Fluidified solidified soil for electromagnetic shielding protection and method for preparing the same

By converting the iron olivine and FeO-SiO₂ glass phase in smelting slag into a symbiotic structure of magnetite and amorphous silica through low-temperature redox roasting, and combining it with high residual carbon coarse fly ash and a curing agent, a low-cost and highly stable electromagnetic shielding fluidized solidified soil was prepared. This solved the problems of high cost and unstable effect in the existing technology, and achieved the improvement of electromagnetic shielding and mechanical properties.

CN123131111APending Publication Date: 2026-11-20SHANGHAI CIVIL ENG GRP CO LTD OF CREC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611635581.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing electromagnetic shielding materials rely on expensive functional materials, resulting in high costs and unstable shielding effects. Fluidized solidified soil does not have electromagnetic shielding function, and existing copper slag treatment processes are energy-intensive and have long processes, making it difficult to simultaneously improve electromagnetic shielding and mechanical properties.

Method used

By using low-temperature oxidative roasting and reduction roasting, the iron olivine and FeO-SiO₂ glass phase in the smelting slag are transformed in situ into a symbiotic structure of magnetite and amorphous silica. Combined with high residual carbon coarse fly ash and a curing agent, electromagnetically shielded fluidized solidified soil is prepared to avoid high-temperature melting and magnetic separation.

Benefits of technology

It achieves low-cost and stable electromagnetic shielding, simplifies the process, reduces energy consumption, improves electromagnetic shielding effectiveness and mechanical properties, and realizes the high-value utilization of smelting slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131111A_ABST
    Figure CN123131111A_ABST
Patent Text Reader

Abstract

This invention discloses a fluidized solidified soil for electromagnetic shielding and its preparation method, relating to the field of building materials technology. The preparation method includes: providing smelting slag containing fir olivine and / or FeO-SiO2 glass phase; grinding and sieving the smelting slag; placing the ground slag in an oxidizing atmosphere and calcining it at 600℃~700℃ without adding flux, causing the fir olivine and / or FeO-SiO2 glass phase to decompose in situ, obtaining a mixture; placing the mixture in a reducing atmosphere and calcining it at 480℃~550℃, then cooling it to room temperature, obtaining a composite filler; mixing and stirring 10~15 parts by weight of high residual carbon coarse fly ash, 30~40 parts by weight of the composite filler, 15~35 parts by weight of solidifying agent, and 130~150 parts by weight of water per 100 parts by weight of dry soil sample to obtain the fluidized solidified soil. The fluidized solidified soil of this invention possesses good electromagnetic shielding effectiveness, mechanical properties, and system stability, while also realizing the high-value utilization of smelting slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, and in particular to a fluidized solidified soil for electromagnetic shielding and its preparation method. Background Technology

[0002] With the rapid development of electronic devices and communication technologies, electromagnetic radiation pollution has become increasingly serious, leading to a growing demand for electromagnetic protection materials.

[0003] Currently, electromagnetic shielding concrete achieves its electromagnetic shielding function by incorporating conductive or magnetically conductive materials such as steel fibers, graphite powder, and magnetite powder. However, these purchased functional materials are costly, and the high-density magnetically conductive materials such as magnetite powder have a significant density difference from cement paste, leading to sedimentation, stratification, and uneven dispersion in the fluid system, resulting in decreased stability of the electromagnetic shielding effect. US Patent US8968461B1 discloses an electromagnetic shielding concrete composed of cement, aggregate, water, graphite / conductive carbon, fly ash or slag, and magnetically conductive materials such as magnetite. While this solution achieves a certain electromagnetic shielding effect, its electromagnetic shielding performance still depends on the incorporation of graphite / conductive carbon and magnetite, failing to escape the reliance on expensive functional materials.

[0004] To reduce material costs, existing technologies attempt to prepare electromagnetic shielding materials using copper slag as a raw material. One study (An Innovated Application of Reutilize Copper Smelter Slag for Cement-based Electromagnetic Interference Composites, Scientific Reports, 2018, 8(1): 16155) directly incorporated copper slag into cement as a magnetically conductive material to prepare electromagnetic shielding materials. However, the iron in copper slag mainly exists in the form of fir olivine and FeO-SiO2 glass phases. Fir olivine and FeO-SiO2 glass phases themselves do not possess electromagnetic shielding capabilities; copper slag only has a weak electromagnetic shielding ability due to the presence of a small amount of natural magnetite. In this scheme, even with a copper slag content of 45%, its shielding effectiveness in the 500MHz–1.5GHz frequency band only increases from 3.5dB–4.5dB of pure cement to approximately 7dB–8dB. It is evident that the electromagnetic shielding effect of using copper slag directly is very limited, and the cementing activity of copper slag is relatively low. When used as an admixture, it is insufficient to effectively bind soil particles, resulting in the inability to simultaneously meet the requirements of electromagnetic shielding and mechanical properties.

[0005] To achieve the magnetization conversion of iron components in copper slag, existing technologies mostly pre-treat the copper slag with the aim of recovering iron concentrate. Chinese patent application CN102260787A discloses a two-stage roasting-magnetic separation method for copper smelting slag. In this method, the oxidative roasting temperature is 1150℃~1300℃, requiring the addition of calcium oxide flux. After reduction roasting, magnetic separation is performed to recover the magnetite generated after roasting conversion from the copper slag to obtain iron concentrate. However, this process relies on high-temperature melting roasting and consumes flux, resulting in high energy consumption, a long process, and high processing costs. Furthermore, the magnetic separation separates the iron and silicon components into two products. The resulting magnetic component retains only its magnetic function, and the cementing activity of the silicon component cannot be simultaneously utilized in the magnetic component, making it difficult to directly use as a filler with both electromagnetic shielding and cementing activity.

[0006] Chinese patent application CN112142415A discloses a scheme to prepare cement-based electromagnetic shielding materials by wet grinding copper slag to 0.8μm to 1.5μm and combining it with recycled carbon fiber and rubber powder. However, this scheme still relies on expensive externally purchased functional materials such as recycled carbon fiber. Moreover, wet grinding copper slag to extremely fine particles of 0.8μm to 1.5μm consumes a lot of energy.

