An interpenetrating network hydrogel and a preparation method and application thereof
By constructing an interpenetrating network hydrogel, combined with curcumin and genetically engineered mesenchymal matrix cells, a match between mechanical properties and degradation rate was achieved, enhancing cell loading and activity maintenance capabilities, endowing active immune regulation function, and realizing long-term controlled release of drugs. This solved the comprehensive problems of existing hydrogels in the repair of diabetic wounds, and achieved efficient and safe wound healing.
Patent Information
- Application Number
- CN202611361096.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-20
AI Technical Summary
Existing hydrogels have shortcomings in terms of mechanical properties, degradation rate, cell load and activity maintenance capacity, immune regulation function and intelligent drug release capacity, making it difficult to meet the comprehensive repair needs of diabetic chronic wounds.
An interpenetrating network hydrogel was constructed, in which curcumin and genetically engineered mesenchymal stromal cells (MSCs-3IL) were loaded through an interpenetrating network structure of GelMA, HAMA, PNIPAAM and FN, achieving synergistic effects of mechanical support, immune regulation, angiogenesis and tissue regeneration.
This invention provides a highly efficient, safe, and controllable multifunctional synergistic hydrogel system that significantly accelerates the healing of diabetic wounds, overcoming the shortcomings of existing materials in terms of mechanical adaptability, controllable degradation, immunomodulation, and intelligent drug release capabilities.
Smart Images

Figure CN123131631A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of interpenetrating network hydrogel preparation technology, and in particular to an interpenetrating network hydrogel, its preparation method and application. Background Technology
[0002] Commonly used hydrogels in existing technologies include methacrylamide gelatin (GelMA) hydrogels, methacrylamide hyaluronic acid (HAMA) hydrogels, fibronectin (FN) composite modified hydrogel systems, and thermosensitive poly(N-isopropylacrylamide) (PNIPAAm) based hydrogels. However, GelMA hydrogels have weak mechanical properties and a rapid degradation rate, making them unsuitable for the mechanical environment and long-term repair cycle of chronic wounds. They also lack the ability to actively regulate immune cell polarization and the inflammatory microenvironment, and do not possess temperature-responsive drug release capabilities. HAMA hydrogels, lacking RGD cell adhesion sites, suffer from poor cell adhesion, low mechanical strength, and a tendency to swell and collapse. They also have limited biological functions and lack thermosensitive controlled-release properties, leading to potential burst release of drugs. While fibronectin composite modified systems can promote cell migration, FN proteins themselves are unstable, easily degraded, and cannot target and induce macrophage polarization towards an anti-inflammatory phenotype. Even when blended with GelMA or HAMA, the imbalance between mechanical and degradation properties remains difficult to resolve. Thermosensitive PNIPAAm-based hydrogels suffer from poor biocompatibility, lack of active sites, weak cell adhesion and proliferation capabilities, and structural shrinkage after phase transition leading to pore collapse, which is unfavorable for long-term cell colonization. Furthermore, as a synthetic polymer, they have poor degradability, posing a risk of toxicity in vivo, making them unsuitable for long-term repair applications. Overall, existing systems have significant shortcomings in terms of mechanical compatibility, controllable degradation, immunomodulatory function, and intelligent drug release capabilities, making it difficult to meet the comprehensive needs of diabetic chronic wound repair.
[0003] Based on the above-mentioned shortcomings of existing hydrogels in terms of mechanical properties, degradation rate, immune regulation, and intelligent response, the present invention aims to solve the following technical problems: Improving mechanical properties and controllable degradation: To address the problems of insufficient mechanical strength and rapid degradation of GelMA, easy swelling and collapse of HAMA, and structural shrinkage after the phase transition of PNIPAMA, this invention constructs an interpenetrating network structure of GelMA, HAMA, fibronectin and PNIPAMA to obtain a composite hydrogel carrier that has suitable mechanical strength, stable structure and degradation rate that matches the wound repair cycle.
[0004] Enhancing cell load and activity maintenance: Addressing the problems of existing materials lacking active adhesion sites, weak cell adhesion and proliferation capabilities, and difficulty in long-term preservation of engineered cells, this invention utilizes interpenetrating network hydrogels to provide an excellent microenvironment for adhesion, proliferation, and secretion of genetically engineered mesenchymal matrix cells, enabling them to stably overexpress anti-inflammatory factors and continuously exert therapeutic effects.
[0005] Imparting active immune regulation function: In response to the problem that existing materials cannot regulate macrophage phenotype and are difficult to reverse persistent inflammation in diabetic wounds, this invention uses hydrogel-loaded MSCs-3IL cells to overexpress IL-4, IL-10 and IL-13, which targets and induces macrophages to polarize from pro-inflammatory M1 type to anti-inflammatory M2 type, thereby actively improving the inflammatory microenvironment of the wound.
[0006] Achieving long-term controlled release and synergistic therapy: Addressing the issues of easy burst release and lack of thermo-responsive drug release capabilities in existing materials, this invention encapsulates curcumin in a hydrogel. By leveraging the sustained-release properties of the interpenetrating network structure and the environmental responsiveness of the thermo-sensitive component, stable and long-term drug release is achieved. This synergizes with the anti-inflammatory effects of MSCs-3IL, jointly promoting angiogenesis, collagen deposition, and tissue remodeling.
[0007] Achieving synergistic integration of multiple functions: In response to the problem that existing systems have single functions and cannot meet the comprehensive repair needs of chronic wounds, this invention constructs a three-in-one composite system of "biomaterial carrier - functionalized cells - natural anti-inflammatory components", which simultaneously achieves synergistic effects of mechanical support, immune regulation, angiogenesis promotion and tissue regeneration, significantly accelerating the healing of diabetic wounds and providing a feasible solution for clinical translation.
[0008] Therefore, this invention proposes a composite system based on interpenetrating network thermosensitive hydrogel loaded with genetically engineered mesenchymal matrix cells and curcumin, aiming to systematically solve the above-mentioned technical problems and achieve synergistic integration of multiple functions such as mechanical properties, degradation rate, immune regulation and intelligent drug release, thereby providing a novel treatment strategy for the repair of diabetic chronic wounds that is efficient, safe, controllable and has clinical translational potential. Summary of the Invention
[0009] The purpose of this invention is to overcome the shortcomings of the prior art and provide an interpenetrating network hydrogel, its preparation method and application.
