Decarburized coal gangue-based multi-solid waste collaborative porcelain raw material based on iron / calcium in-situ chelation pre-organization and preparation method thereof
By using phytic acid chelation and aluminum dihydrogen phosphate to induce crystal nuclei, the problem of disordered crystal phases and expansion caused by the premature migration of iron and calcium elements in the co-production of ceramics from various solid wastes was solved, thus enabling the production of high-performance, low-cost ceramic products.
Patent Information
- Application Number
- CN202611588964.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies for the co-preparation of ceramics from solid wastes such as decarbonized coal gangue, iron tailings, steel slag, and fly ash have several drawbacks. These include the premature migration of iron and calcium elements leading to disordered crystal phase precipitation, a narrow densification window, volume expansion of free CaO, and high pretreatment costs.
By selectively chelating phytic acid to delay Fe/Ca activity, combined with aluminum dihydrogen phosphate to induce crystal nuclei, a shell is formed through phytic acid chelation and sintered in an oxidizing atmosphere, achieving synergistic ceramic formation from multiple solid wastes.
It effectively inhibits the rapid release of Fe and Ca at low temperatures, promotes the orderly nucleation and columnar growth of mullite, eliminates the risk of free CaO expansion, improves the mechanical properties and stability of ceramics, and reduces costs.
Smart Images

Figure CN123131128A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a ceramic raw material based on decarbonized coal gangue with multiple solid wastes and its preparation method, which is based on iron / calcium in-situ chelation pre-organization and belongs to the field of ceramic materials and industrial solid waste resource recycling technology. Background Technology
[0002] With the rapid development of industrialization and urbanization in my country, industries such as coal, steel, and mining generate a large amount of solid waste. Among these, decarbonized coal gangue, iron tailings, steel slag, and fly ash are the typical industrial solid wastes with the largest emissions and the most prominent storage pressure. These solid wastes are rich in elements such as silicon, aluminum, iron, and calcium, and have potential value as raw materials for ceramics. The synergistic utilization of multi-source solid waste in the preparation of high-end ceramics can not only dispose of massive amounts of solid waste but also reduce the consumption of natural minerals in the ceramics industry, aligning with the development direction of green manufacturing and a circular economy.
[0003] Currently, a few studies have attempted to prepare building ceramics or low-grade refractory materials by compounding decarbonized coal gangue with fly ash, steel slag, etc. However, when these four solid wastes (decarbonized coal gangue, iron tailings, steel slag, and fly ash) are used together, the following prominent problems arise due to the significant differences in the occurrence forms and thermochemical behaviors of elements in the different solid wastes: (1) Iron and calcium migrate ahead of silicon and aluminum: Iron in iron tailings mainly exists in the form of hematite and limonite, while steel slag contains a large amount of free calcium oxide and calcium silicate. Combining thermodynamic phase diagrams and thermal analysis, it can be seen that in the initial stage of sintering heating, when the temperature reaches the initiation temperature of a specific phase transformation (usually 800-950℃), Fe... 3+ and Ca 2+ It readily reacts with SiO2 in the system to form low-melting-point calcium ferrite and calcium silicate liquid phases. The premature appearance of this low-viscosity liquid phase will rapidly encapsulate the aluminosilicate particles that have not yet undergone solid-phase reaction, severely altering the non-isothermal kinetic path of the system, hindering the precipitation and secondary growth of the mullite and corundum main crystalline phases, resulting in an extremely narrow ceramic densification temperature window, disordered crystalline phases, and unstable mechanical properties.
[0004] (2) Risk of free calcium oxide volume expansion: If the free CaO remaining in the steel slag fails to participate in the reaction and enter the crystal lattice after ceramic firing, it will slowly absorb moisture from the air during the storage or use of the product, and undergo a hydration reaction to generate Ca(OH)2. This process is accompanied by a violent volume expansion (expansion rate close to 100%), which leads to microcracks inside the ceramic product, greatly weakening its durability and safety in the field of engineering structures. Therefore, it is necessary to transform it into a stable phase in situ through phase engineering methods.
