Low-shrinkage high-durability inorganic-organic composite anchoring cementitious system and preparation method thereof
By combining components A and B of a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the problems of high curing shrinkage, low interfacial bonding strength, and insufficient durability of inorganic anchoring materials are solved, achieving a synergistic improvement in low shrinkage, high bonding strength, and excellent durability.
Patent Information
- Application Number
- CN202611228484.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-20
AI Technical Summary
Existing inorganic anchoring cementitious materials suffer from problems such as high curing shrinkage, low interfacial bonding strength, poor compatibility between inorganic and organic phases, and insufficient long-term durability, making it difficult to meet the long-term anchoring requirements under complex working conditions.
A low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system is adopted. Component A and component B are compounded in a specific non-equilibrium mass ratio. Components A and B are constructed using a composite inorganic cementitious substrate, modified organic composite emulsion, functional composite filler, and additives to achieve synergistic reinforcement between the inorganic cementitious phase and the organic polymer phase.
It achieves a 28-day curing shrinkage rate of less than 0.027%, a tensile bond strength of 4.71~5.27MPa with C30 concrete, a shear bond strength of 18.14~19.86MPa with HRB400 steel bars, and a strength loss rate of only 6.27%~7.81% after 300 freeze-thaw cycles, demonstrating good construction adaptability and long-term durability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of building structure anchoring and bonding materials, specifically relating to a low-shrinkage, high-durability inorganic-organic composite anchoring cementing system and its preparation method. Background Technology
[0002] Anchoring and bonding technologies are key methods for achieving structural connections, reinforcement, and repair in building engineering, and are widely used in scenarios such as rebar installation, anchor bolt anchoring, crack repair, slab bonding, and heavy-duty fixing. Currently, building anchoring cementitious materials are mainly divided into two categories: organic resin type and inorganic cement-based type. Both have their own performance advantages, but they also have inherent defects that are difficult to overcome.
[0003] Organic resin-based anchoring materials, represented by epoxy resin, unsaturated polyester resin, and polyurethane resin, have the outstanding advantages of fast curing speed, high early strength, and excellent adhesion to steel and concrete substrates, thus gaining widespread application in engineering. However, these materials also have significant drawbacks: First, organic resins release volatile organic compounds (VOCs) during the curing process, resulting in high toxicity in the construction environment and significant health hazards to operators, failing to meet increasingly stringent green construction and environmental protection requirements; second, the resin materials themselves are flammable, easily softening or even burning at high temperatures, exhibiting poor fire resistance, and causing a sharp decrease in anchoring load-bearing capacity under fire conditions, posing serious safety hazards; third, organic resins are thermosetting materials, and during service, they are prone to aging and cracking due to environmental factors such as ultraviolet light, temperature cycling, and humidity changes, resulting in significant long-term degradation of mechanical properties, making it difficult to meet the requirements for long-term structural service.
[0004] Inorganic cement-based anchoring materials use rapid-hardening cements such as aluminate cement and sulfoaluminate cement as the base material. Their advantages include being environmentally friendly, non-toxic, non-flammable, non-explosive, and having excellent high-temperature resistance. Furthermore, the raw materials are widely available and relatively inexpensive. However, traditional inorganic anchoring materials suffer from several key technical bottlenecks: First, the chemical and drying shrinkage during the hydration and hardening process of cement-based materials is significant, resulting in a generally high curing shrinkage rate. This leads to shrinkage microcracks at the anchoring interface, reducing bonding reliability. Second, inorganic materials have poor interfacial chemical affinity with reinforcing steel and concrete substrates, resulting in bonding strength far lower than that of organic resin systems, making it difficult to meet heavy-duty anchoring requirements. Third, the early strength development of traditional cement-based materials is uneven, with a prominent contradiction between final setting time and workable time, leading to poor construction adaptability. In addition, ordinary cement-based anchoring materials lack sufficient resistance to freeze-thaw cycles, chloride ion penetration, and carbonation, making it difficult to guarantee durability in complex service environments such as humidity, low temperatures, and corrosion.
[0005] In recent years, some studies have attempted to employ a two-component inhibition-trigger type inorganic anchoring system, which uses inhibition-type aluminate cement combined with an alkaline activator to achieve storage stability and in-situ triggered curing. However, this technical approach still suffers from the following problems: the cured gel is brittle and has weak resistance to vibration loads and impacts; some solutions introduce organic polymers for modification, but the poor compatibility between the polymer and the inorganic cementitious phase leads to uneven dispersion, resulting in long-term strength decay and even interfacial debonding. Furthermore, existing technologies generally lack a comprehensive approach that balances low shrinkage, high early strength, high weather resistance, good construction adaptability, and long-term durability, making it difficult to meet the long-term anchoring requirements under complex working conditions. Summary of the Invention
[0006] In order to overcome the shortcomings of the prior art, the present invention aims to provide a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system and its preparation method, so as to solve the technical problems of high curing shrinkage, low interfacial bonding strength, poor compatibility between inorganic and organic phases, and insufficient long-term durability of existing inorganic anchoring cementitious materials.
[0007] To achieve the above objectives, the present invention employs the following technical solution: In a first aspect, the present invention provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, comprising component A and component B, wherein component A and component B are mixed at a mass ratio of 3.92 to 4.15:1. The A component comprises the following raw materials in parts by weight: 518-641 parts of composite inorganic cementitious substrate, 85-127 parts of modified organic composite emulsion, 191-251 parts of functional composite filler, 22-37 parts of functional additive A, and 128-178 parts of deionized water. The B component comprises the following raw materials in parts by weight: 235-278 parts of composite hydration activator, 55-79 parts of bifunctional interface enhancer, 44-67 parts of micro-expansion and shrinkage compensation component, 13-22 parts of B functional additive, and 581-642 parts of deionized water.
[0008] A further improvement of the present invention is that the composite inorganic cementitious substrate is a mixture of modified barium calcium sulfoaluminate cement, calcined activated metakaolin, and nano-grade active silica fume in a mass ratio of (296~348):(133~177):(84~119).