[0010] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides an interpenetrating network hydrogel, which is made by means of a hydrogel mixture comprising: 4% to 6% by weight (by volume) of methacrylamide gelatin (GelMA), 0.4% to 0.6% by weight (by volume) of methacrylamide hyaluronic acid (HAMA), 0.5% to 25% by weight (by volume) of N-isopropylacrylamide (PNIPAAm), and 0.0008% to 0.0012% by weight (by volume) of fibronectin (FN).
[0011] The roles of each component and its dosage in this invention are as follows: GelMA contains a natural RGD cell adhesion sequence, providing adhesion sites for stem cells and fibroblasts, ensuring three-dimensional cell colonization; photocrosslinking forms the basic hydrogel framework, giving the scaffold basic biocompatibility. This invention limits its content to 4%~6% because experiments have shown that when its mass-volume percentage is below 0.4%, the crosslinking network is sparse, mechanical strength decreases significantly, degradation is too rapid, and cell adhesion sites are insufficient; while above 0.6%, the precursor solution has extremely high viscosity, making filtration and sterilization difficult, and the pores become dense after photocrosslinking, hindering the diffusion of nutrients and cytokines.
[0012] HAMA is used to construct biomimetic porous three-dimensional microenvironments, which can improve the swelling imbalance problem of pure GelMA; it regulates the pore structure of hydrogels, promotes nutrient penetration and cell ingrowth, and is suitable for skin and soft tissue repair. This invention limits its content to 0.4%~0.6% because experiments have shown that when its mass-volume percentage is below 0.4%, the three-dimensional porous structure is not obvious, and there are few interconnected channels inside the scaffold; while above 0.6%, the hydrogel swelling rate is too high, the wound surface easily absorbs water and collapses, and the mechanical compressive modulus is significantly reduced.
[0013] PNIPAAm undergoes a reversible hydrophilic-hydrophobic phase transition within the 37°C body temperature range, enabling temperature-responsive drug release from the wound microenvironment and constructing a second thermosensitive interpenetrating network to enhance the overall toughness of the scaffold. This invention limits its content to 0.5%~25% because experiments have shown that when its mass-volume percentage is below 0.5%, the thermosensitive phase transition effect is weak, resulting in no significant controlled drug release, while above 25%, the proportion of polymer synthesis is too high, leading to decreased overall biocompatibility and significantly reduced cell adhesion and survival capabilities.
[0014] FN can supplement active targets that promote cell migration, proliferation, and tissue remodeling, enhance the chemotactic ability of fibroblasts and vascular endothelial cells, and assist in collagen deposition in wounds. This invention limits its content to 0.0008% ~ 0.0012% because experiments have shown that when its mass-volume percentage is below 0.0008%, its cell migration-promoting activity is insufficient, while when it is above 0.0012%, excessive protein easily aggregates before cross-linking, clogging hydrogel pores. Simultaneously, it is easily and rapidly degraded by proteases in vivo, resulting in wasted activity.
[0015] This invention overcomes the problems of existing single GelMA (weak mechanical properties, rapid degradation, and simple pore structure), pure HAMA (lacking cell adhesion sites, prone to collapse after water absorption and swelling), and simple PNIPAMA (poor biocompatibility and pore collapse after phase transition) by constructing a photocrosslinked-thermosensitive interpenetrating composite network.
[0016] This invention integrates a GelMA covalent network, a HAMA porous framework, and a PNIPAMAm thermosensitive network into a triple interpenetrating scaffold, significantly improving its compressive modulus and structural stability. It is suitable for the active traction and large exudation environment of diabetic wounds, preventing dressings from easily breaking or falling off. The balanced swelling ratio is controllable, preventing excessive water absorption and collapse, and preventing cracking due to water loss. The enzymatic degradation rate matches the skin wound repair cycle, maintaining the scaffold support function for more than 14 days, solving the problem of single materials degrading too quickly or leaving difficult-to-degrade residues.
[0017] PNIPAAm thermosensitive technology responds to body temperature to control drug release, solving the problems of sudden drug release and short-lived effects associated with traditional hydrogels. Traditional drug-loaded hydrogels lack thermosensitive properties, resulting in a rapid, large-scale release of drugs upon contact with body fluids, followed by a short-term loss of efficacy, failing to sustainably inhibit chronic inflammation in wounds. While pure PNIPAAm possesses thermosensitivity, it cannot function as a standalone cell carrier. This invention's PNIPAAm thermosensitive network undergoes a hydrophilic-hydrophobic phase transition in the 37°C wound microenvironment, slowly releasing the drug, avoiding initial explosive drug release, and reducing local cytotoxicity. It achieves long-lasting local anti-inflammatory and antioxidant effects for over ten days, continuously inhibiting the activation of M1 pro-inflammatory macrophages. The drug is released locally at the wound site, reducing systemic side effects and is well-suited to the persistent low-grade inflammation characteristics of diabetic wounds.
[0018] Simultaneous introduction of fibronectin FN for synergistic modification, superimposed cell migration-promoting active sites on the intrinsic RGD sequence of GelMA, to make up for the shortcomings of HAMA lacking cell adhesion sites and PNIPAMAm being a completely non-biologically active peptide.
[0019] As a preferred embodiment of the first aspect of the present invention, the hydrogel mixture of the interpenetrating network hydrogel further includes: an anti-inflammatory active drug at a mass-volume percentage of 0.04% to 0.06%, a photoinitiator at a mass-volume percentage of 0.2% to 0.3%, a crosslinking agent, and an initiator; wherein the mass ratio of the crosslinking agent to N-isopropylacrylamide is (2~4):50; and the mass ratio of the initiator to N-isopropylacrylamide is (0.5~1.5):10.
