High modulus polyimide material for flexible display and preparation method thereof

By polymerizing aromatic cyclic diamines and nitrogen-containing heterocyclic diamines with fused-ring aromatic dianhydrides in a specific molar ratio, rigid planar molecular chains are formed, which solves the problem of creases in polyimide films during repeated bending, improves tensile strength and strain resistance, and maintains the flexibility and transparency of the material.

CN123131602APending Publication Date: 2026-11-20SUZHOU ZUNER PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611203213.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing polyimide films are prone to creases during repeated bending, and their strain resistance is insufficient, which affects the reliability and service life of flexible display devices. Moreover, existing methods often sacrifice transparency, flexibility, or elongation at break when improving the elastic modulus.

Method used

Aromatic cyclic diamines and nitrogen-containing heterocyclic diamines are polymerized with fused-ring aromatic dianhydrides in a specific molar ratio to form rigid planar molecular chains. The nitrogen-containing heterocyclic diamines guide the parallel orientation of the molecular chains, enhance the inter-chain interaction forces and aggregation density, prevent irreversible orientation rearrangement of the molecular chains when bent, and improve the elastic modulus and strain resistance.

Benefits of technology

It significantly improves the tensile strength and strain resistance of polyimide films, prevents crease formation, maintains the flexibility and transparency of the material, and ensures that it maintains full elastic deformation during repeated bending.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application relates to the technical field of flexible display materials, in particular to a high-modulus polyimide material for flexible display and a preparation method thereof. The high-modulus polyimide material for flexible display is prepared by polymerization reaction of diamines and dianhydrides; the diamines comprise aromatic ring diamines and nitrogen-containing heterocyclic diamines; the dianhydrides comprise fused ring aromatic dianhydrides; and the molar ratio of the diamines and the dianhydrides is 1: (1-1.2). In order to effectively improve the bending fatigue resistance of the polyimide film and the comprehensive performance, the prepared high-modulus PI film material for flexible display has tensile strength, elastic modulus and elongation at break, and the elastic modulus ensures that the bending strain is in the elastic region and plastic deformation is not generated, so that the film can always keep complete elastic deformation in the repeated bending process, and slight creases are prevented from being generated and accumulated and deepened along the stress concentration direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of flexible display materials technology, specifically to high-modulus polyimide materials for flexible displays and their preparation methods. Background Technology

[0002] Polyimide (PI) films, due to their excellent thermal stability, mechanical properties, and chemical stability, have become an indispensable key material in the field of flexible displays. In flexible display devices, PI materials are mainly used as flexible substrates, cover plates, and substrate layers for touch panels. Traditional rigid display devices use glass as the substrate and cover material, but the thickness, weight, hardness, and fragility of glass cannot meet the demands of flexible displays for bendability and thinness. With the rapid development of flexible display products such as foldable smartphones, polyimide materials, with their excellent flexibility and foldability, have become the most promising material solution to replace glass. However, foldable display devices need to withstand tens of thousands or even hundreds of thousands of repeated bends in practical use, placing extremely high demands on the bending fatigue resistance of PI materials.

[0003] Existing polyimide films commonly exhibit crease problems during repeated bending. When the screen is repeatedly folded, the molecular chains in the PI substrate undergo irreversible orientation rearrangement under cyclic stress, leading to accumulated plastic deformation and deformation memory, ultimately forming visible creases in the bending area. Once formed, these creases deepen continuously, severely impacting the reliability and lifespan of the display. The essence of the crease problem lies in the insufficient strain resistance of the PI material. Therefore, improving the elastic modulus of the PI film is key to solving the crease problem at the material level. However, improving the elastic modulus of existing polyimide materials often comes at the cost of sacrificing transparency, flexibility, or elongation at break. How to significantly improve the elastic modulus and bending fatigue resistance of PI films while maintaining their good overall performance has become a pressing technical challenge in the field of flexible display materials. Summary of the Invention

[0004] In order to effectively improve the above-mentioned problems of polyimide, this application provides a high-modulus polyimide material for flexible display and a method for preparing the same.

[0005] This application provides a high-modulus polyimide material for flexible displays and a method for preparing the same, using the following technical solution: A high-modulus polyimide material for flexible displays is prepared by polymerization of a diamine and a dianhydride; the diamine includes aromatic cyclic diamines and nitrogen-containing heterocyclic diamines; the dianhydride includes fused-ring aromatic dianhydrides; and the molar ratio of the diamine to the dianhydride is 1:(1-1.2).

