A method of simulating lunar soil material modification enhancement
By adjusting the mass ratio of oxides in lunar soil and using grinding and melting methods, modified lunar soil materials were prepared, solving the problems of high porosity and poor mechanical properties in the molding of lunar building materials. This achieved efficient and low-cost material preparation, improved the mechanical properties of lunar soil materials, and met the needs of lunar construction.
Patent Information
- Application Number
- CN202611159273.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-01
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies for molding building materials using lunar soil on the moon suffer from problems such as high porosity, poor mechanical properties, the need to add reinforcing materials transported from Earth (which violates the principle of in-situ resource utilization), and stringent sintering process requirements and low molding efficiency.
By adjusting the mass ratio of metal oxides to non-metal oxides in simulated lunar soil, modified and enhanced simulated lunar soil materials were prepared using wet grinding and melt molding methods. Naturally occurring oxides in lunar soil, such as Al₂O₃ and SiO₂, were utilized to achieve densification and a uniform microstructure in the materials.
It enables the efficient and low-cost fabrication of dense, uniformly microstructured printed parts on the moon, improving the compressive strength, flexural strength, and impact toughness of the material, achieving a truly zero-transportation-cost material design.
Smart Images

Figure CN123131124A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building materials technology, and in particular to a method for modifying and enhancing materials by simulating lunar soil. Background Technology
[0002] As global lunar exploration activities shift from short-term scientific expeditions to long-term stays and resource development, establishing permanent lunar bases has become a core strategic goal for major spacefaring nations. However, transporting building materials from Earth to the Moon is extremely costly—the cost of Earth-Moon transport can reach hundreds of thousands of US dollars per kilogram—making the traditional Earth-supply construction model economically unfeasible. Therefore, the concept of In-Situ Resource Utilization (ISRU) has emerged, which involves directly producing building materials using existing lunar resources. This is a key technological path to reduce lunar construction costs and achieve sustainable development. Lunar regolith, a loose clastic layer widely distributed across the lunar surface and covering the solid bedrock, can be 5-10 meters thick. It is the richest and most readily available in-situ resource on the Moon, naturally becoming the preferred raw material for lunar construction. However, traditional building materials and their molding processes partially or completely fail in the extreme lunar environment. This makes the development of material molding technologies adapted to the lunar environment and capable of 100% utilizing lunar regolith in situ a critical scientific problem that urgently needs to be solved.
[0003] Currently, the main technical routes for in-situ construction using lunar regolith fall into four categories: reaction solidification methods that use chemical reactions to generate cementitious materials to bind lunar regolith particles; sintering-melting methods that use high-temperature treatment to partially or completely melt lunar regolith particles and then bond them together; bonding solidification methods that add binders to cement lunar regolith particles into shape; and constraint-forming methods that use flexible fabrics to restrain loose lunar regolith. Among these, sintering-melting technology is considered one of the most promising lunar construction technologies due to its advantages of 100% in-situ resource utilization, no need for external additives, and relatively simple process.
[0004] Previous studies have explored various sintering and melting methods, which can be summarized into the following technical solutions. Pure lunar soil sintering technology utilizes the fusion and bonding of lunar soil's own components to achieve molding; however, due to the poor thermal conductivity of lunar soil, sintering efficiency is low, resulting in high porosity of the molded samples and consequently poor mechanical properties. Existing high-performance lunar soil composite materials generally require the addition of reinforcing materials such as Fe powder, fibers, and graphene, which need to be transported from Earth. For example, metal-reinforced composite technology uses metal powders such as Fe powder as reinforcing phases, utilizing the ductility, toughness, and crack bridging mechanisms of metals to improve mechanical properties; however, Fe powder needs to be transported from Earth, violating the principle of maximizing in-situ resource utilization.
[0005] Meanwhile, the difference in thermal expansion coefficients between the metallic phase and the lunar regolith matrix may lead to interfacial cracking, posing interfacial compatibility issues. Furthermore, it places stringent requirements on the sintering process, necessitating precise temperature control to prevent metal oxidation or excessive reaction. Geopolymerization reaction solidification technology utilizes the aluminosilicates in lunar regolith to undergo a geopolymerization reaction under alkaline conditions, forming a three-dimensional network gel structure. However, this also requires the addition of alkaline activators such as sodium hydroxide and solid sodium silicate, increasing the burden on Earth-Moon transport. In addition, laser / solar 3D printing sintering technology uses lasers or focused solar energy to melt lunar regolith powder layer by layer, achieving additive manufacturing of components. However, it is limited by low forming efficiency and insufficient strength; the compressive strength of solar-fired sintered bricks is generally below 5 MPa.
