Preparation method of petrochemical solid waste-based high-strength ceramsite

By mixing petrochemical oily sludge, FCC waste catalyst, petrochemical contaminated soil, and waste glass powder, high-strength ceramsite was prepared, solving the problem of waste utilization in the petrochemical industry and achieving efficient resource utilization and environmentally friendly ceramsite preparation.

CN123131127APending Publication Date: 2026-11-20CHINA PETROLEUM & CHEMICAL CORP +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611457257.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Typical industrial solid wastes from the petrochemical industry, such as petrochemical oily sludge, FCC spent catalysts, and petrochemical contaminated soil, lack large-scale conversion and utilization schemes, leading to environmental pollution and resource waste.

Method used

Petrochemical oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder are mixed and then pre-carbonized, ball-milled, granulated and sintered at high temperature to prepare high-strength ceramic particles. Waste glass powder is used as a sintering aid to promote liquid phase formation and micropore generation, and to avoid rapid volatilization of oil.

Benefits of technology

High-strength, low-density petrochemical solid waste-based ceramsite was prepared, enabling a high-proportion stable treatment of petrochemical industry waste, reducing resource dependence, improving resource utilization, reducing environmental pollution, and meeting the requirements of sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131127A_ABST
    Figure CN123131127A_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of petrochemical solid waste-based high-strength ceramsite, and utilizes petrochemical oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder as sintering aid to cooperatively prepare high-strength building ceramsite; the mass percentage of each raw material is as follows: the oily sludge is 20-40 wt%, the contaminated soil is 30-50 wt%, the FCC waste catalyst is 10 wt%, and the waste glass powder is 20 wt%. The petrochemical solid waste-based high-strength ceramsite is obtained through the following steps in sequence: raw material treatment, ball milling and mixing, pelletizing, drying and high-temperature sintering, and has the characteristics of high strength and low water absorption, is a new type of building material which is economic, environment-friendly and has high resource utilization rate, can effectively solve the problem of large storage of petrochemical solid waste, reduces the serious dependence on non-renewable resources such as quartz, clay and feldspar, and builds a building material with excellent use performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste resource utilization technology. More specifically, this invention relates to a method for preparing high-strength ceramsite based on petrochemical solid waste. Background Technology

[0002] As the global energy structure transformation continues, the status of fossil fuels as the primary energy source will remain difficult to shake in the short term, and the treatment of industrial waste derived from them has become a key bottleneck restricting the sustainable development of the industry.

[0003] Petrochemical oily sludge is a hazardous waste generated during the petrochemical industry. It is mainly composed of crude oil, refined oil, water, solid particles (such as silt, corrosion products, catalysts, etc.), and small amounts of chemical additives. Due to its high content of petroleum-derived organic matter (such as hydrocarbons and polycyclic aromatic hydrocarbons) and heavy metals, it is toxic, flammable, and environmentally persistent. Improper handling can cause serious pollution to soil, water bodies, and the atmosphere. Because of its complex composition and the presence of various organic pollutants and substances harmful to human health, it has been included in the "National Hazardous Waste List" (National Hazardous Waste List HW08).

[0004] Fluidized catalytic cracking (FCC) spent catalysts are solid waste generated during light oil processing from FCC catalysts through hydrothermal deactivation, metal poisoning deactivation, and deposition deactivation. Due to their high heavy metal content, they have been included in China's "National Hazardous Waste List" (National Hazardous Waste List HW50). With the increasing demand for light oil, the annual production of FCC spent catalysts is also rapidly increasing. If not properly disposed of, it will cause serious secondary pollution. Therefore, the recycling and utilization of FCC spent catalysts can improve resource utilization while reducing the environmental problems they cause, promoting sustainable development.

[0005] Petrochemical contaminated soil refers to soil contaminated by petroleum hydrocarbons during petroleum production, storage, transportation, and accidents. Its main sources include long-term oil seepage, leaks from production facilities, accidental spills, and improper discharge of oily wastewater. Contaminated soil has complex characteristics, with pollutants tightly bound to soil particles. The pollutants mainly fall into two categories: the first is petroleum hydrocarbon organic matter, such as petroleum hydrocarbons (TPH), benzene compounds (BTEX), and polycyclic aromatic hydrocarbons (PAHs), which are hydrophobic and toxic, damaging soil ecological functions; the second is heavy metals, commonly including lead (Pb), chromium (Cr), cadmium (Cd), nickel (Ni), and arsenic (As), which are persistent and bioaccumulative.