[0020] Anti-inflammatory drugs (e.g., curcumin) possess broad-spectrum anti-inflammatory and antioxidant properties, inhibiting excessive activation of M1 pro-inflammatory macrophages in wounds and synergistically promoting M2 polarization with MSCs-3IL; thermosensitive phase transition enables localized long-term sustained release from the wound. This invention limits its content to 0.04%~0.06% because experiments have shown that when its mass-volume percentage is below 0.04%, the anti-inflammatory efficacy is insufficient, while above 0.06%, it produces cytotoxicity, inhibiting the proliferation of stem cells and fibroblasts. The photoinitiator can crosslink the hydrogel mixture under 405 nm blue light-mediated crosslinking, providing gentle crosslinking without damaging the loaded stem cells, constructing a stable GelMA / HAMA covalent crosslinked network. The crosslinking agent is a PNIPAMAm polymeric crosslinking agent, forming a thermosensitive polymer network that forms an interpenetrating double network with GelMA / HAMA. The initiator initiates PNIPAMAm free radical polymerization at room temperature, synergistically forming an interpenetrating network with the photocrosslinking. The amount of PNIPAMA added is limited to 1% of the mass of the GHF matrix precursor solution, and is matched with a matching ratio of MBA crosslinking agent and APS initiator to balance the temperature-sensitive drug release performance and biocompatibility. If the amount of PNIPAMA added is too low, there will be no temperature response, while if it is too high, it will significantly reduce the survival ability of stem cells. This specific ratio is the key balance point to achieve temperature-sensitive sustained release and high-efficiency cell loading.
[0021] In a preferred embodiment of the first aspect of the present invention, the N-isopropylacrylamide has a mass-volume percentage of 1%; or / and, the mass ratio of the crosslinking agent to N-isopropylacrylamide is 3:50; and the mass ratio of the initiator to N-isopropylacrylamide is 1:10.
[0022] This invention, through optimization, reveals that when the mass-volume percentage of N-isopropylacrylamide is 1%, the thermosensitive phase transition temperature is precisely close to human body temperature. This allows for controlled drug release without losing responsiveness due to excessively high phase transition temperatures, while also avoiding increased gel brittleness caused by excessive concentration. A mass ratio of crosslinking agent to PNIPAAm of 3:50 and an initiator to PNIPAAm of 1:10 forms a thermosensitive network with a suitable crosslinking density. This ensures sufficient mechanical strength of the gel to support the wound surface without excessive crosslinking inhibiting cell migration and nutrient exchange. By optimizing the ratio of PNIPAAm to the crosslinking agent and initiator, this invention ensures that the thermosensitive network maintains an appropriate crosslinking density while possessing sufficient free radical polymerization activity. This results in a uniformly structured thermosensitive network with a sensitive phase transition response, avoiding excessive network rigidity due to over-crosslinking, which could negatively impact drug release behavior.
[0023] Preferably, the anti-inflammatory active drug is curcumin; the photoinitiator is lithium phenyl-2,4,6-trimethylbenzoylphosphonate (LAP); the crosslinking agent is N,N′-methylenebisacrylamide (MBA); and the initiator is ammonium persulfate (APS).
[0024] Secondly, this invention provides an interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells, comprising the aforementioned interpenetrating network hydrogel loaded with mesenchymal matrix cells, wherein the density of the mesenchymal matrix cells is 1×10⁻⁶. 4 ~3×10 4 cells / cm 2 .
[0025] This invention, based on the aforementioned interpenetrating network hydrogel, further loads engineered mesenchymal stromal cells (MSCs-3ILs) to form a cell-hydrogel composite system. This system synergistically promotes multiple healing pathways, significantly improving the closure efficiency of diabetic wounds. On one hand, it promotes fibroblast migration and proliferation, enhances type I collagen deposition, and accelerates re-epithelialization; on the other hand, it promotes vascular endothelial cell tube formation, improving local wound ischemia. In vivo experiments have demonstrated that the composite system significantly improves wound closure speed compared to simple hydrogels and simple stem cell groups, while simultaneously reducing systemic inflammatory factor levels and decreasing the risk of recurrent wound ulceration. The interpenetrating network hydrogel loaded with engineered mesenchymal stromal cells is an integrated dressing, convenient for clinical use. The precursor solution can be photocrosslinked in situ without additional fixation. It combines the functions of a cell carrier, anti-inflammatory drug reservoir, and immune regulation scaffold, eliminating the need for fractionated drug administration and cell injection, simplifying dressing changes for chronic diabetic wounds.
[0026] As a preferred embodiment of the second aspect of the present invention, the mesenchymal cells overexpress anti-inflammatory factors.
[0027] As a preferred embodiment of the second aspect of the present invention, the anti-inflammatory factor is a combination of interleukin-4, interleukin-10 and interleukin-13.
[0028] The MSCs-3IL loaded in this invention stably and continuously secrete anti-inflammatory factors such as IL-4, IL-10, and TNF-α, and, in combination with curcumin, synergistically regulate RAW264.7 macrophages, downregulate the IL-6 pro-inflammatory gene, and upregulate M2 markers such as IL-10; significantly improve the highly inflammatory microenvironment of diabetic wounds, and overcome the shortcomings of existing hydrogels that only serve as scaffolds and lack immune regulation capabilities.
[0029] Thirdly, this invention provides the application of the described interpenetrating network hydrogel or the described interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells in any of the following: (1) Application in the preparation of materials for treating or repairing wounds; (2) Application in the preparation of biological scaffold materials that promote tissue regeneration; (3) Application in the preparation of anti-inflammatory or immunomodulatory medical dressings.
[0030] This invention has experimentally demonstrated that the interpenetrating network hydrogel and its composite system loaded with engineered mesenchymal matrix cells exhibit significant healing-promoting effects in a diabetic wound model. Specifically, this manifests as a significantly improved wound closure rate, accelerated reepithelialization, and increased collagen deposition. It also reduces the percentage of iNOS-positive macrophages in the wound and increases CD206-positive macrophages at the wound site. Simultaneously, it effectively inhibits local inflammatory responses, showing low levels of IL-6 and high levels of IL-10 in diabetic wounds, indicating excessive inflammation. This suggests that the interpenetrating network hydrogel, or the interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells, can induce macrophage phenotypic polarization from M1 to M2, release anti-inflammatory factors, and promote the transition of the wound from the inflammatory phase to the remodeling phase. Therefore, the interpenetrating network hydrogel or the interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells of this invention has therapeutic or wound-repairing effects, as well as anti-inflammatory or immunomodulatory functions. It provides an integrated solution for the treatment of diabetic wounds, combining structural support and immune regulation. Furthermore, the composite system demonstrated good biocompatibility in both in vivo and in vitro experiments, without causing significant cytotoxicity or tissue rejection, further validating its clinical translation potential.
[0031] In a preferred embodiment of the third aspect of the present invention, the wound is a diabetic chronic wound or a burn wound.
