Cyan-containing polysiloxane resin and use thereof in gel polymer electrolytes
By preparing cyano-containing polysiloxane resins and constructing gel polymer electrolytes, the problems of low ion migration efficiency and interfacial instability in traditional electrolytes in lithium metal batteries are solved, achieving a balance between efficient ion transport and electrochemical stability, and improving the cycle stability and safety of the battery.
Patent Information
- Application Number
- CN202611229863.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional polymer-based electrolytes in lithium metal batteries suffer from low ion migration efficiency, interfacial instability, and difficulty in balancing structural design, making it difficult to achieve a balance between efficient ion transport and electrochemical stability.
A cyano-containing polysiloxane resin was prepared by hydrolysis and polycondensation reaction, and then mixed with a liquid electrolyte to form a gel polymer electrolyte by photocuring or thermal curing, thus constructing a three-dimensional cross-linked network structure.
It improves the dissociation degree and ion transport capacity of lithium salt, reduces the occurrence of side reactions, enhances the cycle stability and safety of the battery, and maintains high ionic conductivity.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the fields of organosilicon polymer materials and electrochemical energy materials, specifically to a cyano-containing polysiloxane resin, a gel polymer electrolyte constructed based on the resin, and its application in lithium metal batteries. Background Technology
[0002] With the development of lithium metal batteries, higher requirements have been placed on electrolyte systems in terms of ion transport performance, electrochemical stability, and interfacial stability. Gel polymer electrolytes, combining the high ionic conductivity of liquid electrolytes with the good safety of solid electrolytes, are considered a promising electrolyte system. However, traditional polymer matrices (such as polyethylene oxide and polyvinylidene fluoride) generally suffer from insufficient polarity or simple structures, making it difficult to simultaneously achieve efficient ion transport and stable interfacial behavior. Specifically, these electrolytes suffer from limited lithium salt dissociation and low ion migration efficiency; furthermore, they are prone to side reactions at the electrode interface, leading to interfacial instability and affecting battery cycle performance and lifespan. In addition, existing gel electrolytes lack effective molecular control methods in structural design, making it difficult to achieve a balance between ion transport, electrochemical stability, and interfacial stability. Therefore, the development of a functionalized polymer matrix with controllable polarity and tunable structure is crucial for improving the overall performance of gel polymer electrolytes. Summary of the Invention
[0003] The technical solution provided by this invention is as follows: A cyano-containing polysiloxane resin, the raw materials of which include: a cyano-containing silane monomer, a difunctional silane monomer, and a capping agent; wherein, The end-capping agent is selected from thermosetting end-capping agents and photosetting end-capping agents.
[0004] Preferably, the thermosetting end-capping agent is selected from vinyl-containing siloxane end-capping agents.
[0005] Preferably, the photocurable end-capping agent is selected from at least one of acrylic acid-containing siloxane end-capping agents, methacrylic acid-containing siloxane end-capping agents, and epoxy group-containing siloxane end-capping agents.
[0006] According to an embodiment of the present invention, the raw material is subjected to hydrolysis and polycondensation to obtain cyanopolysiloxane resin.
[0007] According to an embodiment of the present invention, the molar ratio of the cyanosilane monomer, the difunctional silane and the capping agent in the raw materials is 1:(0~5):(0.01~1.5), preferably 1:(0.1~3):(0.1~1.5), for example 1:0.4:0.15 or 1:0.35:0.5.
[0008] According to an embodiment of the present invention, the difunctional silane monomer has a structure as shown in Formula I: Formula I Each R1 is either identical or different, and is independently selected from C. 1-6 Alkyl groups (such as methyl, ethyl, or propyl), C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl.
[0009] Preferably, the difunctional silane monomer is selected from dimethyldiethoxysilane.
[0010] According to an embodiment of the present invention, the cyanosilane monomer has a structure as shown in Formula II: Formula II Each R2 is either identical or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl.
[0011] Preferably, the cyanosilane monomer is selected from cyanopropyltriethoxysilane (also known as 3-cyanopropyltriethoxysilane).