[0006] In recent years, transforming hazardous solid waste into building materials has become a major research focus for many researchers. Among these efforts, expanded clay aggregate (ECA) resource utilization technology involves preparing ECA by co-firing solid waste, achieving resource utilization of waste while stabilizing its treatment. ECA, as a type of artificial aggregate, is widely used due to its low density, high strength, corrosion resistance, and good thermal insulation properties. Therefore, combining three typical industrial solid wastes from the petrochemical industry—oil-containing sludge, FCC spent catalysts, and petrochemical-contaminated soil—with waste glass powder as a sintering aid and high-temperature sintering to prepare high-strength ECA not only effectively improves resource utilization but also contributes to the sustainable development of resources, energy, the environment, and the economy. Summary of the Invention

[0007] One object of the present invention is to solve at least the above-mentioned problems and to provide at least the advantages that will be described later.

[0008] Another objective of this invention is to provide a method for preparing high-strength ceramsite based on petrochemical solid waste, in order to solve the technical problem that there is a lack of large-scale conversion and utilization solutions for typical industrial solid waste in the petrochemical industry in the existing technology.

[0009] To achieve these objectives and other advantages according to the present invention, a method for preparing high-strength ceramsite based on petrochemical solid waste is provided, comprising the following steps: S1. Raw material processing: The oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder are dried to constant weight. Then, the dried oily sludge is heated to 280~300 ℃ under an inert atmosphere and kept at that temperature for 30~45 min for pre-carbonization treatment. After that, the pre-carbonized oily sludge, dried FCC waste catalyst, petrochemical contaminated soil and waste glass powder are ground and sieved in sequence. S2. Ball milling and mixing: The oily sludge, contaminated soil, FCC waste catalyst, and waste glass powder pretreated in step S1 are mixed according to the following mass percentages: oily sludge 20-40 wt%, contaminated soil 30-50 wt%, FCC waste catalyst 10 wt%, and waste glass powder 20 wt%. The mixture is then ball milled to ensure homogeneity. S3. Granulation: Add water to the material mixed in step S2 and mix evenly. The amount of water added is 20-30 wt% of the material mixed in step S2, so that the viscosity of the raw material is slurry and has plasticity. Then, granulate it in a disc granulator to obtain raw material balls with a diameter of nearly 5 cm. S4. Drying: Dry the formed raw material balls; S5. High-temperature sintering: The dried raw material balls are sintered at high temperature and then naturally cooled to obtain the finished petrochemical solid waste-based high-strength ceramsite.

[0010] Preferably, in step S1, the pre-carbonization treatment is carried out under a nitrogen atmosphere, with a nitrogen introduction rate of 0.5 L / min and a heating rate of 5 °C / min.

[0011] Preferably, in step S1, the drying temperature for oily sludge, FCC waste catalyst, and petrochemical contaminated soil is set to 105~110 ℃, and the drying time is 22~26 h.

[0012] Preferably, in step S1, when grinding oily sludge, FCC waste catalyst, petrochemical contaminated soil, and waste glass powder, a planetary ball mill is used with a rotation speed of 300-500 r / min, a ball milling time of 1 h, a ball-to-material ratio of 2:1, and the material is sieved through a 200-mesh sieve.

[0013] Preferably, in step S2, a planetary ball mill is used for grinding, with a rotation speed of 300-500 r / min, a grinding time of 2-4 h, and a ball-to-material ratio of 2:1.

[0014] Preferably, in step S4, the drying temperature is 105 °C and the drying time is 10-12 h.

[0015] Preferably, in step S5, when performing high-temperature sintering, preheating is first performed at a heating rate of 10 ℃ / min, the target preheating temperature is set to 550 ℃, and the holding time is set to 30 min; the sintering temperature is set to 1120-1160 ℃, the holding time is set to 30 min, and the heating rate from the preheating temperature to the sintering temperature is 5 ℃ / min.