[0006] In this application, the aromatic ring of the aromatic ring diamine has an all-carbon conjugated structure. After polymerization, the imide ring formed is coplanar with the aromatic ring, giving the entire repeating unit a rigid planar configuration and endowing the molecular chain with a rigid backbone. The nitrogen-containing heterocyclic diamine guides the parallel orientation of the molecular chain. The rigid backbone ensures that the molecular chain remains straight under stress and does not undergo segmental rotation. The parallel orientation causes multiple molecular chains to align in the same direction in the aggregated state. The combination of the aromatic ring diamine and the nitrogen-containing heterocyclic diamine increases the elastic modulus, reduces the free volume, and ensures uniform stress transmission. The increased elastic modulus reduces bending strain, thus preventing irreversible orientation rearrangement of the molecular chain and preventing [further stress]. To prevent creases, the reduced free volume requires higher thermal energy for chain segment movement, thus increasing the glass transition temperature. Furthermore, the polymerization of fused-ring aromatic dianhydrides with the two diamines further strengthens the rigid framework and regular arrangement of the molecular chains, making it less prone to conformational changes and relative slippage during bending, thereby further improving resistance to plastic deformation. The proportions of diamines and dianhydrides in this application ensure a high degree of polymerization, resulting in high molecular weight polyimide. This leads to entanglement between molecular chains, reducing structural defects caused by oligomer or end-group enrichment, thereby avoiding stress concentration and significantly improving the tensile strength of the film.

[0007] Preferably, the aromatic cyclic diamine is selected from at least one of m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, benzidine, and 2,6-naphthyldiamine.

[0008] Preferably, the nitrogen-containing heterocyclic diamine is selected from at least one of 4,4'-(pyrimidin-2,5-diyl)diphenylamine, 2-(4-aminophenyl)-5-aminobenzoxazole, 2-(4-aminophenyl)-5-aminobenzimidazole, and 1,3,5-triazine-2,4-diamine.

[0009] Preferably, the nitrogen-containing heterocyclic diamines are 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2.

[0010] Preferably, the aromatic cyclic diamine is p-phenylenediamine; More preferably, the molar ratio of aromatic cyclic diamine to nitrogen-containing heterocyclic diamine is 1:(2-2.5).

[0011] This application uses p-phenylenediamine as the aromatic cyclic diamine to provide the intrinsic rigid framework of the molecular chain. Its molecular structure has the characteristics of monocyclic symmetry. After polymerization, the imide ring formed is coplanar with the benzene ring, giving the molecular chain a rigid linear rod-like configuration. Moreover, the molecular chain has no additional side groups or linking groups, so it can be arranged with minimal spatial distance in the aggregated state, providing the basic elastic modulus and deformation resistance of the film. On this basis, a nitrogen-containing heterocyclic structure is introduced through a nitrogen-containing heterocyclic diamine. This structure provides electron-deficient centers for inter-chain dipole interaction and charge transfer complexation, thereby enhancing the inter-chain interaction force and aggregation density. The effective orientation chain ratio and film uniformity are further improved, and the stress is uniformly transmitted along the molecular chain direction to prevent the generation of obvious stress concentration points, thereby significantly improving the tensile strength and strain resistance of the polyimide material.

[0012] In this study, 4,4'-(pyrimidin-2,5-diyl)diphenylamine was introduced into nitrogen-containing heterocyclic diamines. Its pyrimidine ring contains two symmetrically distributed nitrogen atoms, and the molecular polarity is concentrated along a specific direction, exerting a specific directional constraint on adjacent molecular chains. This prevents the molecular chains from deviating from their original orientation when subjected to bending stress, thus maintaining the proportion of effectively oriented chains without decreasing with increasing bending cycles. The triazine ring of 1,3,5-triazine-2,4-diamine contains three uniformly distributed nitrogen atoms, which act as interchain dipole interaction sites, increasing the aggregation density between molecular chains and enhancing their ability to withstand bending stress. Under stress, interchain relative displacement is less likely to occur, thus further enhancing the ability to suppress interchain slip. Furthermore, the nitrogen-containing heterocyclic diamine complex ensures that the molecular chains maintain their original orientation after repeated bending, preventing rearrangement and further enhancing the ability to suppress interchain slip. This significantly increases the elastic modulus of the film, reducing strain during bending, preventing plastic deformation, and dispersing stress. Consequently, the tensile strength of the polyimide film material is significantly improved, and it exhibits high consistency under external force, maintaining a high elongation at break. This ensures that the film maintains fully elastic deformation during repeated bending, avoiding creases. Therefore, if the aromatic ring diamine content is too low, insufficient rigid framework support leads to a decrease in overall molecular chain rigidity, resulting in a lower elastic modulus and glass transition temperature. If the nitrogen-containing heterocyclic diamine content is too low, the interchain dipole constraint is reduced, making the molecular chains prone to relative slip and orientation deflection during bending, thus lowering the elastic modulus.