[0009] A further improvement of the present invention is that the modified organic composite emulsion is a compound of a core-shell structured styrene-acrylic-epoxy composite emulsion and a hydrophilic chain-extended waterborne polyurethane dispersion in a mass ratio of (51~69):(33~59).
[0010] A further improvement of the present invention is that the functional composite filler is a mixture of whisker-shaped nano-calcium carbonate, silane-modified quartz sand and anatase nano-titanium dioxide in a mass ratio of (73~97):(114~146):(3~8).
[0011] A further improvement of the present invention is that the functional additive A is a compound retarder stabilizer, a polycarboxylic acid ether high-efficiency water-reducing agent, a non-silicone mineral oil defoamer and an organic bentonite-hydroxyethyl cellulose composite thixotropic agent in a mass ratio of (8~15):(4~7):(3~6):(6~10).
[0012] A further improvement of the present invention is that the composite hydration activator is a compound of lithium sulfate-lithium acetate double salt and modified aluminate alkaline activator in a mass ratio of (87~117):(145~162); The bifunctional interface enhancer is a compound of silane-modified phosphate coupling agent and medium-viscosity hydroxymethyl cellulose ether in a mass ratio of (34~48):(21~31); The micro-expansion and shrinkage compensation component is an ultrafine calcium sulfoaluminate expander; Functional additive B is a compound of isothiazolinone bactericide, polyacrylate dispersant and propylene glycol-calcium formate composite antifreeze in a mass ratio of (2~4):(5~8):(5~11).
[0013] Secondly, the present invention also provides a method for preparing a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, comprising the following steps: S1, mix the formulated amount of composite inorganic cementitious substrate and functional composite filler to obtain a uniform dry-mixed powder; mix the formulated amount of deionized water with functional additive A to obtain a uniform aqueous phase liquid; add the dry-mixed powder to the aqueous phase liquid, control the system temperature, stir and mix, add the modified organic composite emulsion, continue stirring, and degas under vacuum to obtain component A. S2, mix the prescribed amount of deionized water with functional additive B, add the composite hydration activator and stir until completely dissolved, then add the bifunctional interface enhancer and micro-expansion and shrinkage compensation component, stir until uniformly dispersed, and filter to obtain component B; S3. Mix component A and component B at a mass ratio of 3.92~4.15:1 to obtain the low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system.
[0014] A further improvement of the present invention is that the composite inorganic cementitious substrate and the functional composite filler described in S1 are mixed using a double-helix conical mixer with a filling rate of 65% to 72%, a mixing speed of 36 to 42 r / min, and a mixing time of 10 to 20 min.
[0015] A further improvement of the present invention is that the vacuum degree of vacuum degassing in S1 is -0.072 to -0.065 MPa, and the degassing time is 5 to 8 minutes; the filtration in S2 uses a 100 to 150 mesh stainless steel filter screen for pressure filtration.
[0016] A further improvement of the present invention is that the stirring speed in S3 is 360~420 r / min, the stirring time is 3.2~3.8 min, and the working time of the mixed paste is 28~38 min.
[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system. Component A and component B are compounded at a specific non-equilibrium mass ratio of 3.92 to 4.15:1. Component A is constructed using a composite inorganic cementitious substrate, a modified organic composite emulsion, a functional composite filler, and functional additive A. Component B is constructed using a composite hydration activator, a bifunctional interface reinforcing agent, a micro-expansion and shrinkage compensation component, and functional additive B. This achieves synergistic reinforcement between the inorganic cementitious phase and the organic polymer phase. Compared to existing inorganic anchoring materials, the 28-day curing shrinkage rate of this invention is only 0.022%~0.027%, the tensile bond strength with C30 concrete reaches 4.71~5.27 MPa, the shear bond strength with HRB400 steel bars reaches 18.14~19.86 MPa, and the strength loss rate after 300 freeze-thaw cycles is only 6.27%~7.81%. Meanwhile, the 1-day compressive strength reaches 36.2~42.7 MPa, and the 28-day compressive strength reaches 77.3~85.2 MPa. These data demonstrate that this invention effectively overcomes the technical difficulties of high curing shrinkage rate, low interfacial bond strength, and insufficient durability of traditional inorganic anchoring cementitious materials, achieving a synergistic improvement in low shrinkage, high bonding strength, and excellent durability.
[0018] This invention also provides a method for preparing a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system. This method involves pre-mixing a composite inorganic cementitious substrate with a functional composite filler to obtain a uniform dry-mixed powder. Then, deionized water is mixed with functional additive A to obtain a homogeneous aqueous phase. The dry-mixed powder is then added to the aqueous phase and stirred under controlled temperature. A modified organic composite emulsion is added and stirring continues. After vacuum degassing, component A is obtained. Simultaneously, deionized water is mixed with functional additive B, and a composite hydration activator, a bifunctional interface enhancer, and a micro-expansion / shrinkage compensation component are added sequentially. After stirring, dispersion, and filtration, component B is obtained. Finally, components A and B are mixed in a specific ratio to obtain the finished product. Compared to existing preparation methods, this invention features tightly integrated processes, complete core steps, and eliminates the need for high temperature, high pressure, or organic solvents, producing no harmful byproducts. The cementitious system prepared by this method exhibits a 28-day curing shrinkage rate of only 0.022%~0.027%, a tensile bond strength of 4.71~5.27 MPa with C30 concrete, and a shear bond strength of 18.14~19.86 MPa with HRB400 steel bars. After 300 freeze-thaw cycles, the strength loss rate is only 6.27%~7.81%, indicating that this method effectively solves the core process problems of poor compatibility between organic and inorganic phases, easy agglomeration of nanofillers, and insufficient storage stability in existing technologies. Furthermore, the A component prepared by this method has a storage stability period of ≥180 days at 25℃, and the B component has a stability period of ≥360 days. The batch-to-batch performance deviation is small, the process adaptability is strong, and it is suitable for large-scale industrial production, demonstrating good industrialization prospects. Detailed Implementation
[0019] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0020] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0021] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0022] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”
[0023] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0024] This invention provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system. This system is a non-reactive, inhibitory-triggering two-component system, consisting of independently prepared and sealed components A and B. On-site, it can be used after mixing at a mass ratio of A:B = 3.92~4.15:1, with a preferred mass ratio of 4.05:1, and is compatible with most construction equipment. This cementitious system is suitable for ambient temperatures ranging from -6 to 38℃ and is applicable to substrates including ordinary concrete, high-strength concrete, natural stone, sintered masonry, and aerated concrete. It can be widely used in applications such as rebar installation, anchor bolt anchoring, structural crack sealing, slab bonding, heavy-load fixing, and anchoring reinforcement in humid, low-temperature, and corrosive environments. Component A is a continuous phase paste-like cementitious substrate, and component B is a water-based activated and regulated liquid phase.