[0016] The present invention has at least the following beneficial effects: (1) The raw materials used in the preparation method of high-strength ceramsite based on petrochemical solid waste of the present invention include petrochemical oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder. The mass percentages of each raw material are as follows: oily sludge 20-40 wt%, contaminated soil 30-50 wt%, FCC waste catalyst 10 wt%, and waste glass powder 20 wt%. High-strength building ceramsite is prepared by synergistic processing of multiple solid wastes through raw material processing, ball milling and mixing, granulation, drying, and high-temperature sintering. At the same bulk density, its compressive strength and water absorption are far superior to ceramsite prepared by existing waste utilization methods. This process achieves high-proportion stable treatment of three typical industrial solid wastes from the petrochemical industry: oily sludge, FCC spent catalysts, and petrochemical-contaminated soil. The process is simple, low-cost, and the density meets aggregate requirements. It is an economical, environmentally friendly, and resource-efficient new building material that can effectively solve the problem of large-scale stockpiling of petrochemical solid waste and reduce the heavy reliance on non-renewable resources such as quartz, clay, and feldspar. It not only effectively improves resource utilization but also contributes to the sustainable development of resources, energy, environment, and economy.

[0017] (2) The preparation method of high-strength ceramsite based on petrochemical solid waste of the present invention uses waste glass powder as a sintering aid. The main components of waste glass powder are rich in SiO2 and fluxing oxides, which can reduce the melting point of the system while improving the skeleton composition of the system, thereby promoting the formation of liquid phase. First, the oily sludge is pre-carbonized. The heavy oil in the oily sludge is converted into a stable carbon skeleton in the pre-carbonization stage, instead of volatilizing rapidly in high-temperature sintering, thereby reducing some organic matter and providing skeleton strength of ceramsite in sintering process. The carbon skeleton is slowly oxidized to generate gas when the temperature is raised to 500-600℃. Due to the slow and uniform release rate, a large number of uniform and closed micron-sized spherical pores can be formed inside the ceramsite, avoiding the interconnected large pores and local collapse caused by the rapid volatilization of oil in direct sintering. The raw materials are fully coordinated and cooperated to finally obtain high-strength ceramsite that meets the requirements of aggregate.

[0018] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Attached Figure Description

[0019] Figure 1 This is a microstructure diagram of the high-strength ceramsite obtained in Example 1 of the present invention; Figure 2 This is a microstructure diagram of the high-strength ceramsite obtained in Example 2 of the present invention; Figure 3 This is a microstructure diagram of the high-strength ceramsite obtained in Example 3 of the present invention; Figure 4 This is a microstructure diagram of the high-strength ceramsite obtained in Example 4 of the present invention; Figure 5 This is a microstructure diagram of the high-strength ceramsite obtained in Example 5 of the present invention. Detailed Implementation

[0020] The present invention will now be described in further detail with reference to the accompanying drawings, so that those skilled in the art can implement it based on the description.

[0021] It should be noted that, unless otherwise specified, the experimental methods described in the following embodiments are all conventional methods, and the reagents and materials described are all commercially available unless otherwise specified. In the description of this invention, the terms "lateral", "longitudinal", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", and "outer" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0022] like Figure 1-5 As shown, this invention provides a method for preparing high-strength ceramsite based on petrochemical solid waste, comprising the following steps: S1. Raw material processing: The oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder are dried to constant weight. Then, the dried oily sludge is heated to 280~300 ℃ under an inert atmosphere and kept at that temperature for 30~45 min for pre-carbonization treatment. After that, the pre-carbonized oily sludge, dried FCC waste catalyst, petrochemical contaminated soil and waste glass powder are ground and sieved in sequence.

[0023] Oily sludge is formed by mixing drilling fluid (oil-based mud) used in the drilling process with underground rock cuttings. This type of oily sludge is characterized by high water and oil content and low ash content. FCC waste catalyst is solid waste generated during the processing of light oil. Petrochemical contaminated soil is soil around oil refineries that has been contaminated by rainwater from the oil refineries for a long time. Waste glass powder is a powdery substance formed after waste glass has been crushed, ground and processed. As a sintering aid, waste glass powder is rich in SiO2 and fluxing oxides, which can improve the system skeleton composition while lowering the melting point of the system, thereby promoting the formation of the liquid phase.

[0024] Specifically, the pre-carbonization treatment is carried out under a nitrogen atmosphere, with a nitrogen introduction rate of 0.5 L / min, a heating rate of 5 ℃ / min, a holding temperature of 280 ℃, and a holding time of 30~45 min.

