A novel organic phosphorus-nitrogen flame retardant and a preparation process thereof

By optimizing the phosphorus and nitrogen flame retardant composition and surface treatment technology, the problem of uneven expanded char layer was solved, achieving uniform distribution of flame retardant and improved material properties, thus enhancing flame retardant effect and mechanical properties.

CN123131679APending Publication Date: 2026-11-20LUXI YIXING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611261584.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing phosphorus-nitrogen flame retardants, the decomposition temperature, reaction rate, and migration behavior of the acid source, gas source, and carbon source are difficult to match, resulting in uneven formation of the expanded carbon layer, which affects the flame retardant effect. Furthermore, the inorganic and organic components are not compatible enough, leading to uneven distribution of the flame retardant and a decline in material performance.

Method used

Piperazine pyrophosphate, melamine polyphosphate and ammonium type II polyphosphate are used as the main phosphorus and nitrogen flame retardant components, combined with triazine trihydroxyethyl piperazine phosphonate, phytic acid melamine piperazine composite salt and zinc borate, etc. The compatibility between the components is improved by surface treatment to form a uniform expanded carbon layer, and methyl phenyl silicone resin and hydrophilic fumed silica are used to improve the density of the carbon layer.

Benefits of technology

It achieves uniform distribution of flame retardant and good continuity of expanded char layer, improves the flame retardant and mechanical properties of material, reduces melt dripping, and enhances the crack resistance and interfacial bonding of char layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application belongs to the technical field of flame retardants, and particularly relates to a novel organic phosphorus-nitrogen flame retardant and a preparation process thereof. The flame retardant comprises piperazine pyrophosphate, melamine polyphosphate, ammonium polyphosphate, triazine trihydroxyethyl piperazine phosphonate, phytic acid melamine piperazine composite salt, dipentaerythritol, zinc borate, methylphenyl silicone resin, hydrophilic fumed silica, aminopropyl triethoxysilane and ethylene bis-stearamide. The triazine trihydroxyethyl piperazine phosphonate is prepared by substituting cyanuric chloride with hydroxyethyl piperazine in steps and then salifying with aminotrimethylene phosphonic acid. The phytic acid melamine piperazine composite salt is prepared by dispersing, neutralizing and precipitating phytic acid, melamine and piperazine. In the preparation, the base flame-retardant component is first subjected to silane surface treatment, and then mixed with the organic phosphorus-nitrogen component, the carbon-forming component and the processing aid. The obtained flame retardant has the characteristics of phosphorus-nitrogen synergy, good carbon-forming performance, uniform dispersion, simple preparation process and easily available raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of flame retardant technology, specifically relating to a novel organophosphorus nitrogen flame retardant and its preparation process. Background Technology

[0002] Organic polymer materials are widely used in building decoration, electronics, wires and cables, transportation, packaging materials, and household products due to their lightweight, good processing performance, chemical resistance, and low overall cost. However, most organic polymer materials contain numerous carbon-hydrogen bonds in their molecular structure, making them prone to softening, melting, and thermal decomposition upon heating, releasing flammable small molecules. Under the combined action of oxygen and an external heat source, these flammable decomposition products can easily continue to burn, accompanied by molten dripping, rapid heat release, and smoke generation. This not only accelerates flame propagation but may also ignite surrounding materials. To reduce the fire risk of organic polymer materials, flame retardants are typically added. Traditional halogenated flame retardants are characterized by relatively low addition amounts and high flame retardant efficiency, but their combustion process may produce corrosive and irritating hydrogen halide gases and generate significant amounts of smoke. Therefore, halogen-free, low-smoke, and environmentally adaptable phosphorus-nitrogen flame retardant systems are gradually becoming an important research direction in the field of flame retardant materials.

[0003] Existing phosphorus-nitrogen flame retardants typically consist of an intumescent flame retardant system composed of phosphates, polyphosphates, nitrogen-containing compounds, and polyhydroxy charring agents. Upon heating, the phosphorus-containing components decompose to form acidic substances with dehydration catalytic activity, promoting dehydration, cyclization, and cross-linking of the polymer matrix or charring agent; the nitrogen-containing components release flammable gases, causing the initially formed char layer to expand; and the charring components provide the carbon source for char layer formation. Piperazine pyrophosphate, melamine polyphosphate, and ammonium polyphosphate are commonly used phosphorus-nitrogen flame retardant components. Dipentaerythritol, with its numerous hydroxyl groups, can be used as a stable charring agent. When these components are combined, an intumescent char layer can form on the material surface, thereby blocking the transfer of heat, oxygen, and flammable pyrolysis products. However, in traditional compound phosphorus-nitrogen flame retardants, the acid source, gas source, and char source usually exist in a simple physical mixture state. The decomposition temperature, reaction rate, and migration behavior of each component are difficult to perfectly match, easily leading to problems such as premature decomposition of the acid source, inconsistency between gas release time and char layer formation time, and char layer cracking after expansion. In addition, polyphosphates and inorganic synergists have strong surface polarity and insufficient compatibility with non-polar or weakly polar polymer matrices. They are prone to agglomeration during the mixing process, which leads to uneven distribution of flame retardants, increased local defects in materials, and decreased mechanical properties.

