Temperature-controlled composite membrane, method of making and use thereof
By designing a three-layer structure for a temperature-controlled composite membrane, utilizing a eutectic system formed by hydrated magnesium sulfate crystals and oxalate metal ions coordinated with sulfate ions, combined with porous materials and water-absorbing inorganic salts, adaptive temperature control and reversible heat absorption and release functions in high and low temperature environments are achieved. This solves the problem of damage to existing radiative cooling membranes in low-temperature environments and extends their service life.
Patent Information
- Application Number
- CN202611434164.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-20
Smart Images

Figure CN123131671A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of energy storage technology, and in particular to a temperature-controlled composite membrane, its preparation method, and its application. Background Technology
[0002] Electronic devices face challenges from both high and low temperatures when used outdoors. High temperatures can cause overheating and frequency reduction in electronic components, thermal aging of materials (such as plastic deformation and solder joint breakage), risk of battery thermal runaway, and overheating. Low temperatures can lead to material brittleness, a sharp drop in battery life, icing that blocks functional components (sensors, interfaces), and internal condensation short circuits, significantly reducing the lifespan of electronic devices.
[0003] Radiative cooling is a passive cooling technology that utilizes the thermal radiation of an object to dissipate heat in the form of electromagnetic waves (mainly infrared radiation) into a low-temperature external environment (such as outer space), thereby achieving self-cooling. By coating electronic devices with radiative cooling materials, the temperature of these devices can spontaneously decrease. For example, CN116394610A uses polydimethylsiloxane as a mid-infrared emitting layer to achieve mid-infrared emission, silver as a near-infrared reflective layer to achieve reflection of the near-infrared 0.8μm~2.5μm solar spectrum, and polycarbonate as a visible light anti-reflection layer. By constructing a polymer-metal-polymer structure, it achieves visible light transmission and high near-infrared reflectivity. When applied to outdoor electronic devices, this material can significantly reduce the temperature of the electronic devices when the outdoor ambient temperature is too high.
[0004] However, conventional radiation cooling films cannot solve the damage to equipment caused by low-temperature environments, and existing radiation cooling transparent film systems usually use polymer materials, which are easy to degrade and have poor adhesion to the film, thus limiting their outdoor applications. Summary of the Invention
[0005] Therefore, it is necessary to provide a temperature-controlled composite film, its preparation method, and its application to address the above problems. The temperature-controlled composite film described in this application has reversible heat absorption and heat release functions. When applied in high and low temperature or large temperature difference environments, it can simultaneously perform cooling and heating functions, achieve adaptive temperature control, and has a long service life.
[0006] A temperature-controlled composite membrane includes a functional layer, a water-proof and breathable membrane, and a water-conducting layer stacked sequentially.
[0007] The functional layer includes hydrated magnesium sulfate crystals and a structural framework coated on the surface of the hydrated magnesium sulfate crystals. The structural framework includes MgC2O4 precipitate and a coordination network of oxalate metal ions and sulfate ions. The melting point of the eutectic system formed in the functional layer is less than or equal to 48°C.
[0008] The water-conducting layer includes a composite filler fixed by a film-forming agent, the composite filler comprising a porous material and a water-absorbing inorganic salt loaded in the porous material.
[0009] In one embodiment, the thickness of the functional layer is 300 μm to 500 μm;
[0010] And / or, the thickness of the water-conducting layer is 100μm~150μm.
[0011] In one embodiment, the mass ratio of the porous material to the water-absorbing inorganic salt is 1:0.1 to 1:0.5;
[0012] And / or, the water-absorbing inorganic salt is selected from at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide;
[0013] And / or, the porous material is selected from at least one of porous silica and porous alumina.
[0014] In one embodiment, the thickness of the waterproof and breathable membrane is 50 μm to 80 μm;
[0015] And / or, the pore size of the waterproof and breathable membrane is 0.2μm~0.3μm;
[0016] And / or, the material of the waterproof and breathable membrane is selected from polytetrafluoroethylene or polypropylene.
[0017] A method for preparing a temperature-controlled composite film includes the following steps:
[0018] A mixture of hydrated magnesium sulfate and ionic salt is prepared, and then oxalate dispersion and binder are added to prepare a first slurry. The melting point of the eutectic system formed in the first slurry is less than or equal to 48°C.
[0019] A composite filler was prepared by injecting a water-absorbing inorganic salt solution into a porous material and maintaining pressure using a vacuum impregnation method. The composite filler was then mixed with a film-forming agent dispersion to prepare a second slurry.
[0020] The first slurry is coated onto the substrate to form a functional layer. Then, a water-proof and breathable membrane is adhered to the surface of the functional layer. The second slurry is then coated onto the water-proof and breathable membrane to form a water-conducting layer, thus obtaining a temperature-controlled composite membrane on the substrate.