[0025] This step begins with a low-temperature pre-carbonization treatment of the oily sludge. During the pre-carbonization stage, the heavy oil in the oily sludge is transformed into a stable carbonaceous skeleton, rather than rapidly volatilizing during high-temperature sintering. This reduces some organic matter and provides the skeleton strength of the ceramsite during sintering. This carbon skeleton is then slowly oxidized to generate gas when the temperature is subsequently raised to 500-600 ℃. Due to the gradual and uniform release rate, a large number of uniform, closed micron-sized spherical pores can be formed inside the ceramsite, avoiding the interconnected large pores and local collapse caused by the rapid volatilization of oil during direct sintering.

[0026] Preferably, the drying temperature for oily sludge, FCC waste catalyst, and petrochemical contaminated soil is set at 105~110℃, and the drying time is 22~26 h. This ensures that the free water and most of the bound water in the soil are fully removed so that the subsequent grinding process can proceed smoothly and avoids problems such as material agglomeration, difficulty in sieving, or decreased ball milling efficiency caused by excessive moisture content.

[0027] Preferably, in step S1, when grinding the oily sludge, FCC waste catalyst, petrochemical contaminated soil, and waste glass powder, a planetary ball mill is used to mechanically grind the mixture. The ball mill speed is set to 300-500 r / min, the ball milling time is 1 h, the ball-to-material ratio is 2:1, and the mixture is sieved through a 200-mesh sieve. This grinding process ensures that the components are sufficiently refined and uniformly mixed in a short time. After ball milling, the resulting mixed powder is treated to remove any small amount of coarse particles that were not ground finely, ensuring the consistency and uniformity of powder particle size in subsequent mixing and molding processes.

[0028] S2. Ball Milling and Mixing: The oily sludge, contaminated soil, FCC waste catalyst, and waste glass powder pretreated in step S1 are mixed according to the following mass percentages: oily sludge 20-40 wt%, contaminated soil 30-50 wt%, FCC waste catalyst 10 wt%, and waste glass powder 20 wt%. The mixture is then ball-milled to ensure thorough grinding and homogenization. This allows the four components—oily sludge, contaminated soil, FCC waste catalyst, and waste glass powder—to disperse and fully contact each other under mechanical force, eliminating local component segregation. This results in a uniformly distributed powder with consistent particle size, providing a homogenized raw material base for the subsequent water addition and granulation process.

[0029] Specifically, during grinding, a planetary ball mill is used with a rotation speed of 300-500 r / min, a grinding time of 2-4 h, and a ball-to-material ratio of 2:1.

[0030] S3. Granulation: Add water to the material mixed in step S2 and mix evenly. The amount of water added is 20-30 wt% of the material (dry material) mixed in step S2, so that the viscosity of the raw material is slurry and has plasticity. Then, granulate it in a disc granulator to form uniform raw material balls (about 5cm in diameter).

[0031] S4. Drying: Dry the formed raw material balls. This allows excess moisture in the raw material balls to evaporate and be removed, thereby improving the strength of the raw material balls and preventing cracking of the green body due to rapid moisture evaporation during subsequent high-temperature sintering.

[0032] Specifically, the drying temperature is 105 ℃ and the drying time is 10-12 h to ensure that the moisture inside and outside the raw material balls is removed evenly.

[0033] S5. High-temperature sintering: The dried raw material balls are sintered at high temperature and then naturally cooled to obtain the finished petrochemical solid waste-based high-strength ceramsite.

[0034] Specifically, during high-temperature sintering, preheating is first performed to make the internal temperature of the raw material pellets more uniform. The heating rate is 10 ℃ / min, the target preheating temperature is set at 550 ℃, and the holding time is set at 30 min. The sintering temperature is set at 1120-1160 ℃, the holding time is set at 30 min, and the heating rate from the preheating temperature to the sintering temperature is 5 ℃ / min, so that the raw material pellets can fully undergo the sintering reaction in the high-temperature range and form a stable ceramsite structure.

[0035] The method for preparing high-strength ceramsite based on petrochemical solid waste of the present invention treats oily sludge, contaminated soil, and FCC waste catalyst with a total mass percentage of up to 80%, effectively utilizing these three typical industrial solid wastes from the petrochemical industry. High-strength ceramsite is prepared by high-temperature sintering with waste glass powder as a sintering aid. The resulting ceramsite has a compressive strength of approximately 15 MPa and a bulk density of less than 1100 kg / m³. 3 It meets the requirements for lightweight aggregates, has high strength, and can be used as a substitute for traditional aggregates. It can be applied to highway pavements, sponge cities, high-performance concrete, permeable bricks and other fields, which contributes to the sustainable development of resources, energy, environment and economy.