[0004] To improve the overall performance of phosphorus-nitrogen flame retardant systems, existing technologies propose introducing triazine rings, piperazine rings, phosphonic acid groups, phytic acid groups, and melamine structures into flame retardant components. This allows the phosphorus source, nitrogen source, and char-forming structure to be combined in the same molecular or ionic composite structure, thereby enhancing the synergistic effect of each functional group during heating. Triazine and piperazine rings have high nitrogen content and can participate in gas release and cross-linking to form char; phosphonic acid groups and phosphate groups in phytic acid can promote dehydration and char formation; melamine can supplement the nitrogen source and promote expansion. However, some organophosphorus-nitrogen flame retardants require expensive or scarce phosphorus-containing intermediates, and their preparation involves multi-step substitution, complex catalysis, strict anhydrous conditions, or cumbersome purification, which is not conducive to industrial production. Meanwhile, although zinc borate, organosilicon resins, and fumed silica can improve the density and high-temperature stability of the char layer, if directly mixed with other flame retardant powders, they may still be unevenly dispersed due to differences in surface properties. Surface treatment of hydrophilic inorganic powders with silane coupling agents can improve the interfacial bonding between inorganic and organic components. However, existing processes still suffer from problems such as unstable silane hydrolysis, uneven powder coating, and re-agglomeration after treatment. Therefore, it is necessary to develop an organophosphorus-nitrogen flame retardant that has widely available raw materials, a relatively simple synthesis route, is easy to prepare on a large scale, and can simultaneously achieve char formation, expansion, smoke suppression, interfacial compatibility, and processing dispersibility. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a novel organophosphorus nitrogen flame retardant, comprising the following components in parts by weight:

[0006] Piperazine pyrophosphate 26-34 parts, melamine polyphosphate 12-18 parts, ammonium type II polyphosphate 8-14 parts, triazine trihydroxyethyl piperazine phosphonate 15-21 parts, phytic acid melamine piperazine complex salt 9-15 parts, dipentaerythritol 5-9 parts, zinc borate 1-3 parts, methylphenyl silicone resin 1-3 parts, hydrophilic fumed silica 0.5-1.5 parts, 3-aminopropyltriethoxysilane 0.3-0.8 parts, and ethylene bis-stearamide 0.3-0.8 parts.

[0007] According to a preferred embodiment of the present invention, the method for preparing the triazine trihydroxyethylpiperazine phosphonate includes:

[0008] A1. By weight, add 95-105 parts of cyanuric chloride to 450-550 parts of acetone, and cool under nitrogen protection to obtain a cyanuric chloride dispersion; add 68-76 parts of 1-(2-hydroxyethyl)piperazine to 350-450 parts of deionized water, and adjust the pH to 7.5-8.0 with sodium carbonate aqueous solution to obtain a first piperazine solution; under stirring, add the first piperazine solution dropwise to the cyanuric chloride dispersion, and carry out the first substitution reaction at 0-5℃. During the reaction, adjust the pH to 6.5-7.2 with sodium carbonate aqueous solution; after the reaction is completed, heat for aging, and distill under reduced pressure to obtain the first substitution reaction solution;

[0009] A2. Mix 136-152 parts of 1-(2-hydroxyethyl)piperazine with 250-350 parts of deionized water to obtain a second piperazine solution; add the second piperazine solution dropwise to the first substitution reaction solution and carry out the second substitution reaction at 35-45℃; after the addition is complete, raise the temperature to 95-100℃ to carry out the third substitution reaction; after the reaction is complete, cool down to 35-45℃, add 160-180 parts of aminotrimethylenephosphonic acid, and stir until the pH is 3.5-4.5; concentrate, filter, and obtain the filtrate; add ethanol to the filtrate to precipitate, filter, wash with ethanol, dry, pulverize, and vibrate sieve.

