term moisture compensation mechanism inside the concrete matrix. The phenomenon of surface micro-cracks caused by shrinkage and dehydration of the product is still common, and the overall volume stability is poor. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a low-carbon concrete brick made from co-utilized solid waste and its preparation method, which solves the problems of gas evolution expansion deformation and drying shrinkage cracking caused by the presence of porous slag and other components in existing solid waste-based concrete products.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] In a first aspect, the present invention provides a low-carbon concrete brick for the co-utilization of solid waste, which is made from raw materials comprising the following parts by weight:

[0009] 15.0 to 17.3 parts of waste concrete pavement crushed material; 3.5 to 5.0 parts of natural crushed stone; 25.0 to 33.0 parts of stone powder; 1.5 to 3.0 parts of natural river sand; 30.0 to 45.0 parts of pretreated lightweight fine aggregate; 0.014 to 0.026 parts of polycarboxylate superplasticizer; 8.0 to 12.0 parts of ordinary Portland cement; 0.5 to 2.0 parts of fly ash; 3.83 to 4.9 parts of mixing water;

[0010] Polycarboxylate superplasticizers play a steric hindrance role between solid material particles, reducing physical frictional resistance to improve molding and workability; pretreated lightweight aggregates act as a slow-release carrier for internal curing moisture, compensating for volume deformation caused by later drying and ensuring the volume stability of brick products.

[0011] By adopting the above technical solution, due to the introduction of specific amounts of pretreated light and fine aggregates and polycarboxylate superplasticizers into the formulation system, the two play corresponding physical and chemical roles in the material preparation process.

[0012] Specifically, polycarboxylate superplasticizer molecules adsorb onto the surface of solid particles. The steric hindrance effect of the main chain and side chains can reduce the physical frictional resistance between particles to a certain extent, thereby improving the molding and workability of the plastic mixture. At the same time, the pretreated lightweight fine aggregate has a porous structure and reaches a moisture saturation state during pretreatment. When the relative humidity inside the concrete brick decreases in the later stage of hydration, the water stored inside will be slowly released to the surrounding cement paste due to the capillary tension difference. The internal curing water release process can alleviate the volume shrinkage deformation caused by the cementitious system due to the later drying and continuous hydration consumption, thereby improving the volume stability of the product.

[0013] Preferably, the pretreated lightweight aggregate is municipal solid waste incinerator slag that has undergone magnetic separation for iron removal, eddy current separation for non-ferrous metal removal, crushing and screening, and water-wetting, aging, and degassing treatment. During the preparation of the pretreated lightweight aggregate, the overall moisture content of the municipal solid waste incinerator slag pile is controlled to reach 22 to 28 wt%, and it is aged in a naturally ventilated environment for 15 to 30 days. During the aging process, the pretreated lightweight aggregate relies on the moisture in the system to react with the residual metallic aluminum to remove free hydrogen. The particle size of the pretreated lightweight aggregate is less than 5 mm, and the particles are saturated with moisture.

[0014] By adopting the above technical solution, the slag from municipal solid waste incineration undergoes a degassing reaction during the water-wetting and aging stage. The residual active metal aluminum in the slag reacts with the moisture in the system. By pre-controlling the moisture content and aging time, the residual active metal can be consumed and free hydrogen can be released in advance before the material is mixed in. This helps to reduce the physical damage risk of gas release and expansion stress in the matrix after the original slag is directly added to the system. At the same time, the aging process allows moisture to penetrate into the micropores of the slag and reach a saturated state, changing the tendency of the porous medium to absorb external mixing water in the subsequent mixing process, thus making it more conducive to maintaining the stability of the actual water-cement ratio of the matrix.

[0015] Secondly, the present invention provides a method for preparing low-carbon concrete bricks through the co-utilization of solid waste, comprising the following steps:

[0016] Waste concrete blocks are crushed and screened in a closed circuit to obtain the undersize material, which is then used as waste concrete pavement crushing material. Polycarboxylate superplasticizer is pre-dispersed in the mixing water to prepare a modified mixing liquid. Waste concrete pavement crushing material, natural crushed stone, stone powder, natural river sand, and pretreated lightweight fine aggregates are fed into a mixer for anhydrous dry mixing. Then, ordinary silicate cement and fly ash are added, and the modified mixing liquid is pumped in simultaneously for forced wet mixing to prepare a plastic mixture. The plastic mixture is then transported to the mold cavity of a molding machine for demolding to obtain wet brick blanks. The wet brick blanks are then placed in a temperature-controlled indoor environment for static curing. After stacking, the entire brick stack is sealed and wrapped with high-density polyethylene film. After static curing inside the sealed film, the sealing film is removed to obtain low-carbon concrete bricks.

[0017] By adopting the above technical solution, the feeding process combining anhydrous dry mixing and forced wet mixing allows the dry powder material and aggregate to be initially homogenized before contacting the liquid system, which helps to reduce powder agglomeration. The molded wet brick blanks are statically cured in a sealed wrapping state. The high-density polyethylene film restricts the evaporation of moisture from the system to the outside air, maintaining a relatively high humidity microenvironment around the brick stack. Combined with the mechanism of water release from the pretreated light and fine aggregates, the synergistic internal and external moisture compensation conditions can promote the hydration reaction process of silicate minerals and better control the generation of surface shrinkage microcracks caused by water loss.