[0036] Example 1: A method for preparing high-strength building ceramsite based on petrochemical solid waste is provided. The raw materials for preparation are as follows by weight percentage (dry state): 20 wt% oily sludge, 50 wt% contaminated soil, 10 wt% FCC waste catalyst, and 20 wt% waste glass powder. The mass of water added during granulation and slurry preparation is 20% of the total weight of the mixture.

[0037] The specific preparation steps are as follows: (1) Raw material processing: Oily sludge, FCC waste catalyst and petrochemical contaminated soil were placed in a forced-air drying oven and dried at 105℃ to constant weight. Then, the dried oily sludge was placed in a tube furnace and nitrogen gas was introduced (flow rate 0.5 L / min). The temperature was raised to 280℃ at 5℃ / min and held for 30min for pre-carbonization treatment. After natural cooling, it was taken out. Then, the pre-carbonized oily sludge and the dried petrochemical contaminated soil were placed in a planetary ball mill and ground for 1 h. The speed of the planetary ball mill was 300-500 r / min, the ball-to-material ratio was 2:1, and the sieve was sieved through a 200-mesh sieve (particle size less than 0.075 mm). (2) Ball milling and mixing: 20 wt% oily sludge, 50 wt% contaminated soil, 10 wt% FCC waste catalyst and 20 wt% waste glass powder are mixed and placed in a planetary ball mill for ball milling and mixing. The speed of the planetary ball mill is 300-500 r / min, the ball milling time is 2-4 h, and the ball-to-material ratio is 2:1. (3) Granulation: Add 20% of the total weight of water to the material that was mixed evenly in step (2) and mix evenly. The amount of water added should be such that the viscosity of the raw material is such that the slurry has a certain plasticity. Then, granulate by hand. (4) Drying: Place the formed raw material balls in an oven to dry. The temperature of the oven is set to 105 ℃ and the drying time is 10 h. (5) High-temperature sintering: The dried raw material balls are placed in a box-type resistance furnace for sintering. The preheating temperature of the box-type resistance furnace is set to 550 ℃, the holding time is set to 30 min, and the heating rate is 10℃ / min. The sintering temperature is set to 1140 ℃, the holding time is set to 30 min, and the heating rate is 5℃ / min. Then the furnace is naturally cooled to obtain the finished ceramsite.

[0038] After the finished ceramsite is removed, its properties such as compressive strength, bulk density, and water absorption rate are measured.

[0039] Example 2: A method for preparing high-strength building ceramsite based on petrochemical solid waste is provided. The raw materials for preparation are as follows by weight percentage (dry state): 30 wt% oily sludge, 40 wt% contaminated soil, 10 wt% FCC waste catalyst, 20 wt% waste glass powder, and the mass of water added during granulation and slurry preparation is 25% of the total weight of the mixture.

[0040] The specific preparation steps are as follows: (1) Raw material processing: Oily sludge, FCC waste catalyst and petrochemical contaminated soil were placed in a forced-air drying oven and dried at 105℃ to constant weight; then the dried oily sludge was placed in a tube furnace, nitrogen gas was introduced (flow rate 0.5 L / min), the temperature was raised to 280℃ at 5℃ / min, and the temperature was held for 30min for pre-carbonization treatment. After natural cooling, it was taken out; then the pre-carbonized oily sludge and the dried petrochemical contaminated soil were placed in a planetary ball mill and ground for 1 h. The speed of the planetary ball mill was 300-500 r / min, the ball-to-material ratio was 2:1, and the sieve was passed through a 200-mesh sieve (particle size less than 0.075 mm). (2) Ball milling and mixing: 20 wt% oily sludge, 50 wt% contaminated soil, 10 wt% FCC waste catalyst and 20 wt% waste glass powder are mixed and placed in a planetary ball mill for ball milling and mixing. The speed of the planetary ball mill is 300-500 r / min, the ball milling time is 2-4 h, and the ball-to-material ratio is 2:1. (3) Granulation: Add 20% of the total weight of water to the material that was mixed evenly in step (2) and mix evenly. The amount of water added should be such that the viscosity of the raw material is such that the slurry has a certain plasticity. Then, granulate by hand. (4) Drying: Place the formed raw material balls in an oven to dry. The temperature of the oven is set to 105 ℃ and the drying time is 10 h. (5) High-temperature sintering: The dried raw material balls are placed in a box-type resistance furnace for sintering. The preheating temperature of the box-type resistance furnace is set to 550 ℃, the holding time is set to 30 min, and the heating rate is 10℃ / min. The sintering temperature is set to 1140 ℃, the holding time is set to 30 min, and the heating rate is 5℃ / min. Then the furnace is naturally cooled to obtain the finished ceramsite.