[0005] (3) Difficulty in controlling crystal phase composition: Existing technologies mostly employ simple physical-mechanical mixing followed by direct high-temperature sintering. Due to the lack of active intervention on the migration paths of highly reactive interfering elements such as Fe and Ca during the heating process, the sintered product has an excessively high glass phase content, resulting in coarse and unevenly distributed crystals. The flexural strength of the obtained ceramics is usually below 70 MPa, and the coefficient of thermal expansion is too high (>7×10). -6 The system composition ( / K) cannot meet the standards for high-end engineering ceramics. Some studies have attempted to adjust the system composition through acid washing or the addition of additives, but these methods significantly increase costs or introduce new metal ions that interfere with crystal phase formation. Some surface grafting modification techniques rely heavily on expensive reagents and do not consider the complex coupling effects between multiple sources of solid waste.
[0006] Therefore, there is an urgent need to develop a pretreatment method specifically for the co-processing of ceramic raw materials from four types of solid waste: decarbonized coal gangue, iron tailings, steel slag, and fly ash. This method should be based on the phase transition laws of multi-solid waste systems, selectively delaying the early reactivity of Fe and Ca through low-cost chemical pre-organization techniques, while simultaneously inducing the directional nucleation of the target crystalline phase, thereby achieving ordered densification and crystalline phase reconstruction of the multi-solid waste system.
[0007] In view of this, the present invention provides a decarbonized coal gangue-based multi-solid waste synergistic ceramic raw material based on iron / calcium in-situ chelation pre-organization and its preparation method. Summary of the Invention
[0008] To address the problems encountered in ceramic preparation from four solid wastes—decarbonized coal gangue, iron tailings, steel slag, and fly ash—where Fe and Ca migrate ahead of Si and Al, leading to disordered crystal phase precipitation, narrow densification windows, and volume expansion of free CaO, as well as the high cost and reliance on added rare metal salts in existing pretreatment methods, this invention provides a decarbonized coal gangue-based multi-solid waste synergistic ceramic raw material and its preparation method based on in-situ iron / calcium chelate pre-organization. This method temporarily delays Fe / Ca activity through selective chelation with phytic acid, combined with aluminum dihydrogen phosphate-induced crystal nucleation, achieving synergistic ceramic formation from multiple solid wastes.
[0009] The decarbonized coal gangue involved in this invention is silicon-aluminum-rich waste rock after decarbonization treatment in the coal industry; iron tailings is tailings after iron ore beneficiation; steel slag is alkaline slag produced in steelmaking; and fly ash is fly ash from coal-fired power plants.
[0010] The present invention provides a method for preparing decarbonized coal gangue-based multi-solid waste synergistic ceramic raw materials based on iron / calcium in-situ chelation pre-organization, comprising the following steps: S1. Mix four types of solid waste—decarbonized coal gangue, iron tailings, steel slag, and fly ash—in a certain proportion, and then crush and ball-mill them to obtain a mixed powder. S2. Disperse the mixed powder in water, add phytic acid as a multidentate chelating agent, so that the phytic acid reacts with the Fe in the mixed powder. 3+ and Ca2+ Selective chelation occurs, forming a phytic acid-metal chelate shell on the particle surface. After filtration, washing, and drying, pre-structured powder is obtained. S3. Add aluminum dihydrogen phosphate to the pre-organized powder and dry mix evenly to obtain the compound raw material powder; S4. The compound raw material powder is mixed with the molding aid, and after molding and drying, it is sintered in an oxidizing atmosphere to obtain a ceramic material.
[0011] In step S1, the mass percentages of the four types of solid waste are: decarbonized coal gangue 40-50%, iron tailings 20-30%, steel slag 10-20%, and fly ash 15-25%. The particle size D90 of the mixed powder is ≤20 μm.
[0012] In step S2, after adding the phytic acid, the pH of the system is adjusted to 4.0-5.0, and the mixture is stirred at 50-70℃ for 1-3 hours to carry out chelation. During the reaction, multiple phosphate groups of the phytic acid molecules preferentially react with Fe exposed on the surface of the mixed powder. 3+ Ca 2+ Selective in-situ chelation occurs.
[0013] In step S2, the amount of phytic acid added is 5-10% of the mass of the mixed powder; The thickness of the phytic acid-metal chelate shell is 50-200 nm. The phytic acid (C6H) used in this invention 18 O 24 P6 (also known as inositol hexaphosphate) is a naturally sourced green chelating agent that has a strong effect on Fe. 3+ Ca 2+ The chelation constant is much higher than that for Al 3+ The chelation constant, therefore preferentially with Fe 3+ Ca 2+ It combines with the main Si and Al framework in the system, but has little effect on them.