[0013] Preferably, the fused-ring aromatic dianhydride includes 1,4,5,8-naphthalenetetracarboxylic anhydride.

[0014] 1,4,5,8-Naphthalenetetracarboxylic anhydride has a fully coplanar structure of two fused benzene rings. After polymerization, the coplanarity of the imide ring and the naphthalene ring makes the entire repeating unit present a rigid planar configuration, which significantly enhances the rigidity and aromaticity of the molecular chain backbone, thereby improving the rigidity of the single chain. The electron-rich fused ring structure of the naphthalene ring forms a charge transfer complexation effect with the electron-deficient heterocycle of the nitrogen-containing heterocyclic diamine, which enhances the interaction force between molecular chains and thus improves the ability to inhibit interchain slippage. This significantly improves the elastic modulus and tensile strength of the film and prevents cumulative creases.

[0015] Secondly, this application provides a method for preparing high-modulus polyimide materials for flexible displays, employing the following technical solution: The preparation method of high-modulus polyimide material for flexible displays includes the following steps: under nitrogen protection, diamine and solvent are mixed evenly, then dianhydride is added, the reaction temperature is adjusted to 20-25℃, the reaction is carried out for 24-48 hours, filtered, cast into a film, vacuum treated, gradient cured, and naturally cooled and annealed to room temperature to obtain polyimide material.

[0016] Preferably, the solvent is selected from at least one of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide.

[0017] Preferably, the gradient curing process involves heating at 100-110℃ for 30-45 minutes, followed by a 20-30 minute increase to 180-200℃ for 30-45 minutes, and then a 60-80 minute increase to 400-450℃ for 30-45 minutes.

[0018] Preferably, the vacuum treatment conditions are a vacuum degree of 10-20 Pa, a temperature of 70-85℃, and a time of 1-2 h.

[0019] This application involves preparing the film through low-temperature polymerization, followed by slit coating and static film formation to achieve initial orientation of the molecular chains. Vacuum treatment prevents the formation of bubbles and micropores. The gradient curing process plays a key regulatory role in the final aggregated structure of the formed rigid molecular chains. Stepwise heating allows the molecular chains to gradually complete orientation and imidization ring closure at different temperature stages. Slow heating in the low-temperature stage allows residual solvent to be fully removed to avoid bubble formation and reduce internal defects in the film. In the medium-temperature stage, the molecular chains gain initial mobility and spontaneously orient along the film surface, thereby increasing the proportion of effectively oriented chains. In the high-temperature stage, the imidization reaction is fully carried out, and the molecular chains move further at high temperatures, correcting local orientation deviations and further improving the uniformity of the film. Ultimately, the internal defects of the film are reduced, the proportion of effectively oriented chains is increased, the film uniformity is improved, and the elastic modulus and tensile strength are enhanced.

[0020] In summary, this application includes at least one of the following beneficial technical effects: 1. By selecting diamines and dianhydrides within a specific molar ratio range for polymerization, the structural characteristics of polyimide molecular chains can be effectively controlled. The diamines are a combination of aromatic cyclic diamines and nitrogen-containing heterocyclic diamines. The aromatic ring of the aromatic cyclic diamine has a fully carbon conjugated structure. After polymerization, the imide ring formed is coplanar with the aromatic ring, giving the entire repeating unit a rigid planar configuration and endowing the molecular chain with a rigid skeleton. The nitrogen-containing heterocyclic diamine guides the parallel orientation of the molecular chain. The rigid skeleton ensures that the molecular chain remains straight under stress and does not undergo chain segment rotation. The parallel orientation allows multiple molecular chains to be arranged in the same direction in the aggregated state. The combination of aromatic cyclic diamines and nitrogen-containing heterocyclic diamines increases the elastic modulus, reduces the free volume, and ensures uniform stress transmission. The increase in elastic modulus reduces bending strain, thus preventing irreversible orientation rearrangement of the molecular chain and preventing creases.