[0041] After the finished ceramsite is removed, its properties such as compressive strength, bulk density, and water absorption rate are measured.

[0042] Example 3: A method for preparing high-strength building ceramsite based on petrochemical solid waste is provided. The raw materials for preparation are as follows by weight percentage (dry state): 40 wt% oily sludge, 30 wt% contaminated soil, 10 wt% FCC waste catalyst, 20 wt% waste glass powder, and the mass of water added during granulation and slurry preparation is 30% of the total weight of the mixture.

[0043] The specific preparation steps are as follows: (1) Raw material processing: Oily sludge, FCC waste catalyst and petrochemical contaminated soil were placed in a forced-air drying oven and dried at 105℃ to constant weight; then the dried oily sludge was placed in a tube furnace, nitrogen gas was introduced (flow rate 0.5 L / min), the temperature was raised to 280℃ at 5℃ / min, and the temperature was held for 30min for pre-carbonization treatment. After natural cooling, it was taken out; then the pre-carbonized oily sludge and the dried petrochemical contaminated soil were placed in a planetary ball mill and ground for 1 h. The speed of the planetary ball mill was 300-500 r / min, the ball-to-material ratio was 2:1, and the sieve was passed through a 200-mesh sieve (particle size less than 0.075 mm). (2) Ball milling and mixing: 20 wt% oily sludge, 50 wt% contaminated soil, 10 wt% FCC waste catalyst and 20 wt% waste glass powder are mixed and placed in a planetary ball mill for ball milling and mixing. The speed of the planetary ball mill is 300-500 r / min, the ball milling time is 2-4 h, and the ball-to-material ratio is 2:1. (3) Granulation: Add 20% of the total weight of water to the material that was mixed evenly in step (2) and mix evenly. The amount of water added should be such that the viscosity of the raw material is such that the slurry has a certain plasticity. Then, granulate by hand. (4) Drying: Place the formed raw material balls in an oven to dry. The temperature of the oven is set to 105 ℃ and the drying time is 10 h. (5) High-temperature sintering: The dried raw material balls are placed in a box-type resistance furnace for sintering. The preheating temperature of the box-type resistance furnace is set to 550 ℃, the holding time is set to 30 min, and the heating rate is 10 ℃ / min. The sintering temperature is set to 1140 ℃, the holding time is set to 30 min, and the heating rate is 5 ℃ / min. Then the furnace is naturally cooled to obtain the finished ceramsite.

[0044] After the finished ceramsite is removed, its properties such as compressive strength, bulk density, and water absorption rate are measured.

[0045] Example 4: A method for preparing high-strength building ceramsite based on petrochemical solid waste is provided. The raw materials for preparation are as follows by weight percentage (dry state): 30 wt% oily sludge, 40 wt% contaminated soil, 10 wt% FCC waste catalyst, 20 wt% waste glass powder, and the mass of water added during granulation and slurry preparation is 25% of the total weight of the mixture.

[0046] The specific preparation steps are the same as in Example 1, except that the firing temperature is 1120 °C.

[0047] Example 5: A method for preparing high-strength building ceramsite based on petrochemical solid waste is provided. The raw materials for preparation are as follows by weight percentage (dry state): 30 wt% oily sludge, 40 wt% contaminated soil, 10 wt% FCC waste catalyst, 20 wt% waste glass powder, and the mass of water added during granulation and slurry preparation is 25% of the total weight of the mixture.

[0048] The specific preparation steps are the same as in Example 1, except that the firing temperature is 1160 °C.

