An inorganic particle covalently bonded polyolefin composite separator and a method for preparing the same
By using a method for preparing a polyolefin composite membrane covalently bonded to inorganic particles, the problems of gas cross-diffusion and inorganic particle agglomeration in the composite membrane were solved, achieving high mechanical strength, alkali resistance, and long-term stability, thereby improving the efficiency and safety of alkaline water electrolysis.
Patent Information
- Application Number
- CN202611517899.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-20
AI Technical Summary
Existing composite membranes have high porosity in alkaline water electrolysis, which leads to a high probability of gas cross-diffusion, affecting hydrogen purity and equipment safety. At the same time, inorganic particle agglomeration and long-term operation desorption problems result in decreased mechanical properties and reduced electrolysis efficiency.
An inorganic particle covalently bonded polyolefin composite membrane is prepared by modifying the surface of inorganic particles with a silane coupling agent to form a branched silane coupling agent layer. Combined with quaternary ammonium groups and a crosslinking agent, in-situ crosslinking and secondary crosslinking are carried out to establish covalent connections at the molecular level and construct a highly crosslinked composite membrane.
It significantly improves the mechanical strength and alkali resistance of the composite membrane, inhibits the agglomeration of inorganic particles, reduces desorption during long-term operation, and enhances the stability and electrolysis efficiency of the membrane.
Smart Images

Figure CN123131663A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of membrane technology, and in particular to an inorganic particle covalently bonded polyolefin composite membrane and its preparation method. Background Technology
[0002] Alkaline water electrolysis (AWE) using composite membranes is one of the most mature water electrolysis technologies currently available. Compared to proton exchange membrane electrolysis, AWE uses low-cost non-platinum group metal catalysts, and its polymer backbone does not contain fluorine, making it more environmentally friendly. To improve electrolysis performance, AWE electrolyzers typically use a 30 wt% KOH solution combined with a porous composite membrane. Zirconia is added to the composite membrane to utilize its high hydrophilicity and the formation of larger pores by its inorganic particles, thereby improving the membrane's absorption capacity for alkaline solutions. However, high porosity is a double-edged sword: while it increases the efficiency of alkaline water electrolysis, it also increases the probability of gas cross-diffusion, adversely affecting hydrogen purity and the safety of the electrolysis equipment. Furthermore, the agglomeration of zirconium oxide during membrane preparation and its desorption during long-term operation can also significantly affect membrane performance.
[0003] To address the aforementioned issues, several solutions exist. One approach is to spray a dense layer of cross-linked polyvinyl alcohol (PVA) onto the surface of the Zirfon membrane to block gas cross-transmission and improve equipment safety. However, this method also hinders alkali absorption to some extent, reducing electrolysis efficiency. Another approach involves preparing asymmetric composite membrane structures using a solvent-inducible phase separation method. A dense gas barrier layer is constructed on one side of the membrane to prevent gas cross-transmission and increase the membrane's bubble point pressure, while finger-like pores are constructed on the other side to balance electrolyte absorption and gas permeability. However, this asymmetric structure also has limitations, namely, a relatively loose overall structure and significantly reduced mechanical properties. Therefore, preparing a composite membrane with high alkali absorption capacity, high gas barrier properties, and high mechanical properties to replace existing Zirfon composite membranes has significant scientific and industrial value. Summary of the Invention
[0004] In view of this, this application provides an inorganic particle covalently bonded polyolefin composite membrane and its preparation method. The prepared polyolefin composite membrane has the advantages of high mechanical strength, alkali resistance and long-term stable operation, which effectively solves the problems of easy gelation and difficult film formation of composite membrane slurry, as well as the problems of inorganic particle agglomeration and desorption during long-term operation in traditional composite membranes.
[0005] This application provides a method for preparing an inorganic particle covalently bonded polyolefin composite separator, comprising the following steps: Step 1: Styrene, acrylonitrile, and 4-chloromethylstyrene are polymerized to obtain the initial casting solution; Step 2: Quaternize the initial casting solution to obtain an olefin anion film solution; Step 3: After mixing the olefin anion membrane solution, silane coupling modified inorganic particles and crosslinking agent, an in-situ crosslinking reaction is carried out, followed by ultrasonic crushing to obtain a mixed slurry; Step 4: Prepare olefin-based cross-linked membranes using a mixed slurry and a composite membrane support; Step 5: Perform secondary cross-linking on the olefin-based cross-linked membrane to obtain an olefin-based composite membrane.
[0006] In some specific implementations, in step 1, the molar ratio of styrene, acrylonitrile, and 4-chloromethylstyrene is (0.1~5):(0.1~12):(0.1~5).
[0007] In some specific implementations, in step 2, the quaternizing agent for the quaternization reaction is N-methylpyrrolidine, N-methylpiperidine, 1-methylazacycloheptane, 4-methylmorpholine, quinine ring, 1,4-dimethylpiperidine, 1,3,5-trimethylpiperidine, 1,2,6-trimethylpiperidine, N-methyldipropylamine, or trimethylamine; The mass of the quaternizing reagent is 5% to 60% of the mass of 4-chloromethylstyrene.