[0021] In one embodiment, the mass ratio of the hydrated magnesium sulfate to the ionic salt is 5:1 to 10:1;
[0022] And / or, the ionic salt is selected from at least one of magnesium chloride, magnesium nitrate, sodium chloride, potassium chloride, and aluminum nitrate;
[0023] And / or, the total concentration of hydrated magnesium sulfate and ionic salt in the mixture is 0.5 g / mL to 1 g / mL;
[0024] And / or, the temperature for mixing hydrated magnesium sulfate with ionic salt is 30℃~35℃, and the rotation speed is 200rps~300rps;
[0025] And / or, the mass ratio of the hydrated magnesium sulfate to the oxalate in the oxalate dispersion is 20:1 to 30:1;
[0026] And / or, the concentration of oxalate in the oxalate dispersion is 0.01 g / mL to 0.1 g / mL;
[0027] And / or, the oxalate in the oxalate dispersion is selected from at least one of aluminum oxalate, iron oxalate, and chromium oxalate.
[0028] In one embodiment, the mass ratio of hydrated magnesium sulfate to the binder is 15:1 to 20:1;
[0029] And / or, the adhesive is selected from at least one of polyvinyl butyral and polytetrafluoroethylene-polyurethane.
[0030] In one embodiment, the mass ratio of the porous material to the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is 1:0.1 to 1:0.5;
[0031] And / or, the concentration of the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is 0.05 g / mL to 0.15 g / mL;
[0032] And / or, the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is selected from at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide;
[0033] And / or, the porous material is selected from at least one of porous silica and porous alumina;
[0034] And / or, the pressure holding includes: introducing protective gas to bring the pressure to 0.3MPa~0.35MPa and maintaining it for 10min~15min.
[0035] In one embodiment, the mass ratio of the porous material to the film-forming agent in the film-forming agent dispersion is 1:0.1 to 1:0.5;
[0036] And / or, the concentration of the film-forming agent in the film-forming agent dispersion is 0.01 g / mL to 0.05 g / mL.
[0037] An electronic device comprising the temperature-controlled composite film as described above.
[0038] The temperature-controlled composite membrane described in this application has a unique three-layer structure. The main material of the functional layer is hydrated magnesium sulfate, which can achieve environmental adaptive temperature control by acquiring and releasing water molecules from the environment. At the same time, the addition of oxalate reacts to generate local MgC2O4 precipitate and oxalate metal ions coordinate with sulfate ions to form a spatial framework that encapsulates unreacted hydrated magnesium sulfate crystals, constituting a low-melting-point eutectic system. This effectively prevents the loss of functional components and low melting point, which is beneficial for expanding the operating temperature range and extending service life. The water-proof and breathable membrane allows water vapor to enter the functional layer while isolating liquid water, which is beneficial for further preventing the loss of the main material of the functional layer and improving the reliability of the membrane. The porous material loaded with water-absorbing inorganic salts in the water-conducting layer increases the water vapor exchange rate between the functional layer and the environment, thereby improving the heat absorption and release efficiency.
[0039] Therefore, based on the synergistic effect of the three-layer structure, the temperature-controlled composite film described in this application has reversible heat absorption and heat release functions. When applied to high and low temperature or large temperature difference environments, it can have both cooling and heating functions, achieve adaptive temperature control, and has a long service life. Attached Figure Description
[0040] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0041] Figure 1 This is a laser confocal image of the longitudinal section of the temperature-controlled composite film prepared in Example 1. Detailed Implementation
[0042] To facilitate understanding of this application, it will be described in more detail below. However, it should be understood that this application can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to provide a more thorough and complete understanding of the disclosure of this application.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein in the specification of this application is for the purpose of describing particular implementations or embodiments only and is not intended to be limiting of this application. The optional range of the term "and / or" as used herein includes any one of two or more of the related listed items, as well as any and all combinations of the related listed items, including any two related listed items, any more related listed items, or a combination of all related listed items. In this application, when numerical ranges are involved, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, and every value between such minimum and maximum values. Further, when a range refers to an integer, it includes every integer between the minimum and maximum values of the range. Furthermore, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all sub-ranges to which they are incorporated.
[0044] This application provides a temperature-controlled composite membrane, comprising a functional layer, a water-proof and breathable membrane, and a water-conducting layer stacked sequentially.
[0045] The functional layer includes hydrated magnesium sulfate crystals and a structural framework coated on the surface of the hydrated magnesium sulfate crystals. The structural framework includes MgC2O4 precipitate and a coordination network of oxalate metal ions and sulfate ions. The melting point of the eutectic system formed in the functional layer is less than or equal to 48°C.
[0046] The water-conducting layer includes a composite filler fixed by a film-forming agent, the composite filler comprising a porous material and a water-absorbing inorganic salt loaded in the porous material.
