Wood grain ceramic stable grain firing method

By introducing TiO₂ and plant ash into the glaze and adopting a segmented firing process, the problem of insufficient stability of the wood leaf pattern on ceramics was solved, achieving stable display and integrity of the wood leaf pattern and reducing the defect rate.

CN123131184APending Publication Date: 2026-11-20JIAN COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611314650.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The existing technology for wood-leaf pattern ceramics has insufficient stability in terms of pattern display, resulting in large fluctuations in the integrity and clarity of the wood-leaf pattern among ceramic products fired in the same kiln. Some products have defects such as incomplete leaf patterns, blurred leaf veins, and leaf shape erosion and disappearance.

Method used

Using a glaze containing TiO₂ and plant ash, combined with a segmented firing process including a low-temperature drainage section, a medium-temperature melting section, and a high-temperature texture development section, the bonding reaction between leaf ash and the glaze surface is controlled. Through the formation of glaze crystal phases and interfacial bonding reactions, the stable display of wood and leaf texture is ensured.

Benefits of technology

It improves the bonding stability of leaf patterns, reduces the incompleteness rate of leaf patterns, ensures clear and continuous boundaries of leaf textures, and reduces leaf pattern loss and vein breakage caused by poor bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131184A_ABST
    Figure CN123131184A_ABST
Patent Text Reader

Abstract

The application discloses a wood leaf pattern ceramic stable pattern showing firing method, which comprises the following steps: preparing glaze, mixing TiO2 and plant ash to prepare glaze slurry by adding water; applying the glaze slurry on the ceramic body to form a bottom glaze layer; attaching leaves with pretreatment and surface coating of glaze slurry on the bottom glaze layer; putting the ceramic body with leaves into a kiln for firing, which comprises a low-temperature drainage section, a medium-temperature melting section and a high-temperature pattern showing section; the temperature range of the low-temperature drainage section is room temperature to 600 DEG C; the temperature range of the medium-temperature melting section is 600 DEG C to 1000 DEG C and comprises a 1000 DEG C holding section; the temperature range of the high-temperature pattern showing section is 1000 DEG C to 1260 DEG C and comprises a 1260 DEG C holding section; and cooling after the firing is completed. Thus, the combination stability of wood leaf ash and glaze surface can be effectively improved during the firing process, so that the defect rate of wood leaf pattern decoration is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the technical field of ceramic firing, and in particular to a method for firing ceramics with stable wood-leaf texture. Background Technology

[0002] Wood-leaf porcelain is the most representative variety of Jizhou kiln. It is made by placing natural leaves on a ceramic body covered with black glaze after processing, and firing it at high temperature once. The leaves are ashed in the glaze but the leaf shape is retained. The ash accumulation forms a wood-leaf pattern with leaf stem and vein texture, which has high artistic value.

[0003] In related technologies, the preparation of wood-leaf pattern ceramics usually involves applying a black glaze as a base color to the surface of the ceramic body, followed by high-temperature firing to ash the leaves, leaving leaf-shaped traces on the glaze surface. However, this preparation method faces the problem of insufficient pattern stability in actual production. Specifically, the integrity and clarity of the wood-leaf pattern vary greatly among ceramic products fired in the same kiln. Some products exhibit defects such as incomplete leaf patterns, blurred leaf veins, and the disappearance of leaf shapes due to burning. The formation of wood-leaf patterns involves the ashing process of leaves at high temperatures. The bonding state between the leaf ash and the glaze layer during this process directly determines the final pattern presentation effect. Since the composition of leaves varies with tree species, leaf maturity, and growth environment, their ashing behavior at high temperatures and the interaction between ash and the glaze surface are difficult to control precisely, resulting in a large degree of uncertainty in the pattern presentation effect. Summary of the Invention

[0004] This application aims to at least partially address one of the technical problems in the related art.

[0005] Therefore, one objective of this application is to provide a stable firing method for wood leaf pattern ceramics, which can effectively improve the bonding stability between wood leaf ash and glaze during the firing process, thereby reducing the defect rate of wood leaf pattern decoration.