[0008] In some specific implementations, in step 3, the method for preparing the silane coupling modified inorganic particles is as follows: a silane coupling reagent, deionized water and inorganic particles are subjected to a silane coupling reaction. The silane coupling agent is one or more selected from 3-(2,3-epoxypropoxy)propyltrimethoxysilane, epoxycyclohexyltrimethoxysilane and epoxycyclohexyltriethoxysilane; The inorganic particles are nano-zirconia particles with a particle size of 10 nm to 200 nm.
[0009] In some specific implementations, in step 3, the mass of the silane-coupled modified inorganic particles accounts for 40% to 90% of the total mass of the mixed slurry.
[0010] In some specific implementations, the crosslinking agent is selected from one or more of polyethyleneimine, small molecule polytertiary amines, and amino-terminated polyethers; The small molecule polytertiary amine is N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, 4,4'-trimethylenebis(1-methylpiperidine), N,N,N',N'',N''-pentamethyldiethylenetriamine or tris(2-dimethylaminoethyl)amine; The terminal amino polyether is O,O′-bis(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol, O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol-block-polyethylene glycol, or O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol; The crosslinking agent accounts for 0.01% to 1.0% of the total mass of the mixed slurry.
[0011] In some specific implementations, in step 4, the thickness of the composite membrane support is 20 μm to 200 μm; The composite membrane support is one or more of polyphenylene sulfide, polyether ether ketone, polysulfone, and polytetrafluoroethylene.
[0012] In some specific implementations, in step 5, the secondary crosslinking reaction is: immersing the olefin crosslinked membrane in a crosslinking agent solution and then performing heat treatment; The crosslinking agent solution comprises a crosslinking agent and a solvent, wherein the crosslinking agent is polyethyleneimine; The mass ratio of the crosslinking agent to the solvent is 1:(1~200). Soaking time is 10 min to 72 h.
[0013] In some specific implementations, the temperature of the heat treatment is 30℃~80℃.
[0014] This application also provides an inorganic particle covalently bonded polyolefin composite membrane, which is obtained according to the preparation method described in any of the above technical solutions.
[0015] The crosslinking system provided in this application is novel and its preparation method is simple. Through the rational design of the inorganic nanoparticle structure, covalent bonding between inorganic particles and an organic framework is achieved, and its beneficial effects are reflected in the following aspects: The method for preparing an inorganic particle covalently bonded polyolefin composite membrane provided in this application utilizes a silane coupling agent to surface-treat the inorganic particles, forming a branched silane coupling agent physical shielding layer on the particle surface and introducing reactive epoxy groups. Simultaneously, olefin polymer monomers without aromatic ether bonds are selected to construct the membrane framework, and during polymerization, functional groups such as chloromethyl crosslinking sites and quaternary ammonium groups are grafted onto the framework, endowing the membrane framework with excellent alkali resistance and flexible design potential. Then, the silane coupling agent-modified inorganic particles are dispersed in a polyolefin framework slurry containing chloromethyl groups, and a portion of a crosslinking agent is added. A first in-situ crosslinking is performed before membrane formation, initially constructing a crosslinked network, effectively preventing slurry gelation and successfully preparing a porous composite membrane. Finally, the obtained porous membrane is immersed in a water-soluble crosslinking agent solution and heated. Molecular thermal motion allows the crosslinking agent to fully penetrate, completing a secondary crosslinking through a nucleophilic substitution reaction, establishing a molecular-level covalent connection between the organic segments and inorganic particles, thereby obtaining a highly crosslinked composite membrane.
[0016] The inorganic particle covalently bonded polyolefin composite membrane provided in this application features a physical shielding layer formed by the silane coupling agent coating the surface of inorganic particles with a branched silane coupling agent layer. This significantly reduces the surface energy of the particles, allowing them to disperse uniformly within the membrane, effectively inhibiting agglomeration, reducing stress concentration within the composite membrane, and improving mechanical properties. The chloromethyl groups on the membrane backbone covalently bond with the epoxy groups on the modified particle surface under the action of a crosslinking agent, adding molecular-level chemical bridging to the traditional physical coating. This significantly reduces desorption of inorganic particles during long-term operation, ensuring the membrane's long-term operational stability. The membrane backbone is composed of a non-aromatic olefin polymer, and its carbon-carbon backbone structure provides excellent alkali resistance. Furthermore, the benzyl chloride crosslinking sites and functional groups that can be grafted onto the backbone allow for precise control of the composite membrane's performance through flexible adjustment of monomers and dosages. Furthermore, by employing a stepwise crosslinking process, pre-crosslinking is performed before film formation and then deep crosslinking is performed after film formation. This solves the common problem of high-activity crosslinking systems being prone to gelation and difficult to form films. The resulting composite membrane has a high degree of crosslinking and a dense and stable structure, providing a new technical path for the construction of high-stability composite membranes. Attached Figure Description
[0017] Figure 1 The silane-coupled modified zirconium oxide prepared in step 3 of Example 1; Figure 2 The polyolefin composite membrane prepared in Example 1; Figure 3 This is a schematic diagram of the polyolefin composite membrane prepared in Example 1; Figure 4 The nuclear magnetic resonance spectrum of the polyolefin composite membrane prepared in Example 1; Figure 5This is a diagram of the alkaline membrane water electrolysis device used in Experiment Example 9. Figure 6 Electrolysis test results of the polyolefin composite membrane prepared in Example 1 and the commercial Zirfon membrane; Figure 7 The image shows the electrolytic water stability test results of the polyolefin composite membrane prepared in Example 1. Detailed Implementation
[0018] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.