[0049] The microstructure images of the ceramsite products obtained in Examples 1-5 under a scanning electron microscope (SEM) correspond to the following: Figure 1-5 As shown; referring to GB / T17431.2-2010 "Lightweight aggregates and their test methods Part 2: Lightweight aggregates test methods", the compressive strength, bulk density and water absorption of the lightweight high-strength ceramsite prepared in the above embodiments were tested, and the results are as follows: Table 1 Test results of Examples 1-5 As can be seen from the above examples, the building ceramsite prepared using the method of the present invention with three typical industrial solid wastes from the petrochemical industry—oil-containing sludge, FCC waste catalyst, and petrochemical contaminated soil—combined with waste glass powder as a sintering aid, can achieve compressive strength and mass that can reach or even exceed those of building ceramsite prepared from non-waste raw materials using conventional techniques. Among them, the bulk density of Examples 1-5 is in the medium-high density range, and the compressive strength reaches 11-15 MPa. The compressive strength of Examples 2, 3, and 5 is relatively high, and the skeletal structure outline is clearer in the microstructure. The compressive strength of Example 2 is the highest, far exceeding the 6.5-8 MPa compressive strength of conventional high-strength ceramsite. In terms of water absorption rate, it remains below 4%. The water absorption rate of Example 2 is slightly higher than 1%, and the water absorption rate of Examples 3 and 5 is less than 0.5%, which is far better than the water absorption rate range of ordinary ceramsite. From a microscopic perspective, the micron-sized pores are uniformly distributed within the structure and are not interconnected, providing structural assurance for the material's durability and frost resistance. It is particularly suitable for lightweight aggregate concrete in load-bearing structures, reducing the structure's self-weight while providing sufficient strength and excellent durability. It also provides a new approach to treating these types of industrial solid wastes, which aligns with the sustainable development strategy of recycling.

[0050] Although embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details and illustrations shown and described herein.

Claims

1. A method for preparing high-strength ceramsite based on petrochemical solid waste, characterized in that, Includes the following steps: S1. Raw material processing: The oily sludge, FCC waste catalyst, petrochemical contaminated soil and waste glass powder are dried to constant weight. Then, the dried oily sludge is heated to 280~300 ℃ under an inert atmosphere and kept at that temperature for 30~45 min for pre-carbonization treatment. After that, the pre-carbonized oily sludge, dried FCC waste catalyst, petrochemical contaminated soil and waste glass powder are ground and sieved in sequence. S2. Ball milling and mixing: The oily sludge and contaminated soil pretreated in step S1 are mixed with FCC waste catalyst and waste glass powder in the following mass percentages: oily sludge 20-40 wt%, contaminated soil 30-50 wt%, FCC waste catalyst 10 wt%, and waste glass powder 20 wt%. The mixture is then ball milled to mix it evenly. S3. Granulation: Add water to the material mixed in step S2 and mix evenly. The amount of water added is 20-30 wt% of the material mixed in step S2, so that the viscosity of the raw material is slurry and has plasticity. Then, granulate it in a disc granulator to obtain raw material balls with a diameter of nearly 5 cm. S4. Drying: Dry the formed raw material balls; S5. High-temperature sintering: The dried raw material balls are sintered at high temperature and then naturally cooled to obtain the finished petrochemical solid waste-based high-strength ceramsite.

2. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S1, the pre-carbonization treatment is carried out under a nitrogen atmosphere, with a nitrogen introduction rate of 0.5 L / min and a heating rate of 5 °C / min.

3. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S1, the drying temperature for oily sludge, FCC waste catalyst, and petrochemical contaminated soil is set to 105~110 ℃, and the drying time is 22~26 h.

4. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S1, when grinding oily sludge, FCC waste catalyst, petrochemical contaminated soil, and waste glass powder, a planetary ball mill is used with a rotation speed of 300-500 r / min, a ball milling time of 1 h, a ball-to-material ratio of 2:1, and the material is sieved through a 200-mesh sieve.

5. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S2, a planetary ball mill is used for grinding, with a rotation speed of 300-500 r / min, a grinding time of 2-4 h, and a ball-to-material ratio of 2:

1.

6. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S4, the drying temperature is 105 ℃ and the drying time is 10-12 h.

7. The method for preparing high-strength ceramsite based on petrochemical solid waste as described in claim 1, characterized in that, In step S5, when performing high-temperature sintering, preheating is first performed at a heating rate of 10 ℃ / min, with the target preheating temperature set at 550 ℃ and the holding time set at 30 min; the sintering temperature is set at 1120-1160 ℃, the holding time is set at 30 min, and the heating rate from the preheating temperature to the sintering temperature is 5 ℃ / min.