[0032] Fourthly, this invention provides a method for preparing the aforementioned interpenetrating network hydrogel, comprising the following steps: (1) Methacrylamide gelatin, methacrylamide hyaluronic acid, fibronectin and N-isopropylacrylamide were added sequentially to the photoinitiator solution and mixed evenly to obtain a prepolymer solution; (2) Add crosslinking agent, initiator and curcumin solution to the prepolymer solution; (3) The mixture obtained in step (2) is injected into the mold and cross-linked by ultraviolet light to form an interpenetrating network hydrogel.
[0033] Fifthly, this invention provides a method for preparing the aforementioned interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells, comprising the following steps: (1) Culture engineered mesenchymal stromal cells overexpressing anti-inflammatory factors and collect the cells; (2) The cells are directly seeded onto the surface of the interpenetrating network hydrogel as described in claim 1; (3) Place the inoculated hydrogel in an incubator for static culture so that the cells can fully adhere to the surface and pores of the hydrogel to obtain an interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells.
[0034] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention constructs an interpenetrating network hydrogel composed of methacrylamide gelatin, methacrylamide hyaluronic acid, fibronectin, and poly-N-isopropylacrylamide, and encapsulates curcumin and genetically engineered human umbilical cord mesenchymal matrix cells, forming a composite system of "biomaterial carrier-functionalized cells-natural anti-inflammatory components". The interpenetrating network hydrogel supports cell survival, growth, and factor secretion. The IL-4 / IL-10 / IL-13 co-expressed by the engineered umbilical cord mesenchymal matrix cells form a dual anti-inflammatory synergistic system with curcumin, showing good potential for the treatment of diabetic wounds and regenerative medicine applications.
[0035] The composite hydrogel with porous biomimetic microenvironment combined with multilayer cell adhesion sites can stably anchor MSCs-3IL, maintaining high cell viability even after 5 days of in vitro co-culture, thus preventing rapid loss of stem cells; carrying genetically modified MSCs-3IL, it can sustainably and stably express key anti-inflammatory factors such as IL-10, which ordinary unmodified MSCs cannot achieve the same secretion level.
[0036] This invention forms a dual anti-inflammatory synergistic system. Curcumin is released slowly to inhibit the NF-κB pathway and downregulate M1 pro-inflammatory factors such as IL-6. MSCs-3IL continuously secrete IL-10, specifically inducing macrophages to polarize towards the anti-inflammatory and repair-oriented M2 type and upregulating IL-10 expression. The combined effect of the two is significantly better than curcumin alone or ordinary stem cells, effectively improving the highly inflammatory microenvironment of diabetic wounds and eliminating the core obstacle to wound repair.
[0037] The composite system of this invention provides multi-pathway synergistic repair: 1) The RGD sequence of FN and GelMA significantly promotes fibroblast migration and proliferation, accelerating skin re-epithelialization; 2) MSCs-3IL secretion of active factors significantly enhances the tube-forming ability of endothelial cells, improving local ischemia in diabetic wounds; 3) Continuous anti-inflammatory effects reduce damage to fibroblasts and vascular endothelium caused by inflammation, increase type I collagen deposition, and enhance collagen maturity in wounds; 4) In vivo experiments have confirmed that the wound closure rate is significantly better than that of commercial dressings, hydrogel alone, and stem cell suspension alone.
[0038] High biocompatibility, simple process, convenient clinical use, and biocompatibility advantages: all matrix raw materials are medical-grade bioactive materials, and the hemolysis rate is far lower than the medical dressing standard; cross-linking uses a low-cytotoxic LAP photoinitiator, and 405nm gentle blue light cross-linking will not damage the loaded stem cells; compared with PNIPAAm pure polymer materials, this system is dominated by natural biological matrix and has no long-term residual toxicity in vivo.
[0039] Advantages in preparation and use: The precursor solution has good fluidity, allowing for in-situ injection and photocuring, making it suitable for irregular wounds; one set of materials simultaneously achieves the triple functions of scaffold, drug carrier, and stem cell carrier, eliminating the need for step-by-step dressing changes and multiple cell injections, simplifying clinical procedures and reducing the risk of infection. Existing technologies all focus on studying one or two of GelMA, HAMA, FN, and PNIPAAm individually, and there is currently no technical solution that integrates the five functional components (photocrosslinked matrix, hyaluronic acid, fibronectin, thermosensitive polymer, and anti-inflammatory drugs) with genetically engineered stem cells. Attached Figure Description
[0040] Figure 1 Schematic diagram of the physicochemical properties of interpenetrating network hydrogels (A: Flowchart of GHF+1%PNI@CUR hydrogel preparation process; B: SEM image of each hydrogel; C: Average pore size distribution of each hydrogel; D: Mechanical compression test results of each hydrogel; E: Free flow state of each hydrogel before and after 405nm UV irradiation; F: In vitro enzymatic degradation results of each hydrogel; G: Swelling performance test results of each hydrogel; H: Rheological test results of each hydrogel). Figure 2 Schematic diagram of wound repair results in diabetic mice (A: Flowchart of the diabetes model construction process; B: Photographs of wound repair results in each group; C: Wound healing over time; D: Comparison of wound closure rates in each group; E: Comparison of levels of inflammatory factors IL-6, TNF-α, and IL-4 in each group). Figure 3 Schematic diagram of histological examination results of diabetic mice (A: H&E staining results of each group; B: Masson collagen staining results of each group; C: Percentage of iNOS-positive macrophages on day 3 of each group; D: Percentage of iNOS-positive macrophages on day 7 of each group; E: Percentage of CD206-positive macrophages on day 3 of each group; F: Percentage of CD206-positive macrophages on day 7 of each group; G: Expression level of IL-6 on day 3 of each group; G: Expression level of IL-6 on day 7 of each group; I: Expression level of IL-10 on day 3 of each group; J: Expression level of IL-10 on day 7 of each group). Detailed Implementation
[0041] To better illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0042] The basic solvent system is sterile PBS buffer (0.01 mol / L, pH 7.2~7.4); unless otherwise specified, the standard volume of the formulation is 10 mL of PBS.