[0019] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.
[0020] It should be understood that the order of steps or the sequence of actions is not important as long as this application remains operational. Furthermore, two or more steps or actions may be performed simultaneously.
[0021] The use of any and all instances or exemplary language such as “e.g.” or “including” herein is merely intended to better illustrate the application and does not constitute a limitation on the scope of the application unless the claims are made. No language in this specification should be construed as indicating that any unclaimed element is essential to the practice of this application.
[0022] Furthermore, the numerical ranges and parameters used to define this application are approximate values, and the relevant values in the specific embodiments have been presented as precisely as possible. However, any numerical value inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise explicitly stated, it should be understood that all ranges, quantities, values, and percentages used in this disclosure are modified with the word "approximately." Here, "approximately" generally means that the actual value is within plus or minus 10%, 5%, 1%, or 0.5% of a specific value or range.
[0023] This application provides a method for preparing an inorganic particle covalently bonded polyolefin composite separator, comprising the following steps: Step 1: Styrene, acrylonitrile, and 4-chloromethylstyrene are polymerized to obtain the initial casting solution; Step 2: Quaternize the initial casting solution to obtain an olefin anion film solution; Step 3: After mixing the olefin anion membrane solution, silane coupling modified inorganic particles and crosslinking agent, an in-situ crosslinking reaction is carried out, followed by ultrasonic crushing to obtain a mixed slurry; Step 4: Prepare olefin-based cross-linked membranes using a mixed slurry and a composite membrane support; Step 5: Perform secondary cross-linking on the olefin-based cross-linked membrane to obtain an olefin-based composite membrane.
[0024] This application describes a polymerization reaction of styrene, acrylonitrile, and 4-chloromethylstyrene to obtain an initial casting solution.
[0025] Specifically, styrene (ST), acrylonitrile (AN), and 4-chloromethylstyrene (VBC) are mixed in a solvent, and an initiator is added to carry out a preliminary polymerization reaction to obtain an initial casting solution. This application does not limit the sources of styrene (ST), acrylonitrile (AN), 4-chloromethylstyrene (VBC), the solvent, and the initiator. In some specific implementations, the solvent is one or more of N-methylpyrrolidone, dimethylformamide, dimethylacetamide, and dimethyl sulfoxide, preferably dimethyl sulfoxide. In some specific implementations, the initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, and dicumyl peroxide, preferably azobisisobutyronitrile. In some specific implementations, this application also includes purification treatment of styrene, acrylonitrile, 4-chloromethylstyrene, and the initiator. In some specific implementations, the purification process involves extracting styrene, acrylonitrile, and 4-chloromethylstyrene with an aqueous sodium hydroxide solution, wherein the concentration of the sodium hydroxide solution is 0.1 mol / L to 1.5 mol / L, preferably 0.5 mol / L to 1.0 mol / L. In some specific implementations, the purification process involves recrystallizing the initiator with a methanol solution.
[0026] In some specific implementations, the molar ratio of styrene, acrylonitrile, and 4-chloromethylstyrene is (0.1~5):(0.1~12):(0.1~5), preferably (0.1~4):(0.1~8):(0.1~4). In some specific implementations, the mass of the initiator is 0.001 to 0.4 times the total mass of the three monomers (styrene, acrylonitrile, and 4-chloromethylstyrene), preferably 0.001 to 0.3 times. In some specific implementations, the polymerization reaction is preferably carried out under nitrogen protection. In some specific implementations, the polymerization reaction temperature is 50℃ to 100℃, preferably 60℃ to 80℃, more preferably 70℃. In some specific implementations, the polymerization reaction time is 3 h to 7 h, preferably 4 h to 6 h. In some specific implementations, the polymerization reaction is preferably carried out under stirring conditions, with a stirring speed of 500 rpm to 700 rpm.
[0027] After obtaining the initial casting solution, the initial casting solution is subjected to a quaternization reaction to obtain an olefin anion film solution.
[0028] Specifically, after heating and stirring the initial casting solution, when a large number of bubbles are generated in the initial casting solution, a quaternizing agent is added to carry out a quaternization reaction to obtain an olefin anion film solution. This application does not limit the stirring conditions. In some specific implementations, the quaternizing agent for the quaternization reaction is N-methylpyrrolidine, N-methylpiperidine, 1-methylazacycloheptane, 4-methylmorpholine, quinine ring, 1,4-dimethylpiperidine, 1,3,5-trimethylpiperidine, 1,2,6-trimethylpiperidine, N-methyldipropylamine, or trimethylamine, preferably N-methylpiperidine. In some specific implementations, the mass of the quaternizing agent is 5% to 60% of the mass of 4-chloromethylstyrene, preferably 35% to 55%, and more preferably 45%.
[0029] In some specific implementations, the temperature of the quaternization reaction is 30℃~60℃, preferably 35℃~45℃. In some specific implementations, the time of the quaternization reaction is 20 h~48 h, preferably 24 h~30 h.