[0007] On the other hand, fluidized solidified soil is a building material with good fluidity, strong self-compacting properties, and convenient construction, and is widely used in engineering fields such as foundation pit backfilling and trench filling. However, existing fluidized solidified soil formulations do not contain conductive or magnetic functional components and lack electromagnetic shielding capabilities, making it difficult to meet the electromagnetic protection requirements of special occasions such as communication cable trenches.

[0008] The statements herein provide only background information in relation to the present invention and do not necessarily constitute prior art. Summary of the Invention

[0009] The purpose of this invention is to provide a fluidized solidified soil for electromagnetic shielding and a method for its preparation.

[0010] To achieve the above objectives, the present invention provides a method for preparing fluidized solidified soil for electromagnetic shielding, comprising: Step 1: Provide smelting slag, grind and sieve the smelting slag, wherein the smelting slag contains fir olivine and / or FeO-SiO2 glass phase; Step 2: Without adding flux, the ground smelting slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 10%~15% and a water vapor volume fraction of 3%~5%, and roasted at 600℃~700℃ to decompose the iron olivine and / or the FeO-SiO2 glass phase in situ, to obtain a mixture containing magnetite, amorphous silica and hematite. Step 3: The mixture is placed in a reducing atmosphere with an oxygen volume fraction greater than 0 and not more than 5% and a carbon monoxide volume fraction not less than 10%, and calcined at 480℃ to 550℃. Then it is cooled to room temperature under a nitrogen atmosphere to obtain a composite filler. The composite filler contains a symbiotic structure of magnetite and amorphous silica, and the magnetite and amorphous silica are formed in situ from the same smelting slag particles. Step 4: Based on 100 parts by weight of dry soil sample, mix and stir 10-15 parts by weight of high residual carbon coarse fly ash, 30-40 parts by weight of the composite filler, 15-35 parts by weight of curing agent and 130-150 parts by weight of water to obtain fluidized solidified soil for electromagnetic shielding protection.

[0011] Optionally, in step 1, grinding and sieving the smelting slag includes: grinding the smelting slag until the residue on an 80μm square hole sieve does not exceed 10% by mass percentage.

[0012] Optionally, in step 2, the roasting time is 60 min to 120 min; in step 3, the roasting time is 50 min to 100 min.

[0013] Optionally, in step 3, the volume fraction of carbon monoxide is less than or equal to 20%.

[0014] Optionally, step 4 may also include 0.5 to 2 parts by weight of graphite carbon powder, calculated based on 100 parts by weight of dry soil sample.

[0015] Optionally, in step 4, the loss on ignition of the high residual carbon coarse fly ash is greater than or equal to 8%; and the high residual carbon coarse fly ash is fly ash that, after grinding, has a residue of greater than or equal to 10% and less than or equal to 20% on a 45μm square hole sieve, expressed as a percentage by mass.

[0016] Optionally, in step 4, the dry soil sample is any one or a combination of several of the following: engineering waste soil, weathered rock soil, and silt, and the organic matter content in the dry soil sample is less than or equal to 4% by mass.

[0017] Optionally, the curing agent is an SS-WS type curing agent, which includes cement, slag powder, water-reducing agent and activator.

[0018] Optionally, the smelting slag includes at least one of copper slag and nickel slag.

[0019] The present invention also provides a fluidized solidified soil for electromagnetic shielding protection, wherein the fluidized solidified soil is prepared by the preparation method described above.

[0020] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects: To address the shortcomings of existing electromagnetic shielding concrete, which relies on the purchase of expensive functional materials such as steel fibers, graphite powder, and magnetite powder, resulting in high costs, this invention uses smelting slag (such as copper slag or nickel slag) as raw material. Through low-temperature oxidation roasting (600℃~700℃) and low-temperature reduction roasting (480~550℃), the fir olivine (Fe2SiO4) and / or FeO-SiO2 glass phase are transformed in situ into a symbiotic structure of magnetite and amorphous silica, resulting in a high magnetite content (up to 38%~51%). Magnetite, as a magnetically conductive component, provides electromagnetic shielding functionality, thus eliminating the need for the addition of expensive functional materials. Instead, the required amount of electromagnetic shielding functional components is generated by the smelting slag itself, significantly reducing raw material costs.

[0021] The symbiotic structure of magnetite and amorphous silica avoids the risks of sedimentation, stratification, and uneven dispersion between magnetic materials and solidified soil slurry. Specifically, under the preparation conditions of this invention, on the one hand, fir olivine and / or FeO-SiO2 glass phases decompose in situ within the same smelting slag particles, with iron transforming into magnetite and silicon into amorphous silica. The two coexist closely at the particle scale, anchoring the magnetite to the amorphous silica. Since the density of amorphous silica is lower than that of magnetite, the symbiosis results in the apparent density of the composite filler being lower than that of pure magnetite, reducing the density difference with the solidified soil slurry, thereby effectively suppressing the local enrichment and sedimentation stratification of the magnetically conductive material in the fluidized system. On the other hand, during the hydration and hardening process of the fluidized solidified soil, amorphous silica, as a cementing active component, participates in the hydration reaction and, together with the hydration products of the curing agent, constructs a cementing network structure, improving the interfacial bonding between magnetite and the fluidized system. This anchors the magnetite in the hardened matrix, enhancing structural stability and significantly improving the stability of the electromagnetic shielding effect.

[0022] Compared to existing technologies that require high-temperature melting and roasting, the addition of flux (e.g., calcium oxide), and magnetic separation, this invention performs oxidative roasting at 600–700°C without adding flux, followed by reduction roasting at 480–550°C. The composite filler is then obtained directly without magnetic separation. This significantly reduces the roasting temperature, eliminates the need for flux, and removes a series of subsequent processing steps such as cooling, crushing, regrinding, and magnetic separation. The process is significantly simplified, and energy consumption and processing costs are greatly reduced. More importantly, the absence of magnetic separation allows the in-situ symbiotic structure of magnetite and amorphous silica on the same particle to be fully preserved, giving the composite filler both electromagnetic shielding and gelling activity.