[0043] Example 1 This embodiment provides an interpenetrating network hydrogel, which is made by a hydrogel mixture comprising: 5% by weight (v / v) methacrylamide gelatin (GelMA), 0.5% by weight (v / v) methacrylamide hyaluronic acid (HAMA), 1% by weight (v / v) N-isopropylacrylamide (PNIPAAm), and 0.001% by weight (v / v) fibronectin (FN). Furthermore, the hydrogel mixture of the interpenetrating network hydrogel also includes the following components: 0.25% by mass of lithium phenyl-2,4,6-trimethylbenzoylphosphonate (LAP) photoinitiator, N,N'-methylenebisacrylamide (MBA) crosslinking agent, and ammonium persulfate (APS) initiator, wherein the mass ratio of PNIPAAm to MBA is 100:6, and the mass ratio of PNIPAAm to APS is 10:1.
[0044] Example 2 The only difference between Example 2 and Example 1 is the amount of PNIPAAM used, which is 0.1% by mass volume.
[0045] Example 3 The only difference between Example 3 and Example 1 is the amount of PNIPAAM used, which is 2.5% by mass volume.
[0046] Example 4 This embodiment provides a method for preparing the interpenetrating network hydrogel of Example 1, including the following steps: Step 1: Prepare a 0.25% (w / v) LAP photoinitiator stock solution: Dissolve 0.05g of LAP powder in 20mL of sterile PBS, heat in a 45℃ water bath for 15min, and shake repeatedly until completely clear. Store in the dark for later use.
[0047] Step 2: Preparation of GelMA precursor solution: Add 0.5g of GelMA powder to 10mL of the above LAP stock solution, heat in a 60℃ water bath in the dark for 30min, and shake intermittently until completely dissolved to obtain a transparent GelMA basic precursor solution.
[0048] Step 3: Preparation of GH binary composite precursor solution: Add 0.05g of HAMA powder to the GelMA precursor solution and stir magnetically at room temperature for 30 minutes to mix thoroughly.
[0049] Step 4: Preparation of GHF ternary precursor solution: Prepare a 1 mg / mL sterile aqueous solution of FN (dissolve at 37℃ for 30 min), add 100 μL of FN stock solution to the above GH binary composite precursor solution, stir and mix well; filter with a 0.22 μm sterile filter membrane to obtain the GHF ternary basic precursor solution.
[0050] Step 5: Introduce a temperature-sensitive polymerization system to prepare GHF + 1% PNI precursor solution: Add 100 mg PNIPAAm, 6 mg MBA, and 10 mg APS sequentially to 10 mL of sterilized GHF ternary precursor solution, and stir at room temperature until the solids are completely dissolved.
[0051] Step 6: One-step photocrosslinking molding of hydrogel dressing: The above-mentioned precursor liquid was injected into the mold and cross-linked by 405nm ultraviolet blue light irradiation; the light irradiation process parameters were 10 mW / cm², 30s; after cross-linking, the interpenetrating network composite hydrogel was obtained, denoted as GHF+1%PNI.
[0052] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 is a pure GelMA single-network hydrogel, and its preparation method is as follows: Step 1: Prepare a 0.25% (w / v) LAP photoinitiator stock solution: Dissolve 0.05g of LAP powder in 20mL of sterile PBS, heat in a 45℃ water bath for 15min, and shake repeatedly until completely clear. Store in the dark for later use.
[0053] Step 2: Preparation of GelMA precursor solution: Add 0.5g of GelMA powder to 10mL of the above LAP stock solution, heat in a 60℃ water bath in the dark for 30min, and shake intermittently until completely dissolved to obtain a transparent GelMA basic precursor solution.
[0054] Step 3: One-step photocrosslinking to form hydrogel dressing: The above-mentioned precursor liquid was injected into the mold and cross-linked by 405nm ultraviolet blue light irradiation; the light irradiation process parameters were 10 mW / cm², 30s; after cross-linking, the interpenetrating network composite hydrogel was obtained, denoted as GelMA.
[0055] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that Comparative Example 2 is a GelMA+HAMA binary composite hydrogel, and its preparation method is as follows: Step 1: Prepare a 0.25% (w / v) LAP photoinitiator stock solution: Dissolve 0.05g of LAP powder in 20mL of sterile PBS, heat in a 45℃ water bath for 15min, and shake repeatedly until completely clear. Store in the dark for later use.
[0056] Step 2: Preparation of GelMA precursor solution: Add 0.5g of GelMA powder to 10mL of the above LAP stock solution, heat in a 60℃ water bath in the dark for 30min, and shake intermittently until completely dissolved to obtain a transparent GelMA basic precursor solution.
[0057] Step 3: Preparation of GH binary composite precursor solution: Add 0.05g of HAMA powder to the GelMA precursor solution and stir magnetically at room temperature for 30 minutes to mix thoroughly.
[0058] Step 4: One-step photocrosslinking to form hydrogel dressing: The above-mentioned precursor liquid was injected into the mold and cross-linked by 405nm ultraviolet blue light irradiation; the light irradiation process parameters were 10 mW / cm², 30s; after cross-linking, the interpenetrating network composite hydrogel was obtained, denoted as GHF.
[0059] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that Comparative Example 3 is a GelMA+HAMA+FN composite hydrogel, and its preparation method is as follows: Step 1: Prepare a 0.25% (w / v) LAP photoinitiator stock solution: Dissolve 0.05g of LAP powder in 20mL of sterile PBS, heat in a 45℃ water bath for 15min, and shake repeatedly until completely clear. Store in the dark for later use.
[0060] Step 2: Preparation of GelMA precursor solution: Add 0.5g of GelMA powder to 10mL of the above LAP stock solution, heat in a 60℃ water bath in the dark for 30min, and shake intermittently until completely dissolved to obtain a transparent GelMA basic precursor solution.
[0061] Step 3: Preparation of GH binary composite precursor solution: Add 0.05g of HAMA powder to the GelMA precursor solution and stir magnetically at room temperature for 30 minutes to mix thoroughly.
[0062] Step 4: Preparation of GHF ternary precursor solution: Prepare a 1 mg / mL sterile aqueous solution of FN (dissolve at 37℃ for 30 min), add 100 μL of FN stock solution to the above GH binary composite precursor solution, stir and mix well; filter with a 0.22 μm sterile filter membrane to obtain the GHF ternary basic precursor solution.
[0063] Step 5: One-step photocrosslinking to form hydrogel dressing: The above-mentioned precursor liquid was injected into the mold and cross-linked by 405nm ultraviolet blue light irradiation; the light irradiation process parameters were 10 mW / cm², 30s; after cross-linking, the interpenetrating network composite hydrogel was obtained, denoted as GHF.