[0030] After obtaining the olefin anion membrane solution, the olefin anion membrane solution, silane coupling modified inorganic particles and crosslinking agent are mixed and then subjected to in-situ crosslinking reaction. After ultrasonic crushing, a mixed slurry is obtained.
[0031] The above reaction is carried out in a solvent, including but not limited to dimethyl sulfoxide. In some specific implementations, the mass of the silane-coupled modified inorganic particles accounts for 40% to 90% of the total mass of the mixed slurry, preferably 50% to 80%. In some specific implementations, the mass of the crosslinking agent accounts for 0.01% to 1.0% of the total mass of the mixed slurry, preferably 0.05% to 0.8%. In some specific implementations, the crosslinking agent is selected from one or more of polyethyleneimine, small molecule polytertiary amines, and amino-terminated polyethers, preferably polyethyleneimine. In some specific implementations, the small molecule polytertiary amine is N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, 4,4'-trimethylenebis(1-methylpiperidine), N,N,N',N'',N''-pentamethyldiethylenetriamine, or tris(2-dimethylaminoethyl)amine. In some specific implementations, the terminal amino polyether is O,O′-bis(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol, O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol-block-polyethylene glycol, or O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol. In some specific implementations, the temperature of the in-situ crosslinking reaction is 70℃~90℃, preferably 80℃.
[0032] In some specific implementations, the method for preparing the silane coupling modified inorganic particles is as follows: a silane coupling reagent, deionized water, and inorganic particles are subjected to a silane coupling reaction.
[0033] Specifically, the silane coupling reagent is hydrolyzed and then added to a solvent to carry out the silane coupling reaction. After the reaction is completed, the modified inorganic particles are washed, dried, bottled, and stored for later use.
[0034] The above reaction is carried out in a solvent, including but not limited to anhydrous ethanol. In some specific implementations, the hydrolysis is performed by mixing the silane coupling agent with deionized water, wherein the mixing ratio of the silane coupling agent to water is 1:(0.1~10). In some specific implementations, the silane coupling agent is one or more of glyceroxypropyltrimethoxysilane, glyceroxypropyltriethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, cyclohexyloxysilane, and cyclohexyloxytriethoxysilane, preferably 3-(2,3-epoxypropoxy)propyltrimethoxysilane. In some specific implementations, the inorganic particles are one or more of nano-alumina, nano-zinc oxide, nano-titanium dioxide, nano-silica, and nano-zirconia, preferably nano-zirconia. In some specific implementations, the particle size of the inorganic particles is 10 nm~200 nm, preferably 10 nm~150 nm.
[0035] In some specific implementations, the mass ratio of the silane coupling agent to the solvent is 1:(10~200), preferably 1:(10~120). In some specific implementations, the silane coupling reaction is preferably carried out under nitrogen protection, with the mixed liquid heated to 70℃~110℃, refluxed, and stirred for 3 h~6 h. In some specific implementations, the cleaning method is as follows: the nano-zirconia anhydrous ethanol mixed solution is centrifuged, the supernatant is discarded, anhydrous ethanol is added, and the mixture is ultrasonically cleaned repeatedly by centrifugation and ultrasonication 3~6 times, and finally dried in a vacuum drying oven for later use. After obtaining the mixed slurry, an olefin-based cross-linked membrane is prepared using the mixed slurry and the composite membrane support.
[0036] Specifically, the composite membrane support is fixed on a glass plate, a mixed slurry is applied to the glass plate, and then the slurry is smoothed with a scraper. The glass plate is then moved to a heating stage for pre-evaporation, and then moved to a phase inversion liquid for solvent-induced phase separation. After phase inversion, the glass plate is removed, and the residual phase inversion liquid is rinsed off with deionized water to obtain an olefin-based crosslinked membrane.
[0037] In some specific implementations, the thickness of the composite membrane support is 20 μm to 200 μm, preferably 30 μm to 100 μm. In some specific implementations, the composite membrane support is one or more of polyphenylene sulfide, polyetheretherketone, polysulfone, and polytetrafluoroethylene, preferably polyphenylene sulfide. In some specific implementations, the pre-evaporation time is 3 min to 10 min, preferably 5 min. In some specific implementations, the pre-evaporation temperature is 60℃ to 100℃, preferably 80℃. In some specific implementations, the phase inversion liquid is a mixture of isopropanol and deionized water in a volume ratio of 1:(1~3), preferably 1:1.
[0038] After obtaining the olefin-based cross-linked membrane, the olefin-based cross-linked membrane is subjected to secondary cross-linking to obtain an olefin-based composite membrane.
[0039] In some specific implementations, the secondary crosslinking reaction involves immersing the olefin-based crosslinked membrane in a crosslinking agent solution followed by heat treatment. In some specific implementations, the crosslinking agent solution comprises the crosslinking agent and solvent described in the above technical solutions. The crosslinking agent is selected from polyethyleneimine, and the polyethyleneimine types include, but are not limited to, branched-MW-1800, branched-MW-10000, branched-MW-25000, average-MW-1300, average-MW-1800, average-MW-10000, or average-MW-25000.