[0006] To achieve the above objectives, the first aspect of this application proposes a method for firing ceramics with stable leaf-pattern texture, comprising the following steps:

[0007] S1. Prepare the glaze by mixing raw materials containing TiO2 and plant ash and adding water to obtain the glaze slurry.

[0008] S2. Apply the glaze slurry onto the ceramic body to form a base glaze layer;

[0009] S3. Attach the pretreated leaves, whose surfaces are coated with glaze slurry, onto the base glaze layer;

[0010] S4. The ceramic body with the attached leaves is fired in a kiln. The firing process includes a low-temperature drainage section, a medium-temperature melting section, and a high-temperature texture development section. The temperature range of the low-temperature drainage section is room temperature to 600°C. The temperature range of the medium-temperature melting section is 600°C to 1000°C and includes a 1000°C holding section. The temperature range of the high-temperature texture development section is 1000°C to 1260°C and includes a 1260°C holding section.

[0011] S5. Cool after firing.

[0012] In addition, the method for stabilizing and firing wood-leaf pattern ceramics according to the above-mentioned method proposed in this application may also have the following additional technical features:

[0013] In one embodiment of this application, in step S1, the glaze is composed of the following components by mass fraction: 55wt% potassium feldspar, 6wt% kaolin, 13wt% talc, 10wt% quartz, 5wt% limestone, 8wt% Fe2O3, 1wt% TiO2, and 2wt% plant ash.

[0014] In one embodiment of this application, in step S4, firing is performed according to the following temperature curve: heating from room temperature to 300°C for 100 min; heating from 300°C to 600°C for 120 min; heating from 600°C to 900°C for 120 min; heating from 900°C to 1000°C for 30 min; holding at 1000°C for 60 min; heating from 1000°C to 1200°C for 120 min; heating from 1200°C to 1260°C for 60 min; and holding at 1260°C for 40 min.

[0015] In one embodiment of this application, the leaves are mulberry leaves, and the pretreatment includes: picking mature leaves from the middle of the mulberry tree, steaming them with boiling water for 3 to 8 minutes, then pressing them flat with a plate in a cool and ventilated place and drying them until the leaves are completely dehydrated and flat.

[0016] In one embodiment of this application, the preprocessing further includes: classifying and grouping the leaves according to the age of the mulberry tree and the tenderness of the leaves, and grouping the leaves of the same age and tenderness into the same group;

[0017] The age of the mulberry trees is classified as follows: 1 to 3 years old is the young tree grade, 5 to 15 years old is the mature tree grade, and 20 years and above is the old tree grade.

[0018] The maturity of the leaves is classified as follows: newly sprouted shoots at the top of the mulberry tree that have not yet fully unfolded are classified as young leaves; fully unfolded leaves in the middle of the mulberry tree that are dark green and have a flexible texture are classified as mature leaves; and leaves near the base of the mulberry tree near the petiole that are dark in color and have a hard and brittle texture are classified as old leaves.

[0019] In one embodiment of this application, the thickness of the base glaze layer is 0.2 mm to 0.5 mm, and the glaze-containing slurry is the glaze.

[0020] In one embodiment of this application, a top glaze application step is included before step S4: a top glaze is applied to the surface of the base glaze layer and the leaf to form a decorative surface layer, the top glaze having the same composition as the glaze, and the thickness of the decorative surface layer being 0.2 mm to 0.5 mm.

[0021] In one embodiment of this application, a bisque firing step is included before step S2: the shaped and air-dried ceramic blank is placed in a bisque firing at 850°C and then cooled.

[0022] In one embodiment of this application, before step S1, there is a step of adding TiO2 to the blank of the ceramic body, wherein the mass fraction of TiO2 in the blank is 1 wt%.

[0023] A second aspect of this application provides a ceramic product with a wood-leaf pattern, which is obtained by firing using the above method. The product comprises:

[0024] Ceramic body;

[0025] A base glaze layer covers the surface of the ceramic body;

[0026] The leaf texture layer is located on the base glaze layer. The leaf texture layer has leaf stem and vein textures, which protrude 0.2 mm to 1 mm from the surface of the base glaze layer.