[0014] In step S3, the amount of aluminum dihydrogen phosphate added is 2-5% of the mass of the pre-organized powder; The aluminum dihydrogen phosphate used in this invention decomposes to generate P2O5 during the subsequent sintering process. P2O5 reacts in situ with Al2O3 released from the mixed powder to generate AlPO4 crystal nuclei. These crystal nuclei have a high degree of matching with the mullite lattice and can induce the mullite to grow in a long columnar orientation.
[0015] In step S4, the molding aid includes at least one of kaolin and polyvinyl alcohol; preferably, the molding aid is a combination of kaolin and polyvinyl alcohol, wherein the amount of kaolin added is 10-15% of the mass of the compound raw material powder, and the amount of polyvinyl alcohol added is 3-5% of the mass of the compound raw material powder.
[0016] In step S4, the sintering process involves heating to 900-1000℃ at a rate of 1-3℃ / min and holding at that temperature for 0.5-1.5 h. During this stage, the phytic acid-metal chelate shell gradually undergoes pyrolysis under an oxidizing atmosphere, accompanied by shell structure destruction and changes in Fe and Ca migration behavior. Temperature-specific ICP-OES analysis shows that, compared to the mixed powder without phytic acid chelation, the release of Fe and Ca in the phytic acid pre-structured powder is significantly inhibited below 900℃, while the release gradually increases in the 900–1000℃ temperature range. This indicates that phytic acid chelation pre-structured powder can effectively delay the rapid release of Fe and Ca, preventing large-scale premature migration of eutectic compounds below 900℃. Then raise the temperature to 1200-1250℃ at a rate of 3-6℃ / min, hold for 1-3 hours, and then let it cool naturally to room temperature in the furnace. The oxygen volume concentration in the oxidizing atmosphere is ≥15%; The sintering in the oxidizing atmosphere completely oxidizes and decomposes the phytic acid in the chelated shell, and the Fe in the shell... 3+ Ca 2+ The slow release prevents the premature formation of a large amount of low-melting-point liquid phase; at the same time, the phosphorus element in the shell participates in the nucleation reaction in the form of P2O5.
[0017] The main crystalline phase of the ceramic product obtained by this invention is mullite with a long columnar interwoven structure. The free CaO in the steel slag is completely transformed into a stable calcium feldspar phase, with no residual expansion risk.
[0018] In terms of macroscopic performance, the product has a bending strength ≥100 MPa (far exceeding the <70 MPa of conventional solid waste ceramics) and a coefficient of thermal expansion ≤5.0×10⁻⁶. -6 / K, and after high-temperature hydrothermal aging, the volume expansion rate is <0.05%, and the surface is intact without cracks.
[0019] At the mechanistic level, the phytic acid chelate shell delays the release of Fe and Ca activity until 900℃, avoiding premature interference of the low-melting-point liquid phase with ceramic formation; the AlPO4 crystal nuclei generated by the decomposition of aluminum dihydrogen phosphate directionally induce mullite to grow with a high aspect ratio. The two work together to achieve phase reconstruction and performance leap of multi-solid waste into high-performance ceramics.
[0020] Compared with the prior art, the present invention has the following beneficial effects: Selective inhibition of Fe and Ca advanced migration: utilizing phytic acid on Fe3+ Ca 2+ The chelation effect forms a phytic acid-metal pre-structured layer on the surface of solid waste particles. Quantitative analysis using ICP-OES at specific temperatures shows that the phytic acid pre-structure significantly reduces the release rate of Fe and Ca below 900 °C and shifts the main release process to the 900–1000 °C temperature range. This reduces the possibility of Fe and Ca prematurely participating in the reaction at low temperatures to form a low-melting-point liquid phase, providing a relatively stable reaction environment for further reconstruction of the Si-Al framework and the formation of the target crystal phase.
[0021] In-situ induced ordered precipitation of crystalline phases: The introduced aluminum dihydrogen phosphate decomposes to produce P2O5, which reacts with Al2O3 in the system to form AlPO4 crystal nuclei. These nuclei effectively lower the nucleation barrier of mullite, inducing mullite to form a long columnar interwoven structure, significantly improving the mechanical properties of the ceramic. Experimental results show that the flexural strength of the obtained ceramic is ≥100 MPa, and the coefficient of thermal expansion is ≤5.0×10⁻⁶. -6 / K.