[0023] Furthermore, in fluidized solidified soil, the residual carbon in high residual carbon coarse fly ash acts as a conductive material, synergistically forming a conductive-magnetic composite shielding mechanism with magnetite in the composite filler. That is, magnetite provides magnetic loss, and residual carbon provides electrical conductivity loss. Both of these factors effectively attenuate the electric field and magnetic field components in electromagnetic waves, enabling the electromagnetic shielding effectiveness of fluidized solidified soil to reach 26dB to 39dB in the frequency range of 0.3GHz to 3GHz, further enhancing the electromagnetic shielding effect.

[0024] Therefore, this invention enables fluidized solidified soil to possess good electromagnetic shielding performance, mechanical properties and system stability simultaneously, without the need for high-cost functional fillers such as magnetic powder and steel fiber, and without the need for high-temperature melting and magnetic separation, and realizes the high-value utilization of smelting slag. Attached Figure Description

[0025] Figure 1 This is a process flow diagram of a method for preparing fluidized solidified soil for electromagnetic shielding according to the present invention. Detailed Implementation

[0026] The following detailed description, in conjunction with the accompanying drawings and specific embodiments, provides a further detailed explanation of the fluidized solidified soil for electromagnetic shielding and its preparation method proposed in this invention. The advantages and features of this invention will become clearer from the following description. It should be noted that the accompanying drawings are in a very simplified form and use non-precise proportions, used only to facilitate and clearly illustrate the embodiments of this invention. Please refer to the accompanying drawings to make the objectives, features, and advantages of this invention more apparent and understandable. It should be understood that the structures, proportions, sizes, etc., depicted in the accompanying drawings are only for illustrative purposes to aid those skilled in the art and are not intended to limit the implementation conditions of this invention. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in proportions, or adjustments to the size, without affecting the effects and objectives achieved by this invention, should still fall within the scope of the technical content disclosed in this invention.

[0027] The “FeO-SiO2 glass phase” mentioned in this article refers to an amorphous phase with FeO and SiO2 as the main components. When the silicate slag formed in pyrometallurgy is discharged and cooled, the melt fails to crystallize fully, and the iron, silicon and other components exist in an amorphous (amorphous) form, that is, a glass phase network structure with Fe-O-Si bonds is formed.

[0028] The “in-situ symbiosis” or “symbiosis” mentioned in this article refers to the formation of magnetite and amorphous silica within the same smelting slag (e.g., copper slag or nickel slag) particles through an in-situ oxidation-reduction roasting reaction (steps S2 and S3 below), with the two particles interpenetrating within the same particle matrix.

[0029] The “gelling activity” mentioned in this article refers to the ability of a material to generate hydration products with cementing capacity through its own hydration reaction or chemical reaction with alkaline activating components under aqueous conditions, thereby enabling the system to solidify, harden, and generate strength.

[0030] As described in the background section, existing electromagnetic shielding materials rely on externally added high-cost conductive or magnetic materials such as graphite / conductive carbon, magnetite, and steel fibers, resulting in high costs. Furthermore, high-density magnetic fillers are prone to sedimentation and stratification in fluid systems, leading to a decrease in electromagnetic shielding effectiveness. Additionally, when smelting slags such as copper and nickel slag are used directly as fillers, their shielding efficiency is extremely low. Moreover, the magnetization conversion process for smelting slag requires high-temperature melting and roasting at 1150℃–1300℃ with the addition of flux, followed by reduction roasting and magnetic separation, resulting in high energy consumption, a long process, and high processing costs.

[0031] Therefore, this invention provides a method for preparing fluidized solidified soil for electromagnetic shielding. Without adding flux, the method involves in-situ decomposition of the fir olivine and / or FeO-SiO2 glass phase in smelting slag through low-temperature oxidative roasting with water vapor at 600℃~700℃. This is followed by controlled reduction at 480℃~550℃ and slow cooling with nitrogen to form a composite filler containing a symbiotic structure of magnetite and amorphous silica. The resulting composite filler is not subjected to magnetic separation, retaining the symbiotic structure of magnetite and amorphous silica, thus enabling the composite filler to simultaneously possess electromagnetic shielding function and cementing activity. Furthermore, the composite filler is combined with high-residual-carbon coarse fly ash, a solidifying agent, and water, and mixed with a dry soil sample to obtain fluidized solidified soil. The resulting fluidized solidified soil possesses both electromagnetic shielding and mechanical properties, simultaneously achieving low-energy, high-value utilization of both smelting slag and high-residual-carbon coarse fly ash solid wastes.

[0032] The technical solution of the present invention will be further described in detail below with reference to specific embodiments and accompanying drawings.

[0033] like Figure 1 As shown, the present invention provides a method for preparing fluidized solidified soil for electromagnetic shielding, comprising the following steps: Step S1: Provide smelting slag, grind and sieve the smelting slag, the smelting slag contains fir olivine and / or FeO-SiO2 glass phase.

[0034] Smelting slag refers to the slag produced during pyrometallurgical processes. In pyrometallurgical processes, gangue components in ores (e.g., chalcopyrite, nickel pyrite, etc.) react with iron oxides under high-temperature smelting conditions to form silicate slag. Upon cooling and solidification, this slag forms smelting slag, in which iron is present as fir olivine (Fe₂SiO₄) and / or FeO-SiO₂ glassy phases. Smelting slag includes at least one of the following pyrometallurgical slags: copper slag, nickel slag, etc.

[0035] In this embodiment, the smelting slag is either copper slag or nickel slag. In copper slag, the TFe (Total Iron) content is typically 30%–45%, the silica content is typically 30%–40%, and the copper content is typically between 0.3% and 1.5%. In nickel slag, the TFe (Total Iron) content is typically 20%–40%, the silica content is typically 40%–55%, and the nickel content is typically between 0.1% and 0.5%.