[0047] The temperature-controlled composite membrane described in this application has a unique three-layer structure. The main material of the functional layer is hydrated magnesium sulfate, which can achieve environmental adaptive temperature control by acquiring and releasing water molecules from the environment. At the same time, the addition of oxalate reacts to generate local MgC2O4 precipitate and oxalate metal ions coordinate with sulfate ions to form a spatial framework that encapsulates unreacted hydrated magnesium sulfate crystals, constituting a low-melting-point eutectic system. This effectively prevents the loss of functional components and low melting point, which is beneficial for expanding the operating temperature range and extending service life. The water-proof and breathable membrane allows water vapor to enter the functional layer while isolating liquid water, which is beneficial for further preventing the loss of the main material of the functional layer and improving the reliability of the membrane. The porous material loaded with water-absorbing inorganic salts in the water-conducting layer increases the water vapor exchange rate between the functional layer and the environment, thereby improving the heat absorption and release efficiency.
[0048] Therefore, based on the synergistic effect of the three-layer structure, the temperature-controlled composite film described in this application has reversible heat absorption and heat release functions. When applied to high and low temperature or large temperature difference environments, it can have both cooling and heating functions, achieve adaptive temperature control, and has a long service life.
[0049] In one embodiment of this application, the thickness of the functional layer is preferably 300μm to 500μm, including but not limited to any one of 300μm, 350μm, 400μm, 450μm, and 500μm or any range between two of them.
[0050] In one embodiment of this application, the thickness of the water-conducting layer is preferably 100μm to 150μm, including but not limited to any one of 100μm, 110μm, 120μm, 130μm, 140μm, and 150μm or any range between two of them.
[0051] In one embodiment of this application, the mass ratio of the porous material to the water-absorbing inorganic salt is preferably 1:0.1 to 1:0.5, including but not limited to any one of 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any range between the two.
[0052] In one embodiment of this application, the water-absorbing inorganic salt is selected from at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide.
[0053] In one embodiment of this application, the porous material is selected from at least one of porous silica and porous alumina.
[0054] Considering that direct contact between hydrated magnesium sulfate and water may cause loss of functional components, this application sets a water-proof and breathable membrane between the functional layer and the water-conducting layer, which is beneficial to further improve the reliability of the temperature-controlled composite membrane.
[0055] In one embodiment of this application, the thickness of the waterproof and breathable membrane is preferably 50μm to 80μm, including but not limited to any one of 50μm, 60μm, 70μm, and 80μm or any range between two of them.
[0056] In one embodiment of this application, the pore size of the water-proof and breathable membrane is preferably 0.2μm to 0.3μm, including but not limited to any one of 0.2μm, 0.22μm, 0.25μm, 0.28μm, 0.3μm or any range between two of them.
[0057] In one embodiment of this application, the material of the waterproof and breathable membrane includes, but is not limited to, polytetrafluoroethylene (PTFE) or polypropylene (PP).
[0058] This application also provides a method for preparing a temperature-controlled composite film, comprising the following steps:
[0059] Step 1: Prepare a mixture of hydrated magnesium sulfate and ionic salt, add oxalate dispersion and binder to prepare a first slurry, wherein the melting point of the eutectic system formed in the first slurry is less than or equal to 48°C.
[0060] Step 2: A water-absorbing inorganic salt solution is injected into a porous material using a vacuum impregnation method and pressure is maintained to obtain a composite filler. The composite filler is then mixed with a film-forming agent dispersion to obtain a second slurry.
[0061] Step 3: Coat the first slurry onto the substrate to form a functional layer, then attach the water-proof and breathable membrane to the surface of the functional layer, and then coat the second slurry onto the water-proof and breathable membrane to form a water-conducting layer, thus obtaining a temperature-controlled composite membrane on the substrate.
[0062] In step one, hydrated magnesium sulfate can absorb heat and lose water molecules in high-temperature environments to lower the temperature, and absorb moisture from the environment and release heat in low-temperature environments to raise the temperature, thus achieving reversible endothermic and exothermic functions. On the one hand, the reaction of oxalate with hydrated magnesium sulfate to generate local MgC2O4 precipitate and the coordination network of oxalate metal ions and sulfate ions forms a spatial barrier and structural framework, which encapsulates and separates a large number of unreacted hydrated magnesium sulfate crystals, helping to prevent their loss, thereby ensuring the exothermic and endothermic functions and extending the service life. On the other hand, the melting point of the eutectic system formed in the first slurry is less than or equal to 48°C, which is conducive to forming a high ion concentration liquid environment. This not only allows for rapid conduction of water molecules, but also allows the salt ions of the low eutectic system to "fill" the lattice gaps, which helps maintain the structural stability of the phase change process, thereby further extending the service life of the temperature-controlled composite membrane.
[0063] It is understood that this application does not limit the specific proportion of water molecules in hydrated magnesium sulfate, including but not limited to magnesium sulfate heptahydrate.
[0064] In one embodiment of this application, the mass ratio of hydrated magnesium sulfate to the ionic salt is preferably 5:1 to 10:1. By adjusting the ratio of hydrated magnesium sulfate to the ionic salt, it is not only beneficial to accurately control the working temperature, but also to further improve structural stability and extend service life.