[0012] According to an embodiment of the present invention, the capping agent has a structure as shown in Formula III or Formula IV:
[0013] Formula III Formula IV in, In Equation III, each R3 is either the same or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl, -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; and at least one R3 in Formula III is selected from -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate group, -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; In Equation IV, each R4 is either the same or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl; R5 is selected from one of the following groups: -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate group, -OC 1-6 Alkyl-C 2-4 Epoxyalkyl.
[0014] For example, the end-capping agent is selected from 1,3-divinyltetramethyldisiloxane, vinyldimethylethoxysilane, and 3-(methoxydimethylsilyl)propyl acrylate.
[0015] The present invention also provides a method for preparing the above-mentioned cyano-containing polysiloxane resin, the method comprising the following steps: (1) Mix the cyanosilane monomer with the difunctional silane and stir at 40-60°C for 0.5-2 h; (2) Add a mixture of water and acid catalyst dropwise to the system obtained in step (1), and control the dropwise addition time to 0.5~2h. After the dropwise addition is completed, continue the hydrolysis reaction at 60~70℃ for 1~4h. (3) After the hydrolysis reaction in step (2) is completed, add the end-capping agent and carry out the polycondensation reaction at 60~90°C for 4~18 h to obtain the cyano-containing polysiloxane resin.
[0016] According to an embodiment of the present invention, in step (1), the molar ratio of the cyanosilane monomer to the difunctional silane is 1: (0~5), for example, 1:0.01, 1:0.1, 1:0.3, 1:0.4, 1:0.5, 1:1, 1:3 or any two of the above values.
[0017] According to an embodiment of the present invention, in step (2), the amount of water added is 0.8 to 1.5 times the total number of moles of Si–OR groups in the system obtained in step (1).
[0018] According to an embodiment of the present invention, in step (2), the acid catalyst is selected from at least one of hydrochloric acid, trifluoroacetic acid, sulfuric acid, formic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, acetic acid, and phosphoric acid, preferably hydrochloric acid. Further, the concentration of the hydrochloric acid can be selected from concentrations known in the art, for example, 36–38 wt% (mass concentration).
[0019] According to an embodiment of the present invention, in step (2), the amount of acid catalyst used is 0.5 to 5 wt% of the total mass of the system obtained in step (1), for example, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt% or any two of the above values.
[0020] According to an embodiment of the present invention, the molar ratio of the cyanosilane monomer in step (1) to the end-capping agent added in step (3) is 1:(0~1.5), for example, 1:0.1, 1:0.15, 1:0.5, 1:1, 1:1.5 or any two of the above values.
[0021] According to an embodiment of the present invention, in step (3), after the polycondensation reaction is completed, an elution operation can be performed, such as layering, water washing, alcohol washing, and solvent removal under reduced pressure.
[0022] The present invention also provides the application of the above-mentioned cyano-containing polysiloxane resin in gel polymer electrolytes.
[0023] The present invention also provides a gel polymer electrolyte, wherein the raw materials of the gel polymer electrolyte include: a precursor solution and an initiator; the precursor solution includes the above-mentioned cyano-containing polysiloxane resin and liquid electrolyte.
[0024] According to an embodiment of the present invention, the liquid electrolyte comprises a lithium salt and an organic solvent.
[0025] According to an embodiment of the present invention, the lithium salt is selected from one or more of LiPF6, LiBF4, LiClO4, LiTFSI, LiFSI, and LiDFOB.
[0026] According to an embodiment of the present invention, in the liquid electrolyte, the molar concentration of the lithium salt is selected from concentrations known in the art, for example, 1 mol / L.
[0027] According to embodiments of the present invention, the organic solvent includes carbonate solvents and / or ether solvents.
[0028] Preferably, the carbonate solvent is selected from one or more of cyclic carbonates and chain carbonates. Further, the cyclic carbonate includes ethylene carbonate (EC) and / or propylene carbonate (PC). Further, the chain carbonate is selected from one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC).
[0029] Preferably, the ether solvent is selected from one or more of the following substances: 1,2-dimethoxyethane (DME), 1,3-dioxolane (DOL), tetrahydrofuran (THF), ethylene glycol dimethyl ether (EGDME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (Triglyme), and tetraethylene glycol dimethyl ether (Tetraglyme).