[0040] In some specific implementations, the crosslinking agent solution comprises a crosslinking agent and a solvent, wherein the crosslinking agent is polyethyleneimine, and the mass ratio of the crosslinking agent to the solvent is 1:(1~200), preferably 1:(1~150). In some specific implementations, the soaking time is 10 min~72 h, preferably 30 min~36 h, more preferably 12 h~30 h. In some specific implementations, after soaking, heat treatment is performed at a temperature of 30℃~80℃, preferably 40℃~60℃. In some specific implementations, the heat treatment time is 12 h~36 h, preferably 18 h~28 h.
[0041] This application also provides an inorganic particle covalently bonded polyolefin composite membrane, which is obtained according to the preparation method described in any of the above technical solutions.
[0042] This application provides a method for preparing an inorganic particle covalently bonded polyolefin composite membrane, relating to the field of alkaline water electrolysis hydrogen production membrane technology. The composite membrane consists of inorganic oxide particles surface-modified with a silane coupling agent and carrying epoxy groups, a polyolefin backbone containing chloromethyl and functional groups without aromatic ether bonds, and a crosslinking agent. The preparation employs a stepwise crosslinking process to covalently link the modified oxide particles and the olefin membrane backbone. Modification with a silane coupling agent reduces the surface energy of the inorganic particles to prevent agglomeration, effectively solving the problems of inorganic particle agglomeration and long-term desorption in traditional composite membranes. This significantly improves the membrane's mechanical strength, alkali resistance, and long-term operational stability, providing technical support for industrial preparation and application.
[0043] The present application is further illustrated below with reference to embodiments. The scope of protection of the present application is not limited to the following embodiments.
[0044] Note: KH560 is 3-(2,3-epoxypropoxy)propyltrimethoxysilane; ST is styrene; AN is acrylonitrile; VBC is 4-chloromethylstyrene; AIBN is azobisisobutyronitrile.
[0045] Example 1
[0046] Step 1: Take ST, AN, and VBC as precursors, and extract them separately with 0.5 mol / L sodium hydroxide aqueous solution. Remove residual water from the extracted VBC with anhydrous sodium sulfate, store in glass bottles and refrigerate for later use. At the same time, recrystallize AIBN with methanol to obtain needle-like crystals for later use. Weigh 6.6 g of purified ST, 8.92 g of AN, 18.6 g of VBC and 96.8 mL of dimethyl sulfoxide into a 250 mL round-bottom flask, add 0.4 g of AIBN to initiate the polymerization reaction; under nitrogen protection, place the round-bottom flask in a 70°C oil bath and stir for 5 h to obtain the initial casting solution. Step 2: Add 12.6 g of N-methylpiperidine to the prepared initial membrane solution, cool to 50°C, reduce the stirrer speed, and keep the reaction at this temperature overnight to obtain an olefin anion membrane solution; Step 3: Weigh 0.5 g of KH560 and 2 g of deionized water into a centrifuge tube, add 20 mL of anhydrous ethanol, and stir at room temperature for 1 h to obtain a hydrolyzed KH560 mixture. Transfer the mixture to a 250 mL three-necked flask, add 20 g of 30 nm diameter zirconium oxide particles and 120 mL of anhydrous ethanol, then transfer the three-necked flask to a heated magnetic stirrer, adjust the temperature to 100℃, the rotation speed to 500 rpm, and connect a reflux condenser. Maintain the temperature and stir for 4 h to stop the reaction. Remove the mixture from the three-necked flask, divide it into batches into centrifuge tubes, centrifuge at 8000 rpm for 5 min, discard the supernatant, add 35 mL of anhydrous ethanol again, and perform ultrasonic cleaning and centrifugation. Repeat this step 5 times. After cleaning and centrifugation, dry the product in a vacuum oven and bottle it for later use. The obtained silane-coupled modified zirconium oxide, as shown... Figure 1 As shown; Take 5 g of the olefin anion exchange solution from step 2, 2.25 g of silane-coupled modified zirconium oxide, and 12.5 g of DMSO and add them to a 50 mL centrifuge tube for overnight stirring and mixing. After mixing, take 10 mL of the slurry and sonicate it for 30 min. Then add 0.68 g of PEI crosslinking agent (branched-MW-10000) diluted to 5 wt% with DMSO, and sonicate it for another 5 min to obtain a uniformly mixed composite membrane slurry. Step 4: Take a glass plate with a side length of 10 cm, and fix the polyphenylene sulfide mesh to the glass plate with 50 μm double-sided tape. Take the uniform composite membrane slurry from Step 3, apply it to the glass plate, and then use a scraper to smooth the slurry. Then, move the glass plate to a heating stage for pre-evaporation for 5 min, and then move the glass plate to a phase inversion liquid for non-solvent-induced phase separation. The phase inversion liquid is a mixture of isopropanol and deionized water (volume ratio of 1:1). After overnight phase inversion, remove the glass plate and rinse it with deionized water to remove the residual phase inversion liquid, thus obtaining a composite membrane with a porous structure. Step 5: Dissolve 1 g of branched-MW-10000 PEI crosslinking agent in 20 mL of deionized water, mix well to obtain a crosslinking agent solution, place the crosslinking agent solution in a wide-mouth reagent bottle, then fully immerse the composite membrane obtained in Step 4 in the crosslinking agent solution and heat to 50℃. After maintaining the temperature for 24 h, the secondary crosslinking strengthening is completed, and the final composite membrane is obtained. Figure 2 As shown. The preparation principle of its composite membrane is as follows. Figure 3 As shown, zirconia was first functionalized using hydrolyzed KH560. Hydrolyzed KH560 has a hydroxyl group at one end and an epoxy group at the other. Under high-temperature catalysis, the hydroxyl group and the hydroxyl group originally present on the zirconia surface undergo a condensation reaction, allowing KH560 to graft onto the zirconia particles. Therefore, the modified zirconia carries epoxy groups on its outer surface. Both the epoxy groups and the chloromethyl sites on the olefin membrane chain can undergo substitution reactions with PEI, thereby linking the zirconia, crosslinking agent, and olefin membrane backbone together.