[0065] It is understood that the mass ratio of the hydrated magnesium sulfate to the ionic salt includes, but is not limited to, any one of the following values: 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or any range between the two.
[0066] In one embodiment of this application, the ionic salt includes, but is not limited to, at least one of magnesium chloride, magnesium nitrate, sodium chloride, potassium chloride, and aluminum nitrate, preferably magnesium chloride or magnesium nitrate, wherein the Cl in the ionic salt... - Able to replace part of SO4 2- These sites fill lattice voids, which helps maintain the structural stability of the phase transition process.
[0067] In one embodiment of this application, the total concentration of hydrated magnesium sulfate and ionic salt in the mixture is preferably 0.5 g / mL to 1 g / mL, including but not limited to any one of 0.5 g / mL, 0.6 g / mL, 0.7 g / mL, 0.8 g / mL, 0.9 g / mL, 1 g / mL or any range between two.
[0068] In one embodiment of this application, the preferred temperature for mixing hydrated magnesium sulfate and ionic salt is 30°C to 35°C, and the preferred rotation speed is 200 rpm to 300 rpm, which is beneficial for the hydrated magnesium sulfate and ionic salt to be fully and evenly mixed.
[0069] It should be noted that this application does not restrict the solvents used to mix hydrated magnesium sulfate with ionic salts, including but not limited to deionized water.
[0070] In one embodiment of this application, the mass ratio of hydrated magnesium sulfate to oxalate in the oxalate dispersion is preferably 20:1 to 30:1. By adjusting the amount of hydrated magnesium sulfate and oxalate, it is beneficial to control the distribution of an appropriate amount of magnesium oxalate precipitate and the coordination network between oxalate metal ions and sulfate ions in the functional layer. While utilizing the spatial barriers and structural framework formed therein to encapsulate and separate the hydrated magnesium sulfate crystals, it ensures that there is sufficient magnesium sulfate in the functional layer, thereby giving the temperature-controlled composite membrane a better heat absorption and release function and a longer service life.
[0071] It is understood that the mass ratio of the hydrated magnesium sulfate to the oxalate in the oxalate dispersion includes, but is not limited to, any one of the following values or any range between 20:1, 21:1, 23:1, 25:1, 26:1, 28:1, and 30:1.
[0072] In one embodiment of this application, the concentration of oxalate in the oxalate dispersion is preferably 0.01 g / mL to 0.1 g / mL, including but not limited to any one of 0.01 g / mL, 0.02 g / mL, 0.04 g / mL, 0.05 g / mL, 0.06 g / mL, 0.08 g / mL, 0.1 g / mL, or any range between two values.
[0073] In one embodiment of this application, the oxalate in the oxalate dispersion includes, but is not limited to, at least one of aluminum oxalate, iron oxalate, and chromium oxalate, with aluminum oxalate being preferred.
[0074] It should be noted that this application does not impose any restrictions on the preparation process of the oxalate dispersion; conventional process conditions can be used, such as dispersing oxalate in an organic solvent and sonicating at a constant temperature of 45℃~55℃ for 30min~50min.
[0075] In one embodiment of this application, the mass ratio of the hydrated magnesium sulfate to the binder is preferably 15:1 to 20:1, including but not limited to any one of 15:1, 16:1, 17:1, 18:1, 19:1, 20:1 or any range between the two.
[0076] In one embodiment of this application, the adhesive includes, but is not limited to, at least one of polyvinyl butyral (PVB) and polytetrafluoroethylene-polyurethane (PTFE-PU).
[0077] In step two, the porous material is loaded with water-absorbing inorganic salts by vacuum impregnation, which helps to reduce the surface tension of water, increase the capillary adsorption rate, thereby increasing the water vapor exchange rate between the functional layer and the environment, and thus improving the heat absorption and release efficiency.
[0078] In one embodiment of this application, the mass ratio of the porous material to the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is preferably 1:0.1 to 1:0.5. By adjusting the ratio of the porous material to the water-absorbing inorganic salt, it is beneficial to further optimize the water vapor transmission efficiency of the water-conducting layer under high temperature and low temperature environments.
[0079] It is understood that the mass ratio of the porous material to the water-absorbing inorganic salt in the water-absorbing inorganic salt solution includes, but is not limited to, any one of the following values or any range between 1:0.1, 1:0.2, 1:0.3, 1:0.4, and 1:0.5.
[0080] In one embodiment of this application, the concentration of the hygroscopic inorganic salt in the hygroscopic inorganic salt solution is preferably 0.05 g / mL to 0.15 g / mL, including but not limited to any one of 0.05 g / mL, 0.06 g / mL, 0.08 g / mL, 0.10 g / mL, 0.12 g / mL, 0.15 g / mL, or any range between two of them.
[0081] In one embodiment of this application, the water-absorbing inorganic salt in the water-absorbing inorganic salt solution includes, but is not limited to, at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide.