[0006] Furthermore, microwave, solar, and laser forming are extremely inefficient, typically limiting their use to the manufacture of only a few precision parts. This severely restricts the application of these technologies in large-scale lunar construction. Lunar regolith liquid 3D printing is a promising solution, based on melting and relying on the self-impact of high-pressure melt flow and layer-by-layer solidification to produce customized shapes. This technology has previously been successfully applied to the forming of metallic materials, solving problems such as compositional inhomogeneity and coarse grain size inherent in traditional casting. Moreover, its efficiency is more than a thousand times that of traditional additive manufacturing methods such as laser / solar 3D printing, providing a promising solution to overcome this bottleneck.
[0007] The inherent compositional heterogeneity of lunar regolith is a key challenge in liquid 3D printing technology. Lunar regolith from different geological topography exhibits significant differences in chemical composition, as shown in Table 1. These compositional differences lead to variations in melting behavior, viscosity, crystallization kinetics, and the mechanical properties of the final printed product. Summary of the Invention
[0008] To address the aforementioned technical problems, embodiments of the present invention provide a method for modifying and enhancing simulated lunar soil materials.
[0009] To achieve the above objectives, the embodiments of the present invention adopt the following technical solutions: On the one hand, the present invention provides a method for simulating lunar soil material modification and enhancement, comprising the following steps: Modified and enhanced simulated lunar soil materials are obtained by adjusting the mass ratio of metal oxides to non-metal oxides or the mass ratio of non-metal oxides to non-metal oxides in simulated lunar soil, followed by grinding and melting molding.
[0010] In some embodiments, the metal oxide includes calcium oxide, ferrous oxide, ferric oxide, iron(II) oxide, or aluminum oxide, and the non-metal oxide includes silicon dioxide.
[0011] In some embodiments, the following steps are specifically adopted: the mass ratio of alumina to silica in the simulated lunar soil is adjusted by adding silica or alumina to the simulated lunar soil.
[0012] In some embodiments, the following steps are specifically adopted: calcium oxide, ferrous oxide, ferric oxide or ferric oxide are added to the simulated lunar soil to adjust the mass ratio of iron oxide to silicon dioxide in the simulated lunar soil, thereby adjusting the mass ratio of calcium oxide to silicon dioxide.
[0013] In some embodiments, the grinding is performed using a wet grinding method.
[0014] In some embodiments, the wet grinding speed is 300~500 r / min, and the ball milling time is 6~10 h.
[0015] In some embodiments, the wet milling process uses anhydrous ethanol or deionized water as a solvent.
[0016] In some embodiments, the melt molding process specifically adopts the following steps: after grinding, vacuum drying, first heating to 1100~1200℃ and holding, then heating to 1250~1350℃, and finally molding.
[0017] In some embodiments, the heat preservation time is 5 to 15 minutes.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: Performance optimization can be achieved by regulating the existing chemical composition of lunar soil. Al2O3, SiO2, calcium oxide, and iron oxides are naturally occurring components in lunar soil. By regulating the mass ratio between these oxides, liquid-phase mass transfer and crystal nucleation can be promoted during sintering, resulting in printed parts with higher densification and more uniform microstructure. These oxides can be obtained through separation and purification or by directly utilizing in-situ lunar resources (such as aluminum-rich regions in the lunar highlands), enabling the in-situ production of reinforcing materials and achieving truly "zero transportation cost" material design. Attached Figure Description
[0019] Figure 1 To provide a comparative example of simulated lunar soil powder, including physical images and SEM images, a schematic diagram of the printing process, and the formed sample; Figure 2 The elemental distribution is shown in the EDS surface scan images of the modified simulated lunar soil powders of Examples 2 and 4. Figure 3 XRD patterns of simulated lunar soil powder and shaped samples were used for comparative examples and corresponding embodiments; Figure 4 The diagram shows simulated lunar soil mechanical properties test results for comparative examples and corresponding embodiments; Figure 5 The diagram shows the state of representative specimens after the compression tests of the comparative examples, Example 2, and Example 4. Detailed Implementation
[0020] The technical solutions in some embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments provided in this disclosure are within the scope of protection of this disclosure.