[0064] Example 5 The only difference between Example 5 and Example 1 is that an active antioxidant, curcumin (CUR), was added; the other parameters are the same as in Example 1, and the mass-volume percentage of curcumin in the hydrogel mixture is 0.05%.
[0065] Example 6 This embodiment provides a method for preparing the interpenetrating network hydrogel of Example 5, including the following steps: Step 1: Prepare a 0.25% (w / v) LAP photoinitiator stock solution: Dissolve 0.05g of LAP powder in 20mL of sterile PBS, heat in a 45℃ water bath for 15min, and shake repeatedly until completely clear. Store in the dark for later use.
[0066] Step 2: Preparation of GelMA precursor solution: Add 0.5g of GelMA powder to 10mL of the above LAP stock solution, heat in a 60℃ water bath in the dark for 30min, and shake intermittently until completely dissolved to obtain a transparent GelMA basic precursor solution.
[0067] Step 3: Preparation of GH binary composite precursor solution: Add 0.05g of HAMA powder to the GelMA precursor solution and stir magnetically at room temperature for 30 minutes to mix thoroughly.
[0068] Step 4: Preparation of GHF ternary precursor solution: Prepare a 1 mg / mL sterile aqueous solution of FN (dissolve at 37℃ for 30 min), add 100 μL of FN stock solution to the above GH binary composite precursor solution, stir and mix well; filter with a 0.22 μm sterile filter membrane to obtain the GHF ternary basic precursor solution.
[0069] Step 5: Introduce a temperature-sensitive polymerization system to prepare GHF + 1% PNI precursor solution: Add 100 mg PNIPAAm, 6 mg MBA, and 10 mg APS sequentially to 10 mL of sterilized GHF ternary precursor solution, and stir at room temperature until the solids are completely dissolved.
[0070] Step 6: Preparation of drug-loaded GHF + 1% PNI@CUR precursor solution by loading curcumin: Prepare a 100 mg / mL curcumin solution with DMSO and sterilize it with a 0.22 μm filter membrane; take 5 μL of CUR stock solution and add it to the above 10 mL LHF + 1% PNI precursor solution, mix gently and let stand in the dark for 5 min.
[0071] Step 7: One-step photocrosslinking to form hydrogel dressing: The above-mentioned precursor liquid was injected into the mold and cross-linked by 405nm ultraviolet blue light irradiation; the light irradiation process parameters were 10 mW / cm², 30s; after cross-linking, the interpenetrating network composite hydrogel was obtained, denoted as GHF+1%PNI@CUR.
[0072] Example 7 This embodiment provides a method for preparing an interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells, comprising the following steps: Step 1: Preparation of engineered mesenchymal stromal cells MSCs-3IL: 1. Origin of primitive cells: Primary human umbilical cord mesenchymal stromal cells (hUMSCs) isolated from fresh, healthy umbilical cord tissue; 2. Gene modification vectors and transfection: Lentiviral vector pLV[Exp]-EF1A>hIL10 [NM_000572.3](ns):T2A:hIL13[NM_002188.3](ns):P2A:hIL4[NM_000589.4]-SV40>EGFP:T2A:Puro: co-expresses three anti-inflammatory cytokines, IL-4, IL-10, and IL-13, and also carries the eGFP fluorescent reporter gene; Transduced MOI gradient: MOI=15; Transfection groups: blank hUMSCs (control group MSCs), empty vector transfected MSCs-V, and MSCs-3IL co-expressed with three factors; Detection and verification: Transfection efficiency was detected by flow cytometry and fluorescence microscopy 48 h after transduction; IL-4 / IL-10 / IL-13 secretion by transfected cells was quantitatively detected by ELISA 72 h after transduction; positive markers CD73 / CD90 / CD105 and negative markers CD14 / CD34 / HLA-DR on stem cell surface were identified by flow cytometry; the engineered mesenchymal stromal cells that met the requirements were named MSCs-3IL.
[0073] Step 2: Seed engineered mesenchymal stromal cells MSCs-3IL in an interpenetrating network hydrogel: With a density of 2×10 4 cells / cm 2MSCs-3IL were directly seeded onto the surface of GHF+1% PNI@CUR hydrogel (Example 5), and cultured at 37°C with 5% CO2 to obtain GHF+1% PNI@CUR+MSCs-3IL.
[0074] Test case I. Physicochemical Properties of GHF+1% PNI and GHF+1% PNI@CUR Hydrogels 1. Detection method: (1) SEM microstructure: The sample was freeze-dried at -50℃ for 24h, sputtered with a 10nm gold-palladium coating, and imaged at 5000x magnification. ImageJ statistical aperture was used.
[0075] (2) Mechanical compression test: cylindrical sample Φ10mm×2mm, loading rate 4~6mm / min, temperature control at 37℃, to determine compression modulus and ultimate compressive strength.
[0076] (3) In vitro enzymatic degradation: 2 U / mL type II collagenase was incubated at 37°C with shaking, and the mass retention rate was calculated by weighing after 24 / 48 / 72 h. Hydrogels are cross-linked networks of hydrophilic polymers that can swell in water and absorb several times their own mass of water, and can undergo hydrolytic degradation in an aqueous environment. The degradation behavior of hydrogels was evaluated by incubating them in a type II collagenase solution (2 U / mL) for up to 14 days.
[0077] (4) Swelling performance: Incubate in PBS at 37℃ for 24h until equilibrium is reached, weigh and calculate the equilibrium swelling ratio (ESR).
[0078] (5) Rheological test: Parallel plate mold Φ25mm, strain scan 0.1~10% to determine the linear viscoelastic region, frequency scan 0.1~10 Hz, and record the storage modulus G'.
[0079] (6) In vitro release of curcumin: under 37℃ leaking conditions, samples were taken at 24h intervals, and the cumulative release rate was quantified by 425nm ultraviolet spectrophotometry; the temperature-sensitive network enables continuous sustained release triggered at 37℃.
[0080] (7) Blood compatibility hemolysis test: according to ASTM F756-17 standard, absorbance was measured at 540nm. The hemolysis rate was <5%, which meets the medical dressing standard.
[0081] 2. Results: like Figure 1 As shown, according to Figure 1 The preparation process flow diagram shown in A was used to prepare GelMA (Comparative Example 1), GH (Comparative Example 2), GHF (Comparative Example 3), GHF+0.1%PNII (Example 2), GHF+1%PNII (Example 1), and GHF+2.5%PNII (Example 3) hydrogels, respectively.