[0025] Component A comprises the following raw materials in parts by weight: 518-641 parts of composite inorganic cementitious substrate, 85-127 parts of modified organic composite emulsion, 191-251 parts of functional composite filler, 22-37 parts of functional additive A, and 128-178 parts of deionized water. Specifically, the composite inorganic cementitious substrate is composed of modified barium calcium sulfoaluminate cement, calcined activated metakaolin, and nano-grade activated silica fume in a mass ratio of (296-348):(133-177):(84-119). The modified barium calcium sulfoaluminate cement has a mineral composition of C4A3≥58wt%, C2S≥22wt%, C4AF≥8wt%, and a specific surface area of 436-472 m². 2 / kg, free calcium oxide and free magnesium oxide are both ≤0.08wt%, initial heat of hydration ≤220J / g (within 45min); the Al2O3 content of the calcined activated metakaolin is 42.6~45.3wt%, and the particle size distribution meets D 50 =7.2~8.8μm, D 90 The particle size is ≤22μm, and the activity index is ≥96%; the SiO2 purity of the nano-sized active silica fume is 92.4~94.7wt%, the average particle size is 94~116nm, and the specific surface area is 17.3~19.6m². 2 / g, loss on ignition ≤1.8wt%.
[0026] The modified organic composite emulsion is formulated by compounding a core-shell structured styrene-acrylic-epoxy composite emulsion and a hydrophilic chain-extended waterborne polyurethane dispersion at a mass ratio of (51~69):(33~59). The core-shell structured styrene-acrylic-epoxy composite emulsion has a solid content of 49.2~51.5wt%, a core glass transition temperature of 28~33℃, a shell glass transition temperature of -12~-7℃, an average particle size of 146~172nm, and a minimum film-forming temperature ≤3℃. The hydrophilic chain-extended waterborne polyurethane dispersion has a solid content of 41.8~44.2wt%, -NCO residue ≤0.12wt%, and an elongation at break of 360%~420%. Furthermore, its compatibility with cement meets the requirements of no demulsification, no floating oil, and no flocculation. The functional composite filler is composed of whisker-shaped nano-calcium carbonate, silane-modified quartz sand, and anatase nano-titanium dioxide in a mass ratio of (73~97):(114~146):(3~8). The whisker-shaped nano-calcium carbonate is aragonite-type with an aspect ratio of 9.6~13.2, a diameter of 0.6~1.8 μm, and an oil absorption value of 18~24 g / 100 g. The silane-modified quartz sand has a Mohs hardness of 7.2~7.4, a continuous gradation of particle size (0.18~0.32 mm), and its surface is modified with KH570 silane coupling agent with a loading of 0.42~0.58 wt%, and a mud content ≤0.15 wt%. The functional additive A is composed of a composite retarder stabilizer, a polycarboxylate ether-based high-efficiency water-reducing agent, a non-silicone mineral oil defoamer, and an organic bentonite-hydroxyethyl cellulose composite thixotropic agent in a mass ratio of (8~15):(4~7):(3~6):(6~10). The composite retarder stabilizer is a mixture of sodium gluconate and aminotrimethylene phosphonic acid in a mass ratio of 1:0.38~0.46, with a retarding efficiency that inhibits the hydration of gelled powder for ≥160 min at 25℃; the polycarboxylate ether-based high-efficiency water-reducing agent has a water reduction rate of 29%~32%; the non-silicone mineral oil defoamer does not demulsify or reduce adhesive strength; and the organic bentonite-hydroxyethyl cellulose composite thixotropic agent has a thixotropic index ≥3.8.
[0027] Component B comprises the following raw materials in parts by weight: 235-278 parts of composite hydration activator, 55-79 parts of bifunctional interface enhancer, 44-67 parts of micro-expansion and shrinkage compensation component, 13-22 parts of B functional additive, and 581-642 parts of deionized water. Specifically, the composite hydration activator is compounded from lithium sulfate-lithium acetate complex salt and modified aluminate alkaline activator in a mass ratio of (87-117):(145-162). In the lithium sulfate-lithium acetate complex salt, the molar ratio of lithium sulfate to lithium acetate is 1:1.32, the purity is ≥98.5wt%, and the complete dissolution time at 25℃ is ≤45s; the modified aluminate alkaline activator has a solid content of 48-52wt%, a pH value of 10.7-11.3, and a corrosion rate of ≤0.01mm / year for Q235 steel and HRB400 steel bars. The bifunctional interfacial reinforcing agent is a compound of silane-modified phosphate coupling agent and medium-viscosity hydroxymethyl cellulose ether in a mass ratio of (34~48):(21~31). The effective content of the silane-modified phosphate coupling agent is 86~92wt%, and the functional groups include -Si(OCH3)3 and -PO3H2, with a bonding strength enhancement rate to concrete ≥42%. The micro-expansion and shrinkage compensation component is 44~67 parts of ultrafine calcium sulfoaluminate expansion agent with a particle size D... 50 =14.6~17.2μm, the limited expansion rate after 7 days of water curing is 0.09%~0.14%, and the shrinkage rate after 21 days in air is ≤-0.02%. The B functional additive is composed of isothiazolinone bactericide, polyacrylate dispersant and propylene glycol-calcium formate composite antifreeze in a mass ratio of (2~4):(5~8):(5~11). Among them, the mass ratio of propylene glycol to calcium formate in the composite antifreeze is 1:0.62, the critical antifreeze temperature is -8℃, and it does not contain chloride ions and has no risk of alkali-aggregate reaction.