[0021] 2. By introducing a nitrogen-containing heterocyclic structure through a nitrogen-containing heterocyclic diamine, the structure provides electron-deficient centers for interchain dipole interaction and charge transfer complexation, thereby enhancing the interchain interaction force and aggregation density. The effective proportion of oriented chains and the uniformity of the film material are further improved, and the stress is uniformly transmitted along the molecular chain direction to prevent the generation of obvious stress concentration points, thus significantly improving the tensile strength and strain resistance of polyimide materials. Detailed Implementation

[0022] All raw materials used in this application are commercially available. Example 1

[0023] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.018 mol of aromatic cyclic diamine and 0.036 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 h to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 min to level. After drying under vacuum at 20 Pa and 75℃ for 2 h, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2; the aromatic cyclic diamine was p-phenylenediamine. Example 2

[0024] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.027 mol of aromatic cyclic diamine and 0.027 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 h to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 min to level. After drying under vacuum at 20 Pa and 75℃ for 2 h, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2; the aromatic cyclic diamine was p-phenylenediamine. Example 3

[0025] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.0135 mol of aromatic cyclic diamine and 0.0405 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 h to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 min to level. After drying under vacuum at 20 Pa and 75℃ for 2 h, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2; the aromatic cyclic diamine was p-phenylenediamine. Example 4

[0026] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.018 mol of aromatic cyclic diamine and 0.036 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 hours to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 minutes to level. After drying under vacuum at 20 Pa and 75℃ for 2 hours, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 4:1; the aromatic cyclic diamine was p-phenylenediamine. Example 5

[0027] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.018 mol of aromatic cyclic diamine and 0.036 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25°C for 24 hours to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 minutes to level. After drying under vacuum at 75°C (20 Pa) for 2 hours, a gradient curing process (100°C / 30 min, 20 min to 180°C, 180°C / 30 min, 80 min to 450°C, 450°C / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamine was 4,4'-(pyrimidin-2,5-diyl)diphenylamine, and the aromatic cyclic diamine was p-phenylenediamine. Example 6

[0028] Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.018 mol of aromatic cyclic diamine and 0.036 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 h to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 min to level. After drying under vacuum at 20 Pa and 75℃ for 2 h, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2. The aromatic cyclic diamine is 1,5-naphthyldiamine.

[0029] Comparative Example 1 Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.054 mol of p-phenylenediamine was added and stirred for 30 min to disperse evenly. Next, 0.054 mol of 1,4,5,8-naphthalenetetracarboxylic anhydride was added, followed by 50 g of NMP. NMP was reacted at 25°C for 24 hours to obtain a polymer solution. The polymer solution was filtered and injected into a slot coating device. A clean glass plate was used as the coating carrier. The coating gap was set to 200 μm and the coating speed was 5 m / min. The wet film was uniformly extruded and coated, and allowed to stand at room temperature for 5 min to level. The film was dried under vacuum at 20 Pa and 75°C for 2 hours. Then, it was subjected to a gradient curing program (100°C / 30 min, 20 min to 180°C, 180°C / 30 min, 80 min to 450°C, 450°C / 30 min) for high-temperature treatment and then naturally cooled and annealed to room temperature. The glass plate with the film was immersed in deionized water to obtain a PI film with a thickness of 20 μm.

[0030] Comparative Example 2 Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.018 mol of aromatic cyclic diamine and 0.036 mol of nitrogen-containing heterocyclic diamine were added sequentially, and the mixture was stirred for 30 min to disperse evenly. Then, 0.054 mol of biphenyltetracarboxylic dianhydride was added, followed by 50 g of NMP. NMP was reacted at 25℃ for 24 h to obtain a polymerization solution. The solution was filtered and injected into a slot coating apparatus. A clean glass plate was used as the coating carrier, with a coating gap of 200 μm and a coating speed of 5 m / min. The solution was uniformly extruded to form a wet film, which was then allowed to stand at room temperature for 5 min to level. After drying under vacuum at 20 Pa and 75℃ for 2 h, a gradient curing process (100℃ / 30 min, 20 min to 180℃, 180℃ / 30 min, 80 min to 450℃, 450℃ / 30 min) was performed, followed by natural cooling and annealing to room temperature. The glass plate with the film was then immersed in deionized water to obtain a PI film with a thickness of 20 μm. The nitrogen-containing heterocyclic diamines were 4,4'-(pyrimidin-2,5-diyl)diphenylamine and 1,3,5-triazine-2,4-diamine in a molar ratio of 3:2; the aromatic cyclic diamine was p-phenylenediamine.