[0082] (1) SEM microstructure test results are as follows Figure 1 As shown in B and C, the scanning electron microscope (SEM) images of the hydrogel ( Figure 1 B) and average pore size distribution ( Figure 1 C) The results show that incorporating different concentrations of N-isopropylacrylamide (PNI) leads to changes in the average pore size and pore size distribution of the resulting hydrogel. Introducing PNI into the GHF hydrogel effectively increases the pore size, thereby promoting cell growth and nutrient diffusion while providing ample space for cells. The GHF+1%PNI hydrogel formulation exhibits the optimal pore structure, with an average pore size of 406.58±58.63 μm. Porosity is a crucial property of hemostatic dressings related to blood absorption rate. Improved porosity helps maintain a moist environment and promotes wound healing, ultimately accelerating wound closure. High porosity and a large internal pore structure (pore size >50 μm) provide ample space for cell growth. Therefore, compared to the control group, the unique microstructure of the GHF+1%PNI hydrogel exhibits superior structural stability and uniformity. The interconnected macroporous network is beneficial for increasing drug loading and promoting cell infiltration, which is crucial for wound healing.
[0083] (2) The results of the mechanical compression test are as follows Figure 1 As shown in Figure D, the GelMA hydrogel exhibits a stress of 40 kPa at 70% compressive strain. The addition of the HAMA component significantly enhances the mechanical properties of the hydrogel, with a marked increase in the compressive stress of the GH hydrogel. Furthermore, in GHF+0.1%PNII, GHF+1%PNII, and GHF+2.5%PNII hydrogels, the compressive stress further increases to over 400 kPa with increasing PNI content. The GHF+1%PNI hydrogel, while maintaining high compressive stress, can withstand a high compressive strain of 74.4 ± 2.2%. In conclusion, due to its uniform pore size, effective cell culture capability, and excellent mechanical strength, the GHF+1%PNI hydrogel was chosen for subsequent experiments.
[0084] (3) Subsequently, according to Figure 1 As shown in method A, curcumin was further synthesized into a GHF+1%PNI@CUR hydrogel based on GHF+1%PNII. The free-flow state test results of PBS, GelMA, GH, GHF, GHF+1%PNII, and GHF+1%PNI@CUR solutions are as follows... Figure 1 As shown in E, they are all in a free-flowing state before being irradiated by 405nm ultraviolet light. Figure 1 E, left), except for the PBS group, all other groups turned into a solid state after UV crosslinking ( Figure 1 E, right).
[0085] (4) Results of in vitro enzymatic degradation are as follows Figure 1 As shown in Figure F, the hydrogels formed from GelMA, GH, and GHF degraded rapidly, with approximately 50% degradation occurring within 2 days and near-complete degradation by day 5. In contrast, the GHF+1%PNI and GHF+1%PNI@CUR hydrogels exhibited slower degradation, with GHF+1%PNI@CUR showing superior performance. GHF+1%PNI@CUR only degraded by approximately 50% by day 9, after which degradation accelerated, reaching complete degradation by day 12. This prolonged degradation time better aligns with the timeline of wound healing. In the biomedical field, hydrogels with appropriate swelling ratios are promising candidate materials for drug delivery systems and tissue engineering scaffolds, facilitating controlled drug release and promoting tissue regeneration and repair.
[0086] (5) The swelling performance test results are as follows Figure 1 As shown in Figure G, each hydrogel exhibited rapid swelling behavior within the first 30 minutes, subsequently stabilizing. The equilibrium swelling ratio reached approximately 130%-150%. Although the introduction of PNI slightly reduced the swelling capacity of the GHF+1%PNI@CUR hydrogel due to increased crosslinking density, there was no significant difference between the groups (p>0.05). These results indicate that all hydrogel formulations possess good tissue regeneration and repair properties.
[0087] (6) Rheological test results are as follows Figure 1 As shown in H, the elastic modulus of each hydrogel formulation is approximately 1.14 kPa. Statistical analysis showed no significant difference between groups (p>0.05), closely resembling the mechanical properties of human skin. Gelation behavior was confirmed by G' being higher than G'' throughout the entire test time and angular frequency range, indicating the formation of a stable hydrogel. This mechanical stability was maintained throughout the measurement period. Rheological analysis revealed the effects of shear rate and temperature on the storage modulus (G', representing elastic behavior) and loss modulus (G'', representing viscous behavior). The elastic modulus of biological tissues is crucial for cell function; the elastic modulus of human skin typically ranges from 0.9 to 20 kPa. Pathological conditions are often associated with alterations in tissue mechanical properties. Therefore, achieving an appropriate elastic modulus is essential for supporting normal cell growth, differentiation, and function when designing hydrogel materials for regenerative applications. Thus, the GHF+1%PNI@CUR hydrogel prepared in this invention possesses the potential to support normal cell growth, differentiation, and function, providing a mechanical basis for its application in wound repair.
[0088] In summary, the GHF+1%PNI@CUR hydrogel of this invention possesses optimal physicochemical properties, including suitable adhesion, controllable degradation, appropriate swelling behavior, and good rheological properties. These combined properties make this material ideally suited for wound treatment applications, as all measured parameters meet the requirements for effective tissue repair. Experimental data demonstrate that the GHF+1%PNI@CUR hydrogel exhibits optimal physicochemical properties, including strong mechanical strength, favorable degradation kinetics synchronized with drug release profiles, and excellent cell adhesion. These comprehensive characteristics establish this hydrogel system as a promising therapeutic platform for controlled drug delivery and tissue engineering applications.
[0089] II. Validation of the wound repair effect of GHF+1% PNI@CUR+MSCs-3IL in diabetic mice 1. Method: (1) Diabetes model construction: C57BL / 6 male mice aged 6-8 weeks were injected intraperitoneally with streptozotocin (STZ) at a dose of 150 mg / kg. The model was considered successful when the fasting blood glucose was ≥16.7 mmol / L. (2) Wound model: A full-thickness skin wound with a diameter of 8 mm was created on the back of each mouse; Groups: blank group, hydrogel group (GHF+1% PNI@CUR), cell suspension group (MSCs-3IL), and cell-loaded hydrogel group (GHF+1% PNI@CUR+MSCs-3IL). (3) Wound healing and systemic inflammation detection: On days 0, 3, 7 and 14, gross images of mouse skin wounds were taken at a specific focal length to assess the wound healing process; at the end point, blood was collected from the orbital ELISA to detect the serum levels of IL-6, TNF-α and IL-4 systemic inflammation. 2. Results: (1) The establishment and experimental procedure of the mouse diabetic wound model are as follows: Figure 2 As shown in Figure A, compared with the healthy control group, on day 10 after STZ injection, the fasting blood glucose level of C57BL / 6J mice exceeded 16.7 mmol / L, and the model group mice showed symptoms of weight loss, polyuria, polydipsia and polyphagia, confirming the successful induction of the model.