[0082] In one embodiment of this application, the porous material is preferably a hydrophilic porous material, including but not limited to at least one of porous silica and porous alumina, more preferably porous silica. By utilizing the strong infrared emission characteristics of silica, porous silica can serve as a water-conducting layer while also achieving radiative cooling, which is beneficial to further improve the cooling efficiency.
[0083] In one embodiment of this application, a composite filler is preferably obtained by vacuum impregnation, where a lithium chloride dispersion is injected into porous silica and pressed, or by injecting a magnesium chloride dispersion into porous alumina and pressing, where a composite filler is obtained.
[0084] Step two employs a vacuum impregnation method. On one hand, this facilitates the removal of air and other gas molecules from the pores of the porous material, providing ample space for the subsequent entry of water-absorbing inorganic salt ions. On the other hand, the pressure difference created by the negative pressure promotes the entry of the water-absorbing inorganic salt solution into the pores. Furthermore, the subsequent pressure holding not only aids liquid permeation but also helps stabilize the liquid's filling state within the porous structure, preventing partial discharge due to uneven capillary action.
[0085] In one embodiment of this application, the pressure holding preferably includes: introducing a protective gas to bring the pressure to 0.3MPa~0.35MPa and maintaining it for 10min~15min, wherein the protective gas includes, but is not limited to, nitrogen or argon.
[0086] In one embodiment of this application, the mass ratio of the porous material to the film-forming agent in the film-forming agent dispersion is preferably 1:0.1 to 1:0.5, including but not limited to any one of 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or any range between the two.
[0087] In one embodiment of this application, the concentration of the film-forming agent in the film-forming agent dispersion is 0.01 g / mL to 0.05 g / mL, including but not limited to any one of 0.01 g / mL, 0.02 g / mL, 0.03 g / mL, 0.04 g / mL, and 0.05 g / mL, or a range between any two. Specifically, the film-forming agent includes, but is not limited to, polyvinylpyrrolidone (PVP).
[0088] It is understood that this application does not restrict the preparation order of step one and step two. Step one can be prepared first and then step two, or step two can be prepared first and then step one, or both steps one and step two can be prepared simultaneously.
[0089] To prevent the loss of functional components caused by direct contact between hydrated magnesium sulfate and water, this application provides a water-proof and breathable membrane between the functional layer and the water-conducting layer prepared from the first slurry and the second slurry in step three, which further improves the reliability of the temperature-controlled composite membrane.
[0090] In one embodiment of this application, the thickness of the waterproof and breathable membrane is preferably 50μm to 80μm, including but not limited to any one of 50μm, 60μm, 70μm, and 80μm or any range between two of them.
[0091] In one embodiment of this application, the pore size of the water-proof and breathable membrane is preferably 0.2μm to 0.3μm, including but not limited to any one of 0.2μm, 0.22μm, 0.25μm, 0.28μm, 0.3μm or any range between two of them.
[0092] In one embodiment of this application, the material of the waterproof and breathable membrane includes, but is not limited to, polytetrafluoroethylene (PTFE) or polypropylene (PP).
[0093] It should be noted that before using the waterproof and breathable membrane, it is preferable to perform plasma activation treatment on the membrane, which is beneficial to improve its hydrophilicity.
[0094] In one embodiment of this application, the thickness of the functional layer is preferably 300μm to 500μm, including but not limited to any one of 300μm, 350μm, 400μm, 450μm, and 500μm or any range between two of them.
[0095] In one embodiment of this application, the thickness of the water-conducting layer is preferably 100μm to 150μm, including but not limited to any one of 100μm, 110μm, 120μm, 130μm, 140μm, and 150μm or any range between two of them.
[0096] The temperature-controlled composite membrane provided in this application achieves high stability, high reliability, and efficient heat absorption and release by constructing a three-layer structure consisting of a functional layer, a water-proof and breathable membrane, and a water-conducting layer. Furthermore, the raw materials are simple to obtain and have low cost, and the membrane preparation is simple, making it easy to mass-produce and apply.
[0097] This application also provides a temperature-controlled composite film as described above, which can be applied to electronic devices to achieve both cooling and heating functions in high and low temperature or large temperature difference environments, enabling adaptive temperature control and a long service life. It is understood that, when the temperature-controlled composite film provided in this application is applied to electronic devices, the functional layer of the temperature-controlled composite film is in contact with the substrate of the electronic device, and the water-conducting layer is in contact with the environment. That is, from the inside out, the film is sequentially stacked including the substrate of the electronic device, the functional layer, the water-proof and breathable membrane, and the water-conducting layer.
[0098] The following specific embodiments will further illustrate the temperature-controlled composite film, its preparation method, and its applications. However, those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of this application. Unless otherwise specified, specific conditions in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used without specified manufacturers are all commercially available conventional products.