[0030] For example, the organic solvent includes EC, DEC and DMC in a volume ratio of 1:1:1.
[0031] According to an embodiment of the present invention, in the precursor solution, the mass ratio of cyano-containing polysiloxane resin to liquid electrolyte is 0.1-1:0.1-5, preferably 0.1-1:0.1-3, for example 1:1 or 1:2.25.
[0032] According to an embodiment of the present invention, the cyano-containing polysiloxane resin has a mass percentage content of 10 to 80 wt% in the gel polymer electrolyte, for example, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, or any two of the above values.
[0033] According to an embodiment of the present invention, the initiator is selected from photoinitiators and / or thermal initiators.
[0034] Preferably, the photoinitiator is selected from at least one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), 2,4,6-trimethylbenzoyl diphenylphosphine oxide (TPO), ethyl 2,4,6-trimethylbenzoylphosphonate (TPO-L), 2-isopropylthioxanthone (ITX), 1-hydroxy-cyclohexyl-phenyl ketone (184), 2,2-dimethoxy-2-phenylacetophenone (BDK), phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (819), methyl o-benzoylbenzoate (OMBB), 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone (907), and ethyl 4-dimethylaminobenzoate (EDB).
[0035] Preferably, the thermal initiator is selected from at least one or more of benzoyl peroxide (BPO), dicumyl peroxide (DCP), tert-butyl peroxide (TBPB), di-tert-butyl peroxide (DTBP), tert-butyl cumyl peroxide, (2,4-dichlorobenzoyl peroxide), di(4-methylbenzoyl peroxide), azobisisobutyronitrile (AIBN), and azobisisoheptanenitrile (ABVN).
[0036] According to an embodiment of the present invention, in the raw materials of the gel polymer electrolyte, the amount of initiator added is 0.05 wt.% to 10 wt.% of the total mass of the precursor solution, for example, 0.1 wt.%, 0.5 wt.%, 1 wt.%, 2 wt.%, 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, 8 wt.%, 9 wt.%, 10 wt.%, or any range between two of the above values.
[0037] According to an embodiment of the present invention, after the gel polymer electrolyte is cured, the cyano-containing polysiloxane resin locks in the liquid electrolyte to form a gel, thereby having a three-dimensional cross-linked network structure.
[0038] The present invention also provides a method for preparing the above-mentioned gel polymer electrolyte, the method comprising: mixing the cyano-containing polysiloxane resin with a liquid electrolyte, adding an initiator to form a homogeneous system, and then forming the gel polymer electrolyte by photocuring and / or thermal curing.
[0039] According to embodiments of the present invention, the cyano-containing polysiloxane resin, liquid electrolyte, initiator, and their amounts have the meanings described above.
[0040] According to an embodiment of the present invention, the photocuring process can be performed using methods known in the art, such as 365 nm ultraviolet light irradiation.
[0041] According to an embodiment of the present invention, the thermosetting treatment can be performed using methods known in the art, such as AIBN catalytic heating curing.
[0042] The present invention also provides the application of the above-mentioned cyano-containing polysiloxane resin and / or gel polymer electrolyte in secondary ion batteries.
[0043] Beneficial effects This invention introduces a polar cyano (–CN) functional group into a polysiloxane structure and combines it with a controllable end-capping structure to achieve regulation of the material's molecular structure and construction of a cross-linked network, thereby obtaining a gel polymer electrolyte system that combines good ion transport performance and interfacial stability. The cyano functional group has strong polarity and electron attraction capabilities, which helps to enhance the overall polarity of the electrolyte system, promote lithium salt dissociation and improve ion transport capacity, while also reducing side reactions to a certain extent and improving electrochemical stability. Furthermore, this structure is beneficial for improving the interfacial compatibility between the electrolyte and the electrode, thereby improving the cycle stability of the battery.
[0044] This invention introduces end-capping agents containing vinyl, acrylate, or epoxy groups, enabling the resulting polysiloxane resin to possess photocurable and / or thermocurable capabilities. This allows it to adapt to various processing requirements and, under external conditions, form a three-dimensional cross-linked network structure, thereby constructing a stable gel polymer electrolyte. This network structure effectively immobilizes the liquid electrolyte, optimizes interfacial reaction pathways, improves SEI stability, significantly enhances the cycle stability and system safety of lithium metal batteries, while maintaining continuous ion conduction channels.