[0027] A decorative surface layer covers the surface of the base glaze layer and the leaf texture layer.

[0028] Compared with the prior art, this application has at least the following beneficial effects:

[0029] 1. This application introduces TiO2 into the glaze and allows TiO2 to coexist with Fe2O3 and plant ash in a specific ratio. During the high-temperature firing process, TiO2 participates in the formation of the glaze crystal phase and can regulate the surface tension of the glaze at high temperatures. When leaf ash comes into contact with the glaze, the glaze system composed of the above components is conducive to a stable interfacial bonding reaction between the mineral components in the ash and the glaze layer. As a result, after the glaze is cured, it forms a clear, continuous and complete leaf vein texture, reducing leaf pattern loss and vein breakage caused by poor bonding between ash and glaze.

[0030] 2. This application achieves segmented control of the firing process by allowing the orderly removal of moisture and organic components from the body and glaze at a set heating rate during the low-temperature stage. This prevents bubbles and glaze cracking in the leaf pattern area due to excessively rapid volatile release. During the 1000℃ holding stage, the glaze enters a molten state at this temperature, allowing sufficient reaction time between the leaf ash and the glaze. This facilitates the initial spreading of the ash on the glaze and the formation of a stable interfacial bonding layer. During the 1260℃ holding stage, the glaze completes its final melting and solidification at this temperature, allowing the formed wood and leaf texture to be fixed in the glaze. This reduces leaf shape deformation and texture blurring caused by temperature fluctuations during firing.

[0031] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0032] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the following description of the embodiments taken in conjunction with the accompanying drawings, wherein:

[0033] Figure 1 This is a schematic flowchart of a method for firing a wood-leaf pattern ceramic according to an embodiment of this application.

[0034] Figure 2 This is a schematic diagram of the glaze formulation according to an embodiment of this application;

[0035] Figure 3 This is a schematic diagram of the firing temperature profile according to an embodiment of this application. Detailed Implementation

[0036] Embodiments of this application are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain this application, and should not be construed as limiting this application. Rather, embodiments of this application include all variations, modifications, and equivalents falling within the spirit and scope of the appended claims.

[0037] The following describes a method for firing a wood-leaf pattern ceramic with stable texture according to an embodiment of this application, with reference to the accompanying drawings.

[0038] like Figures 1-3As shown in the embodiment of this application, a method for stable firing of leaf-patterned ceramics is based on the coordination of glaze composition and firing regime. In terms of glaze, TiO2 and plant ash are introduced as necessary components to give the glaze suitable physicochemical properties during high-temperature firing, which is conducive to the formation of a stable bonding interface between the leaf ash and the glaze layer. In terms of firing regime, the firing process is controlled in stages, and a firing curve including a low-temperature drainage stage, a medium-temperature melting stage and a high-temperature pattern-developing stage is set. A heat preservation stage is set in the medium-temperature stage and the high-temperature stage respectively, so that the reaction between the leaf ash and the glaze layer proceeds in an orderly manner and is finally shaped.

[0039] In one embodiment of this application, when preparing the glaze, solid raw materials containing TiO2 and plant ash are weighed and mixed according to the formula ratio, and an appropriate amount of water is added (for example, the amount of water added is 80wt% to 120wt% of the total mass of the solid raw materials). The components are fully mixed and the required fineness is achieved by wet ball milling. The slurry after ball milling is sieved to remove coarse particles that are not fully ground, and then iron removal treatment is performed to remove iron impurities in the slurry. Finally, the slurry is left to stand and age to fully homogenize the components in the slurry, thus obtaining the glaze slurry.

[0040] TiO2 participates in the formation of glaze crystal phases during high-temperature firing and can regulate the surface tension of the glaze at high temperatures. When leaf ash comes into contact with the glaze, it facilitates a stable interfacial bonding reaction between the mineral components in the ash and the glaze layer. Plant ash, as a fluxing component, can regulate the melting temperature range of the glaze.