[0036] In some embodiments, the smelting slag is ground until the residue on an 80μm square-hole sieve does not exceed 10% by mass percentage. The fir olivine and / or FeO-SiO2 glass phase in the smelting slag need to be decomposed in situ via solid-state reaction in subsequent step S3, and the rate and conversion of the solid-state reaction are closely related to the particle specific surface area. Grinding the smelting slag until the residue on an 80μm square-hole sieve does not exceed 10% means that at least 90% of the particles have a diameter smaller than 80μm, significantly increasing the particle specific surface area. This allows oxygen and water vapor in the oxidizing atmosphere to fully penetrate into the particles, enabling the fir olivine and / or FeO-SiO2 glass phase to fully decompose at a low temperature of 600–700°C, avoiding incomplete reaction and insufficient magnetite formation due to excessively coarse particles. If the residue exceeds 10%, the proportion of coarse particles is too high, making it difficult to fully contact with oxygen in the oxidizing atmosphere, ultimately reducing the magnetite content in the composite filler and weakening the electromagnetic shielding effectiveness. Furthermore, unreacted coarse particles easily become inert impurities, reducing the mechanical properties of the fluidized solidified soil. The roasting object in step S2 below is all the smelting slag powder obtained after grinding in this step, including no more than 10% of the coarse particles remaining on the 80μm square hole sieve after grinding.

[0037] Step S2: Without adding flux, the ground smelting slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 10%~15% and a water vapor volume fraction of 3%~5%, and roasted at 600℃~700℃ to decompose the fir olivine and / or FeO-SiO2 glass phase in situ, resulting in a mixture containing magnetite, amorphous silica and hematite.

[0038] Unlike existing technologies that rely on high-temperature melting environments to destroy the structure of the fir olivine and / or FeO-SiO2 glass phase, this step utilizes a low-temperature oxidizing atmosphere to directly achieve solid-phase decomposition of the fir olivine and / or FeO-SiO2 glass phase, without the need for fluxes (e.g., calcium oxide) to create a molten liquid phase environment. Specifically, the iron in the fir olivine and FeO-SiO2 glass phase is converted into Fe... 2+ Fe exists in the oxidizing atmosphere of this step. 2+ Oxidized to Fe 3+ This causes the original mineral lattice to become unstable and decompose, Fe 3+ Recombining to form magnetite crystal nuclei, while SiO44- The tetrahedral structure disintegrates, and the silicon component precipitates out in the form of amorphous silicon dioxide.

[0039] In this step, the addition of water vapor provides an additional oxygen source and, as a mass transfer medium, promotes the diffusion of oxygen into the interior of the smelting slag particles, allowing the solid-phase oxidation reaction to proceed fully at a relatively low temperature of 600℃ to 700℃.

[0040] Experiments revealed that when the oxygen volume fraction is less than 10%, the oxidation driving force is insufficient, resulting in incomplete decomposition of fir olivine and / or FeO-SiO2 glass phases and insufficient magnetite formation. When the oxygen volume fraction is greater than 15%, excess oxygen makes the newly formed magnetite more susceptible to further oxidation into weakly magnetic hematite, increasing the burden on subsequent reduction (step S3 below). When the water vapor volume fraction is less than 3%, the mass transfer promoting effect is limited; when the water vapor volume fraction is greater than 5%, the excessively high water vapor partial pressure may affect the equilibrium of the oxidation reaction.

[0041] In this step, by not adding flux, the introduction of foreign components such as calcium oxide is avoided, reducing raw material costs and the burden of subsequent processing. In addition, since the reaction takes place in a solid phase without the participation of a liquid phase, the growth of magnetite grains is suppressed, and the grain coarsening and enrichment phenomena commonly seen under high-temperature melting conditions do not occur. Instead, the grains coexist closely with amorphous silica in the form of fine particles at the original particle scale.

[0042] In some embodiments, in order to control the degree of oxidation and decomposition of the fir olivine and / or FeO-SiO2 glass phase, it is further necessary to control the calcination time, which is 60 min to 120 min.

[0043] Step S3: The mixture is placed in a reducing atmosphere with an oxygen volume fraction greater than 0 and not more than 5% and a carbon monoxide volume fraction not less than 10%, and calcined at 480℃ to 550℃. Then it is cooled to room temperature under a nitrogen atmosphere to obtain a composite filler. The composite filler contains a symbiotic structure of magnetite and amorphous silica, and the magnetite and amorphous silica are formed by in-situ transformation of the same smelting slag particles.

[0044] During the oxidative roasting process in step S2, a small portion of magnetite will be further oxidized to hematite (α-Fe2O3). However, hematite has a much lower magnetic loss capacity than magnetite and is not suitable for use as a magnetic filler (magnetic material). Therefore, in this step, the reducing property of carbon monoxide is used to reduce hematite to magnetite. The reaction principle is 3Fe2O3 + CO → 2Fe3O4 + CO2, thereby restoring and increasing the magnetite content in the composite filler.

[0045] It should be noted that this step defines the intensity control range of the reducing atmosphere by using the upper limit of the oxygen volume fraction (≤5%) and the lower limit of the carbon monoxide volume fraction (≥10%). The reducing intensity of the reducing atmosphere depends on the relative ratio of carbon monoxide to oxygen. When the carbon monoxide volume fraction is not less than 10% and the oxygen volume fraction is greater than 0 but not more than 5%, the reducing potential of the reducing atmosphere is sufficient to convert hematite into magnetite, but not too strong. Experiments have shown that the presence of a small amount of oxygen can, to some extent, inhibit over-reduction, stabilizing the iron phase within the magnetite mineral phase range. From the perspective of the Fe-O phase system, the stable existence of magnetite requires a suitable oxygen potential window. When there is absolutely no oxygen and the carbon monoxide concentration is too high, the reducing potential is too strong, and hematite and magnetite may be further reduced to flostenite or even metallic iron, resulting in the loss of magnetic loss phases and reducing the electromagnetic shielding function of the composite filler. Furthermore, as an example, the carbon monoxide volume fraction is greater than or equal to 10% and less than or equal to 20%.