[0018] Preferably, the steps of crushing and screening the waste concrete blocks to obtain the undersize material as waste concrete pavement crushing material include: using a jaw crusher for primary crushing, using a hammer crusher for secondary impact crushing, and controlling the water mist dust suppression throughout the process.

[0019] By adopting the above technical solution, the two-stage mechanical crushing process can promote the removal of old cement mortar adhering to the surface of waste concrete coarse aggregate, reduce some weak interfaces, and improve the particle shape geometry parameters and surface roughness of recycled aggregate to a certain extent.

[0020] Preferably, the steps of feeding waste concrete pavement crushed material, natural crushed stone, stone powder, natural river sand and pretreated lightweight fine aggregate into a mixer for anhydrous dry mixing, followed by adding ordinary Portland cement and fly ash, and simultaneously pumping in modified mixing liquid to continue forced wet mixing to prepare a plastic mixture include: controlling the anhydrous dry mixing time to 30 to 60 seconds and controlling the forced wet mixing time to 120 to 180 seconds.

[0021] By adopting the above technical solution, the segmented stirring cycle control is beneficial for polycarboxylate superplasticizer molecules to complete adsorption and dispersion at the solid-phase interface with different particle size distributions, thereby improving the uniformity of the slurry distribution of the mixture system.

[0022] Preferably, the step of conveying the plastic mixture into the mold cavity of the molding machine for demolding and molding to obtain a wet brick blank includes: demolding and molding by combining low-frequency vibration with top pressure, with the top pressure controlled at 15 to 25 MPa.

[0023] By adopting the above technical solution, the bottom mechanical vibration causes the particles of the mixture to liquefy locally and rearrange to fill the pores. Combined with the top static load pressure, it promotes the discharge of trapped air inside the system, which is beneficial to improving the packing density of the matrix.

[0024] Preferably, the steps of placing wet brick blanks in an indoor environment with controlled ambient temperature for static curing, stacking them, wrapping the entire brick stack with high-density polyethylene film, and removing the sealing film after static curing inside the sealed film to obtain low-carbon concrete bricks include: controlling the indoor ambient temperature to 30 to 40°C, wrapping with high-density polyethylene film with a thickness of 0.02 to 0.05 mm, and controlling the static curing time inside the sealed film to 48 to 72 hours.

[0025] By adopting the above technical solution, an ambient temperature higher than room temperature helps to accelerate the hydration heat release rate of cement minerals. A polyethylene film of a certain thickness exhibits good structural toughness when subjected to the internal vapor pressure caused by the heat of hydration to avoid physical cracking and maintain the physical airtightness of the film microenvironment. It can basically meet the thermodynamic and humidity conditions required for the early mechanical strength development of the product.

[0026] This invention provides a low-carbon concrete brick made from co-utilized solid waste and its preparation method. It has the following beneficial effects:

[0027] 1. This invention improves the workability and later volume stability of plastic mixtures by introducing pretreated lightweight aggregates and polycarboxylate superplasticizers into the raw material system. The polycarboxylate superplasticizer in the formula moderately reduces the physical frictional resistance between solid particles by relying on the steric hindrance effect generated by the molecular structure, which facilitates the demolding and molding of the mixture. The pretreated lightweight aggregates, which have reached a state of internal moisture saturation, can slowly release water to the surrounding cement paste by relying on the capillary tension difference when the internal humidity decreases in the later stage of hydration. The internal curing process compensates for the volume shrinkage of the cementitious system caused by drying and continuous hydration by moisture, which helps to reduce the cracking rate of the product.

[0028] 2. This invention improves the structural stability of concrete bricks by controlling the moisture content of municipal solid waste incineration slag and pre-treating it with natural ventilation. The aging and degassing process causes the residual active aluminum metal in the slag to react chemically with water in advance and release free hydrogen gas. This avoids the gas precipitation and expansion stress in the matrix caused by directly putting the slag into the mold in the raw state. At the same time, the pre-treatment process makes the porous medium reach the moisture saturation state in advance, changing the tendency to absorb a large amount of external mixing water during mixing, thereby maintaining the stability of the actual water-cement ratio of the matrix.

[0029] 3. This invention reduces the probability of surface shrinkage microcracks and promotes early strength development by using a curing process of tightly wrapped high-density polyethylene film. The tightly wrapped high-density polyethylene film restricts the rapid evaporation of moisture from the internal system into the air during the early stages of molding, maintaining a relatively high humidity environment in the brick stack to meet the needs of early hydration. Combined with the mechanism of slow water release from the pretreated light and fine aggregates, the combined internal and external moisture retention conditions enable silicate minerals to undergo a more complete hydration reaction, meeting the thermodynamic and humidity conditions required for the early mechanical property development of the product. Attached Figure Description

[0030] Figure 1 This is a graph showing the changes in the degassing and microenvironment maintenance characteristics of the present invention over time, wherein... Figure 1 (a) is a graph showing the change in gas evolution over time in a simulated alkaline solution. The test objects include raw municipal solid waste incinerator slag and pretreated light and fine aggregates A to C. Figure 1 (b) is a graph showing the change in core temperature over time during the static curing of the brick stack;

[0031] Figure 2 This is a comparison diagram of the equipment load and the apparent density of the brick blank according to the present invention, wherein, Figure 2 (a) is a comparison chart of motor operating current during the forced wet mixing stage. Figure 2 (b) is a comparison diagram of the apparent density of wet brick blanks during molding;