[0010] According to a preferred embodiment of the present invention, in step A1, the first substitution reaction is carried out at 0-5°C for 2-3 hours, and the aging temperature is 20-25°C for 1-2 hours.

[0011] According to a preferred embodiment of the present invention, in step A2, during both the second and third substitution reactions, an aqueous sodium carbonate solution is added to adjust the pH to 7.0-8.0; the second substitution reaction is carried out at 35-45°C for 2-3 hours, and the third substitution reaction is carried out at 95-100°C for 4-6 hours.

[0012] According to a preferred embodiment of the present invention, the preparation method of the phytic acid-melamine-piperazine composite salt includes:

[0013] B1. By weight, add 95-105 parts of a phytic acid aqueous solution with a mass fraction of 68-72% to 400-500 parts of deionized water and stir to obtain a diluted phytic acid solution; add 24-32 parts of melamine to 180-220 parts of deionized water and stir to disperse at 70-80℃ to obtain a melamine aqueous dispersion; add the melamine aqueous dispersion to the diluted phytic acid solution and stir to react at 80-85℃ to obtain a phytic acid-melamine reaction solution;

[0014] B2. Dissolve 28-36 parts of anhydrous piperazine in 120-160 parts of deionized water to obtain a piperazine aqueous solution; under nitrogen protection, add the piperazine aqueous solution dropwise to the phytic acid melamine reaction solution, adjust the pH to 4.8-5.5, and carry out the neutralization reaction at 40-50℃; after the reaction is completed, concentrate, add ethanol for precipitation, filter, wash, dry, pulverize and vibrate sieve.

[0015] According to a preferred embodiment of the present invention, in step B1, the stirring reaction time at 80-85°C is 2-4 hours.

[0016] According to a preferred embodiment of the present invention, in step B2, the neutralization reaction is carried out at 40-50°C for 1-2 hours.

[0017] This invention also provides a method for preparing the novel organophosphorus nitrogen flame retardant, comprising the following steps:

[0018] S1. Piperazine pyrophosphate, melamine polyphosphate, ammonium type II polyphosphate, zinc borate, and hydrophilic fumed silica are dried and mixed to obtain a basic flame retardant mixture. 3-Aminopropyltriethoxysilane is added to a mixture of ethanol and deionized water, and the pH is adjusted to 4.0-5.0 with acetic acid. After stirring and hydrolysis, a silane treatment solution is obtained. The silane treatment solution is sprayed into the basic flame retardant mixture and stirred at 55-70℃ to obtain a surface-treated flame retardant mixture. Triazine trihydroxyethylpiperazine phosphonate, phytic acid melamine piperazine composite salt, and dipentaerythritol are mixed to obtain an organophosphorus nitrogen premix. The organophosphorus nitrogen premix is ​​added to the surface-treated flame retardant mixture and stirred to obtain a composite flame retardant mixture.

[0019] S2. Add methylphenyl silicone resin and ethylene bis-stearamide to the composite flame retardant mixture, stir, cool, crush and vibrate screen.

[0020] According to a preferred embodiment of the present invention, in step S1, the zinc borate is type 2335 zinc borate; the stirring time at 55-70°C is 15-25 min.

[0021] According to a preferred embodiment of the present invention, in step S2, the stirring temperature is 55-65°C and the stirring time is 10-20 min.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) This invention uses piperazine pyrophosphate, melamine polyphosphate, and ammonium type II polyphosphate as the main phosphorus and nitrogen flame retardant components, and combines them with pentaerythritol to form an intumescent flame retardant system. During heating, piperazine pyrophosphate, melamine polyphosphate, and ammonium type II polyphosphate can form phosphorus-containing substances with dehydration catalytic activity, promoting dehydration, cross-linking, and carbonization of pentaerythritol and the surface of polymer materials; at the same time, piperazine pyrophosphate and melamine polyphosphate release flammable gases when heated, causing the softened carbon layer to expand uniformly. The formed expanded carbon layer can reduce the transfer of heat and oxygen to the interior of the material and limit the outward diffusion of combustible decomposition products, thereby slowing down the combustion of the material and the spread of flames, and reducing the phenomenon of molten dripping.