[0031] Comparative Example 3 Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring, followed by 0.054 mol of p-phenylenediamine, and the mixture was stirred for 30 min to disperse evenly. Then, 0.054 mol of biphenyltetracarboxylic dianhydride was added, followed by 50 g of NMP. The reaction was carried out at 25 °C for 24 h to obtain a polymerization solution. After filtration, the polymerization solution was injected into a slot coating device, using a clean glass plate as the coating carrier. The coating gap was set to 200 μm, and the coating speed was 5 m / m. The film is uniformly extruded and coated to form a wet film, and allowed to stand at room temperature for 5 minutes to level. It is then dried under vacuum at 20 Pa and 75°C for 2 hours, followed by a gradient curing process (100°C / 30 min, 20 min to 180°C, 180°C / 30 min, 80 min to 450°C, 450°C / 30 min) and naturally cooled to room temperature. The glass plate with the film is then immersed in deionized water to obtain a PI film with a thickness of 20 μm.

[0032] Comparative Example 4 Under nitrogen protection, 100 g of NMP was added to a 250 mL three-necked flask equipped with mechanical stirring. Then, 0.054 mol of 4,4'-(pyrimidin-2,5-diyl)diphenylamine was added and stirred for 30 min to disperse evenly. Next, 0.054 mol of biphenyltetracarboxylic dianhydride was added, followed by 50 g of NMP. NMP was reacted at 25°C for 24 hours to obtain a polymer solution. The polymer solution was filtered and injected into a slot coating device. A clean glass plate was used as the coating carrier. The coating gap was set to 200 μm and the coating speed was 5 m / min. The wet film was uniformly extruded and coated, and allowed to stand at room temperature for 5 min to level. The film was dried under vacuum at 20 Pa and 75°C for 2 hours. Then, it was subjected to a gradient curing program (100°C / 30 min, 20 min to 180°C, 180°C / 30 min, 80 min to 450°C, 450°C / 30 min) for high-temperature treatment and then naturally cooled and annealed to room temperature. The glass plate with the film was immersed in deionized water to obtain a PI film with a thickness of 20 μm.

[0033] The performance testing of the high-modulus PI thin film materials for flexible displays prepared in the examples and comparative examples was conducted using the following methods: (1) Tensile strength, elastic modulus, and elongation at break tests: Tensile strength was tested using Shimadzu AG-X plus, 1KN. The PI film was cut into rectangular strips of 20mm × 200mm along the casting direction, ensuring smooth edges, no gaps, and parallel sides. The samples were placed in an environment of 23±2℃ and 50±5%RH for at least 24 hours for conditioning. At least 5 points were measured in the effective area of ​​the sample using a micrometer, and the average value was taken as the sample thickness. The sample was installed in the fixture of the universal testing machine with an initial fixture spacing of 100mm. The sample was stretched at a tensile rate of 12.5mm / min until it broke. At least 5 samples were tested in each group, and the average value was taken. The stress-strain curve was recorded. The tensile strength was calculated by dividing the maximum force by the original cross-sectional area. The elastic modulus was calculated by the slope of the initial linear segment of the curve. The elongation at break was the percentage of the gauge length elongation at break divided by the original gauge length.

[0034] (2) Glass transition temperature (Tg) was measured using a dynamic mechanical analyzer (DMA850) under the following conditions: load of 0.05 N, heating rate of 5 °C / min, and measurement was conducted in a nitrogen atmosphere within a temperature range of 30–650 °C. The inflection point of the curve with the maximum value was recorded as the glass transition temperature. The comparison results are shown in Table 1 below: Table 1 Performance Test Results

[0035] The high-modulus PI thin film material for flexible displays prepared in this application has high tensile strength, elastic modulus, and elongation at break. The elastic modulus ensures that the bending strain is within the elastic zone and no plastic deformation occurs. The tensile strength ensures that stress concentration does not lead to the propagation of microcracks. The elongation at break ensures that the material has sufficient toughness and does not break brittlely. This satisfies the requirement that the film maintains complete elastic deformation during repeated bending, and prevents the formation of micro-creases that accumulate and deepen along the stress concentration direction.