[0047] Example 2
[0048] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 1, the content of ST is 7.6 g; In step 3, the content of KH560 is 1.5 g, the heat preservation and stirring time is 4.5 h, and the molecular weight of PEI crosslinking agent is MW-1800.
[0049] Example 3
[0050] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 1, the content of AN is 7.6 g and the content of AIBN is 0.6 g; In step 3, the content of KH560 is 2.5 g; the content of silane-coupled modified zirconium oxide is 2.6 g; In step 4, the volume ratio of isopropanol to deionized water is 2:1.
[0051] Example 4
[0052] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 1, the content of VBC is 12.6 g and the content of AIBN is 0.6 g; In step 3, the diameter of the zirconium oxide particles is 50 nm; the content of silane-coupled modified zirconium oxide is 3.2 g, and the content of PEI crosslinking agent is 0.56 g; In step 4, the volume ratio of isopropanol to deionized water is 3:1.
[0053] Example 5
[0054] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 2, the content of N-methylpiperidine is 8.6 g; In step 3, the zirconium oxide is a blend of zirconium oxide with a diameter of 50 nm and zirconium oxide with a diameter of 30 nm in a mass ratio of 1:1; the content of silane coupling modified zirconium oxide is 3.0 g, and the crosslinking agent is O,O′-bis(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol. In step 4, the pre-evaporation time is 10 minutes.
[0055] Example 6
[0056] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 2, the heating time is 6 hours, and the magnetic stirrer speed is not reduced after adding N-methylpiperidine; In step 3, the zirconium oxide is a blend of zirconium oxide with a diameter of 100 nm and zirconium oxide with a diameter of 30 nm in a mass ratio of 1:2; the content of silane coupling modified zirconium oxide is 2.8 g, and the crosslinking agent is O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol-block-polyethylene glycol. In step 5, the temperature of the crosslinking agent liquid is 60°C.
[0057] Example 7
[0058] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 2, the heating time is 5.5 h, and the content of N-methylpiperidine is 16.6 g; In step 3, the content of anhydrous ethanol is 160 mL; the content of silane coupling modified zirconium oxide is 2.6 g; and the crosslinking agent is O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol. In step 5, the amount of deionized water is 50 mL.
[0059] Example 8
[0060] This embodiment uses the same preparation method as Example 1 to prepare the polyolefin composite film, the only difference being: In step 2, the concentration of DMSO was 78.8 mL; In step 3, the diameter of the zirconium oxide particles is 100 nm; the content of silane-coupled modified zirconium oxide is 5 g; and the crosslinking agent is PEI-branched-MW-10000. In step 5, the heating and heat preservation time is 72 hours.
[0061] Experimental Example 1
[0062] An appropriate amount of the sample prepared in Example 1 was dissolved in a deuterated solvent (DMSO-d6), and nuclear magnetic resonance spectroscopy was performed at room temperature. 1 The 1H NMR test was performed, and the resulting spectrum can be found in [reference]. Figure 4 , Figure 4 The image shows the nuclear magnetic resonance spectrum of the polyolefin composite membrane prepared in Example 1. The experimental results indicate that the composite membrane was successfully prepared.
[0063] Experimental Example 2: Conductivity Test
[0064] The conductivity of the ion exchange membrane was tested using an Auto Lab electrochemical workstation.
[0065] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane were cut into strips of 1 cm × 4 cm. Each membrane was then independently ion-exchanged with a 1 mol / L KOH solution to fully exchange ion with OH radicals. - The sample is then thoroughly washed with deionized water to remove free ions. During testing, the ion-exchange membrane sample is clamped in a PTFE fixture, and the electrochemical impedance spectroscopy is measured in constant current mode, with a frequency range of 100 Hz to 1 MHz. The measured resistance is recorded as R. The formula for calculating conductivity is as follows: ; Where L represents the distance between the two sensing electrodes (cm); R represents the resistance; W is the width of the ion membrane sample (cm); and d is the thickness of the ion membrane sample (cm).
[0066] The conductivity of the polyolefin composite membranes and Zirfon membranes prepared in Examples 1-8 was calculated, and the test results are shown in Table 1. According to the experimental results, the conductivity of the polyolefin composite membranes prepared in Examples 1-8 of this application is higher than that of the commercially available Zirfon membrane.