[0022] Eliminating the risk of free CaO volume expansion: Free CaO in steel slag is encapsulated by phytic acid in the chelated shell, and during sintering, Ca... 2+ The release is delayed, and it reacts fully with SiO2 and Al2O3 in the system to form a stable anorthite (CaAl2Si2O8) phase, thus completely avoiding the cracking problem caused by CaO absorbing water and expanding.
[0023] Green and environmentally friendly, low cost: The phytic acid used is a natural plant extract, which is non-toxic and biodegradable; there is no need to use expensive silane coupling agents and rare metal salts (such as lithium nitrate, cobalt nitrate, etc.); the four types of solid waste are all bulk industrial wastes, with extremely low raw material costs, which meet the requirements of green manufacturing.
[0024] The process is simple and easy to industrialize: it only requires adding one step of liquid phase chelation and dry mixing, has low equipment requirements, good compatibility with existing ceramic powder processing production lines, and is easy to scale up. Attached Figure Description
[0025] Figure 1 This is a flowchart of the preparation method of the multi-solid waste synergistic ceramic raw material based on iron / calcium in-situ chelation pre-organization of decarbonized coal gangue.
[0026] Figure 2 The image shows the XRD pattern of the ceramic prepared in Example 3 of this invention.
[0027] Figure 3 This is a SEM image of the ceramic prepared in Example 3 of the present invention. Detailed Implementation
[0028] To further illustrate the technical solution and beneficial effects of the present invention, a detailed description is provided below with reference to specific embodiments and comparative examples. The following embodiments are for illustrative purposes only and do not constitute any limitation on the scope of protection of the present invention. Any modifications, equivalent substitutions, or improvements made by those skilled in the art without departing from the principles of the present invention should fall within the scope of protection of the present invention.
[0029] Unless otherwise specified, in the following examples and comparative examples, the decarbonized coal gangue used is silica-alumina-rich waste rock from the coal industry after decarbonization treatment; iron tailings are tailings from iron ore beneficiation; steel slag is alkaline slag produced in steelmaking; and fly ash is fly ash from coal-fired power plants. All of the above solid waste raw materials have been crushed and ground, and their chemical composition is within the conventional fluctuation range in the field.
[0030] Table 1 Composition of various solid waste raw materials
[0031] I. Implementation Examples Example 1 Step 1: Preparation of mixed powders Weigh out 45% decarburized coal gangue, 25% iron tailings, 15% steel slag, and 15% fly ash by mass percentage, with a total mass of 1 kg. Mix the above solid wastes and place them in a planetary ball mill, using zirconia balls as the grinding medium, with a ball-to-material ratio of 3:1, a rotation speed of 300 rpm, and ball milling for 4 h to obtain a mixed powder with a particle size D90 = 18 μm.
[0032] Step 2: Selective chelation of pre-organized tissue The mixed powder obtained in step 1 was dispersed in 2 L of deionized water, and 70 g of phytic acid (active ingredient ≥50% aqueous solution, calculated as pure phytic acid) (7% of the mixed powder mass) was added. The pH was slowly adjusted to 4.5 with dilute ammonia (volume ratio 1:1), and the reaction was stirred in a 60℃ water bath for 2 h. After the reaction was completed, the mixture was filtered, washed three times with deionized water until the pH of the filtrate was 7, and dried at 105℃ for 12 h to obtain pre-structured powder. Scanning electron microscopy revealed that a continuous chelate shell with a thickness of approximately 120 nm was formed on the surface of the particles.
[0033] Step 3: Introduction of aluminum phosphate nucleus precursor Add 35 g of aluminum dihydrogen phosphate (analytical grade) (3.5% of the mass of the pre-organized powder) to the pre-organized powder obtained in step 2, and dry mix in a V-type mixer for 30 min to obtain the compound raw material powder.
[0034] Step 4: Shaping and Sintering Kaolin (125 g, 12.5% of the total powder mass) and polyvinyl alcohol (PVA, 40 g, 4%) were added to the compound raw material powder obtained in step 3. After being dry-mixed evenly, the mixture was dry-pressed into Φ50 mm × 5 mm round green blanks under a pressure of 30 MPa. The green blanks were dried at 110℃ for 12 h and then placed in a high-temperature box furnace for sintering in an air atmosphere (O2 volume concentration of approximately 21%). The sintering regime was as follows: the temperature was increased to 950℃ at a rate of 2℃ / min and held for 1 h; then increased to 1230℃ at a rate of 5℃ / min and held for 2 h; and then cooled to room temperature in the furnace.