[0032] Figure 3 This is a comparison diagram of the mechanical properties of the present invention, wherein, Figure 3(a) is a comparison chart of the compressive strength test results of specimens at 28 days of age. Figure 3 (b) is a comparison chart of the flexural strength test results of specimens at 28 days old;

[0033] Figure 4 This is a comparison chart of the volume stability and dimensional change rate of the present invention, wherein, Figure 4 (a) is a comparison chart of the dimensional change rate of specimens at 28 days of age. Figure 4 (b) is a comparison chart of the mass loss rate of specimens at 28 days of age;

[0034] Figure 5 This is a comparison chart of the environmental protection and carbon reduction and techno-economic indicators of the present invention. Detailed Implementation

[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.

[0037] The polycarboxylate superplasticizer is a commercially available comb-shaped block copolymer aqueous solution. The main chain is polymerized from methacrylic acid monomer, and the side chain is polyethylene glycol monomethyl ether monomer. The weight-average molecular weight ranges from 30,000 g / mol to 50,000 g / mol, the solid content is 40 wt%, and the water reduction rate is greater than 25 wt%.

[0038] High-density polyethylene film; the CAS number for high-density polyethylene is 9002-88-4.

[0039] Municipal solid waste incineration ash is taken from the bottom ash discharged from municipal solid waste incineration power plants. Its original appearance is a heterogeneous mixture of gray-brown porous irregular particles. Its main chemical components include SiO2, Al2O3, CaO and Fe2O3, and its initial moisture content is between 15wt% and 20wt%.

[0040] The waste concrete blocks were taken from the demolished cement concrete pavement during road reconstruction projects. Their initial compressive strength grade is not lower than C30, and their apparent density is 2400 kg / m³. 3 The maximum geometric dimension of a single block is less than 1000mm;

[0041] Stone powder is the tailings powder produced during the processing of commercially available limestone crushed stone.

[0042] In this invention, the units of measurement for all materials and solvents are uniformly referred to as parts by weight.

[0043] Preparation Example 1:

[0044] This preparation example provides a method for preparing pretreated lightweight fine aggregates, including the following steps:

[0045] The raw municipal solid waste incineration slag is sequentially passed through a magnetic separator and an eddy current separator to separate magnetic ferrous and non-magnetic non-ferrous metal impurities. The slag after impurity removal is then processed by a crusher and sieved to obtain slag particles with a diameter of less than 5 mm. These slag particles with a diameter of less than 5 mm are piled in a seepage-proof storage silo, and a spray system is activated to evenly spray water onto the pile, controlling the overall moisture content of the pile to reach 22 wt%. Under this moistened state, the pile is aged for 15 days in a naturally ventilated environment. The moisture in the system causes the residual metallic aluminum to react and remove free hydrogen, and the porous slag particles to reach a moisture saturation state, thus obtaining pretreated light and fine aggregate for later use. This pretreated light and fine aggregate is named Pretreated Light and Fine Aggregate A.

[0046] Preparation Example 2:

[0047] This preparation example provides a method for preparing pretreated lightweight fine aggregates, including the following steps:

[0048] The raw municipal solid waste incineration slag is sequentially passed through a magnetic separator and an eddy current separator to separate magnetic ferrous and non-magnetic non-ferrous metal impurities. The slag after impurity removal is then processed by a crusher and screened to obtain slag particles with a diameter of less than 5 mm. These slag particles are then piled in a seepage-proof storage silo, and a spray system is activated to evenly spray water onto the pile, controlling the overall moisture content of the pile to reach 25 wt%. Under this moistened state, the pile is aged for 22 days in a naturally ventilated environment. The moisture in the system causes the residual metallic aluminum to react and remove free hydrogen, and the porous slag particles reach a moisture saturation state, thus obtaining pretreated light and fine aggregate for later use. This pretreated light and fine aggregate is named Pretreated Light and Fine Aggregate B.

[0049] Preparation Example 3:

[0050] This preparation example provides a method for preparing pretreated lightweight fine aggregates, including the following steps:

[0051] The raw municipal solid waste incineration slag is sequentially passed through a magnetic separator and an eddy current separator to separate magnetic ferrous and non-magnetic non-ferrous metal impurities. The slag after impurity removal is then processed by a crusher and screened to obtain slag particles with a diameter of less than 5 mm. These slag particles with a diameter of less than 5 mm are piled in a seepage-proof storage silo, and a spray system is activated to evenly spray water onto the pile, controlling the overall moisture content of the pile to reach 28 wt%. Under this moistened state, the pile is aged for 30 days in a naturally ventilated environment. The moisture in the system causes the residual metallic aluminum to react and remove free hydrogen, and the porous slag particles reach a moisture saturation state, thus obtaining pretreated light and fine aggregate for later use. This pretreated light and fine aggregate is named Pretreated Light and Fine Aggregate C.

[0052] Example 1:

[0053] This embodiment provides a method for preparing low-carbon concrete bricks through the co-utilization of solid waste, including the following steps:

[0054] Waste concrete blocks are fed into a jaw crusher for primary crushing, with the discharge port parameters controlled to keep the output particle size within 80mm. The material is then conveyed under a closed belt to a hammer crusher for secondary crushing, with the output particle size controlled to be less than 20mm. Finally, it enters a vibrating screening system for closed-circuit screening with a 15mm aperture. The oversize material is returned for re-crushing, while the undersize material is used as waste concrete pavement crushing material for later use. Water mist dust suppression is activated throughout the process.