[0045] The gel polymer electrolyte constructed in this invention exhibits good electrochemical stability while maintaining high ionic conductivity, making it suitable for electrochemical energy storage devices such as lithium metal batteries. Attached Figure Description
[0046] Figure 1 The image shows the silica spectrum of the resin in Example 1.
[0047] Figure 2 The image shows the resin silicon spectrum of Example 2.
[0048] Figure 3 The image shows the resin silicon spectrum of Example 3.
[0049] Figure 4 The change in ionic conductivity of the gel electrolyte as a function of temperature in Example 4.
[0050] Figure 5 The linear sweep voltammetry curve of the gel electrolyte in Example 4 is shown.
[0051] Figure 6 The change in ionic conductivity of the gel electrolyte as a function of temperature in Example 5.
[0052] Figure 7 The linear sweep voltammetry curve of the gel electrolyte in Example 5 is shown.
[0053] Figure 8 The image shows the lithium stability test curve of the gel electrolyte in Example 5. Detailed Implementation
[0054] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0055] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0056] Example 1 The raw materials for cyanopolysiloxane resin include: The mixture contains 30 g of cyanopropyltriethoxysilane, 7.8 g of dimethyldiethoxysilane, 3.94 g of 3-(methoxydimethylsilyl)propyl acrylate, 9.24 g of water, and 0.83 g of hydrochloric acid. The molar ratio of cyanopropyltriethoxysilane to dimethyldiethoxysilane to 3-(methoxydimethylsilyl)propyl acrylate is 1:0.4:0.15. The amount of water added is 1.0 times the total molar number of Si-OR groups in the system. The amount of hydrochloric acid used is 2 wt% of the total mass of the other raw materials excluding water.
[0057] The preparation method of cyanopolysiloxane resin is as follows: (1) Add cyanopropyltriethoxysilane and dimethyldiethoxysilane to the reaction vessel and stir at 45°C for 1 h to make the system uniformly mixed; (2) Prepare a mixed solution of water and hydrochloric acid, and slowly add it dropwise to the reaction system under stirring. Control the dropwise addition time to about 1 h. After the dropwise addition is completed, continue the reaction for 2 h to complete the hydrolysis process. (3) Add the end-capping agent 3-(methoxydimethylsilyl)propyl acrylate to the above system, connect the water separator and introduce nitrogen for protection, heat the system to 75°C and react for 10 h to carry out polycondensation. (4) After the reaction is complete, the system is allowed to stand and separate into layers. The lower layer of oily product is taken out and washed with deionized water until neutral (pH≈7), and then washed with ethanol to remove small molecule byproducts. (5) After removing the residual solvent by depressurization, a transparent oily cyanopolysiloxane resin is obtained.
[0058] Example 2 The raw materials for cyanopolysiloxane resin include: The mixture contains 30 g of cyanopropyltriethoxysilane, 7.8 g of dimethyldiethoxysilane, 3.6 g of 1,3-divinyltetramethyldisiloxane, 8.89 g of water, and 0.83 g of hydrochloric acid. The molar ratio of cyanopropyltriethoxysilane to dimethyldiethoxysilane to 1,3-divinyltetramethyldisiloxane is 1:0.4:0.15. The amount of water added is 1.0 times the total molar number of Si-OR groups in the system. The amount of hydrochloric acid used is 2 wt% of the total mass of the other raw materials excluding water.
[0059] The preparation method of cyanopolysiloxane resin is as follows: (1) Add cyanopropyltriethoxysilane and dimethyldiethoxysilane to the reaction vessel and stir at 45°C for 1 h to make the system uniformly mixed; (2) Prepare a mixed solution of water and hydrochloric acid, and slowly add it dropwise to the reaction system under stirring. Control the dropwise addition time to about 1 h. After the dropwise addition is completed, continue the reaction for 2 h to complete the hydrolysis process. (3) Add the end-capping agent 1,3-divinyltetramethyldisiloxane to the above system, connect the water separator and introduce nitrogen for protection, heat the system to 75°C and react for 10 h to carry out polycondensation. (4) After the reaction is complete, the system is allowed to stand and separate into layers. The lower layer of oily product is taken out and washed with deionized water until neutral (pH≈7), and then washed with ethanol to remove small molecule byproducts. (5) After removing the residual solvent by depressurization, a transparent oily cyanopolysiloxane resin is obtained.