[0035] Example 2 This embodiment is basically the same as Embodiment 1, except that: in step 2, the amount of phytic acid added is adjusted to 5% (i.e., 50 g) of the mass of the mixed powder, the chelation reaction time is adjusted to 1.5 h, and the thickness of the resulting chelated shell is approximately 65 nm. The remaining steps and parameters are the same as in Embodiment 1.
[0036] Example 3 This embodiment is basically the same as Embodiment 1, except that: the mass percentages of the four solid wastes in step 1 are adjusted to: decarbonized coal gangue 50%, iron tailings 20%, steel slag 10%, and fly ash 20%. In step 3, the amount of aluminum dihydrogen phosphate added is adjusted to 5% of the pre-organized powder mass (approximately 52 g). In step 4, the high-temperature sintering temperature is adjusted to 1250℃, and the holding time is 1.5 h. The remaining steps and parameters are the same as in Embodiment 1.
[0037] The XRD pattern of the ceramic prepared in this embodiment is as follows: Figure 2 As shown, the SEM image is as follows: Figure 3 As shown.
[0038] Depend on Figure 2 It can be seen that the main crystalline phase of the product is mullite, and it also exhibits characteristic peaks of anorthite, without diffraction peaks of free CaO and low-melting-point impurities such as calcium ferrite. This indicates that the free CaO in the steel slag, which poses a risk of volume expansion, has been completely transformed into the stable anorthite phase. Figure 3It is evident that the mullite crystals exhibit a long columnar interwoven structure with well-developed grains, a high aspect ratio, tight grain boundary bonding, and minimal residual pores, which are distributed as closed pores, indicating that the material has achieved sufficient densification. XRD and SEM results jointly demonstrate that the phytic acid chelation pre-structure effectively inhibited the premature reaction of Fe and Ca at low temperatures (based on the temperature-dependent ICP-OES data in Table 2, the release rates of Fe and Ca decreased by approximately 58.8% and 58.3%, respectively, at 900℃), avoiding premature formation of the low-melting-point liquid phase and its interference with subsequent mullitization and densification. Simultaneously, the AlPO4 crystal nuclei generated from the decomposition of aluminum dihydrogen phosphate directionally induced the mullite to grow into long columnar shapes with a high aspect ratio. These two factors synergistically achieved phase reconstruction and structural optimization of the multi-solid-waste system into high-performance ceramics, resulting in the ceramic of Example 3 exhibiting a flexural strength of 120 MPa and a thermal expansion coefficient of only 4.5 × 10⁻⁶. -6 The performance results of / K and a volume expansion rate of <0.04% after hydrothermal aging provide direct microstructural support.
[0039] Example 4 This embodiment is basically the same as Example 1, except that: in step 2, the pH of the chelation reaction is adjusted to 4.0, the reaction temperature is adjusted to 50°C, the reaction time is 3 h, and the amount of phytic acid added is 10% (i.e., 100 g) of the mass of the mixed powder. The remaining steps and parameters are the same as in Example 1.
[0040] II. Comparative Example Comparative Example 1: Direct mechanical mixing and sintering, without in-situ chelation and nucleation induction. The four solid wastes (45% decarbonized coal gangue, 25% iron tailings, 15% steel slag, and 15% fly ash) were weighed and ball-milled using the exact same proportions as in Example 1. The phytic acid chelation and coating reaction in step two was omitted, and aluminum dihydrogen phosphate in step three was not added. Instead, kaolin and PVA molding aid were directly added to the ball-milled mixed powder. The ceramic material sample was prepared using the same molding and sintering process as in Example 1.
[0041] Comparative Example 2: Phytic acid chelation present, but no aluminum dihydrogen phosphate nucleation induction. Mechanical mixing and phytic acid chelation reaction were performed using the same raw material ratios and steps one and two as in Example 1. However, no aluminum dihydrogen phosphate was added in step three. The dried pre-structured powder was directly mixed with kaolin and PVA and prepared using the same pressure molding and gradient sintering process as in Example 1.
[0042] Comparative Example 3: Contains aluminum dihydrogen phosphate, but lacks phytic acid chelation. The mixed powder was prepared using the same raw material ratio and step one as in Example 1. Instead of performing the phytic acid chelation reaction in step two, the unmodified mixed powder was directly dry-mixed with 3.5% by mass of aluminum dihydrogen phosphate, followed by the addition of a molding aid and pressing. The powder was then prepared using the same sintering process as in Example 1.