[0099] Example 1
[0100] 0.1 g of Al2(C2O4)3 was dispersed in 2 mL of ethylene glycol and sonicated at 55 °C for 30 min to obtain an oxalate dispersion. 3 g of MgSO4·7H2O and 0.5 g of MgCl2 were dissolved in 5 mL of deionized water and stirred at a constant temperature of 30 °C at 200 rpm to obtain a mixture. The oxalate dispersion and 0.15 g of PVP were slowly added dropwise to the mixture while continuously stirring to form a first slurry. The melting point of the eutectic system formed in the first slurry was determined to be approximately 46 °C by differential scanning spectroscopy.
[0101] 1 g of porous silica was placed in the sample basket of an impregnation vessel and evacuated to 100 Pa. 0.3 g of LiCl was dissolved in 3 g of deionized water and slowly injected into the porous silica. N2 was introduced to 0.3 MPa, and the pressure was maintained for 10 min to obtain the composite filler. 0.1 g of PVP was dispersed in 3 mL of anhydrous ethanol and sonicated for 5 min. The composite filler was then added to the PVP dispersion to form a second slurry.
[0102] The first slurry is uniformly coated onto the substrate to form a functional layer, with the thickness of the functional layer controlled at 500 μm. A PTFE membrane layer with a thickness of 50 μm (pore size of approximately 0.22 μm) is taken and plasma-treated under an argon atmosphere at a power of 100 W for 5 min. Thermoplastic polyurethane is then coated onto the surface of the functional layer, and the treated PTFE membrane layer is pressed at 0.1 MPa for 10 s. The second slurry is coated onto the PTFE membrane layer to form a water-conducting layer, with the thickness of the water-conducting layer controlled at 150 μm.
[0103] The longitudinal section of the temperature-controlled composite film prepared in Example 1 was characterized by laser confocal microscopy, and the results are as follows: Figure 1 As shown, it can be clearly observed that the composite membrane has a multi-layer structure, with the bottom layer being the substrate, and the functional layer, the water-proof and breathable membrane, and the water-conducting layer being stacked sequentially on the substrate.
[0104] Example 2
[0105] 0.1 g of Al2(C2O4)3 was dispersed in 2 mL of ethylene glycol and sonicated at 55 °C for 30 min to obtain an oxalate dispersion. 3 g of MgSO4·7H2O and 0.6 g of Mg(NO3)2 were dissolved in 5 mL of deionized water and stirred at a constant temperature of 30 °C at 200 rpm to obtain a mixture. The oxalate dispersion and 0.15 g of PVP were slowly added dropwise to the mixture while continuously stirring to form a first slurry. The melting point of the eutectic system formed in the first slurry was determined to be approximately 39 °C by differential scanning spectroscopy.
[0106] 1 g of porous silica was placed in the sample basket of an impregnation vessel and evacuated to 100 Pa. 0.3 g of LiCl was dissolved in 3 g of deionized water and slowly injected into the porous silica. N2 was introduced to 0.3 MPa, and the pressure was maintained for 10 min to obtain the composite filler. 0.1 g of PVP was dispersed in 3 mL of anhydrous ethanol and sonicated for 5 min. The composite filler was then added to the PVP dispersion to form a second slurry.
[0107] The first slurry is uniformly coated onto the substrate to form a functional layer, with the thickness of the functional layer controlled at 450 μm. A 60 μm thick PP membrane layer (pore size approximately 0.25 μm) is taken and plasma-treated in a nitrogen atmosphere at a power of 100 W for 5 min. Thermoplastic polyurethane is then coated onto the surface of the functional layer, and the treated PP membrane layer is pressed at 0.1 MPa for 10 s. The second slurry is coated onto the PP membrane layer to form a water-conducting layer, with the thickness of the water-conducting layer controlled at 140 μm.
[0108] Example 3
[0109] 0.12 g of Fe2(C2O4)3 was dispersed in 2 mL of ethylene glycol and sonicated at 55 °C for 30 min to obtain an oxalate dispersion. 3 g of MgSO4·7H2O and 0.4 g of NaCl were dissolved in 5 mL of deionized water and stirred at a constant temperature of 32 °C at 250 rpm to obtain a mixture. The oxalate dispersion and 0.2 g of PVP were slowly added dropwise to the mixture while continuously stirring to form a first slurry. The melting point of the eutectic system formed in the first slurry was determined to be approximately 43 °C by differential scanning spectroscopy.
[0110] 1 g of porous alumina was placed in the sample basket of an impregnation vessel and evacuated to 100 Pa. 0.1 g of MgCl2 was dissolved in 3 g of deionized water and slowly injected into the porous alumina. N2 was introduced to 0.35 MPa, and the pressure was maintained for 15 min to obtain the composite filler. 0.15 g of PVP was dispersed in 3 mL of anhydrous ethanol and sonicated for 5 min. The composite filler was then added to the PVP dispersion to form a second slurry.