[0090] (2) Wound repair results are as follows Figure 2As shown in BD, on day 3, the wound closure rate of the GHF+1%PNI@CUR+MSCs-3IL group (27%) was significantly better than that of other groups, which may indicate that GHF+1%PNI@CUR+MSCs-3IL has shown good effects in reducing inflammation and regulating the wound microenvironment in the early stage of wound healing. Furthermore, on day 7, the closure rate of GHF+1%PNI@CUR+MSCs-3IL (50%) was higher than that of the control group (28%) and the MSCs-3IL group (35%). In addition, compared with the control group, the GHF+1%PNI@CUR hydrogel group showed faster wound closure after day 7. On day 14, the wound closure rate of the GHF+1%PNI@CUR+MSCs-3IL group was 94%, which was significantly higher than that of the blank group (44%), the GHF+1%PNI@CUR group (71%) and the MSCs-3IL group (69%). Compared with the blank group, the GHF+1%PNI@CUR+MSCs-3IL group accelerated the healing of diabetic wounds by 40%.
[0091] (3) Results of systemic inflammation level Figure 2 As shown in Figure E, compared with the control group, the GHF+1%PNI@CUR+MSCs-3IL group had lower levels of inflammatory factors (IL-6, TNF-α, IL-4), indicating that systemic inflammation was not significant. GHF+1%PNI@CUR+MSCs-3IL may provide durable anti-inflammatory and regenerative signals to accelerate and promote the healing of full-thickness skin defects, thus demonstrating synergistic therapeutic potential in the repair of diabetic wounds.
[0092] (4) Histological examination results as follows Figure 3 As shown, where Figure 3 A, 3C-F showed that, compared with the control group, on days 3 and 7, the GHF+1%PNI@CUR+MSCs-3IL group significantly reduced the percentage of iNOS-positive macrophages (a 17.9-fold decrease on day 7, P<0.001) and increased CD206-positive macrophages at the wound site, especially on day 7 (a 14.8-fold increase in CD206), indicating a reduced inflammatory state; Figure 3 As shown in B and 3G-J, compared with the control group, the GHF+1%PNI@CUR+MSCs-3IL group exhibited low levels of IL-6 and high levels of IL-10 in diabetic wounds on days 3 and 7, indicating excessive inflammation. These findings suggest that GHF+1%PNI@CUR+MSCs-3IL induces macrophage phenotypic polarization from M1 to M2, releases anti-inflammatory factors, and promotes the transition of wounds from the inflammatory phase to the remodeling phase.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. An interpenetrating network hydrogel, characterized in that, It is made by a hydrogel mixture comprising: 4% to 6% by weight and volume of methacrylamide gelatin, 0.4% to 0.6% by weight and volume of methacrylamide hyaluronic acid, 0.5% to 25% by weight and volume of N-isopropylacrylamide, and 0.0008% to 0.0012% by weight and volume of fibronectin.
2. The interpenetrating network hydrogel as described in claim 1, characterized in that, The hydrogel mixture of the interpenetrating network hydrogel further includes: an anti-inflammatory active drug at a mass-volume percentage of 0.04% to 0.06%, a photoinitiator at a mass-volume percentage of 0.2% to 0.3%, a crosslinking agent, and an initiator; wherein the mass ratio of the crosslinking agent to N-isopropylacrylamide is (2~4):50; and the mass ratio of the initiator to N-isopropylacrylamide is (0.5~1.5):
10.
3. The interpenetrating network hydrogel according to claim 1 or 2, characterized in that, The N-isopropylacrylamide has a mass-volume percentage of 1%; or / and the mass ratio of the crosslinking agent to N-isopropylacrylamide is 3:50; the mass ratio of the initiator to N-isopropylacrylamide is 1:
10.
4. A hydrogel with an interpenetrating network of engineered mesenchymal matrix cells, characterized in that, It is composed of an interpenetrating network hydrogel load as described in any one of claims 1-3 and a filler matrix cell, wherein the filler matrix cell density is 1×10⁻⁶. 4 ~3×10 4 cells / cm 2 .
5. The interpenetrating network hydrogel as described in claim 4, characterized in that, The mesenchymal cells overexpress anti-inflammatory factors.
6. The interpenetrating network hydrogel as described in claim 5, characterized in that, The anti-inflammatory factor is a combination of interleukin-4, interleukin-10 and interleukin-13.
7. The use of the interpenetrating network hydrogel according to any one of claims 1-3 or the interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells according to any one of claims 4-6 in any of the following: (1) Application in the preparation of materials for treating or repairing wounds; (2) Application in the preparation of biological scaffold materials that promote tissue regeneration; (3) Application in the preparation of anti-inflammatory or immunomodulatory medical dressings.
8. The application as described in claim 7, characterized in that, The wound is a chronic diabetic wound or a burn wound.
9. The method for preparing the interpenetrating network hydrogel as described in claim 2, characterized in that, Includes the following steps: (1) Methacrylamide gelatin, methacrylamide hyaluronic acid, fibronectin and N-isopropylacrylamide were added sequentially to the photoinitiator solution and mixed evenly to obtain a prepolymer solution; (2) Add crosslinking agent, initiator and curcumin solution to the prepolymer solution; (3) The mixture obtained in step (2) is injected into the mold and cross-linked by ultraviolet light to form an interpenetrating network hydrogel.
10. The method for preparing the interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells as described in claim 4, characterized in that, Includes the following steps: (1) Culture engineered mesenchymal stromal cells overexpressing anti-inflammatory factors and collect the cells; (2) The cells are directly seeded onto the surface of the interpenetrating network hydrogel as described in claim 2; (3) Place the inoculated hydrogel in an incubator for static culture so that the cells can fully adhere to the surface and pores of the hydrogel to obtain an interpenetrating network hydrogel loaded with engineered mesenchymal matrix cells.