[0043] III. Performance Testing and Effect Comparison The ceramic samples prepared in each embodiment and comparative example were tested for flexural strength and coefficient of thermal expansion (the coefficient of thermal expansion of the samples was determined according to GB / T16535-2008 "Test Method for Linear Thermal Expansion Coefficient of Fine Ceramics - Top Rod Method", using a DIL402PC thermal dilatometer, with sample size of 4mm×4mm×25mm, heated from room temperature to 800℃ at a heating rate of 5℃ / min in air atmosphere; the flexural strength of the samples was tested according to GB / T 6569-2006 "Test Method for Flexural Strength of Fine Ceramics" - three-point bending method, with sample size of 3mm×4mm×36mm, span set to 30mm, and loading rate of 0.5mm / min). The samples were also tested for crack resistance and volume expansion resistance through hydrothermal aging experiments (test method: the samples were placed in a 120℃ autoclave for 24h of steam treatment, and the presence of cracks, peeling, or powdering was observed, and the volume expansion rate of the samples was tested).
[0044] The test results are shown in Table 2: Table 2. Performance comparison of each embodiment and the comparative ceramic sample
[0045] Temperature-dependent ICP-OES quantitative analysis was performed on the ceramics prepared in Example 1 and Comparative Example 1. Specifically, unchelated mixed solid waste powder was used as the control group, and phytate-chelated pre-structured powder was used as the experimental group. Samples were heated to 700, 800, 850, 900, 950, 1000, and 1050 °C under the same heating conditions and then rapidly cooled before sampling. The samples were then treated using a uniform leaching / digestion method, and the release amounts of Fe and Ca at each temperature stage were determined by ICP-OES. The Fe and Ca release rates were calculated, and the release behavior of the two groups of samples at different temperatures was compared.
[0046] The above experiments investigated the inhibitory effect of phytic acid chelation on the rapid release of Fe and Ca at 800-900 ℃, and the changes in the release of Fe and Ca at 900-1000 ℃. If the experimental results show that the release rate of Fe and Ca in the phytic acid group is significantly lower than that in the unchelated group below 900 ℃, while the release amount is significantly increased at 900-1000 ℃, then the delaying effect of phytic acid pre-tissue on the migration behavior of Fe and Ca can be directly verified. The results are shown in Table 3.
[0047] Table 3. Fe and Ca release rates in unchelated and phytic acid-chelated powders at different temperatures
[0048] It can be seen that with increasing temperature, both Fe and Ca in the unchelated group exhibited a relatively obvious premature release behavior. At 700℃, the release rates of Fe and Ca were 15% and 18%, respectively; when the temperature was increased to 800℃ and 900℃, the release rates increased to 35% / 42% and 68% / 72%, respectively, indicating that Fe and Ca had already undergone significant release before 900℃.
[0049] In contrast, the phytic acid chelated group exhibited significantly lower Fe and Ca release rates at low temperatures. At 700 °C, the Fe and Ca release rates were only 5% and 6%, respectively; at 800 °C, they were 9% and 11%; and at 900 °C, they were 28% and 30%, respectively, significantly lower than the unchelated group at the same temperature. Taking 900 °C as an example, phytic acid chelation reduced the Fe and Ca release rates by approximately 58.8% and 58.3%, respectively, indicating that phytic acid pretreatment can effectively inhibit the rapid release of Fe and Ca below 900 °C.
[0050] With further increase in temperature, the release rates of Fe and Ca in the phytic acid group increased significantly, reaching 48% and 52% respectively at 950 ℃, and further increasing to 75% and 78% at 1000 ℃, indicating that the release process of Fe and Ca accelerated significantly in the 900-1000 ℃ temperature range. At 1050 ℃, the release rates of Fe and Ca in the phytic acid group reached 91% and 93% respectively, significantly narrowing the difference with the 95% and 96% of the non-chelated group.
[0051] The above results indicate that phytic acid chelation pre-organization can significantly inhibit the rapid release of Fe and Ca below 900 °C and shift the main release process to the 900-1000 °C temperature range, thereby reducing the possibility of Fe and Ca participating in the reaction prematurely at low temperatures and providing more favorable reaction conditions for subsequent Si-Al framework reconstruction and target crystal phase formation.