[0028] This invention also provides a method for preparing a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, comprising the following steps: S1. First, the composite inorganic cementitious substrate (i.e., modified barium calcium sulfoaluminate cement, calcined activated metakaolin, and nano-grade active silica fume) and functional composite filler (i.e., whisker-like nano-calcium carbonate, silane-modified quartz sand, and anatase nano-titanium dioxide) in the formula amount are put into a double-spiral conical mixer with a filling rate of 65%~72% (preferably 68.5%). The mixture is mixed at a speed of 36~42 r / min (preferably 39 r / min) for 10~20 min (preferably 15 min) to obtain a uniform dry-mixed powder with a powder uniformity deviation of ≤1.2% and no visible agglomerated particles. After mixing, the powder is transferred to a sealed silo, protected by nitrogen, with humidity controlled at ≤35%RH, and the storage time is ≤2h. Add the prescribed amount of deionized water to a stirring vessel and stir at 220~260 r / min (preferably 240 r / min). Then, add the composite retarder stabilizer, polycarboxylate ether high-efficiency water-reducing agent, non-silicone mineral oil defoamer, and organic bentonite-hydroxyethyl cellulose composite thixotropic agent (i.e. functional additive A) in sequence. Stir for 2.5 min after each additive is added, and continue stirring for 5 min after all additives are added to obtain a homogeneous aqueous phase liquid without precipitation or stratification. The dry-mixed powder is then added to the aqueous phase at a rate of 1.8~2.3 kg / min (preferably 2.0 kg / min), while simultaneously increasing the stirring speed to 460~520 r / min (preferably 490 r / min) and controlling the system temperature at 18~26℃ (preferably 22℃). After the powder is added, stirring continues for 10 min to form a uniform paste. The stirring speed is then reduced to 280~320 r / min (preferably 300 r / min), and the core-shell structured styrene-acrylic-epoxy composite emulsion and the hydrophilic chain-extended waterborne polyurethane dispersion (i.e., modified organic composite emulsion) are slowly added. After the addition is complete, stirring continues for 8 min to ensure complete compatibility between the organic and inorganic phases, with no floating oil or particle aggregation. The resulting mixed paste is transferred to a vacuum high-shear mixer and stirred at 240 r / min for 5~8 min (preferably 6.5 min) under a vacuum of -0.072~-0.065 MPa (preferably -0.0685 MPa) to degas the mixture and eliminate internal defects. After degassing, the material is discharged into a sealed aluminum-plastic composite packaging drum, filled with nitrogen, and sealed to obtain component A. The resulting component A paste is uniform and fine, with a density of 1.86~1.94 g / cm³. 3 Stable period at 25℃: ≥180 days.
[0029] S2, add the prescribed amount of deionized water to a stirred tank and stir at 210~240 r / min (preferably 225 r / min). Then, sequentially add isothiazolinone bactericide, polyacrylate dispersant, and propylene glycol-calcium formate composite antifreeze (i.e., functional additive B), stirring for 3.5 min until completely dissolved, resulting in a clear, transparent solution free of suspended matter. Next, add lithium sulfate-lithium acetate double salt and stir for 4 min until completely clear. Then, slowly add the modified aluminate alkaline activator (i.e., composite hydration activator), maintaining a temperature of 16~28℃ (preferably 22℃) throughout the process, stirring for 6.5 min. Subsequently, a silane-modified phosphate coupling agent and medium-viscosity hydroxymethyl cellulose ether (i.e., a bifunctional interfacial enhancer) were added, and the mixture was stirred for 5 minutes. Then, an ultrafine calcium sulfoaluminate expanding agent (i.e., a micro-expansion and shrinkage compensation component) was added at a rate of 1.2 kg / min, and the stirring speed was increased to 320-360 r / min (preferably 340 r / min), and the mixture was stirred for 7.5 minutes to ensure that the solid particles were completely suspended and there was no sedimentation. The resulting mixture was then pressure filtered through a 100-150 mesh (preferably 120 mesh) stainless steel filter. The filtrate was transferred to a corrosion-resistant plastic container, sealed, and stored in a light-proof environment to obtain component B. The obtained component B has a homogeneous liquid phase, without stratification or precipitation, and a density of 1.18-1.24 g / cm³. 3 Storage stability period ≥360 days.
[0030] S3, at the construction site, component A and component B are mixed at a mass ratio of 3.92~4.15:1 (preferably 4.05:1). Mixing can be carried out using a handheld electric mixer (speed 280~450 r / min) or a two-component grouting pump with a static mixing pipe (stage ≥16). During mixing, the stirring speed is 360~420 r / min (preferably 390 r / min), and the stirring time is 3.2~3.8 min (preferably 3.5 min). During the stirring process, the stirring head is moved up and down to ensure that there are no dead corners at the bottom and sides of the bucket. The mixed system is qualified as a uniform light gray paste, without streaks, particles, or visible bubbles. The working time of the mixed paste is 28~38 min (25℃, preferably 33 min). During construction, pour from the bottom of the hole or the bottom of the gap upwards to avoid air entrapment. It fills the gap by its own flow and does not require vibration or compaction. When constructing on vertical or top surfaces, it does not flow or fall, and the slippage is ≤0.8mm / 10min.
[0031] The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system prepared by the above method exhibits the following curing properties at room temperature (20℃): initial setting time 40~52 min, final setting time 90~106 min, 1-day compressive strength ≥36 MPa, 3-day compressive strength ≥57 MPa, and 28-day compressive strength ≥77 MPa. This system can be applied normally in ambient temperatures ranging from -6℃ to 38℃, demonstrating good temperature adaptability.