[0041] In some embodiments, the glaze is composed of the following components by mass fraction: 55wt% potassium feldspar, 6wt% kaolin, 13wt% talc, 10wt% quartz, 5wt% limestone, 8wt% Fe2O3, 1wt% TiO2, and 2wt% plant ash. The above solid components are weighed and mixed according to the mass fraction, water is added, and the mixture is ball-milled, sieved, iron removed, and aged to obtain the glaze slurry.

[0042] In some embodiments, the plant ash is sesame stalk ash. The sesame stalks are fully burned, the ash is collected, and the ash is sieved to remove coarse impurities (e.g., through a 200-mesh sieve) to obtain sesame stalk ash.

[0043] In some embodiments, TiO2 is added to the blank used to prepare the ceramic body before the glaze is prepared, and the mass fraction of TiO2 in the blank is 1 wt%.

[0044] Specifically, TiO2 powder is added to the ceramic raw materials used to prepare the body at a mass fraction of 1 wt%. After conventional body preparation processes such as mixing and kneading, a body containing TiO2 is obtained. After shaping and air drying, it is used in the subsequent glazing process. Introducing TiO2 into the body can further adjust the interfacial bonding characteristics between the body and the glaze layer, which is beneficial to improving the glaze quality.

[0045] In one embodiment of this application, before applying the base glaze, the shaped and air-dried ceramic blank is placed in a kiln and heated to 850°C for bisque firing. After bisque firing, the ceramic blank is removed from the kiln and cooled to obtain the bisque-fired ceramic blank.

[0046] In some implementations, after bisque firing, the kiln power is turned off, allowing the ceramic blanks to cool naturally to room temperature before being removed from the kiln. Natural cooling with the kiln helps reduce thermal stress caused by rapid temperature changes in the blanks, thus lowering the risk of cracking.

[0047] In other embodiments, after bisque firing, the ceramic blank is removed from the kiln and left to cool naturally to room temperature in the air.

[0048] Bisque-fired ceramic bodies have high mechanical strength, which can reduce the risk of cracking and deformation during subsequent glazing and firing. In addition, the bisque-firing process allows some organic impurities in the body to be removed in advance, which helps to reduce the impact of volatiles on the glaze quality during the high-temperature firing stage.

[0049] In one embodiment of this application, after bisque firing, the prepared glaze is applied to the ceramic body to form a base glaze layer. The glazing method can be immersion glazing, in which the ceramic body is immersed in the glaze slurry so that the glaze adheres to the surface of the body. After removal, the thickness of the base glaze layer is adjusted by controlling the immersion time or the glaze concentration. Alternatively, conventional glazing methods such as pouring or spraying glaze can be used, as long as a uniform base glaze layer can be formed on the surface of the body.

[0050] In some embodiments, the thickness of the base glaze layer is controlled to be between 0.2 mm and 0.5 mm. Within this thickness range, the glaze layer can form a uniform glaze surface during subsequent firing, which can provide sufficient reaction medium for the leaf ash without causing glaze run-through or obscuring leaf vein details due to excessive glaze thickness.

[0051] In one embodiment of this application, the leaves need to be pretreated before being attached to give them a suitable shape for firing and a dehydrated state.

[0052] In some implementations, mulberry leaves are selected. When picking mulberry leaves, mature leaves from the middle part of the mulberry tree are selected, while overly tender shoots and leaves from the top of the tree and overly coarse old leaves from the base are discarded. Mature leaves from the middle part have moderate fiber density and thickness, which can retain relatively clear leaf vein texture after high-temperature firing. After picking, the leaves are steamed in time to avoid excessive water loss and cracking.

[0053] When steaming, the picked mulberry leaves are steamed with boiling water for 3 to 8 minutes. The steaming time can be selected according to the thickness of the leaves: thinner leaves can be steamed for a shorter time, such as 3 to 5 minutes; thicker leaves can be steamed for a longer time, such as 5 to 8 minutes.