[0055] 0.014 parts of polycarboxylate superplasticizer were pre-dispersed in 4.9 parts of mixing water to prepare a modified mixing liquid. 15.0 parts of waste concrete pavement crushed material, 5.0 parts of natural crushed stone, 33.0 parts of stone powder, 3.0 parts of natural river sand, and 30.0 parts of pretreated lightweight fine aggregate A were sequentially fed into a twin-shaft forced mixer and dry-mixed for 30 seconds. Then, 12.0 parts of ordinary Portland cement and 2.0 parts of fly ash were pneumatically conveyed into the mixer, and the modified mixing liquid was pumped in simultaneously. Forced wet mixing was continued for 120 seconds to prepare a plastic mixture.

[0056] The mixture is continuously conveyed into the mold cavity of the fully automatic block forming machine. Under the hydraulic drive of the equipment, low-frequency vibration and top pressure are combined to demold and form the block. The top pressure is controlled at 15MPa, and the wet brick blank is obtained by demolding.

[0057] The wet brick blanks are placed in an indoor greenhouse with the ambient temperature controlled at 30℃ and left to stand. After mechanical stacking, the entire brick stack is immediately wrapped and sealed with a 0.02mm thick high-density polyethylene film in 360°. The brick stack is left to cure in the sealed film for 48 hours. After the sealing film is removed, the low-carbon concrete bricks of solid waste co-utilization are obtained.

[0058] Example 2:

[0059] This embodiment provides a method for preparing low-carbon concrete bricks through the co-utilization of solid waste, including the following steps:

[0060] Waste concrete blocks are fed into a jaw crusher for primary crushing, with the discharge port parameters controlled to keep the output particle size within 100mm. The material is then conveyed under a closed belt to a hammer crusher for secondary crushing, with the output particle size controlled to be less than 20mm. Finally, it enters a vibrating screening system for closed-circuit screening with a 15mm aperture. The oversize material is returned for re-crushing, while the undersize material is used as waste concrete pavement crushing material for later use. Water mist dust suppression is activated throughout the process.

[0061] 0.019 parts of polycarboxylate superplasticizer were pre-dispersed in 3.88 parts of mixing water to prepare a modified mixing liquid. 17.3 parts of waste concrete pavement crushed material, 3.5 parts of natural crushed stone, 31.3 parts of stone powder, 1.7 parts of natural river sand, and 36.5 parts of pretreated lightweight fine aggregate B were sequentially fed into a twin-shaft forced mixer and dry-mixed for 45 seconds. Then, 9.0 parts of ordinary Portland cement and 0.7 parts of fly ash were pneumatically conveyed into the mixer, and the modified mixing liquid was pumped in simultaneously. Forced wet mixing was continued for 150 seconds to prepare a plastic mixture.

[0062] The mixture is continuously conveyed into the mold cavity of the fully automatic block forming machine. Under the hydraulic drive of the equipment, low-frequency vibration and top pressure are combined to demold and form the block. The top pressure is controlled at 20MPa, and the wet brick blank is obtained by demolding.

[0063] The wet brick blanks are placed in an indoor greenhouse with the ambient temperature controlled at 35℃ and left to stand. After mechanical stacking, the entire brick stack is immediately wrapped and sealed with a 0.03mm thick high-density polyethylene film in 360°. The brick stack is left to cure in the sealed film for 60 hours. After the sealing film is removed, the low-carbon concrete bricks of solid waste co-utilization are obtained.

[0064] Example 3:

[0065] This embodiment provides a method for preparing low-carbon concrete bricks through the co-utilization of solid waste, including the following steps:

[0066] Waste concrete blocks are fed into a jaw crusher for primary crushing, with the discharge port parameters controlled to keep the output particle size within 120mm. The material is then conveyed under a closed belt to a hammer crusher for secondary crushing, with the output particle size controlled to be less than 20mm. Finally, it enters a vibrating screening system for closed-circuit screening with a 15mm aperture. The oversize material is returned for re-crushing, while the undersize material is used as waste concrete pavement crushing material for later use. Water mist dust suppression is activated throughout the process.

[0067] 0.026 parts of polycarboxylate superplasticizer were pre-dispersed in 3.83 parts of mixing water to prepare a modified mixing liquid. 16.5 parts of waste concrete pavement crushed material, 3.5 parts of natural crushed stone, 25.0 parts of stone powder, 1.5 parts of natural river sand, and 45.0 parts of pretreated lightweight fine aggregate C were sequentially fed into a twin-shaft forced mixer and dry-mixed for 60 seconds. Then, 8.0 parts of ordinary Portland cement and 0.5 parts of fly ash were pneumatically conveyed into the mixer, and the modified mixing liquid was pumped in simultaneously. Forced wet mixing was continued for 180 seconds to prepare a plastic mixture.

[0068] The mixture is continuously conveyed into the mold cavity of the fully automatic block forming machine. Under the hydraulic drive of the equipment, low-frequency vibration and top pressure are combined to demold and form the block. The top pressure is controlled at 25MPa, and the wet brick blank is obtained by demolding.