[0032] This cementitious system achieves a synergistic improvement in low shrinkage and high durability. Its core mechanism is as follows: Regarding volume stability, the composite inorganic cementitious system hydrates to form a three-dimensional framework structure of ettringite, CSH gel, and barium aluminum silicate. The organic phase forms a continuous flexible film in the gaps between the framework. Simultaneously, the ultrafine calcium sulfoaluminate expander in the micro-expansion and shrinkage compensation component releases a micro-expansion effect during the mid-hydration stage, precisely offsetting the chemical and drying shrinkage of the cementitious body. The final linear shrinkage rate can be controlled to ≤0.028%. Regarding interface reinforcement, the silane-modified phosphate coupling agent in the bifunctional interface reinforcer contains -Si(OCH3)3 and -PO3H2 functional groups, which can simultaneously connect the inorganic cementitious phase to the hydroxyl groups on the surface of the reinforcing steel or concrete substrate, forming covalent bonds. This significantly improves the interfacial bond strength and pull-out strength, achieving a tensile bond strength ≥4.7MPa with C30 concrete and a shear bond strength ≥18MPa with HRB400 reinforcing steel. In terms of durability, the system has high density and excellent resistance to chloride ion penetration, carbonization, freeze-thaw cycles and chemical corrosion. The strength loss rate after 300 freeze-thaw cycles is ≤8%, and the strength does not decrease during long-term service.
[0033] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0034] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" represents weight percentage, "parts" represents parts by weight, and "ratio" represents weight proportion.
[0035] Example 1 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0036] Component A: The composition includes: 298.4 parts modified barium calcium sulfoaluminate cement, 134.2 parts calcined activated metakaolin, 85.7 parts nano-activated silica fume, 52.1 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 33.2 parts waterborne polyurethane dispersion, 73.1 parts whisker calcium carbonate, 114.2 parts modified quartz sand, 3.6 parts nano titanium dioxide, 8.5 parts composite retarder stabilizer, 4.3 parts polycarboxylate superplasticizer, 3.4 parts mineral oil defoamer, 6.7 parts composite thixotropic agent, and 128.3 parts deionized water.
[0037] Component B: 88.2 parts lithium sulfate-lithium acetate double salt, 146.3 parts modified aluminate activator, 34.2 parts silane modified phosphate ester, 21.5 parts hydroxymethyl cellulose ether, 44.3 parts ultrafine calcium sulfoaluminate expanding agent, 2.4 parts bactericide, 5.3 parts polyacrylate dispersant, 5.2 parts composite antifreeze agent, and 581.4 parts deionized water.
[0038] At the construction site, component A and component B are mixed at a mass ratio of 3.92:1.
[0039] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 68.5% and mixed at a speed of 39 r / min for 15 min to obtain a uniform dry-mixed powder.
[0040] Add the prescribed amount of deionized water to a stirred tank and stir at 240 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0041] The above dry-mixed powder was added to the aqueous phase at a rate of 2.0 kg / min, while the stirring speed was increased to 490 r / min and the system temperature was controlled at 22℃. After the powder was added, stirring was continued for 10 min. Then the stirring speed was reduced to 300 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 8 min to obtain a mixed paste.
[0042] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 6.5 min under a vacuum of -0.0685 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0043] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 225 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0044] Add lithium sulfate-lithium acetate double salt, stir for 4 minutes until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 22℃, and stir for 6.5 minutes.
[0045] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5 minutes, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 340 r / min, and stir for 7.5 minutes until the solid particles are completely suspended.
[0046] The resulting mixture was filtered under pressure through a 125-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0047] S3. Mix component A and component B at a mass ratio of 3.92:1, and stir at 390 r / min for 3.5 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 33 min.
[0048] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0049] Example 2 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0050] Component A: The composition includes: 307.2 parts modified barium calcium sulfoaluminate cement, 141.7 parts calcined activated metakaolin, 92.3 parts nano-activated silica fume, 55.3 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 37.6 parts waterborne polyurethane dispersion, 78.5 parts whisker calcium carbonate, 119.7 parts modified quartz sand, 4.2 parts nano titanium dioxide, 9.7 parts composite retarder stabilizer, 4.8 parts polycarboxylate superplasticizer, 3.9 parts mineral oil defoamer, 7.2 parts composite thixotropic agent, and 136.5 parts deionized water.
[0051] Component B: 93.6 parts lithium sulfate-lithium acetate double salt, 149.8 parts modified aluminate activator, 37.5 parts silane modified phosphate ester, 23.7 parts hydroxymethyl cellulose ether, 48.7 parts ultrafine calcium sulfoaluminate expander, 2.7 parts bactericide, 5.8 parts polyacrylate dispersant, 6.1 parts composite antifreeze, and 593.2 parts deionized water.
[0052] At the construction site, component A and component B are mixed at a mass ratio of 3.97:1.
[0053] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 65% and mixed at 36 r / min for 20 min to obtain a uniform dry-mixed powder.
[0054] Add the prescribed amount of deionized water to a stirred tank and stir at 220 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0055] The above dry-mixed powder was added to the aqueous phase at a rate of 1.8 kg / min, while the stirring speed was increased to 460 r / min and the system temperature was controlled at 18℃. After the powder was added, stirring was continued for 11.5 min. Then the stirring speed was reduced to 280 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 9.2 min to obtain a mixed paste.
[0056] The mixed paste was transferred into a vacuum high-shear mixer and stirred at 240 r / min for 5 min under a vacuum of -0.072 MPa. The mixture was then discharged, sealed, and packaged to obtain component A.
[0057] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 210 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0058] Add lithium sulfate-lithium acetate double salt, stir for 4.6 min until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 16℃, and stir for 7.5 min.
[0059] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5.8 min, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 320 r / min, and stir for 8.6 min until the solid particles are completely suspended.
[0060] The resulting mixture was filtered under pressure through a 100-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0061] S3. Mix component A and component B at a mass ratio of 3.97:1, and stir at 360 r / min for 3.8 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 38 min.
[0062] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0063] Example 3 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0064] Component A: The composition includes: 315.6 parts modified barium calcium sulfoaluminate cement, 149.3 parts calcined activated metakaolin, 98.6 parts nano-activated silica fume, 58.2 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 42.1 parts waterborne polyurethane dispersion, 83.9 parts whisker calcium carbonate, 125.3 parts modified quartz sand, 4.9 parts nano titanium dioxide, 10.8 parts composite retarder stabilizer, 5.2 parts polycarboxylate superplasticizer, 4.3 parts mineral oil defoamer, 7.8 parts composite thixotropic agent, and 144.7 parts deionized water.