[0021] Example This application uses CUG-1A simulated lunar soil as a comparative example to study the effect of incorporating different masses of alumina or silica on compressive strength. Uniaxial compression testing of the molded specimens was conducted according to GB / T 8489-2006. The top and bottom surfaces were sanded smooth, and the testing environment was room temperature. The compressive stress-strain curves are shown in [reference needed]. Figure 4 The bending test employed a three-point bending method, conforming to GB / T6569-2006. The impact test was conducted using the simply supported beam pendulum method according to GB / T 14389-1993. It should be noted that the Al / Si, Ca / Si, and Fe / Si ratios in the following comparative examples and embodiments are all oxide mass ratios, such as Al / Si representing the mass ratio of aluminum oxide to silicon dioxide.
[0022] Comparative Example: The simulated lunar soil composition was CUG-1A, without any other additives, with an Al / Si ratio of 0.31, a Ca / Si ratio of 0.16, and an Fe / Si ratio of 0.25. The molded specimen exhibited a compressive strength of 39.7 MPa, a flexural strength of 4.2 MPa, and an impact toughness of 0.9 J / cm². 2 .
[0023] Example 1: 5 wt% SiO2 was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 400 r / min. After grinding, the mixture was vacuum dried, resulting in an Al / Si ratio of 0.28. The mixture was then heated to 1200℃ and held for 5 min, followed by heating to 1250℃. Finally, it was molded. The molded sample exhibited a compressive strength of 29.7 MPa and an impact toughness of 1.5 J / cm². 2 .
[0024] Example 2: 10 wt% SiO2 was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 300 r / min. After grinding, the mixture was vacuum dried, resulting in an Al / Si ratio of 0.24. The mixture was first heated to 1200℃ and held for 5 min, then heated to 1250℃, and finally shaped. The resulting sample exhibited a compressive strength of 13.2 MPa, a flexural strength of 2.7 MPa, and an impact toughness of 0.6 J / cm².2 .
[0025] Example 3: 5 wt% Al2O3 was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 450 r / min. After grinding, the mixture was vacuum dried, resulting in an Al / Si ratio of 0.39. The mixture was then heated to 1200℃ and held for 10 min, followed by heating to 1250℃. Finally, it was molded. The molded sample exhibited a compressive strength of 49.4 MPa and an impact toughness of 2.1 J / cm². 2 .
[0026] Example 4: 10 wt% Al2O3 was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 500 r / min. After grinding, the mixture was vacuum dried, resulting in an Al / Si ratio of 0.51. The mixture was first heated to 1150℃ and held for 8 min, then heated to 1250℃, and finally shaped. The compressive strength of the shaped sample was 62.1 MPa, and the impact toughness was 3.3 J / cm. 2 .
[0027] Example 5: 10 wt% CaO was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 300 r / min. After grinding, the mixture was vacuum dried, resulting in a Ca / Si ratio of 0.36. The mixture was first heated to 1200℃ and held for 15 min, then heated to 1350℃, and finally molded. The molded sample exhibited a compressive strength of 51.0 MPa and an impact toughness of 2.5 J / cm². 2 .
[0028] Example 6: 10 wt% FeO was added to CUG-1A, followed by wet ball milling with deionized water for 8 h at 500 r / min. After grinding, the mixture was vacuum dried, resulting in an Fe / Si ratio of 0.45. The mixture was then heated to 1150℃ and held for 10 min, followed by heating to 1250℃. Finally, the mixture was molded. The compressive strength of the molded sample was 45.9 MPa, and the impact toughness was 2.2 J / cm². 2 .
[0029] Example 7: 10 wt% Al2O3 was added to CUG-1A, followed by wet ball milling with deionized water for 6 h at 450 r / min. After grinding, the mixture was vacuum dried, resulting in an Al / Si ratio of 0.51. The mixture was first heated to 1100℃ and held for 12 min, then heated to 1300℃, and finally shaped. The compressive strength of the shaped sample was 46.8 MPa, and the impact toughness was 1.8 J / cm. 2 .
[0030] Table 1. Chemical composition of real lunar soil
[0031] Table 2. Chemical composition of simulated lunar soil and modified soil
[0032] like Figure 1 The morphology of the CUG-1A lunar regolith simulant powder, a comparative raw material, is shown. Scanning electron microscopy images reveal that the initial simulated lunar regolith is sub-angular to angular, with the overall morphology mainly composed of irregular blocks, and a few particles appearing as elongated or flaky shapes. The particle surfaces are generally rough, with tiny adhering particles, and sharp edges caused by breakage can be seen in some areas; this morphology is similar to that of real lunar regolith. Printed samples of lunar regolith simulants of different sizes and shapes are also shown. The equipment can produce continuous bricks of 50mm × 100mm. Its production speed reaches 30-50kg / h, significantly higher than 3D printing technologies such as laser melting manufacturing.