[0046] In some embodiments, in step S3, in order to further avoid excessive reduction of magnetite, the roasting time is controlled to be 50 min to 100 min.

[0047] In step S3, after the reduction roasting is completed, the material temperature is still at a high level. If it is directly exposed to air for cooling, the generated magnetite will come into contact with oxygen in the air again and be oxidized. Therefore, it is cooled to room temperature under a nitrogen atmosphere to isolate it from air and inhibit the re-oxidation of magnetite during the cooling process.

[0048] Furthermore, this step omits magnetic separation, aiming to retain magnetite and amorphous silica together in the composite filler as part of an in-situ transformation of the same particles, thus synergistically exerting their electromagnetic shielding and gelling activity functions. In addition, eliminating the magnetic separation step avoids a series of subsequent processing steps such as cooling, crushing, regrinding, and magnetic separation, simplifying the process and reducing processing costs.

[0049] Step S4: Based on 100 parts by weight of dry soil sample, mix and stir 10-15 parts by weight of high residual carbon coarse fly ash, 30-40 parts by weight of composite filler, 15-35 parts by weight of curing agent and 130-150 parts by weight of water to obtain fluidized solidified soil for electromagnetic shielding protection.

[0050] The fluidized solidified soil obtained by this invention has at least the following advantages: First, in this invention, the magnetite in the composite filler and the residual carbon in the high residual carbon coarse fly ash synergistically form a conductive-magnetic composite shielding mechanism.

[0051] Specifically, magnetite, as a magnetically conductive component, provides magnetic loss; residual carbon, as a conductive component, can construct conductive pathways within the fluidized solidified soil. This allows electromagnetic waves to be simultaneously attenuated by both magnetic and conductive losses within the fluidized solidified soil, effectively achieving electromagnetic shielding and avoiding reliance on expensive externally sourced functional materials such as steel fibers, graphite powder, and magnetite powder. Furthermore, other metallic components remaining in the smelting slag (e.g., copper residue from copper slag and nickel residue from nickel slag) also exist as conductors in the fluidized solidified soil, further contributing to conductive loss and enhancing the electromagnetic shielding effect.

[0052] In some embodiments, the loss on ignition (LOI) of high-residual-carbon coarse fly ash is greater than or equal to 8%, expressed as a percentage by mass. LOI reflects the content of unburned carbon in fly ash; the higher the LOI, the more residual carbon. By using high-residual-carbon coarse fly ash with a LOI of greater than or equal to 8%, the residual carbon content in the final fluidized solidified soil is sufficiently high to construct conductive pathways and thus provide electrical conductivity. In traditional building material applications, the LOI of fly ash is usually strictly controlled (e.g., no more than 5% for Grade I ash) because residual carbon is porous and absorbs water, increasing water demand, adsorbing additives, and reducing strength. This invention takes the opposite approach, directly utilizing high-residual-carbon fly ash to transform it from a traditionally inferior ash into a conductive component required for electromagnetic shielding. This not only saves the cost of purchasing conductive materials such as steel fibers, graphite carbon powder, and magnetic powder, but also achieves the resource utilization of industrial waste.

[0053] In some embodiments, to further enhance the conductive shielding effect, 0.5 to 2 parts by weight of graphite carbon powder (based on 100 parts by weight of dry soil sample) are added in step S4. The graphite carbon powder and the residual carbon in the high residual carbon coarse fly ash synergistically conduct electricity, and the total amount of conductive components can be flexibly adjusted according to specific electromagnetic shielding requirements. As an example, the graphite carbon powder can be industrial-grade graphite carbon powder with a purity ≥99% and a particle size ≤45μm. It should be noted that without the addition of graphite carbon powder, effective electromagnetic shielding performance can also be achieved solely by the magnetite in the composite filler and the residual carbon in the high residual carbon coarse fly ash, as shown in Example 1 below.

[0054] Second, in the prior art, the high-density magnetic filler with external additives is prone to local enrichment and sedimentation stratification in the fluid system. However, the present invention suppresses the sedimentation stratification of the high-density magnetic filler by the symbiotic structure of magnetite and amorphous silica in the composite filler and the micro-aggregate effect of high residual carbon coarse fly ash.

[0055] Specifically, on the one hand, in the composite filler, magnetite and amorphous silica coexist in situ on the same smelting slag (e.g., copper slag or nickel slag) particles. The high-density magnetic phase (i.e., magnetite) is anchored in the smelting slag particles, which reduces the risk of local enrichment and stratification of magnetic materials in the fluid system and improves the slurry stability of the fluid solidified soil.

[0056] On the other hand, in some embodiments, the high residual carbon coarse fly ash used is fly ash that, after grinding, has a sieve residue of ≥10% and ≤20% on a 45μm square-hole sieve. The ≥10% and ≤20% sieve residue on the 45μm square-hole sieve aims to control the particle size of the fly ash, retaining a certain amount of coarse particles. Although these coarse particles have a smaller specific surface area and lower cementitious activity, they act as micro-aggregates filling the slurry, increasing the slurry's yield stress and plastic viscosity, increasing the resistance to the settling of high-density magnetite particles, thereby inhibiting stratification and bleeding.

[0057] Third, in this invention, the amorphous silica in the composite filler and the curing agent synergistically enhance the strength of the fluidized solidified soil.