[0065] Component B: 99.1 parts lithium sulfate-lithium acetate double salt, 153.2 parts modified aluminate activator, 40.8 parts silane modified phosphate ester, 25.9 parts hydroxymethyl cellulose ether, 53.2 parts ultrafine calcium sulfoaluminate expander, 3.1 parts bactericide, 6.2 parts polyacrylate dispersant, 6.9 parts composite antifreeze, and 605.7 parts deionized water.
[0066] At the construction site, component A and component B are mixed at a mass ratio of 4.02:1.
[0067] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added into a double helical conical mixer with a filling rate of 72% and mixed at a speed of 42 r / min for 10 min to obtain a uniform dry-mixed powder.
[0068] Add the prescribed amount of deionized water to a stirred tank and stir at 260 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0069] The dry-mixed powder was added to the aqueous phase at a rate of 2.3 kg / min, while the stirring speed was increased to 520 r / min and the system temperature was controlled at 26℃. After the powder was added, stirring was continued for 8.5 min. Then the stirring speed was reduced to 320 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 6.8 min to obtain a mixed paste.
[0070] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 8 min under a vacuum of -0.065 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0071] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 240 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0072] Add lithium sulfate-lithium acetate double salt, stir for 3.4 min until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 28℃, and stir for 5.5 min.
[0073] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 4.2 min, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 360 r / min, and stir for 6.4 min until the solid particles are completely suspended.
[0074] The resulting mixture was filtered under pressure through a 150-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0075] S3. Mix component A and component B at a mass ratio of 4.02:1, and stir at 420 r / min for 3.2 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 28 min.
[0076] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0077] Example 4 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0078] Component A: The composition includes: 324.3 parts modified barium calcium sulfoaluminate cement, 156.8 parts calcined activated metakaolin, 105.1 parts nano-activated silica fume, 61.4 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 46.5 parts waterborne polyurethane dispersion, 89.2 parts whisker calcium carbonate, 130.8 parts modified quartz sand, 5.5 parts nano titanium dioxide, 11.9 parts composite retarder stabilizer, 5.7 parts polycarboxylate superplasticizer, 4.8 parts mineral oil defoamer, 8.3 parts composite thixotropic agent, and 152.9 parts deionized water.
[0079] Component B: 104.5 parts lithium sulfate-lithium acetate double salt, 156.7 parts modified aluminate activator, 44.1 parts silane modified phosphate ester, 28.1 parts hydroxymethyl cellulose ether, 57.6 parts ultrafine calcium sulfoaluminate expanding agent, 3.4 parts bactericide, 6.7 parts polyacrylate dispersant, 7.8 parts composite antifreeze agent, and 618.2 parts deionized water.
[0080] At the construction site, component A and component B are mixed at a mass ratio of 4.05:1.
[0081] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 68.5% and mixed at a speed of 39 r / min for 15 min to obtain a uniform dry-mixed powder.
[0082] Add the prescribed amount of deionized water to a stirred tank and stir at 240 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0083] The above dry-mixed powder was added to the aqueous phase at a rate of 2.0 kg / min, while the stirring speed was increased to 490 r / min and the system temperature was controlled at 22℃. After the powder was added, stirring was continued for 10 min. Then the stirring speed was reduced to 300 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 8 min to obtain a mixed paste.
[0084] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 6.5 min under a vacuum of -0.0685 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0085] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 225 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0086] Add lithium sulfate-lithium acetate double salt, stir for 4 minutes until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 22℃, and stir for 6.5 minutes.
[0087] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5 minutes, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 340 r / min, and stir for 7.5 minutes until the solid particles are completely suspended.
[0088] The resulting mixture was filtered under pressure through a 125-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0089] S3. Mix component A and component B at a mass ratio of 4.05:1, and stir at 390 r / min for 3.5 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 33 min.
[0090] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0091] Example 5 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0092] Component A: The composition includes: 332.8 parts modified barium calcium sulfoaluminate cement, 164.2 parts calcined activated metakaolin, 111.4 parts nano-activated silica fume, 64.3 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 50.8 parts waterborne polyurethane dispersion, 94.6 parts whisker calcium carbonate, 136.2 parts modified quartz sand, 6.1 parts nano titanium dioxide, 12.7 parts composite retarder stabilizer, 6.1 parts polycarboxylate superplasticizer, 5.1 parts mineral oil defoamer, 8.9 parts composite thixotropic agent, and 161.2 parts deionized water.
[0093] Component B: The composition includes: 109.7 parts lithium sulfate-lithium acetate double salt, 159.4 parts modified aluminate activator, 47.3 parts silane modified phosphate ester, 30.2 parts hydroxymethyl cellulose ether, 62.1 parts ultrafine calcium sulfoaluminate expander, 3.6 parts bactericide, 7.1 parts polyacrylate dispersant, 8.7 parts composite antifreeze, and 630.6 parts deionized water.
[0094] At the construction site, component A and component B are mixed at a mass ratio of 4.08:1.
[0095] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 68.5% and mixed at a speed of 39 r / min for 15 min to obtain a uniform dry-mixed powder.
[0096] Add the prescribed amount of deionized water to a stirred tank and stir at 240 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0097] The above dry-mixed powder was added to the aqueous phase at a rate of 2.0 kg / min, while the stirring speed was increased to 490 r / min and the system temperature was controlled at 22℃. After the powder was added, stirring was continued for 10 min. Then the stirring speed was reduced to 300 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 8 min to obtain a mixed paste.
[0098] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 6.5 min under a vacuum of -0.0685 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0099] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 225 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0100] Add lithium sulfate-lithium acetate double salt, stir for 4 minutes until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 22℃, and stir for 6.5 minutes.
[0101] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5 minutes, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 340 r / min, and stir for 7.5 minutes until the solid particles are completely suspended.
[0102] The resulting mixture was filtered under pressure through a 125-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0103] S3. Mix component A and component B at a mass ratio of 4.08:1, and stir at 390 r / min for 3.5 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 33 min.