[0067] Experimental Example 3: Alkali Absorption Rate Test
[0068] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane were cut into 2 cm × 2 cm samples. Each sample was independently washed and soaked in deionized water 3-5 times, then thoroughly dried in a vacuum drying oven at 80°C. The mass of the sample before alkali absorption (m1) was measured. The sample was then immersed in a 4 mol / L KOH solution for 24 h at 80°C. After removing the sample from the alkali solution, any remaining alkali was removed, and the mass of the sample after alkali absorption (m2) was measured. The alkali absorption rate U was calculated using the following formula: ; The conductivity of the polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane was calculated, and the test results are shown in Table 1. According to the experimental results, except for the alkali absorption rate of the ion-exchange membrane prepared in Example 8 of this application, the alkali absorption rates of the composite membranes prepared in the other examples are all higher than those of the commercial Zirfon membrane.
[0069] Experimental Example 4: Test of Water Contact Angle
[0070] The contact angle of the membrane was measured using the lying drop method. During the test, the polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane samples were placed independently on the sample stage. 1 μL of pure water was dropped onto the membrane surface using a graduated syringe, and the droplet morphology data was recorded immediately. The test results are shown in Table 1.
[0071] According to the experimental results, the water contact angle of the polyolefin composite membranes prepared in Examples 1 to 8 of this application is not significantly different from that of the commercial Zirfon membrane, and all of them are hydrophilic.
[0072] Experimental Example 5: Surface Resistance Test
[0073] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane samples were cut into strips of 4 cm × 4 cm, and each was independently exchanged with 1 mol / L KOH solution to fully convert OH-. - The membrane sample was fixed in the MEA water electrolysis fixture, and the electrochemical impedance spectroscopy was measured in constant current mode. The frequency range was set to 100 Hz to 1 MHz. The in-situ resistance was read and then converted into the sheet resistance. The test results are shown in Table 1.
[0074] According to the experimental results, the sheet resistance of the polyolefin composite membranes prepared in Examples 1-8 of this application did not change significantly compared with the sheet resistance of the commercial Zirfon membrane.
[0075] Test Example 6: Tensile Strength Test
[0076] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane samples were cut into strips of 1 cm × 10 cm and tested on a material tensile testing machine. The experimental results are shown in Table 1.
[0077] According to the experimental results, the tensile strength of the polyolefin composite membranes prepared in Examples 1, 2, 3, 7 and 8 of this application is higher than that of the commercial Zirfon membrane.
[0078] Experimental Example 7: Bubble Point Pressure Test
[0079] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane samples were cut into small pieces, each independently wetted with high-purity water, and placed in an airtight fixture. Nitrogen gas pressure was applied to one side of the membrane, and the pressure value was recorded in real time using a pressure gauge. An electronic soap film flow meter was connected to the other side. When the soap film rise was detected, the pressure was regarded as the bubble point pressure of the membrane. The experimental results are shown in Table 1.
[0080] According to the experimental results, the bubble point pressure of the polyolefin composite membranes prepared in Examples 1 to 8 of this application is higher than that of the commercial Zirfon membrane.
[0081] Test Example 8: Alkali Resistance Stability Test
[0082] Alkali stability is assessed by monitoring changes in its conductivity and mass in alkaline solutions.
[0083] The polyolefin composite membranes prepared in Examples 1-8 and the commercial Zirfon membrane samples were cut and then separately sealed and immersed in a 4 mol / L KOH solution. After being placed in a vacuum oven at 80°C for 72 h, the membrane samples were taken out and their conductivity and mass loss were tested according to the above method. The experimental results are shown in Table 1.
[0084] According to the experimental results, the polyolefin composite membranes prepared in Examples 1 and 5 of this application have higher alkali resistance than the commercial Zirfon membrane.
[0085] Table 1
[0086] Test Example 9: Electrolysis Performance Test of Water
[0087] The alkaline water electrolysis test used a zero-gap MEA electrolyzer, which consists of a platinum-plated titanium alloy bipolar plate with a single linear serpentine path, a polytetrafluoroethylene (PTFE) expanded gasket, and a membrane electrode assembly. The bipolar plate is used for injecting and circulating the electrolyte, and temperature sensing elements and thermocouples are installed on the outside of the bipolar plate to control the electrolysis temperature of the electrolyzer. The membrane electrode assembly includes a diaphragm (4 cm²).2 The device includes a sandwich structure containing two catalyst-supported structures, with the anode being a nickel-iron catalyst and the cathode being a platinum-carbon catalyst. See the diagram of the alkaline membrane water electrolysis device. Figure 5 The apparatus mainly consists of three parts: a pair of platinum-plated flow guide plates, a pair of alloy end plates, and a pair of gaskets. The flow guide plates ensure stable and uniform contact between the electrolyte and the membrane, thus guaranteeing a stable water electrolysis reaction. The end plates fix the entire apparatus, preventing external physical conditions from affecting the reaction. The gaskets ensure the airtightness of the entire apparatus, preventing gas cross-contamination and electrolyte permeation. A Blue Electric CT3002N electrochemical workstation was used as the power source to measure the battery voltage and evaluate battery performance. During the experiment, a gear pump circulated 4 mol / L KOH electrolyte at a flow rate of 50 mL / min. Before recording the first polarization curve, the assembled battery was set at 50 mA / cm². 2 Activated at a current density of 1 h, then by applying 2.5 mA / cm 2 ~1200 mA / cm 2 The voltage was used to record the current density of the battery and obtain the polarization curve.