[0058] Specifically, in some embodiments, the curing agent is an SS-WS type curing agent (supplied as a finished product, which can be mixed with water to form a slurry or used in powder form). The curing agent contains cement, slag powder, water-reducing agent, and activator. The cement includes anhydrous minerals such as tricalcium silicate, dicalcium silicate, and tricalcium aluminate. When the curing agent comes into contact with water, these anhydrous minerals spontaneously react chemically with the water to generate hydration products such as hydrated calcium silicate gel (CSH gel) and calcium hydroxide (Ca(OH)2). These hydration products have extremely low solubility, precipitate from the solution, and continuously grow, forming an interwoven cementitious network structure. Simultaneously, the hydration reaction consumes free water, and the fluidized solidified soil slurry gradually thickens, eventually losing its fluidity and hardening. Because the Ca(OH)2 produced by cement hydration provides an alkaline environment, the active SiO2 and Al2O3 in the slag powder undergo hydration reactions under alkaline activation conditions. Activators (e.g., sodium sulfate, triethanolamine, etc.) further promote the dissolution of active components in the slag powder, enabling them to participate in the secondary hydration reaction and generate additional CSH gel and ettringite, thereby improving the density and strength of the fluidized solidified soil. Water-reducing agents are used to adjust the fluidity of the fluidized solidified soil, ensuring good flowability of the slurry even with low water consumption. In this embodiment, the curing agent used is the SS-WS type curing agent purchased from Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd.

[0059] Amorphous silica in the composite filler reacts with Ca(OH)₂ in an alkaline environment to form hydrated calcium silicate (CSH) gel, which fills the pores of the fluidized solidified soil, making the system more compact and increasing its strength. Furthermore, since amorphous silica and magnetite are derived from the same smelting slag particles in situ, they are closely symbiotic. The gelation reaction of amorphous silica occurs around the magnetite particles, and the resulting gel anchors the magnetite within the gel network, allowing the electromagnetic shielding function of magnetite and the mechanical properties of the gel matrix to work synergistically.

[0060] In some embodiments, the dry soil sample is any one or a combination of several of the following: engineering waste soil, weathered rock soil, and silt. The organic matter content in the dry soil sample is less than or equal to 4% (by mass percentage) to ensure that the hydration and hardening of the curing agent can proceed normally.

[0061] The present invention will be further described below with reference to embodiments and comparative examples.

[0062] The main chemical compositions of the copper slag and nickel slag used in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1 below.

[0063] Table 1. Main chemical components (mass fraction %) of copper slag and nickel slag

[0064] The loss on ignition mentioned in Table 1 refers to the mass fraction of the sample (copper slag or nickel slag) after drying to remove free water and then being fully ignited to constant weight, representing the mass difference before and after ignition relative to the mass of the dried sample.

[0065] Example 1 The specific steps for preparing fluidized solidified soil in this embodiment include: (1) Grind copper slag containing ferroolitic olivine and / or FeO-SiO2 glass phase to a fineness such that 10% residue remains on an 80μm square mesh sieve; (2) Without adding flux, the ground copper slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 10% and a water vapor volume fraction of 3%, and oxidized and roasted at 700°C for 1.5h to decompose the iron olivine and / or FeO-SiO2 glass phase in situ, and a mixture containing magnetite, amorphous silica and a small amount of hematite is obtained. (3) The mixture was placed in a reducing atmosphere with an oxygen volume fraction of 5% and a carbon monoxide volume fraction of 10%, and calcined at 480°C for 100 min. Then it was cooled slowly with nitrogen to isolate it from the air, and a composite filler of magnetite and amorphous silica was obtained. (4) Based on 100 parts by weight of dry soil sample, 15 parts by weight of high residual carbon coarse fly ash, 40 parts by weight of composite filler, 15 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent) and 135 parts by weight of water were mixed and stirred to obtain fluidized solidified soil for electromagnetic shielding protection. In this embodiment, the loss on ignition of high residual carbon coarse fly ash was 9.2%, and the residue on a 45μm square hole sieve after ball milling was 20%; the dry soil sample was engineering slag soil with an organic matter content of 3.4%.

[0066] Example 2 The specific steps for preparing fluidized solidified soil in this embodiment include: (1) Grind nickel slag containing ferroolitic olivine and / or FeO-SiO2 glass phase to a residue of 8.3% on an 80μm square mesh sieve; (2) Without adding flux, the ground nickel slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 15% and a water vapor volume fraction of 4%, and oxidized and roasted at 650°C for 1 hour to decompose the iron olivine and / or FeO-SiO2 glass phase in situ, and a mixture containing magnetite, amorphous silica and a small amount of hematite is obtained. (3) The mixture was placed in a reducing atmosphere with an oxygen volume fraction of 4% and a carbon monoxide volume fraction of 12%, and calcined at 500°C for 90 min. Then it was slowly cooled with nitrogen to isolate it from the air, and a composite filler of magnetite and amorphous silica was obtained. (4) Based on 100 parts by weight of dry soil sample, 0.5 parts by weight of graphite carbon powder, 13 parts by weight of high residual carbon coarse fly ash, 38 parts by weight of composite filler, 20 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent) and 130 parts by weight of water are mixed and stirred to obtain fluidized solidified soil for electromagnetic shielding protection. In this embodiment, the loss on ignition of high residual carbon coarse fly ash is 8%, and its residue on a 45μm square hole sieve after ball milling is 18.1%; the dry soil sample is weathered rock soil with an organic matter content of 3.8%.

[0067] Example 3 The specific steps for preparing fluidized solidified soil in this embodiment include: (1) Grind copper slag containing ferroolitic olivine and / or FeO-SiO2 glass phase to a fineness of 7.6% on an 80μm square mesh sieve; (2) Without adding flux, the ground copper slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 12% and a water vapor volume fraction of 5%, and oxidized and roasted at 600°C for 2 hours to decompose the iron olivine and / or FeO-SiO2 glass phase in situ, and a mixture containing magnetite, amorphous silica and a small amount of hematite is obtained. (3) The mixture was placed in a reducing atmosphere with an oxygen volume fraction of 3% and a carbon monoxide volume fraction of 14%, and calcined at 520°C for 70 min. Then it was cooled slowly with nitrogen to isolate it from the air, and a composite filler of magnetite and amorphous silica was obtained. (4) Based on 100 parts by weight of dry soil sample, 1 part by weight of graphite carbon powder, 13 parts by weight of high residual carbon coarse fly ash, 36 parts by weight of composite filler, 20 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent) and 140 parts by weight of water are mixed and stirred to obtain fluidized solidified soil for electromagnetic shielding protection. In this embodiment, the loss on ignition of high residual carbon coarse fly ash is 10.5%, and its residue on a 45μm square hole sieve after ball milling is 16.9%; the dry soil sample is weathered rock soil with an organic matter content of 3.5%.