[0060] Example 3 The raw materials for cyanopolysiloxane resin include: The mixture contains 30 g of cyanopropyltriethoxysilane, 6.8 g of dimethyldiethoxysilane, 8.5 g of vinyldimethylethoxysilane, 9.8 g of water, and 0.91 g of hydrochloric acid. The molar ratio of cyanopropyltriethoxysilane to dimethyldiethoxysilane to vinyldimethylethoxysilane is 1:0.35:0.5. The amount of water added is approximately 1.0 times the total molar amount of Si-OR groups in the system. The amount of hydrochloric acid used is 2 wt% of the total mass of the raw materials excluding water.
[0061] The preparation method of cyanopolysiloxane resin includes the following steps: (1) Add cyanopropyltriethoxysilane and dimethyldiethoxysilane to the reaction vessel and stir at 45°C for 1 h to make the system uniformly mixed; (2) Prepare a mixed solution of water and hydrochloric acid, and slowly add it dropwise to the reaction system under stirring. Control the dropwise addition time to about 1 h. After the dropwise addition is completed, continue the reaction for 2 h to complete the hydrolysis process. (3) Add the end-capping agent vinyldimethylethoxysilane to the above system, connect the water separator and introduce nitrogen for protection, heat the system to 75°C and react for 10 h to carry out polycondensation. (4) After the reaction is complete, the system is allowed to stand and separate into layers. The lower layer of oily product is taken out and washed with deionized water until neutral (pH≈7), and then washed with ethanol to remove small molecule byproducts. (5) After removing the residual solvent by depressurization, a transparent oily cyanopolysiloxane resin is obtained.
[0062] Test Example 1 Figure 1 , Figure 2 and Figure 3 The images show the resin silica spectra for Examples 1, 2, and 3, respectively. (From...) Figure 1-3It can be seen that the peaks at δ of 15 ~ 5ppm, 5 ~ -5ppm, -12 ~ -20ppm, and -55 ~ -70ppm are respectively attributed to the silicon atoms of CH2=CH-COO-(CH2)3-Si(Me)2-O-, CH2=CH-Si(Me)2-O-, D-linker-Me2SiO-, and cyanopropyl T-linker, indicating the successful synthesis of cyanopolysiloxane resin.
[0063] Example 4 Preparation of gel electrolytes: The cyanopolysiloxane resin prepared in Example 1 was used to prepare a gel electrolyte according to the following steps: In an argon-filled glove box, a liquid electrolyte of 1 mol / L LiPF6 in EC / DEC / DMC (1:1:1, volume ratio) was prepared. The resin and liquid electrolyte were mixed at a mass ratio of 1:1 to obtain a precursor solution. 1 wt% of photoinitiator 1173 (by mass of the precursor solution) was added, and the mixture was stirred for 4 h to form a homogeneous solution. This solution was injected into a membrane mold and cured under 365 nm UV light for 20 s to obtain a gel polymer electrolyte membrane with a thickness of 100 μm.
[0064] Example 5 Preparation of gel electrolytes: The cyanopolysiloxane resin prepared in Example 2 was used to prepare a gel electrolyte according to the following steps: In an argon-filled glove box, the resin and DEGDME were mixed at a mass ratio of 1:1.5 to obtain a precursor solution. 30 wt% LiTFSI and 1 wt% thermal initiator AIBN were added, and the mixture was stirred for 4 h to form a homogeneous solution. This solution was injected into a membrane mold and thermally cured at 80°C for 1 h to obtain a gel polymer electrolyte membrane with a thickness of 200 μm.