[0052] IV. Results Analysis In Comparative Example 1, due to the lack of active barrier and crystal phase induction, Fe and Ca prematurely overflowed at low temperature, failing to form an interwoven columnar mullite network. The excess free CaO absorbed water and expanded during hydrothermal aging, resulting in a bending strength of only 52 MPa and severe cracking.
[0053] In Comparative Example 2, the volume expansion problem was solved because phytic acid was added to temporarily block Ca and Fe. However, due to the lack of AlPO4 crystal nucleus orientation induction, the mullite failed to grow into an ideal high aspect ratio interwoven long column, resulting in limited improvement in mechanical properties.
[0054] Although AlPO4 was introduced to promote nucleation in Comparative Example 3, the lack of phytic acid to block the highly active Ca and Fe meant that the early low-melting-point liquid phase still encapsulated the active components, hindering the orderly nucleation of the main crystalline phase and still posing a risk of cracking.
[0055] In Examples 1-4 of this invention, the flexural strength of all components jumped to over 100 MPa through a dual synergistic mechanism of selective chelation of phytic acid and decomposition of aluminum dihydrogen phosphate, and the expansion rate was almost zero. This completely realizes low-cost, high-performance green multi-solid waste synergistic ceramic production.
Claims
1. A method for preparing a multi-solid waste synergistic ceramic raw material based on iron / calcium in-situ chelation pre-organization of decarbonized coal gangue, comprising the following steps: S1. Mix four types of solid waste—decarbonized coal gangue, iron tailings, steel slag, and fly ash—in a certain proportion, and then crush and ball-mill them to obtain a mixed powder. S2. Disperse the mixed powder in water, add phytic acid as a multidentate chelating agent, so that the phytic acid reacts with the Fe in the mixed powder. 3 + and Ca 2+ Selective chelation occurs, forming a phytic acid-metal chelate shell on the particle surface. After filtration, washing, and drying, pre-structured powder is obtained. S3. Add aluminum dihydrogen phosphate to the pre-organized powder and dry mix evenly to obtain the compound raw material powder; S4. The compound raw material powder is mixed with the molding aid, and after molding and drying, it is sintered in an oxidizing atmosphere to obtain a ceramic material.
2. The preparation method according to claim 1, characterized in that: In step S1, the mass percentages of the four types of solid waste are: decarbonized coal gangue 40-50%, iron tailings 20-30%, steel slag 10-20%, and fly ash 15-25%. The particle size D90 of the mixed powder is ≤20 μm.
3. The preparation method according to claim 1 or 2, characterized in that: In step S2, after adding the phytic acid, the pH of the system is adjusted to 4.0-5.0, and the reaction is carried out by stirring at 50-70℃ for 1-3 hours to achieve chelation.
4. The preparation method according to any one of claims 1-3, characterized in that: In step S2, the amount of phytic acid added is 5-10% of the mass of the mixed powder; The thickness of the phytic acid-metal chelate shell is 50-200 nm.
5. The preparation method according to any one of claims 1-4, characterized in that: In step S3, the amount of aluminum dihydrogen phosphate added is 2-5% of the mass of the pre-organized powder.
6. The preparation method according to any one of claims 1-5, characterized in that: In step S4, the molding aid includes at least one of kaolin and polyvinyl alcohol, wherein the amount of kaolin added is 10-15% of the mass of the compound raw material powder, and the amount of polyvinyl alcohol added is 3-5% of the mass of the compound raw material powder.
7. The preparation method according to any one of claims 1-6, characterized in that: In step S4, the sintering process is as follows: the temperature is increased to 900-1000℃ at a heating rate of 1-3℃ / min, and held for 0.5-1.5 h; then the temperature is increased to 1200-1250℃ at a heating rate of 3-6℃ / min, and held for 1-3 h. The oxygen volume concentration of the oxidizing atmosphere is ≥15%.
8. A ceramic material prepared by the method according to any one of claims 1-7.
9. The decarbonized coal gangue-based multi-solid waste co-firing ceramic raw material according to claim 8, characterized in that: The mullite crystal phase in the ceramic material exhibits a long columnar interwoven structure, with a flexural strength ≥100 MPa and a coefficient of thermal expansion ≤5.0×10⁻⁶. -6 / K, and free calcium oxide is locked in the calcium feldspar phase.
10. The decarbonized coal gangue-based multi-solid waste co-forming ceramic raw material according to claim 8 or 9, characterized in that: The ceramic material contains a phytic acid-metal chelate shell.