[0068] Example 4 The specific steps for preparing fluidized solidified soil in this embodiment include: (1) Grind nickel slag containing ferroolitic olivine and / or FeO-SiO2 glass phase to a sieve residue of 6.2% on an 80μm square hole sieve; (2) Without adding flux, the ground nickel slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 13% and a water vapor volume fraction of 4.5%, and oxidized and roasted at 660°C for 1.8h to decompose the iron olivine and / or FeO-SiO2 glass phase in situ, and a mixture containing magnetite, amorphous silica and a small amount of hematite is obtained. (3) The mixture was placed in a reducing atmosphere with an oxygen volume fraction of 2% and a carbon monoxide volume fraction of 20%, and calcined at 550°C for 50 min. Then it was cooled slowly with nitrogen to isolate the air, and a composite filler of magnetite and amorphous silica was obtained. (4) Based on 100 parts by weight of dry soil sample, 1.5 parts by weight of graphite carbon powder, 13 parts by weight of high residual carbon coarse fly ash, 33 parts by weight of composite filler, 25 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent), and 140 parts by weight of water were mixed and stirred to obtain fluidized solidified soil for electromagnetic shielding protection. In this embodiment, the loss on ignition of high residual carbon coarse fly ash was 11%, and its residue on a 45μm square hole sieve after ball milling was 15.3%; the dry soil sample was engineering slag and silt, and its organic matter content was 4%.

[0069] Example 5 The specific steps for preparing fluidized solidified soil in this embodiment include: (1) The copper slag containing ferroolitic olivine and / or FeO-SiO2 glass phase was ground to a fineness of 3.4% on an 80μm square mesh sieve; (2) Without adding flux, the finely ground copper slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 14% and a water vapor volume fraction of 4%, and oxidized and roasted at 680°C for 1.3h to decompose the iron olivine and / or FeO-SiO2 glass phase in situ, and a mixture containing magnetite, amorphous silica and a small amount of hematite is obtained. (3) The mixture was placed in a reducing atmosphere with an oxygen volume fraction of 2% and a carbon monoxide volume fraction of 18%, and reduced and roasted at 540°C for 60 min. Then it was cooled slowly with nitrogen to isolate it from the air. Without magnetic separation, a composite filler of magnetite and amorphous silica was obtained. (4) Based on 100 parts by weight of dry soil sample, 2 parts by weight of graphite carbon powder, 10 parts by weight of high residual carbon coarse fly ash, 30 parts by weight of composite filler, 30 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent) and 150 parts by weight of water are mixed and stirred to obtain fluidized solidified soil for electromagnetic shielding protection. In this embodiment, the loss on ignition of high residual carbon coarse fly ash is 8%, and its residue on a 45μm square hole sieve after ball milling is 12%; the dry soil sample is weathered rock soil and silt, and its organic matter content is 3.3%.

[0070] Comparative Example 1 Copper slag containing ferric olivine and / or FeO-SiO2 glass phase is ground to a fineness such that the residue on an 80μm square-hole sieve does not exceed 10%, and is used directly without roasting or conversion.

[0071] Based on 100 parts by weight of dry soil sample, 2 parts by weight of graphite carbon powder, 15 parts by weight of high residual carbon coarse fly ash, 40 parts by weight of copper slag, 25 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent), and 140 parts by weight of water were mixed and stirred to obtain fluidized solidified soil. In this comparative example, the loss on ignition of high residual carbon coarse fly ash was 13.1%, and its residue on a 45μm square-hole sieve after ball milling was 14.7%; the dry soil sample was silt with an organic matter content of 3.5%.

[0072] Comparative Example 2 Based on 100 parts by weight of dry soil sample, 2 parts by weight of graphite carbon powder, 15 parts by weight of high residual carbon coarse fly ash, 40 parts by weight of ferric oxide, 25 parts by weight of curing agent (Anhui Ronggong Boda Environmental Protection Technology and Materials Research Institute Co., Ltd., SS-WS type curing agent), and 130 parts by weight of water were mixed and stirred to obtain fluidized solidified soil. The high residual carbon coarse fly ash and dry soil sample in this comparative example are the same as in Comparative Example 1.

[0073] Performance testing X-ray diffraction (XRD) tests were performed on the composite fillers obtained in each embodiment and comparative example. The magnetite content was calculated based on the XRD diffraction intensity. The activity index was the ratio of the 28-day compressive strength of the mortar obtained when the composite filler was added to standard cement at a dosage of 30%. Electromagnetic shielding effectiveness, 28-day compressive strength, fluidity, and bleeding rate were tested on the fluidized solidified soils obtained in Examples 1-5 and Comparative Examples 1-2. The test frequency range for electromagnetic shielding effectiveness was 0.3 GHz to 3 GHz, and the shielding sample thickness was 10 mm. Other performance tests were conducted according to the methods specified in the standard. The test results are shown in Tables 2 and 3.