[0069] The wet brick blanks are placed in an indoor greenhouse with the ambient temperature controlled at 40℃ and left to stand. After mechanical stacking, the entire brick stack is immediately wrapped and sealed with a 0.05mm thick high-density polyethylene film in 360°. The brick stack is left to cure in the sealed film for 72 hours. After the sealing film is removed, the low-carbon concrete bricks of solid waste co-utilization are obtained.

[0070] Example 4:

[0071] This embodiment provides a method for preparing low-carbon concrete bricks through the co-utilization of solid waste, including the following steps:

[0072] Waste concrete blocks are fed into a jaw crusher for primary crushing, with the discharge port parameters controlled to keep the output particle size within 100mm. The material is then conveyed under a closed belt to a hammer crusher for secondary crushing, with the output particle size controlled to be less than 20mm. Finally, it enters a vibrating screening system for closed-circuit screening with a 15mm aperture. The oversize material is returned for re-crushing, while the undersize material is used as waste concrete pavement crushing material for later use. Water mist dust suppression is activated throughout the process.

[0073] 0.019 parts of polycarboxylate superplasticizer were pre-dispersed in 3.88 parts of mixing water to prepare a modified mixing liquid. 17.3 parts of waste concrete pavement crushed material, 3.5 parts of natural crushed stone, 31.3 parts of stone powder, 1.7 parts of natural river sand, and 36.5 parts of pretreated lightweight fine aggregate B were sequentially fed into a twin-shaft forced mixer and dry-mixed for 45 seconds. Then, 9.0 parts of ordinary Portland cement and 0.7 parts of fly ash were pneumatically conveyed into the mixer, and the modified mixing liquid was pumped in simultaneously. Forced wet mixing was continued for 150 seconds to prepare a plastic mixture.

[0074] The mixture is continuously conveyed into the mold cavity of the fully automatic block forming machine. Under the hydraulic drive of the equipment, low-frequency vibration and top pressure are combined to demold and form the block. The top pressure is controlled at 20MPa, and the wet brick blank is obtained by demolding.

[0075] The wet brick blanks are placed in an indoor greenhouse with the ambient temperature controlled at 30℃ and left to stand. After mechanical stacking, the entire brick stack is immediately wrapped and sealed with a 0.03mm thick high-density polyethylene film in 360°. The brick stack is left to cure in the sealed film for 48 hours. After the sealing film is removed, the low-carbon concrete bricks of solid waste co-utilization are obtained.

[0076] Comparative Example 1:

[0077] Compared with Example 2, the difference is that: during the curing stage, high-density polyethylene film is not used for wrapping and sealing. Instead, the wet brick blanks are placed directly in an indoor greenhouse for natural open and static curing. All other aspects are the same.

[0078] Comparative Example 2:

[0079] Compared with Example 2, the difference is that: instead of using high-density polyethylene film to wrap the bricks during the curing stage, the wet brick blanks are sent into a traditional gas-fired steam curing chamber for centralized curing under normal pressure and high-temperature steam conditions at 65°C. All other aspects are the same.

[0080] Comparative Example 3:

[0081] Compared with Example 2, the difference is that: instead of using pretreated light and fine aggregate B that has undergone wet aging and degassing treatment, an equal amount of raw municipal solid waste incinerator slag with an initial moisture content of 15wt% to 20wt% that has not undergone any wet aging treatment is directly added; otherwise, they are the same.

[0082] Comparative Example 4:

[0083] Compared with Example 2, the difference is that no polycarboxylate superplasticizer is added, and the modified mixing liquid pumped in the step is replaced with an equal amount of pure fresh mixing water, while the rest are the same.

[0084] Comparative Example 5:

[0085] Compared with Example 2, the difference is that: the waste concrete pavement crushed material, stone powder and pretreated lightweight fine aggregate B are not used, and the total proportion of 85.1 parts is replaced by 45.0 parts of traditional natural crushed stone and 40.1 parts of natural river sand, while the rest are the same.

[0086] Test Example 1:

[0087] Take 100g each of the pretreated light and fine aggregates A to C obtained from Preparation Examples 1 to 3 and the untreated raw municipal solid waste incinerator slag, place them in conical flasks with gas delivery tubes, add a predetermined amount of calcium hydroxide simulated pore solution with a pH of 12.5, seal the conical flasks and connect the gas delivery tubes to a graduated cylinder inverted in a water trough, and record the amount of gas collected by drainage over 72 hours under a constant temperature water bath at 20°C.

[0088] In the process of stacking wet brick blanks in Example 2 and Comparative Example 1, temperature and humidity sensor probes were pre-embedded on the surface of the bricks at the geometric center of the brick stack. Then, static curing was carried out according to the curing conditions set in each scheme. The core temperature and relative humidity data in the 48 hours before curing were read by a data acquisition recorder, and the maximum temperature rise of the core and the average relative humidity value in 48 hours were extracted.