[0054] Steaming inactivates and kills the greening of the leaves, stops the biochemical reaction, removes some chlorophyll, and softens the fibrous tissue. After steaming, the leaves are quickly removed to avoid simmering.

[0055] When drying, place the steamed mulberry leaves in a cool and ventilated place to air dry, avoiding strong sunlight. During the drying process, cover the leaves with a pressing board to flatten them and prevent them from curling and wrinkling. Dry until the leaves are completely dehydrated, crisp, flat, and with intact veins.

[0056] In some embodiments, during drying, the steamed mulberry leaves are stacked neatly in groups of 10 to 15, with thin paper separating each group of leaves to absorb excess moisture and prevent the leaves from sticking together. A pressure plate is then placed on top of the stacked leaves to apply uniform pressure, and the leaves are left to stand in a cool, ventilated place until they are completely dehydrated. This method of stacking, pressing, and drying allows for the simultaneous processing of multiple leaves while maintaining the flatness of each leaf, thus improving pretreatment efficiency.

[0057] In some implementations, during the pretreatment process, the leaves can be graded and grouped according to the age of the mulberry tree and the maturity of the leaves. The specific grading methods are as follows:

[0058] Regarding the grading of mulberry tree age, mulberry trees can be divided into three grades: saplings, mature trees, and old trees. Saplings refer to mulberry trees aged 1 to 3 years. At this age, mulberry trees are in a period of vigorous growth, with relatively thin leaves and underdeveloped leaf veins and fibers, resulting in shallow textures after firing. Mature trees refer to mulberry trees aged 5 to 15 years. At this age, mulberry trees tend to grow more steadily, with moderately thick leaves, strong leaf veins, and uniform fiber density, resulting in clear and complete leaf vein textures after firing. Old trees refer to mulberry trees aged 20 years or older. At this age, mulberry trees tend to grow more slowly, with thick and coarse leaf fibers and a harder texture, resulting in heavy textures after firing. During harvesting, leaves from mulberry trees of different ages are collected separately according to the above age grades, and the corresponding age grade of each batch of leaves is recorded.

[0059] Regarding the grading of leaf maturity, leaves can be divided into three grades: tender leaves, mature leaves, and old leaves. Tender leaves refer to the newly sprouted shoots at the top of the mulberry tree that have not yet fully unfolded. These leaves have thin leaf tissue and fine veins, and are easily completely burned during firing, leaving no clear texture. Mature leaves refer to the fully unfolded leaves in the middle of the mulberry tree, with a dark green color and a flexible texture. These leaves have thick veins and moderate leaf tissue thickness, and after firing, the vein texture is clear and the leaf shape is intact. Old leaves refer to the old, hard leaves near the base of the mulberry tree, with a dark color and a hard and brittle texture. These leaves have thick fibers and a higher ash temperature, resulting in a heavy texture after firing, but are prone to scorching. During harvesting, leaves from different parts are collected separately according to the above maturity grades, and the maturity grade corresponding to each batch of leaves is recorded.

[0060] During grading and sorting, leaves of the same tree age and maturity level are grouped into the same group. For example, mature leaves from mature trees (5 to 15 years old) are grouped into group A, mature leaves from old trees (over 20 years old) are grouped into group B, and old leaves from mature trees are grouped into group C, and so on. The graded and sorted leaves are numbered and stored separately, and the tree age level, maturity level, harvest date and plant number of each group of leaves are recorded so that leaves of the same grade can be selected in the subsequent firing process. Since the difference in tree age and maturity of leaves directly affects the density of leaf vein fibers and ash composition, grading is beneficial to improving the consistency of wood and leaf patterns in the same batch of products.

[0061] Before actual production, the combination of blade grades with the best texture effect can be selected from the above-mentioned grade groups through comparative firing tests.

[0062] Specifically, leaves of different grades are attached to the same batch of glazed blanks and fired in the same kiln and kiln position under the same firing system. After firing, the integrity of the veins, the clarity of the texture, and the retention of the leaf shape of each group of leaves are compared, and the grade group with the best effect is selected as the leaf selection standard for formal production.