[0065] Test Example 2 The gel polymer electrolyte membrane prepared in the above examples was subjected to the following performance tests: (1) Ionic conductivity test: The gel polymer electrolyte membranes from Examples 4 and 5 were placed between two stainless steel electrodes (SS) to assemble SS / electrolyte / SS symmetrical cells. Electrochemical impedance spectroscopy (EIS) tests were performed using an AutoLab 302N electrochemical workstation at a frequency range of 10 Hz. 6 ~10 1 Impedance spectra were recorded at Hz and in a temperature range of 30–70 °C, and the bulk resistance R of the electrolyte was obtained. b The ionic conductivity (σ) of an electrolyte is calculated using the following formula: σ=L / (R b ×S) Where L represents the electrolyte membrane thickness, R b S is the volume resistance of the electrolyte, and S is the effective contact area between the electrolyte membrane and the electrode.
[0066] (2) Electrochemical window testing: The electrochemical stability of the electrolyte was evaluated using linear sweep voltammetry (LSV). The gel polymer electrolyte membranes from Examples 4 and 5 were sandwiched between lithium metal and stainless steel electrodes, respectively, to assemble Li / electrolyte / SS batteries. The electrochemical stability of the electrolyte was evaluated using a scan rate of 10 mV·s. -1 The test was conducted under the specified conditions, and the electrochemical stability window was determined by recording the current-voltage response curve.
[0067] Figure 4 The change in ionic conductivity of the gel electrolyte with temperature in Example 4; Figure 5 The linear sweep voltammetry curve of the gel electrolyte in Example 4 is shown.
[0068] Figure 6 The change in ionic conductivity of the gel electrolyte with temperature in Example 5; Figure 7 The linear sweep voltammetry curve of the gel electrolyte in Example 5 is shown.
[0069] Figure 8 The figure shows the lithium stability test curve of the gel electrolyte in Example 5, with a corresponding current density of 0.1 mA / cm². -2 .
[0070] Table 1
[0071] Figure 4-8 The data are summarized in Table 1, showing that ionic conductivity increases with increasing temperature. The electrolyte with DEGDME as a plasticizer (Example 5) has a higher electrochemical stability window than the carbonate-plasticized electrolyte (EC / DEC / DMC, Example 4), reaching 5.2 V. Simultaneously, this electrolyte also exhibits excellent lithium stability.
[0072] The exemplary embodiments of the present invention have been described above. However, the scope of protection of the present invention is not limited to the above embodiments. Any modifications, equivalent substitutions, improvements, etc., made by those skilled in the art within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A cyano-containing polysiloxane resin, characterized in that, Its raw materials include: cyanosilane monomers, difunctional silane monomers, and end-capping agents; among which, The end-capping agent is selected from thermosetting end-capping agents and photocuring end-capping agents; The thermosetting end-capping agent is selected from vinyl-containing siloxane end-capping agents; The photocurable end-capping agent is selected from at least one of the following: acrylic acid-containing siloxane end-capping agents, methacrylic acid-containing siloxane end-capping agents, and epoxy group-containing siloxane end-capping agents.
2. The cyano-containing polysiloxane resin according to claim 1, characterized in that, The raw materials are subjected to hydrolysis and polycondensation reactions to obtain cyanopolysiloxane resin; The raw materials contain a cyanosilane monomer, a difunctional silane, and a capping agent in a molar ratio of 1:(0.~3):(0.01~1.5). The difunctional silane monomer has the structure shown in Formula I: Equation I Each R1 is either identical or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 At least one of the aryl groups; The cyanosilane monomer has the structure shown in Formula II: Formula II Each R2 is either identical or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 At least one of the aryl groups; The capping agent has a structure as shown in Formula III or Formula IV: Formula III Formula IV in, In Equation III, each R3 is either the same or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl, -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate or -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; and at least one R3 in Formula III is selected from -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate group, -OC 1-6 Alkyl-C 2-4 Epoxyalkyl; In Equation IV, each R4 is either the same or different, and is independently selected from C. 1-6 Alkyl, C 6-12 aryl-substituted C 1-6 Alkyl, C 6-12 Aryl; R5 is selected from one of the following groups: -C 1-6 Alkyl-vinyl, -C 1-6 Alkyl-acrylate group, -C 1-6 Alkyl-methacrylate group, -OC 1-6 Alkyl-C 2-4 Epoxyalkyl.