[0089] Table 1. Test results of degassing characteristics and microenvironment maintenance parameters:

[0090] Test group Test object 72h gas evolution rate (mL / 100g) Maximum core temperature (°C) 48-hour average relative humidity (%) control group Original municipal solid waste incineration slag 42.6 - - Preparation Example 1 Pre-treated light and fine aggregate A 3.2 - - Preparation Example 2 Pre-treated light and fine aggregate B 0.8 - - Preparation Example 3 Pre-treated light and fine aggregate C 0.3 - - Example 2 Example 2: Wet brick stack - 48.3 96.5 Comparative Example 1 Comparative Example 1: Wet Brick Stacks - 31.2 54.7

[0091] From Table 1 and Appendix Figure 1 It can be seen that: "-" in Table 1 indicates that the corresponding test objects were not measured for the test items. The gas evolution of the original municipal solid waste incinerator slag in the simulated alkaline liquid phase is at a high level. The gas evolution of the pretreated light and fine aggregates A to C after wet aging shows different degrees of decrease with the increase of moisture content and aging time. This indicates that the intervention of the preset spray aging conditions can consume most of the gas-producing substances in the aggregate in advance, reducing the risk of expansion stress caused after the introduction of the product. The core maximum temperature and average relative humidity test values ​​of the brick stack in Example 2 are higher than those in Comparative Example 1. This indicates that the operation of sealing with polyethylene film can physically block the moisture and hydration heat that escape from the mixture, and accumulate in the brick stack to form a warm and humid microenvironment for continuous hydration reaction.

[0092] Test Example 2:

[0093] Plastic mixtures were prepared according to the methods of Example 2 and Comparative Example 4, respectively. An electric parameter tester was connected in series in the power supply line of the drive motor of the twin-shaft forced mixer. During the forced wet mixing stage, the motor operating current signal was continuously collected, and the average operating current and peak operating current during the test period were recorded and extracted.

[0094] Five wet brick blanks from Example 2 and Comparative Example 4 were randomly selected after demolding. The length, width, and height of each brick blank were measured with calipers to calculate the apparent volume. The mass of each brick blank was weighed using an electronic platform scale. The apparent density of each brick blank was calculated based on the ratio of mass to volume. The average value of the five brick blanks in the same group was taken as the apparent density of the wet brick blank in the corresponding group.

[0095] Table 2. Test results of load on forced wet mixing equipment and apparent density of wet brick blanks:

[0096] Test group Test object Average operating current (A) Peak operating current (A) <![CDATA[Wet brick blank forming apparent density (kg / m 3 )]]> Example 2 Example 2: Mixture / Brick Blank 45.3 52.1 2215.4 Comparative Example 4 Comparative Example 4: Mixture / Brick Blank 56.4 65.2 1987.2

[0097] From Table 2 and Appendix Figure 2 It can be seen that in Comparative Example 4 without the addition of polycarboxylate superplasticizer, the average operating current and peak operating current of the forced mixer are at a relatively high level, and the apparent density of the wet brick blank after demolding is relatively low. In Example 2, after introducing a predetermined amount of polycarboxylate superplasticizer, the average operating current and peak operating current in the wet mixing stage show a decreasing trend, and the apparent density of the wet brick blank is relatively increased. Combined with the drag reduction mechanism, it can be seen that polycarboxylate superplasticizer can play a corresponding steric hindrance role in the mixture system containing a high proportion of water-absorbing porous solid waste particles, reduce the physical friction resistance between the mixture particles, improve the workability of the semi-dry hard mixture in the equipment conveying and demolding process, and make the material obtain a relatively denser structure under the action of molding pressure.

[0098] Test Example 3:

[0099] According to the relevant test requirements of the national standard, solid waste co-utilization low-carbon concrete brick specimens obtained from Examples 1 to 4 and Comparative Examples 1 to 5 after completing 28 days of static curing were extracted. Specimens with mechanical damage on the surface were removed and the test surface was kept flat.

[0100] Compressive strength tests were performed on a universal testing machine. The brick specimen was placed in the center of the upper and lower pressure plates of the testing machine. Pressure was continuously and uniformly applied to the specimen at a constant loading rate until the specimen failed. The maximum load value at failure was recorded to calculate the compressive strength. Ten specimens were tested in parallel in each group and the arithmetic mean was taken.

[0101] The flexural strength was tested on a flexural testing machine. The span parameters were set and the specimen was placed on the support. A concentrated load was applied uniformly at the mid-span until fracture. The fracture load was recorded and the corresponding flexural strength was calculated. Five specimens were tested in parallel for each group and the arithmetic mean was taken as the final data of the mechanical property test for the group.

[0102] Table 3. Test results of mechanical properties of low-carbon concrete bricks at 28 days of age:

[0103] Test group Test object Compressive strength (MPa) Flexural strength (MPa) Example 1 Example 1 Specimen 29.5 4.8 Example 2 Example 2 Specimen 24.6 4.3 Example 3 Example 3 Specimen 20.1 3.5 Example 4 Example 4 Specimen 24.3 4.2 Comparative Example 1 Comparative Example 1 specimen 14.2 2.5 Comparative Example 2 Comparative Example 2 Specimen 25.1 4.4 Comparative Example 3 Comparative Example 3 specimen 3.2 0.6 Comparative Example 4 Comparative Example 4 Specimen 13.5 2.1 Comparative Example 5 Comparative Example 5 specimen 25.4 4.6

[0104] From Table 3 and Appendix Figure 3It can be seen that the compressive strength and flexural strength test values ​​of Examples 1 to 4 all show that they meet the data requirements of conventional load-bearing wall material standards. Under the condition that Comparative Example 1 did not use film-sealed curing, the various strength test values ​​showed a downward trend, indicating that the film-coated internal circulation mechanism can ensure the internal hydration process of the product without the intervention of external heat sources. The data obtained by Comparative Example 2 using conventional steam curing is similar to that of Example 2, indicating that the present invention has the technical feasibility of replacing the high-energy-consuming steam curing process. The test strength data of Comparative Example 3 is at a low level due to the use of unaged slag, indicating that the gas expansion caused by the residual active components in the matrix damages the development of structural strength. The strength test value of Comparative Example 4 shows a reduced state when polycarboxylate superplasticizer is lacking. Combined with the drag reduction mechanism, it can be seen that the increase in internal frictional resistance of the material affects the molding density. Example 2 and Comparative Example 5, which uses pure natural sand and gravel aggregate, show similar data performance in mechanical properties, indicating that through component regulation treatment, high-content solid waste can form a stable structural system under non-firing and non-steaming conditions.