[0104] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0105] Example 6 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0106] Component A: The composition includes: 341.5 parts modified barium calcium sulfoaluminate cement, 171.6 parts calcined activated metakaolin, 117.2 parts nano-activated silica fume, 67.1 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 55.3 parts waterborne polyurethane dispersion, 96.8 parts whisker calcium carbonate, 141.7 parts modified quartz sand, 6.9 parts nano titanium dioxide, 13.8 parts composite retarder stabilizer, 6.5 parts polycarboxylate superplasticizer, 5.5 parts mineral oil defoamer, 9.5 parts composite thixotropic agent, and 169.4 parts deionized water.
[0107] Component B: 114.2 parts lithium sulfate-lithium acetate double salt, 161.3 parts modified aluminate activator, 46.9 parts silane modified phosphate, 29.4 parts hydroxymethyl cellulose ether, 65.8 parts ultrafine calcium sulfoaluminate expander, 3.7 parts bactericide, 7.5 parts polyacrylate dispersant, 9.5 parts composite antifreeze, and 641.3 parts deionized water.
[0108] At the construction site, component A and component B are mixed at a mass ratio of 4.12:1.
[0109] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 68.5% and mixed at a speed of 39 r / min for 15 min to obtain a uniform dry-mixed powder.
[0110] Add the prescribed amount of deionized water to a stirred tank and stir at 240 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0111] The above dry-mixed powder was added to the aqueous phase at a rate of 2.0 kg / min, while the stirring speed was increased to 490 r / min and the system temperature was controlled at 22℃. After the powder was added, stirring was continued for 10 min. Then the stirring speed was reduced to 300 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 8 min to obtain a mixed paste.
[0112] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 6.5 min under a vacuum of -0.0685 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0113] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 225 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0114] Add lithium sulfate-lithium acetate double salt, stir for 4 minutes until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 22℃, and stir for 6.5 minutes.
[0115] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5 minutes, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 340 r / min, and stir for 7.5 minutes until the solid particles are completely suspended.
[0116] The resulting mixture was filtered under pressure through a 125-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0117] S3. Mix component A and component B at a mass ratio of 4.12:1, and stir at 390 r / min for 3.5 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 33 min.
[0118] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0119] Example 7 This embodiment provides a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, the raw material ratio of its component A and component B is as follows.
[0120] Component A: The composition includes: 346.9 parts modified barium calcium sulfoaluminate cement, 175.4 parts calcined activated metakaolin, 118.3 parts nano-activated silica fume, 68.5 parts core-shell structured styrene-acrylic-epoxy composite emulsion, 58.2 parts waterborne polyurethane dispersion, 97.1 parts whisker calcium carbonate, 145.8 parts modified quartz sand, 7.7 parts nano titanium dioxide, 14.5 parts composite retarder stabilizer, 6.7 parts polycarboxylate superplasticizer, 5.6 parts mineral oil defoamer, 10.2 parts composite thixotropic agent, and 177.6 parts deionized water.
[0121] Component B: The composition includes: 116.3 parts lithium sulfate-lithium acetate double salt, 161.6 parts modified aluminate activator, 48.1 parts silane modified phosphate ester, 30.4 parts hydroxymethyl cellulose ether, 67.3 parts ultrafine calcium sulfoaluminate expander, 3.8 parts bactericide, 7.6 parts polyacrylate dispersant, 10.1 parts composite antifreeze, and 642.1 parts deionized water.
[0122] At the construction site, component A and component B are mixed at a mass ratio of 4.15:1.
[0123] The preparation method of the gelling system described in this embodiment is as follows: Preparation of S1, component A: The modified barium calcium sulfoaluminate cement, calcined activated metakaolin, nano-activated silica fume, whisker calcium carbonate, modified quartz sand and nano titanium dioxide were added to a double helix conical mixer with a filling rate of 68.5% and mixed at a speed of 39 r / min for 15 min to obtain a uniform dry-mixed powder.
[0124] Add the prescribed amount of deionized water to a stirred tank and stir at 240 r / min. Then add the composite retarder stabilizer, polycarboxylate superplasticizer, mineral oil defoamer and composite thixotropic agent in sequence. Stir for 2.5 min after each addition of an additive. After all additives are added, continue stirring for 5 min to obtain a homogeneous aqueous phase.
[0125] The above dry-mixed powder was added to the aqueous phase at a rate of 2.0 kg / min, while the stirring speed was increased to 490 r / min and the system temperature was controlled at 22℃. After the powder was added, stirring was continued for 10 min. Then the stirring speed was reduced to 300 r / min, and the core-shell structured styrene-acrylic-epoxy composite emulsion and waterborne polyurethane dispersion were slowly added. After the addition was completed, stirring was continued for 8 min to obtain a mixed paste.
[0126] The mixed paste was transferred into a vacuum high-shear mixer and stirred and degassed at 240 r / min for 6.5 min under a vacuum of -0.0685 MPa. The mixture was then discharged and sealed in packaging to obtain component A.
[0127] Preparation of S2, component B: Add the prescribed amount of deionized water to the mixing tank and stir at 225 r / min. Then add the bactericide, polyacrylate dispersant and composite antifreeze in sequence and stir for 3.5 min until completely dissolved.
[0128] Add lithium sulfate-lithium acetate double salt, stir for 4 minutes until completely dissolved, then slowly add modified aluminate activator, control the system temperature at 22℃, and stir for 6.5 minutes.
[0129] Add silane-modified phosphate ester and hydroxymethyl cellulose ether, stir for 5 minutes, then add ultrafine calcium sulfoaluminate expansion agent at a rate of 1.2 kg / min, increase the stirring speed to 340 r / min, and stir for 7.5 minutes until the solid particles are completely suspended.
[0130] The resulting mixture was filtered under pressure through a 125-mesh stainless steel filter screen. The filtrate was then transferred to a corrosion-resistant container, sealed, and stored away from light to obtain component B.
[0131] S3. Mix component A and component B at a mass ratio of 4.15:1, and stir at 390 r / min for 3.5 min until a homogeneous paste is obtained, thus obtaining a low-shrinkage, high-durability inorganic-organic composite anchoring gelling system. The working time of the mixed paste is 33 min.
[0132] The performance of the gelling system prepared in this embodiment was tested, and the results are shown in Table 1.