3. The cyano-containing polysiloxane resin according to claim 1, characterized in that, The cyanosilane monomer is selected from cyanopropyltrialkoxysilane.
4. The method for preparing the cyano-containing polysiloxane resin according to any one of claims 1-3, characterized in that, The preparation method includes the following steps: (1) Mix the cyanosilane monomer with the difunctional silane and stir at 40-60°C for 0.5-2 h; (2) Add a mixture of water and acid catalyst dropwise to the system obtained in step (1), and control the dropwise addition time to be 0.5~2 h. After the dropwise addition is completed, continue the hydrolysis reaction at 60~70℃ for 1~4 h. (3) After the hydrolysis reaction in step (2) is completed, add the end-capping agent and carry out the polycondensation reaction at 60~90°C for 4~18 h to obtain the cyano-containing polysiloxane resin.
5. The preparation method according to claim 4, characterized in that, In step (1), the molar ratio of the cyanosilane monomer to the difunctional silane is 1: (0~5); In step (2), the amount of water added is 0.8 to 1.5 times the total number of moles of Si–OR groups in the system obtained in step (1); In step (2), the acid catalyst is selected from at least one of hydrochloric acid, trifluoroacetic acid, sulfuric acid, formic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, acetic acid, and phosphoric acid; In step (2), the amount of acid catalyst used is 0.5~5 wt% of the total mass of the system obtained in step (1). The molar ratio of the cyanosilane monomer in step (1) to the capping agent added in step (3) is 1:(0~1.5).
6. The use of the cyano-containing polysiloxane resin according to any one of claims 1-3 in gel polymer electrolytes.
7. A gel polymer electrolyte, characterized in that, The raw materials for the gel polymer electrolyte include: a precursor solution and an initiator; the precursor solution includes the cyano-containing polysiloxane resin and liquid electrolyte as described in any one of claims 1-3.
8. The gel polymer electrolyte according to claim 7, characterized in that, The liquid electrolyte includes lithium salt and organic solvent; The lithium salt is selected from one or more of LiPF6, LiBF4, LiClO4, LiTFSI, LiFSI, and LiDFOB; The organic solvents include carbonate solvents and / or ether solvents; The carbonate solvent is selected from one or more of cyclic carbonates and chain carbonates; The ether solvent is selected from one or more of the following substances: 1,2-dimethoxyethane, 1,3-dioxolane, tetrahydrofuran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether. In the precursor solution, the mass ratio of cyano-containing polysiloxane resin to liquid electrolyte is 0.1-1:0.1-5; The cyano-containing polysiloxane resin has a mass percentage content of 10-80 wt% in the gel polymer electrolyte. The initiator is selected from photoinitiators and / or thermal initiators; The photoinitiator is selected from at least one or more of the following: 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), 2,4,6-trimethylbenzoyl diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphosphonate, 2-isopropylthioxanthone, 1-hydroxy-cyclohexyl-phenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, methyl o-benzoylbenzoate, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, and ethyl 4-dimethylaminobenzoate. The thermal initiator is selected from at least one or more of the following: benzoyl peroxide (BPO), dicumyl peroxide, tert-butyl peroxide, di-tert-butyl peroxide, tert-butyl cumyl peroxide, (2,4-dichlorobenzoyl peroxide), di(4-methylbenzoyl peroxide), azobisisobutyronitrile, and azobisisoheptanenitrile. In the raw materials of the gel polymer electrolyte, the amount of initiator added is 0.05 wt.% to 10 wt.% of the total mass of the precursor solution.
9. The method for preparing the gel polymer electrolyte according to claim 7 or 8, characterized in that, The preparation method includes: mixing the cyano-containing polysiloxane resin with a liquid electrolyte, adding an initiator to form a homogeneous system, and then forming the gel polymer electrolyte by photocuring and / or thermal curing.
10. The use of the cyano-containing polysiloxane resin according to any one of claims 1-3 and / or the gel polymer electrolyte according to claim 7 or 8 in a secondary ion battery.