[0111] The first slurry is uniformly coated onto the substrate to form a functional layer, with the thickness of the functional layer controlled at 400 μm. A 70 μm thick PTFE membrane (pore size approximately 0.27 μm) is taken and plasma-treated in a nitrogen atmosphere at a power of 100 W for 5 min. Thermoplastic polyurethane is then coated onto the surface of the functional layer, and the treated PTFE membrane is pressed at 0.1 MPa for 10 s. The second slurry is coated onto the PTFE membrane to form a water-conducting layer, with the thickness of the water-conducting layer controlled at 120 μm.
[0112] Example 4
[0113] 0.15 g of Cr₂(C₂O₄)₃ was dispersed in 2 mL of ethylene glycol and sonicated at 55 °C for 30 min to obtain an oxalate dispersion. 3 g of MgSO₄·7H₂O and 0.3 g of Al(NO₃)₃ were dissolved in 5 mL of deionized water and stirred at a constant temperature of 35 °C at 300 rpm to obtain a mixture. The oxalate dispersion and 0.2 g of PVP were slowly added dropwise to the mixture while continuously stirring to form the first slurry.
[0114] 1 g of porous alumina was placed in the sample basket of an impregnation vessel and evacuated to 100 Pa. 0.45 g of NaOH was dissolved in 3 g of deionized water and slowly injected into the porous alumina. N2 was introduced to 0.35 MPa, and the pressure was maintained for 15 min to obtain the composite filler. 0.15 g of PVP was dispersed in 3 mL of anhydrous ethanol and sonicated for 5 min. The composite filler was then added to the PVP dispersion to form a second slurry.
[0115] The first slurry is uniformly coated onto the substrate to form a functional layer, with the thickness of the functional layer controlled at 300 μm; an 80 μm thick PP membrane layer (pore size approximately 0.29 μm) is taken and plasma-treated in an argon atmosphere at a power of 100 W for 5 min; thermoplastic polyurethane is coated onto the surface of the functional layer; and the treated PP membrane layer is then pressed at 0.1 MPa for 10 s; the second slurry is coated onto the PP membrane layer to form a water-conducting layer, with the thickness of the water-conducting layer controlled at 100 μm.
[0116] Comparative Example 1
[0117] The difference between Comparative Example 1 and Example 1 is that MgCl2 was not added when preparing the first slurry.
[0118] Comparative Example 2
[0119] The difference between Comparative Example 2 and Example 1 is that, in the preparation of the first slurry, the same mass of CaCl2 was used instead of MgCl2.
[0120] Comparative Example 3
[0121] The difference between Comparative Example 3 and Example 1 is that no oxalate dispersion was added when preparing the first slurry.
[0122] Comparative Example 4
[0123] The difference between Comparative Example 4 and Example 1 is that porous silica was directly added to the PVP dispersion as a second slurry, and LiCl solution was not injected into the porous silica.
[0124] Comparative Example 5
[0125] The difference between Comparative Example 5 and Example 1 is that the second slurry was directly coated on the surface of the functional layer without setting a waterproof and breathable membrane.
[0126] Comparative Example 6
[0127] The difference between Comparative Example 6 and Example 1 is that no second slurry was prepared, and the resulting composite membrane only includes a two-layer structure of a functional layer and a water-proof and breathable membrane.
[0128] The composite membranes prepared in all examples and comparative examples were subjected to performance tests:
[0129] (1) Cooling performance: Simulate a high temperature environment, maintain 60℃ for 3h, and record the surface temperature change of the composite film;
[0130] (2) Heating performance: Simulate a low temperature environment, maintain -10℃ for 3h, and record the surface temperature change of the composite film;
[0131] (3) Reliability: Simulate a large temperature difference environment, with 60℃ for 3 hours and -10℃ for 3 hours as one cycle, and record the number of consecutive cycles.
[0132] The results are shown in Table 1.
[0133] Table 1
[0134]
[0135] As shown in Table 1, the temperature-controlled composite membranes prepared in Examples 1-4 can achieve excellent cooling and heating functions in high and low temperature or large temperature difference environments, and have high reliability and long service life. However, Comparative Example 1, due to the absence of MgCl2, has a narrower operating temperature range, poorer cooling and heating effects, and reduced reliability. Furthermore, the calcium chloride used in Comparative Example 2 reacts with sulfate ions in the system to form a precipitation reaction, and calcium chloride cannot function effectively below 60°C.
[0136] The loss of magnesium sulfate caused by the lack of oxalate dispersion in Comparative Example 3 resulted in significant loss of magnesium sulfate during operation, leading to poor reliability. Furthermore, the high melting point of the eutectic layer (60℃) resulted in increased operating temperature, significantly reducing cooling and heating efficiency and reliability. Comparative Example 4, lacking a water-permeable membrane, suffered severe magnesium sulfate loss, resulting in poor cooling and heating performance. Comparative Example 5, lacking a water-permeable membrane, showed a significant decrease in the reliability of the composite membrane. Comparative Example 6, also lacking a water-permeable layer, exhibited significantly worse cooling and heating performance and reliability.