[0133] The testing methods for each performance indicator are as follows: Compressive strength: Tested according to GB / T 17671-2021, at 1d, 3d, and 28d. Curing shrinkage rate: Tested according to GB / T 2419-2017, standard curing time 28 days; Interfacial bond strength: tensile bond strength with C30 concrete, tested according to JGJ 145-2013; Shear bond strength of rebar: Shear test with HRB400 rebar, according to GB 50367-2013; Freeze-thaw resistance: Strength loss rate after 300 freeze-thaw cycles, tested according to GB / T 50082-2009; Initial setting / final setting time: Tested according to GB / T 1346-2011.
[0134] Table 1 Performance test results of Examples 1-7 of the present invention
[0135] According to the test results in Table 1, the low-shrinkage, high-durability inorganic-organic composite anchoring cementitious systems prepared in Examples 1-7 of this invention exhibit excellent performance in all performance indicators. The initial setting time is 35.8~41.7 min, and the final setting time is 84.3~92.4 min, which meets the workability requirements for on-site construction. The compressive strength at 1 day, 3 days, and 28 days reaches 36.2~42.7 MPa, 57.4~65.1 MPa, and 77.3~85.2 MPa, respectively, demonstrating excellent early strength development and later strength growth. The 28-day curing shrinkage rate is only 0.022%~0.027%, which is far lower than that of traditional inorganic anchoring materials. The tensile bond strength with C30 concrete reaches 4.71~5.27 MPa, and the shear bond strength with HRB400 steel bars reaches 18.14~19.86 MPa, indicating that the system has good interfacial bonding performance with both concrete and steel reinforcement substrates. After 300 freeze-thaw cycles, the strength loss rate is only 6.27%~7.81%, demonstrating excellent freeze-thaw resistance and durability. In summary, this invention achieves a good balance between low shrinkage, high strength, high adhesion, and excellent durability, making it suitable for engineering scenarios such as heavy-duty anchoring, rebar installation, and structural reinforcement in complex environments, and has broad prospects for widespread application.
[0136] The above content is only for illustrating the technical concept of the present invention and should not be construed as limiting the scope of protection of the present invention. Any modifications made to the technical solution based on the technical concept proposed in this invention shall fall within the scope of protection of the claims of this invention.
Claims
1. A low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system, characterized in that, It includes component A and component B, wherein component A and component B are mixed at a mass ratio of 3.92 to 4.15:1; The A component comprises the following raw materials in parts by weight: 518-641 parts of composite inorganic cementitious substrate, 85-127 parts of modified organic composite emulsion, 191-251 parts of functional composite filler, 22-37 parts of functional additive A, and 128-178 parts of deionized water. The B component comprises the following raw materials in parts by weight: 235-278 parts of composite hydration activator, 55-79 parts of bifunctional interface enhancer, 44-67 parts of micro-expansion and shrinkage compensation component, 13-22 parts of B functional additive, and 581-642 parts of deionized water.
2. The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 1, characterized in that, The composite inorganic cementitious substrate is composed of modified barium calcium sulfoaluminate cement, calcined activated metakaolin, and nano-grade active silica fume in a mass ratio of (296~348):(133~177):(84~119).
3. The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 1, characterized in that, The modified organic composite emulsion is a compound of a core-shell structured styrene-acrylic-epoxy composite emulsion and a hydrophilic chain-extended waterborne polyurethane dispersion in a mass ratio of (51~69):(33~59).
4. The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 1, characterized in that, The functional composite filler is a mixture of whisker-shaped nano-calcium carbonate, silane-modified quartz sand, and anatase nano-titanium dioxide in a mass ratio of (73~97):(114~146):(3~8).
5. The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 1, characterized in that, The functional additive A is a compound of a composite retarder stabilizer, a polycarboxylic acid ether high-efficiency water-reducing agent, a non-silicone mineral oil defoamer, and an organic bentonite-hydroxyethyl cellulose composite thixotropic agent in a mass ratio of (8~15):(4~7):(3~6):(6~10).
6. The low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 1, characterized in that, The composite hydration activator is a compound of lithium sulfate-lithium acetate double salt and modified aluminate alkaline activator in a mass ratio of (87~117):(145~162); The bifunctional interface enhancer is a compound of silane-modified phosphate coupling agent and medium-viscosity hydroxymethyl cellulose ether in a mass ratio of (34~48):(21~31); The micro-expansion and shrinkage compensation component is an ultrafine calcium sulfoaluminate expander; Functional additive B is a compound of isothiazolinone bactericide, polyacrylate dispersant and propylene glycol-calcium formate composite antifreeze in a mass ratio of (2~4):(5~8):(5~11).
7. A method for preparing a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1, mix the formulated amount of composite inorganic cementitious substrate and functional composite filler to obtain a uniform dry-mixed powder; mix the formulated amount of deionized water with functional additive A to obtain a uniform aqueous phase liquid; add the dry-mixed powder to the aqueous phase liquid, control the system temperature, stir and mix, add the modified organic composite emulsion, continue stirring, and degas under vacuum to obtain component A. S2, mix the prescribed amount of deionized water with functional additive B, add the composite hydration activator and stir until completely dissolved, then add the bifunctional interface enhancer and micro-expansion and shrinkage compensation component, stir until uniformly dispersed, and filter to obtain component B; S3. Mix component A and component B at a mass ratio of 3.92~4.15:1 to obtain the low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system.
8. The preparation method of a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 7, characterized in that, The composite inorganic cementitious substrate and functional composite filler described in S1 are mixed using a double-helix conical mixer with a filling rate of 65%~72%, a mixing speed of 36~42 r / min, and a mixing time of 10~20 min.
9. The preparation method of a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 7, characterized in that, The vacuum degree of vacuum degassing described in S1 is -0.072 to -0.065 MPa, and the degassing time is 5 to 8 minutes; the filtration described in S2 uses a 100 to 150 mesh stainless steel filter screen for pressure filtration.
10. The preparation method of a low-shrinkage, high-durability inorganic-organic composite anchoring cementitious system according to claim 7, characterized in that, The mixing speed described in S3 is 360~420 r / min, the mixing time is 3.2~3.8 min, and the working time of the mixed paste is 28~38 min.