[0033] like Figure 2 The influence of energy dispersive spectroscopy (EDS) on the elemental distribution in the simulated lunar regolith was analyzed. The elemental distribution on the surface of the lunar regolith particles could be altered by controlling the mass ratio between oxides. In Example 2, the signal for Si was stronger than that for Al, while in Example 4, the signal for Al was stronger than that for Si. This indicates that the new phase formed by the addition of oxides during ball milling is mainly distributed on the particle surface.
[0034] like Figure 3 The powder is mainly composed of mineral crystalline phases, with oxides incorporated to form new phases, altering the relative proportions and preferred orientations of the raw materials. Combined with EDS results, it can be seen that the addition of SiO2 in Examples 1 and 2 primarily formed plagioclase with a specific orientation, manifested as an increase in the relative intensity of the diffraction peak at approximately 28° in the XRD pattern. In Examples 3 and 4, the addition of alumina primarily formed pyroxene, manifested as an increase in the relative intensity of the diffraction peak at approximately 30° in the XRD pattern.
[0035] The printed samples in both the comparative and example examples used an amorphous glass phase as the matrix, doped with a small amount of mineral crystalline phase, forming a glass-crystalline phase composite material. Example 2 showed the lowest intensity of the crystalline phase peak, followed by the comparative example, while Example 4 exhibited multiple strong crystalline diffraction peaks. The comparison between Examples 2, 4, and the comparative example demonstrates that increasing the Al / Si ratio helps promote the crystallization tendency of the material, thereby increasing the proportion of the crystalline phase.
[0036] like Figure 4(a) The compressive strength and ultimate fracture strain of Examples 1 and 2 are lower than those of the comparative example, while those of Examples 3 and 4 are higher. (b) The compressive properties of Examples 5 and 6 are improved compared to the comparative example, indicating that the addition of Ca and Fe can also change the compressive strength and mechanical behavior of the material, and should also be included in patent protection. (c) The performance data of Examples 1-4 and the comparative example in a are visually quantified. It shows that within this range, both compressive strength and plasticity are positively correlated with the Al / Si ratio. (d) Flexural strength also shows a similar trend. The sample of Example 2 with a lower Al / Si ratio fractured rapidly after the minimum strain (less than 2%), while the comparative example sample had slightly higher flexural strength (4.2 MPa) and ductility (4.6%). The sample of Example 4 exhibited higher flexural stress (7.6 MPa) and flexural strain rate (11.2%) before fracture.
[0037] like Figure 5 The crushing is shown. The comparative example is a typical brittle fracture, with large fragments. The fracture surface of Example 2 has a green glassy structure, while the fracture surface of Example 4 has a white crystalline fracture structure, indicating that the two fracture modes are different.
[0038] In the description of this specification, specific features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments or examples.
[0039] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for modifying and enhancing simulated lunar soil materials, characterized in that, Includes the following steps: Modified and enhanced simulated lunar soil materials are obtained by adjusting the mass ratio of metal oxides to non-metal oxides or the mass ratio of non-metal oxides to non-metal oxides in simulated lunar soil, followed by grinding and melting molding.
2. The method according to claim 1, characterized in that, The metal oxides include calcium oxide, ferrous oxide, ferric oxide, iron(II) oxide, or aluminum oxide, and the non-metal oxides include silicon dioxide.
3. The method according to claim 1, characterized in that, The specific steps are as follows: the mass ratio of alumina to silica in the simulated lunar soil is adjusted by adding silica or alumina.
4. The method according to claim 1, characterized in that, The specific steps are as follows: calcium oxide, ferrous oxide, ferric oxide, or ferric oxide are added to the simulated lunar soil to adjust the mass ratio of iron oxides to silicon dioxide in the simulated lunar soil, thereby adjusting the mass ratio of calcium oxide to silicon dioxide.
5. The method according to claim 1, characterized in that, The grinding process is wet grinding.
6. The method according to claim 5, characterized in that, The wet grinding speed is 300~500 r / min, and the ball milling time is 6~10 h.
7. The method according to claim 5, characterized in that, The wet grinding process uses anhydrous ethanol or deionized water as a solvent.
8. The method according to claim 1, characterized in that, The melt molding process specifically involves the following steps: after grinding, vacuum drying is performed, followed by heating to 1100~1200℃ and holding at that temperature, then heating to 1250~1350℃, and finally molding.
9. The method according to claim 8, characterized in that, The heat preservation time is 5~15 minutes.