[0074] Table 2: Magnetite content and activity index of composite fillers in Examples 1-5 and Comparative Examples 1-2

[0075] Table 3: Performance test results of fluidized solidified soil in Examples 1-5 and Comparative Examples 1-2

[0076] As shown in Tables 2 and 3, the magnetite content in the composite fillers of Examples 1-5 prepared using the method of this invention reaches 38%-51%, while that in Comparative Example 1 (without roasting conversion) is only 1.9%. The electromagnetic shielding effectiveness of the fluidized solidified soils of Examples 1-5 reaches 26dB-39dB, significantly higher than the 13.5dB of Comparative Example 1, indicating that after the fir olivine and / or FeO-SiO2 glass phase are decomposed in situ and reduced to magnetite, the fluidized solidified soil acquires electromagnetic shielding function. The activity index of the composite fillers of Examples 1-5 is 72%-80%, significantly higher than the 58% of the original copper slag in Comparative Example 1. The 28-day compressive strength of the fluidized solidified soils of Examples 1-5 reaches 1.37MPa-2.37MPa, while that of Comparative Example 1 is only 0.55MPa, indicating that the amorphous silica coexisting with magnetite participates in the cementation reaction and improves the interfacial bonding between the magnetic components (magnetite) and hydration products. Comparative Example 2, which directly incorporates iron(III) oxide (Fe3O4), exhibits electromagnetic shielding effectiveness comparable to Examples 1-5. However, its 28-day compressive strength is only 0.43 MPa, with a bleeding rate of 5.7% and stratification. In contrast, the bleeding rate of the fluidized solidified soils in Examples 1-5 is only 0.6%-1.0%, with no stratification. This indicates that the addition of magnetic filler is prone to settling and stratification issues, demonstrating that the in-situ symbiotic structure of magnetite and amorphous silica in the fluidized solidified soil prepared by the method of this invention can effectively reduce the risk of local enrichment and stratification of magnetic filler in the fluidized system.

[0077] In summary, this invention uses smelting slag as raw material and, through low-temperature oxidation roasting and controlled reduction roasting, produces a composite filler in situ coexisting with magnetite and amorphous silica without adding flux or magnetic separation. This composite filler is then combined with dry soil samples, high-residual-carbon coarse fly ash, a solidifying agent, and water to prepare fluidized solidified soil. This method eliminates the need to purchase high-cost functional materials such as magnetite powder and steel fibers, and avoids the high-energy-consuming processes of high-temperature melting and magnetic separation. The magnetite in the composite filler provides magnetic loss, while the residual carbon in the high-residual-carbon coarse fly ash provides electrical conductivity loss; together, they achieve electromagnetic shielding. Amorphous silica exerts its cementing activity, participating in the hydration reaction and improving the interfacial bonding between magnetite and the cementitious matrix. The symbiotic structure reduces the apparent density of the filler, and, combined with the micro-aggregate effect of coarse particles, effectively suppresses sedimentation and stratification. Therefore, the fluidized solidified soil simultaneously possesses excellent electromagnetic shielding effectiveness, mechanical properties, and system stability, and achieves high-value utilization of smelting slag.

[0078] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0079] Although the present invention has been described in detail through the preferred embodiments above, it should be understood that the above description should not be considered as a limitation of the present invention. Various modifications and substitutions to the present invention will be apparent to those skilled in the art after reading the above description. Therefore, the scope of protection of the present invention should be defined by the appended claims.

Claims

1. A method for preparing fluidized solidified soil for electromagnetic shielding, characterized in that, include: Step 1: Provide smelting slag, grind and sieve the smelting slag, wherein the smelting slag contains fir olivine and / or FeO-SiO2 glass phase; Step 2: Without adding flux, the ground smelting slag is placed in an oxidizing atmosphere with an oxygen volume fraction of 10%~15% and a water vapor volume fraction of 3%~5%, and roasted at 600℃~700℃ to decompose the iron olivine and / or the FeO-SiO2 glass phase in situ, to obtain a mixture containing magnetite, amorphous silica and hematite. Step 3: The mixture is placed in a reducing atmosphere with an oxygen volume fraction greater than 0 and not more than 5% and a carbon monoxide volume fraction not less than 10%, and calcined at 480℃ to 550℃. Then it is cooled to room temperature under a nitrogen atmosphere to obtain a composite filler. The composite filler contains a symbiotic structure of magnetite and amorphous silica, and the magnetite and amorphous silica are formed in situ from the same smelting slag particles. Step 4: Based on 100 parts by weight of dry soil sample, mix and stir 10-15 parts by weight of high residual carbon coarse fly ash, 30-40 parts by weight of the composite filler, 15-35 parts by weight of curing agent and 130-150 parts by weight of water to obtain fluidized solidified soil for electromagnetic shielding protection.

2. The preparation method according to claim 1, characterized in that, In step 1, grinding and sieving the smelting slag includes grinding the smelting slag until the residue on an 80μm square hole sieve does not exceed 10% by mass percentage.

3. The preparation method according to claim 1, characterized in that, In step 2, the roasting time is 60 min to 120 min; in step 3, the roasting time is 50 min to 100 min.

4. The preparation method according to claim 1, characterized in that, In step 3, the volume fraction of carbon monoxide is less than or equal to 20%.

5. The preparation method according to claim 1, characterized in that, In step 4, 0.5 to 2 parts by weight of graphite carbon powder are also added, based on 100 parts by weight of dry soil sample.

6. The preparation method according to claim 1, characterized in that, In step 4, the loss on ignition of the high residual carbon coarse fly ash is greater than or equal to 8%; and the high residual carbon coarse fly ash is fly ash that, after grinding, has a residue of greater than or equal to 10% and less than or equal to 20% on a 45μm square hole sieve, expressed as a percentage by mass.

7. The preparation method according to claim 1, characterized in that, In step 4, the dry soil sample is any one or a combination of several of the following: engineering waste soil, weathered rock soil, and silt, and the organic matter content of the dry soil sample is less than or equal to 4% by mass.

8. The preparation method according to claim 1, characterized in that, The curing agent is an SS-WS type curing agent, which includes cement, slag powder, water-reducing agent and activator.

9. The preparation method according to any one of claims 1 to 8, characterized in that, The smelting slag includes at least one of copper slag and nickel slag.

10. A fluidized solidified soil for electromagnetic shielding, characterized in that, The fluidized solidified soil is prepared using the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Methods for comprehensive iron recovery from copper smelting slag flotation tailings

    CN102260787A

  • Wet-ground copper slag cement-based electromagnetic shielding composite material and preparation method thereof

    CN112142415A

  • Concrete mix for electromagnetic wave / pulse shielding

    US8968461B1