[0063] Select leaves that have undergone the above pretreatment, coat the leaf surface with a glaze slurry, and then attach the glaze-coated leaves to the base glaze layer. When attaching, make sure that the back or front of the leaf is in contact with the base glaze layer. Gently press to ensure close contact between the leaf and the base glaze layer, avoiding air bubbles. The glaze slurry coated on the leaf surface can adjust the interface state between the leaf ash and the base glaze layer during the firing process, which is beneficial to the bonding of the ash and the glaze.

[0064] In some embodiments, the glaze-containing paste applied to the surface of the leaves is the aforementioned prepared glaze.

[0065] In one embodiment of this application, after placing the leaves and before firing, a top glaze is applied to the surface of the base glaze layer and the leaves to form a decorative surface layer covering the base glaze layer and the leaves.

[0066] In some embodiments, the top glaze and the base glaze have the same composition, that is, by mass fraction, the top glaze consists of the following components: 55wt% potassium feldspar, 6wt% kaolin, 13wt% talc, 10wt% quartz, 5wt% limestone, 8wt% Fe2O3, 1wt% TiO2, and 2wt% plant ash.

[0067] When applying the surface glaze, an immersion method can be used, in which the ceramic body with the leaves attached is immersed in the surface glaze slurry, so that the surface glaze is evenly covered on the surface of the base glaze layer and the exposed surface of the leaves. After immersion, the speed at which the body is removed from the glaze slurry is controlled to ensure that the surface glaze flows evenly and avoids excessive accumulation of glaze in certain areas.

[0068] In some embodiments, the thickness of the decorative surface layer is controlled to be 0.2 mm to 0.5 mm. Within this thickness range, the glaze layer can provide complete coverage and protection for the base glaze layer and the leaves without excessively obscuring the texture effect formed after the leaves are ashed. During the firing process, the glaze layer accumulates along with the leaf shape, forming a three-dimensional leaf vein texture together with the leaf ash.

[0069] In one embodiment of this application, after completing the above steps, the ceramic body with attached leaves is fired in a kiln. The firing process includes a low-temperature drainage section, a medium-temperature melting section, and a high-temperature texture development section. The temperature range of the low-temperature drainage section is room temperature to 600°C. During this stage, the moisture and organic components in the body and glaze are gradually discharged. The temperature range of the medium-temperature melting section is 600°C to 1000°C and includes a 1000°C holding section. During this stage, the glaze enters a molten state. The temperature range of the high-temperature texture development section is 1000°C to 1260°C and includes a 1260°C holding section. During this stage, the leaf texture is formed in the glaze.

[0070] It should be noted that in the above firing curve, the heating stage from room temperature to 600°C corresponds to the low-temperature drainage stage, and the heating stages from room temperature to 300°C and from 300°C to 600°C are both components of the low-temperature drainage stage.

[0071] The heating stage from 600℃ to 1000℃ (including the heating sections from 600℃ to 900℃ and from 900℃ to 1000℃) and the holding stage at 1000℃ correspond to the medium-temperature melting stage. That is, the medium-temperature melting stage includes not only the holding stage at 1000℃, but also the entire heating process from 600℃ to 1000℃.

[0072] The heating stage from 1000℃ to 1260℃ (including the heating sections from 1000℃ to 1200℃ and from 1200℃ to 1260℃) and the holding stage at 1260℃ correspond to the high-temperature texture development stage. That is, the high-temperature texture development stage includes not only the holding stage at 1260℃, but also the entire heating process from 1000℃ to 1260℃.

[0073] In some implementations, firing is carried out according to the following temperature profile:

[0074] The temperature was increased from room temperature to 300℃ in 100 minutes; from 300℃ to 600℃ in 120 minutes; from 600℃ to 900℃ in 120 minutes; from 900℃ to 1000℃ in 30 minutes; and held at 1000℃ for 60 minutes. The temperature was increased from 1000℃ to 1200℃ in 120 minutes; from 1200℃ to 1260℃ in 60 minutes; and held at 1260℃ for 40 minutes.