[0105] Test Example 4:

[0106] Wet brick blanks of Example 2, Comparative Example 1, and Comparative Example 3 were prepared and molded. Measuring probes were pre-embedded at the center of both ends to record the initial length and initial mass. Then, they were subjected to preliminary static curing in strict accordance with the pre-set curing conditions of each group. After the film was removed or the specific preliminary curing was completed, they were uniformly transferred to a standard environmental test chamber with a temperature of 20°C and a relative humidity of 60% to continue static curing until the test age of 28 days.

[0107] After the specimens reach the 28-day testing age, the length change of the specimens is read and recorded using a vertical shrinkage meter. The dimensional change rate of each group of specimens is calculated based on the ratio of the length change to the initial measurement gauge length, where shrinkage is recorded as a negative value and expansion as a positive value.

[0108] The apparent quality of the specimens at 28 days of age was measured using a high-precision electronic platform scale. The mass loss rate was calculated based on the percentage difference between the apparent quality and the initial quality. Simultaneously, the macroscopic integrity of the specimen surface was observed and recorded visually. Surfaces without visible macroscopic cracks or peeling were recorded as intact, while surfaces with penetrating microcracks or localized peeling were recorded as damaged.

[0109] Table 4. Results of Volumetric Stability and Dimensional Change Rate Tests:

[0110] Test group Test object Dimensional change rate (%) Quality loss rate (%) Appearance integrity Example 2 Example 2 Specimen -0.042 2.18 intact Comparative Example 1 Comparative Example 1 specimen -0.134 11.67 destroy Comparative Example 3 Comparative Example 3 specimen +0.198 3.52 destroy

[0111] From Table 4 and Appendix Figure 4It can be seen that: the dimensional change rate and mass loss rate of Example 2 are at a low level and the appearance of the specimen remains intact. In Comparative Example 1, due to the lack of a sealed membrane during the static curing stage, the internal moisture evaporates rapidly to the external environment, resulting in a high mass loss rate and a negative dimensional shrinkage rate, accompanied by structural damage to the specimen. Combined with the internal curing reservoir mechanism, it can be seen that the membrane microenvironment combined with the internal moisture release effect of porous slag can compensate for the volume deformation caused by the early hydration and the later drying. In Comparative Example 3, the unaged original slag reacts with residual active metals after the specimen is demolded and generates gas, which generates expansion stress in the matrix, causing structural damage to the specimen and exhibiting positive dimensional expansion deformation. Combined with the degassing mechanism, it can be seen that the pre-wet spray aging treatment is a necessary process step to ensure the volume stability of highly doped porous slag products.

[0112] Test Example 5:

[0113] Extract the product formulation material data of Example 2, Comparative Example 2 and Comparative Example 5, and sum the dry basis mass of the waste components from waste concrete pavement crushed material, fly ash, stone powder and pretreated lightweight fine aggregate in the formulation system, and divide it by the total mass of all solid dry basis raw materials in the corresponding group formulation to calculate the solid waste comprehensive utilization rate data of each group product.

[0114] For each group's corresponding maintenance process implementation stage, the physical amount of external heating energy medium consumed by a single batch of 10,000 standard bricks during the complete maintenance cycle is extracted based on the production equipment operation records. The gas or electricity consumption data involved are converted into standard coal equivalent according to the energy consumption conversion factor stipulated by national standards. The summation calculation yields the external comprehensive energy consumption equivalent to standard coal for each group's production of 10,000 standard bricks during the maintenance stage.

[0115] Table 5. Results of Environmental Protection, Carbon Reduction, and Technological and Economic Indicators Calculation and Testing:

[0116] Test group Test object Solid waste comprehensive utilization rate (%) Additional energy consumption during maintenance (kgce / 10,000 units) Example 2 Example 2 Specimen 85.80 0.00 Comparative Example 2 Comparative Example 2 Specimen 85.80 247.15 Comparative Example 5 Comparative Example 5 specimen 0.70 0.00

[0117] From Table 5 and Appendix Figure 5 It can be seen that the solid waste comprehensive utilization rate of Example 2 and Comparative Example 2 is at a high level. The solid waste comprehensive utilization rate of Comparative Example 5, which uses natural sand and gravel aggregate as material substitute, shows a downward trend. This indicates that the formulation system has the industrial feasibility of converting a variety of urban low-value solid wastes into building materials at a high proportion. Comparative Example 2 generates a high external energy consumption equivalent to standard coal when using traditional gas steam curing conditions. The external energy consumption of Example 2 in the curing process is zero. Combined with the thermodynamic microcirculation mechanism of the membrane, it can be seen that the self-heating effect in the membrane sealing environment can maintain the necessary temperature and humidity reaction conditions and replace the external heat source input, solving the high energy consumption problem and resource waste in the traditional building material production process.