[0036] Comparing Examples 1-6 and Comparative Example 1, it is evident that using 1,4,5,8-naphthalenetetracarboxylic anhydride as the dianhydride and p-phenylenediamine as the aromatic cyclic diamine provides the intrinsic rigid framework of the molecular chains, thus providing the basic elastic modulus and resistance to deformation of the film. The introduction of nitrogen-containing heterocyclic structures through nitrogen-containing heterocyclic diamines significantly improves the tensile strength and strain resistance of the polyimide material. An excessively high proportion of rigid framework increases the free volume between molecular chains, leading to a decrease in aggregation density and elastic modulus. When the content of nitrogen-containing heterocyclic diamines increases, the interchain dipole constraint between molecular chains strengthens, but if the proportion of rigid framework is too low, the overall rigidity of the molecular chains decreases, resulting in insufficient rigidity of individual chains. Simultaneously, excessive nitrogen-containing heterocycles increase the interchain spacing, further reducing the elastic modulus. The enhanced interchain constraint but insufficient framework rigidity makes the molecular chains more prone to stretching under stress, increasing the elongation at break. Compared with Example 4, the specific directional constraint effect of pyrimidine diamine is enhanced, but the multidirectional constraint effect of triazine diamine is weakened. The orientation stability of the molecular chain is improved when bent, but the ability to inhibit inter-chain slippage is reduced, the elastic modulus is reduced, and the elongation at break is increased.

[0037] Comparative Examples 1 and 2-4 show that the naphthalene ring of 1,4,5,8-naphthalenetetracarboxylic anhydride has a fully coplanar structure of two fused benzene rings. After polymerization, the coplanarity of the imide ring and the naphthalene ring makes the entire repeating unit present a rigid planar configuration, which significantly enhances the rigidity and aromaticity of the molecular chain backbone, thereby improving the rigidity of the single chain. The electron-rich fused ring structure of the naphthalene ring forms a charge transfer complexation effect with the electron-deficient heterocycle of the nitrogen-containing heterocyclic diamine, which enhances the interaction force between molecular chains, thereby improving the ability to inhibit interchain slippage, significantly improving the elastic modulus and tensile strength of the film, and preventing cumulative creases.

[0038] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A high-modulus polyimide material for flexible displays, characterized in that: The polyimide membrane material is prepared by polymerization of diamine and dianhydride; the diamine includes aromatic cyclic diamine and nitrogen-containing heterocyclic diamine; the dianhydride includes fused-ring aromatic dianhydride; the molar ratio of the diamine to the dianhydride is 1:(1-1.2).

2. The high-modulus polyimide material for flexible displays according to claim 1, characterized in that: The aromatic cyclic diamine is selected from at least one of m-phenylenediamine, p-phenylenediamine, 2,4-toluenediamine, benzidine, and 2,6-naphthyldiamine.

3. The high-modulus polyimide material for flexible displays according to claim 1, characterized in that: The nitrogen-containing heterocyclic diamine is selected from at least one of 4,4'-(pyrimidin-2,5-diyl)diphenylamine, 2-(4-aminophenyl)-5-aminobenzoxazole, 2-(4-aminophenyl)-5-aminobenzimidazole, and 1,3,5-triazine-2,4-diamine.

4. The high-modulus polyimide material for flexible displays according to claim 1, characterized in that: The molar ratio of the aromatic cyclic diamine and the nitrogen-containing heterocyclic diamine is 1:(2-2.5).

5. The high-modulus polyimide material for flexible displays according to claim 1, characterized in that: The fused-ring aromatic dianhydride includes 1,4,5,8-naphthalenetetracarboxylic anhydride.

6. A method for preparing the high-modulus polyimide material for flexible displays according to any one of claims 1-4, characterized in that, The process includes the following steps: under nitrogen protection, diamine and solvent are mixed evenly, then dianhydride is added, the reaction temperature is adjusted to 20-25℃, the reaction is carried out for 24-48 hours, filtered, cast into a film, vacuum treated, gradient cured, and naturally cooled and annealed to room temperature to obtain polyimide material.

7. The method for preparing high-modulus polyimide material for flexible displays according to claim 5, characterized in that: The solvent is selected from at least one of N-methyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide.

8. The method for preparing high-modulus polyimide material for flexible displays according to claim 5, characterized in that: The gradient curing process involves heating at 100-110℃ for 30-45 minutes, followed by a 20-30 minute increase to 180-200℃ for 30-45 minutes, and then a 60-80 minute increase to 400-450℃ for 30-45 minutes.

9. The high-modulus polyimide material for flexible displays according to claim 5, characterized in that: The vacuum treatment conditions are: vacuum degree 10-20 Pa, temperature 70-85℃, and time 1-2 h.