[0075] In the above firing curve, the heating stage from room temperature to 600℃ corresponds to the low-temperature drainage stage. The total heating time in this stage is 220 min (100 min from room temperature to 300℃ and 120 min from 300℃ to 600℃). The average heating rate is relatively slow, which is conducive to the gradual discharge of moisture and organic components in the body and glaze, and avoids the rapid precipitation of water vapor and volatiles due to excessive heating, which may lead to the formation of bubbles in the glaze or cracking of the glaze surface.

[0076] The heating stage from 600℃ to 1000℃ and the holding stage at 1000℃ correspond to the medium-temperature melting section. The heating time from 600℃ to 900℃ is 120 minutes, the heating time from 900℃ to 1000℃ is 30 minutes, and the holding time at 1000℃ is 60 minutes. During this stage, the glaze gradually melts, and the leaves complete the ashing process within this temperature range. The mineral components in the ash come into full contact with the molten glaze layer during the holding stage and undergo an interfacial reaction, initially spreading on the glaze surface and forming a bonding interface.

[0077] After holding at 1000℃, the temperature is raised to 1260℃ and held thereafter. This stage corresponds to the high-temperature texture development stage. The heating time from 1000℃ to 1200℃ is 120 minutes, the heating time from 1200℃ to 1260℃ is 60 minutes, and the holding time at 1260℃ is 40 minutes. In this stage, the viscosity of the glaze is further reduced at a higher temperature, and the final melting is completed. The interface between the ash and the glaze layer tends to stabilize during this process. After holding at 1260℃, the wood leaf texture that has been formed is solidified and shaped in the glaze.

[0078] In some implementations, firing is carried out in an electric kiln, which can precisely control the heating rate and holding temperature at each stage. This helps to improve the reproducibility of the firing process and the consistency of products between different firing cycles, and avoids the adverse effects of temperature fluctuations caused by insufficient kiln temperature control precision on the wood leaf patterns.

[0079] In one embodiment of this application, after firing, the ceramic body is cooled to room temperature. The cooling method can be natural cooling with the kiln, that is, after firing, the power supply to the kiln is turned off, and the kiln and the ceramic body inside it are allowed to cool down naturally to room temperature before being removed from the kiln. During the natural cooling process, the glaze gradually solidifies from a molten state to a glassy state, and the wood and leaf patterns maintain their fixed texture during this process.

[0080] The wood-leaf textured ceramic product obtained by the above method comprises a ceramic body, a base glaze layer, a wood-leaf texture layer, and a decorative surface layer. The base glaze layer covers the surface of the ceramic body and is formed by firing the aforementioned glaze containing TiO2 and plant ash at high temperature. It has a uniform base color and a suitable surface condition. The wood-leaf texture layer is located on the base glaze layer and has leaf stem and vein textures. After firing, the leaves are ashed at high temperature, and the ash accumulates on the surface of the base glaze layer, combining with the glaze layer to form a wood-leaf texture layer with leaf stem and vein textures. The leaf ash and the surface glaze layer accumulate at the leaf vein positions according to the leaf shape, so that the leaf stem and vein textures protrude from the surface of the base glaze layer by 0.2mm to 1mm. The decorative surface layer covers the surface of the base glaze layer and the wood-leaf texture layer, covering and protecting the wood-leaf texture layer, while making the surface of the product smooth and clean, with a distinct texture effect.

[0081] In summary, the method for firing stable leaf-patterned ceramics according to the embodiments of this application can effectively improve the bonding stability between leaf ash and glaze during the firing process, thereby reducing the defect rate of leaf-patterned decorations.

[0082] In the description of this specification, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0083] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0084] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. A method for firing ceramics with stable leaf-like patterns, characterized in that, Includes the following steps: S1. Prepare the glaze by mixing raw materials containing TiO2 and plant ash and adding water to obtain the glaze slurry. S2. Apply the glaze slurry onto the ceramic body to form a base glaze layer; S3. Attach the pretreated leaves, whose surfaces are coated with glaze slurry, onto the base glaze layer; S4. The ceramic body with the attached leaves is fired in a kiln. The firing process includes a low-temperature drainage section, a medium-temperature melting section, and a high-temperature texture development section. The temperature range of the low-temperature drainage section is room temperature to 600°C. The temperature range of the medium-temperature melting section is 600°C to 1000°C and includes a 1000°C holding section. The temperature range of the high-temperature texture development section is 1000°C to 1260°C and includes a 1260°C holding section. S5. Cool after firing.