[0088] This application uses the polyolefin composite membrane prepared in Example 1 and a commercially available Zirfon membrane to test the electrolysis performance of water at 80°C and 4 mol / L KOH. See [link to relevant documentation]. Figure 6 , Figure 6 Electrolysis water test results for the polyolefin composite membrane prepared in Example 1 and the commercial Zirfon membrane. The experimental results show that a membrane area of 4 cm²... 2 Compared to the commercially available Zirfon membrane, the composite membrane provided in this application exhibits higher current density and lower energy consumption at the same voltage when applied in alkaline water electrolysis.
[0089] This application uses the polyolefin composite membrane prepared in Example 1 to conduct an electrolytic water stability test in a 60°C, 4 mol / L KOH solution. See [link to relevant documentation]. Figure 7 , Figure 7 The image shows the electrolytic water stability test results of the polyolefin composite membrane prepared in Example 1. The experimental results indicate that the polyolefin composite membrane prepared in Example 1 can operate stably for 850 hours in a harsh alkaline environment (60℃, 4 mol / L KOH), with a voltage decay rate of only 0.0996 mVh. -1 This indicates that the membrane effectively solves the problems of inorganic particle agglomeration and long-term desorption in traditional composite membranes, and significantly improves the stability of the membrane during long-term operation.
[0090] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in this application, based on the technical solution and inventive concept of this application, should be included within the scope of protection of this application.
Claims
1. A method for preparing an inorganic particle covalently bonded polyolefin composite separator, characterized in that, Includes the following steps: Step 1: Styrene, acrylonitrile, and 4-chloromethylstyrene are polymerized to obtain the initial casting solution; Step 2: Quaternize the initial casting solution to obtain an olefin anion film solution; Step 3: After mixing the olefin anion membrane solution, silane coupling modified inorganic particles and crosslinking agent, an in-situ crosslinking reaction is carried out, followed by ultrasonic crushing to obtain a mixed slurry; Step 4: Prepare olefin-based cross-linked membranes using a mixed slurry and a composite membrane support; Step 5: Perform secondary cross-linking on the olefin-based cross-linked membrane to obtain an olefin-based composite membrane.
2. The preparation method according to claim 1, characterized in that, In step 1, the molar ratio of styrene, acrylonitrile and 4-chloromethylstyrene is (0.1~5):(0.1~12):(0.1~5).
3. The preparation method according to claim 1, characterized in that, In step 2, the quaternizing agent for the quaternization reaction is N-methylpyrrolidine, N-methylpiperidine, 1-methylazacycloheptane, 4-methylmorpholine, quinine ring, 1,4-dimethylpiperidine, 1,3,5-trimethylpiperidine, 1,2,6-trimethylpiperidine, N-methyldipropylamine, or trimethylamine. The mass of the quaternizing reagent is 5% to 60% of the mass of 4-chloromethylstyrene.
4. The preparation method according to claim 1, characterized in that, In step 3, the method for preparing the silane coupling modified inorganic particles is as follows: a silane coupling reagent, deionized water and inorganic particles are subjected to a silane coupling reaction. The silane coupling agent is one or more selected from 3-(2,3-epoxypropoxy)propyltrimethoxysilane, epoxycyclohexyltrimethoxysilane and epoxycyclohexyltriethoxysilane; The inorganic particles are nano-zirconia particles with a particle size of 10 nm to 200 nm.
5. The preparation method according to claim 1, characterized in that, In step 3, the silane coupling modified inorganic particles account for 40% to 90% of the total mass of the mixed slurry.
6. The preparation method according to claim 1, characterized in that, In step 3, the crosslinking agent is selected from one or more of polyethyleneimine, small molecule polytertiary amines, and amino-terminated polyethers; The small molecule polytertiary amine is N,N,N',N'-tetramethyl-1,6-hexanediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, 4,4'-trimethylenebis(1-methylpiperidine), N,N,N',N'',N''-pentamethyldiethylenetriamine or tris(2-dimethylaminoethyl)amine; The terminal amino polyether is O,O′-bis(2-aminopropyl)polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol, O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol-block-polyethylene glycol, or O,O′-bis(2-aminopropyl)polyethylene glycol-block-polypropylene glycol; The crosslinking agent accounts for 0.01% to 1.0% of the total mass of the mixed slurry.
7. The preparation method according to claim 1, characterized in that, In step 4, the thickness of the composite membrane support is 20 μm to 200 μm; The composite membrane support is one or more of polyphenylene sulfide, polyether ether ketone, polysulfone, and polytetrafluoroethylene.
8. The preparation method according to claim 1, characterized in that, In step 5, the secondary crosslinking reaction is as follows: after immersing the olefin crosslinked membrane in a crosslinking agent solution, it is subjected to heat treatment; The crosslinking agent solution comprises a crosslinking agent and a solvent, wherein the crosslinking agent is polyethyleneimine; The mass ratio of the crosslinking agent to the solvent is 1:(1~200). Soaking time is 10 min to 72 h.
9. The preparation method according to claim 8, characterized in that, The heat treatment temperature is 30℃~80℃.
10. An inorganic particulate covalently bonded polyolefin composite separator, characterized in that, The preparation method according to any one of claims 1 to 9 is used.