[0118] Although embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions, and variations can be made to the equipment structure, process flow, step sequence, operating parameters, or working medium type in these embodiments without departing from the principles and spirit of the present invention. The scope of the present invention is defined by the core technical solutions disclosed above and their equivalent substitutions.

Claims

1. A low-carbon concrete brick for the co-utilization of solid waste, characterized in that, Made from the following ingredients in parts by weight: Waste concrete pavement debris: 15.0 to 17.3 parts; Natural crushed stone: 3.5 to 5.0 parts; Stone powder: 25.0 to 33.0 parts; Natural river sand: 1.5 to 3.0 parts; Pretreated light and fine aggregates: 30.0 to 45.0 parts; Polycarboxylate superplasticizer: 0.014 to 0.026 parts; Ordinary Portland cement: 8.0 to 12.0 parts; Fly ash: 0.5 to 2.0 parts; Mixing water: 3.83 to 4.9 parts; The polycarboxylate superplasticizer acts as a steric hindrance between solid material particles to reduce physical friction resistance and improve molding and workability; the pretreated lightweight aggregate acts as a slow-release carrier for internal curing moisture to compensate for volume deformation caused by subsequent drying and ensure the volume stability of brick products.

2. The low-carbon concrete brick for co-utilization of solid waste according to claim 1, characterized in that, The pretreated light and fine aggregate is municipal solid waste incinerator slag that has undergone magnetic separation to remove iron, eddy current separation to remove non-ferrous metals, crushing and screening, and water wetting, aging and degassing treatment.

3. The low-carbon concrete brick for co-utilization of solid waste according to claim 1, characterized in that, During the preparation of pretreated lightweight aggregates, the overall moisture content of the municipal solid waste incinerator slag pile is controlled to reach 22 to 28 wt%, and it is aged in a naturally ventilated environment for 15 to 30 days.

4. The low-carbon concrete brick for co-utilization of solid waste according to claim 1, characterized in that, During the aging process, the pretreated light and fine aggregates rely on the moisture in the system to react with the residual metallic aluminum and remove free hydrogen.

5. The low-carbon concrete brick for co-utilization of solid waste according to claim 1, characterized in that, The pretreated light and fine aggregate has a particle size of less than 5 mm and the particles are saturated with moisture.

6. A method for preparing low-carbon concrete bricks based on the co-utilization of solid waste according to any one of claims 1-5, characterized in that, The preparation method includes the following steps: The waste concrete blocks are crushed and screened in a closed circuit to obtain the undersize material, which is then used as waste concrete pavement crushing material. Polycarboxylate superplasticizer is pre-dispersed in mixing water to prepare modified mixing liquid; waste concrete pavement crushed material, natural crushed stone, stone powder, natural river sand and pretreated light fine aggregate are fed into a mixer for anhydrous dry mixing, then ordinary silicate cement and fly ash are added, and the modified mixing liquid is pumped in simultaneously to continue forced wet mixing to prepare plastic mixture. The plastic mixture is conveyed into the mold cavity of the molding machine for demolding and molding to obtain a wet brick blank; The wet brick blanks are placed in an indoor environment with controlled temperature for static curing. After stacking, the entire brick stack is sealed and wrapped with high-density polyethylene film. After static curing inside the sealed film, the sealing film is removed to obtain low-carbon concrete bricks.

7. The method for preparing low-carbon concrete bricks through co-utilization of solid waste according to claim 6, characterized in that, The step of crushing and screening the waste concrete blocks to obtain the undersize material for use as waste concrete pavement crushing material includes: The jaw crusher is used for primary crushing, followed by a hammer crusher for secondary crushing, with water mist dust suppression activated throughout the process.

8. The method for preparing low-carbon concrete bricks through co-utilization of solid waste according to claim 6, characterized in that, The steps of feeding waste concrete pavement crushed material, natural crushed stone, stone powder, natural river sand, and pretreated lightweight fine aggregate into a mixer for anhydrous dry mixing, followed by adding ordinary Portland cement and fly ash, and simultaneously pumping in modified mixing liquid for forced wet mixing to prepare a plastic mixture include: The time for dry mixing without water is controlled to be 30 to 60 seconds, and the time for forced wet mixing is controlled to be 120 to 180 seconds.

9. The method for preparing low-carbon concrete bricks through co-utilization of solid waste according to claim 6, characterized in that, The step of conveying the plastic mixture into the mold cavity of the molding machine for demolding and molding to obtain a wet brick blank includes: Demolding and molding are carried out by combining low-frequency vibration with top pressure, with the top pressure controlled between 15 and 25 MPa.

10. The method for preparing low-carbon concrete bricks through co-utilization of solid waste according to claim 6, characterized in that, The steps of sending wet brick blanks to a room with controlled ambient temperature for static setting, stacking them, sealing the entire brick stack with high-density polyethylene film, and then removing the sealing film after static curing inside the sealed film to obtain low-carbon concrete bricks include: The indoor ambient temperature is controlled at 30 to 40°C. The room is wrapped with a high-density polyethylene film with a thickness of 0.02 to 0.05 mm and kept in a sealed environment for 48 to 72 hours for curing.