2. The method for stable firing of wood-leaf texture ceramics according to claim 1, characterized in that, In step S1, the glaze is composed of the following components by mass fraction: 55wt% potassium feldspar, 6wt% kaolin, 13wt% talc, 10wt% quartz, 5wt% limestone, 8wt% Fe2O3, 1wt% TiO2, and 2wt% plant ash.

3. The method for stabilizing and firing wood-leaf textured ceramics according to claim 1, characterized in that, In step S4, firing is performed according to the following temperature curves: temperature rises from room temperature to 300℃ for 100 min; temperature rises from 300℃ to 600℃ for 120 min; temperature rises from 600℃ to 900℃ for 120 min; temperature rises from 900℃ to 1000℃ for 30 min; temperature is held at 1000℃ for 60 min; temperature rises from 1000℃ to 1200℃ for 120 min; temperature rises from 1200℃ to 1260℃ for 60 min; temperature is held at 1260℃ for 40 min.

4. The method for stabilizing and firing wood-leaf textured ceramics according to claim 1, characterized in that, The leaves are mulberry leaves. The pretreatment includes: picking mature leaves from the middle of the mulberry tree, steaming them with boiling water for 3 to 8 minutes, then pressing them flat with a plate in a cool and ventilated place and drying them until the leaves are completely dehydrated and flat.

5. The method for firing stable leaf-patterned ceramics according to claim 4, characterized in that, The preprocessing also includes: classifying and grouping the leaves according to the age of the mulberry tree and the tenderness of the leaves, and grouping the leaves of the same age and tenderness into the same group; The age of the mulberry trees is classified as follows: 1 to 3 years old is the young tree grade, 5 to 15 years old is the mature tree grade, and 20 years and above is the old tree grade. The maturity of the leaves is classified as follows: newly sprouted shoots at the top of the mulberry tree that have not yet fully unfolded are classified as young leaves; fully unfolded leaves in the middle of the mulberry tree that are dark green and have a flexible texture are classified as mature leaves; and leaves near the base of the mulberry tree near the petiole that are dark in color and have a hard and brittle texture are classified as old leaves.

6. The method for stabilizing and firing wood-leaf textured ceramics according to claim 1, characterized in that, The thickness of the base glaze layer is 0.2 mm to 0.5 mm, and the glaze-containing slurry is the glaze material.

7. The method for firing stable leaf-patterned ceramics according to claim 1, characterized in that, Before step S4, a top glaze application step is also included: applying a top glaze to the surface of the base glaze layer and the leaf to form a decorative surface layer, wherein the top glaze has the same composition as the glaze and the thickness of the decorative surface layer is 0.2 mm to 0.5 mm.

8. The method for stable firing of wood-leaf texture ceramics according to claim 1, characterized in that, Before step S2, there is also a bisque firing step: the shaped and air-dried ceramic blank is placed at 850°C for bisque firing and then cooled.

9. The method for stabilizing and firing wood-leaf pattern ceramics according to claim 1, characterized in that, Before step S1, there is also a step of adding TiO2 to the blank of the ceramic body, wherein the mass fraction of TiO2 in the blank is 1 wt%.

10. A ceramic product with a wood-leaf pattern, characterized in that, The article is obtained by firing according to any one of claims 1 to 9, and comprises: Ceramic body; A base glaze layer covers the surface of the ceramic body; The leaf texture layer is located on the base glaze layer. The leaf texture layer has leaf stem and vein textures, which protrude 0.2 mm to 1 mm from the surface of the base glaze layer. A decorative surface layer is applied over the surfaces of the base glaze layer and the leaf texture layer.