[0137] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0138] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.
Claims
1. A temperature-controlled composite membrane, characterized in that, The temperature-controlled composite membrane includes a functional layer, a water-proof and breathable membrane, and a water-conducting layer stacked in sequence. The functional layer includes hydrated magnesium sulfate crystals and a structural framework coated on the surface of the hydrated magnesium sulfate crystals. The structural framework includes MgC2O4 precipitate and a coordination network of oxalate metal ions and sulfate ions. The melting point of the eutectic system formed in the functional layer is less than or equal to 48°C. The water-conducting layer includes a composite filler fixed by a film-forming agent, the composite filler comprising a porous material and a water-absorbing inorganic salt loaded in the porous material.
2. The temperature-controlled composite film according to claim 1, characterized in that, The thickness of the functional layer is 300μm~500μm; And / or, the thickness of the water-conducting layer is 100μm~150μm.
3. The temperature-controlled composite film according to claim 1, characterized in that, The mass ratio of the porous material to the water-absorbing inorganic salt is 1:0.1 to 1:0.5; And / or, the water-absorbing inorganic salt is selected from at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide; And / or, the porous material is selected from at least one of porous silica and porous alumina.
4. The temperature-controlled composite film according to claim 1, characterized in that, The thickness of the waterproof and breathable membrane is 50μm~80μm; And / or, the pore size of the waterproof and breathable membrane is 0.2μm~0.3μm; And / or, the material of the waterproof and breathable membrane is selected from polytetrafluoroethylene or polypropylene.
5. A method for preparing a temperature-controlled composite film as described in any one of claims 1 to 4, characterized in that, Includes the following steps: A mixture of hydrated magnesium sulfate and ionic salt is prepared, and then oxalate dispersion and binder are added to prepare a first slurry. The melting point of the eutectic system formed in the first slurry is less than or equal to 48°C. A composite filler was prepared by injecting a water-absorbing inorganic salt solution into a porous material and maintaining pressure using a vacuum impregnation method. The composite filler was then mixed with a film-forming agent dispersion to prepare a second slurry. The first slurry is coated onto the substrate to form a functional layer. Then, a water-proof and breathable membrane is adhered to the surface of the functional layer. The second slurry is then coated onto the water-proof and breathable membrane to form a water-conducting layer, thus obtaining a temperature-controlled composite membrane on the substrate.
6. The method for preparing the temperature-controlled composite film according to claim 5, characterized in that, The mass ratio of the hydrated magnesium sulfate to the ionic salt is 5:1 to 10:1; And / or, the ionic salt is selected from at least one of magnesium chloride, magnesium nitrate, sodium chloride, potassium chloride, and aluminum nitrate; And / or, the total concentration of hydrated magnesium sulfate and ionic salt in the mixture is 0.5 g / mL to 1 g / mL; And / or, the temperature for mixing hydrated magnesium sulfate with ionic salt is 30℃~35℃, and the rotation speed is 200rps~300rps; And / or, the mass ratio of the hydrated magnesium sulfate to the oxalate in the oxalate dispersion is 20:1 to 30:1; And / or, the concentration of oxalate in the oxalate dispersion is 0.01 g / mL to 0.1 g / mL; And / or, the oxalate in the oxalate dispersion is selected from at least one of aluminum oxalate, iron oxalate, and chromium oxalate.
7. The method for preparing the temperature-controlled composite film according to claim 5, characterized in that, The mass ratio of the hydrated magnesium sulfate to the binder is 15:1 to 20:1; And / or, the adhesive is selected from at least one of polyvinyl butyral and polytetrafluoroethylene-polyurethane.
8. The method for preparing the temperature-controlled composite film according to claim 5, characterized in that, The mass ratio of the porous material to the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is 1:0.1 to 1:0.5; And / or, the concentration of the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is 0.05 g / mL to 0.15 g / mL; And / or, the water-absorbing inorganic salt in the water-absorbing inorganic salt solution is selected from at least one of lithium chloride, calcium chloride, magnesium chloride, manganese chloride, sodium hydroxide, and calcium oxide; And / or, the porous material is selected from at least one of porous silica and porous alumina; And / or, the pressure holding includes: introducing protective gas to bring the pressure to 0.3MPa~0.35MPa and maintaining it for 10min~15min.
9. The method for preparing the temperature-controlled composite film according to claim 5, characterized in that, The mass ratio of the porous material to the film-forming agent in the film-forming agent dispersion is 1:0.1 to 1:0.5; And / or, the concentration of the film-forming agent in the film-forming agent dispersion is 0.01 g / mL to 0.05 g / mL.
10. An electronic device, characterized in that, The electronic device includes the temperature-controlled composite film as described in any one of claims 1 to 4.
Citation Information
Patent Citations
Flexible transparent radiation refrigeration window material
CN116394610A