[0024] (2) Triazine trihydroxyethyl piperazine phosphonate contains triazine, hydroxyethyl, piperazine, and phosphonic acid structures, which can promote char formation, release flame-retardant gases, and form phosphorus-containing protective structures when heated. The phytic acid structure in the phytic acid-melamine-piperazine composite salt can promote the dehydration and carbonization of dipentaerythritol and polymer materials, while the melamine and piperazine structures can provide nitrogen-containing gases and participate in the formation of nitrogen-containing carbon layers. The combination of triazine trihydroxyethyl piperazine phosphonate and phytic acid-melamine-piperazine composite salt can make the phosphorus-containing, nitrogen-containing, and char-forming structures more uniformly distributed in the flame retardant, improve the problem of asynchronous heating reactions of different components, and make the formed expanded carbon layer have better continuity, integrity, and crack resistance.

[0025] (3) Zinc borate can form a heat-resistant boron-containing protective structure during heating, improving the strength and high-temperature stability of the expanded carbon layer; methylphenyl silicone resin and hydrophilic fumed silica can participate in the formation of a silicon-containing protective structure, reducing pores and cracks in the carbon layer, and improving the density and oxidation resistance of the carbon layer. Surface treatment of piperazine pyrophosphate, melamine polyphosphate, ammonium type II polyphosphate, zinc borate, and hydrophilic fumed silica with 3-aminopropyltriethoxysilane can improve the interfacial bonding between powders and between powders and polymer materials, reduce powder agglomeration, and improve the dispersion uniformity of the flame retardant. Ethylene bis-stearamide can improve the flowability and processing lubricity of the powder, reduce friction and adhesion during mixing and melt processing, so that the obtained novel organophosphorus nitrogen flame retardant has both flame-retardant char-forming properties, processing dispersion properties, and process applicability. Detailed Implementation

[0026] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0027] Example 1

[0028] This embodiment provides a preparation process for a novel organophosphorus nitrogen flame retardant, the steps of which include:

[0029] S1. Weigh out 30g piperazine pyrophosphate, 15g melamine polyphosphate, 11g ammonium type II polyphosphate, 18g triazine trihydroxyethyl piperazine phosphonate, 12g phytic acid melamine piperazine complex salt, 7g dipentaerythritol, 2g zinc borate, 2g methylphenyl silicone resin, 1g hydrophilic fumed silica, 0.55g 3-aminopropyltriethoxysilane, and 0.55g ethylene bis-stearamide, wherein the zinc borate is type 2335 zinc borate; 30g piperazine pyrophosphate, 15g melamine polyphosphate, 11g ammonium type II polyphosphate, 18g triazine trihydroxyethyl piperazine phosphonate, 12g phytic acid melamine piperazine complex salt, 7g dipentaerythritol, 2g zinc borate, 2g methylphenyl silicone resin, 1g hydrophilic fumed silica, 0.55g 3-aminopropyltriethoxysilane, and 0.55g ethylene bis-stearamide, wherein the zinc borate is type 2335 zinc borate; Ammonium phosphate, 2g zinc borate, and 1g hydrophilic fumed silica were dried at 80℃ and a vacuum of -0.080MPa for 4 hours, cooled to 25℃, and then added to a high-speed mixer. The mixture was stirred at 800r / min for 10 minutes to obtain a basic flame-retardant mixture. 0.55g of 3-aminopropyltriethoxysilane was added to a mixture of 4.46g ethanol and 0.49g deionized water, and stirred at 300r / min for 5 minutes at 25℃. 0.15g acetic acid was added to 1.35g... A 10% (w / w) acetic acid aqueous solution was obtained from deionized water. This acetic acid aqueous solution was added dropwise to a mixture containing 3-aminopropyltriethoxysilane. The pH was adjusted to 4.5, and the mixture was hydrolyzed at 25°C with stirring at 300 rpm for 30 min to obtain a silane-treated solution. The base flame retardant mixture was heated to 62.5°C and stirred at 1000 rpm. The silane-treated solution was then uniformly sprayed into the base flame retardant mixture via atomization over 5 min. Stirring was continued at 62.5°C for 20 min, followed by... Continue stirring at 62.5℃ until no visible wet lumps remain in the material and the volatile matter mass fraction is no more than 0.5%, to obtain a surface-treated flame-retardant mixture; add 18g of triazine trihydroxyethyl piperazine phosphonate, 12g of phytic acid melamine piperazine composite salt and 7g of dipentaerythritol to a premixing device and mix at 500r / min for 10min to obtain an organophosphorus nitrogen premix; add the organophosphorus nitrogen premix to the surface-treated flame-retardant mixture and stir at 700r / min for 15min at 62.5℃ to obtain a composite flame-retardant mixture;

[0030] S2. Add 2g of methylphenyl silicone resin and 0.55g of ethylene bis-stearamide to the composite flame retardant mixture, adjust the material temperature to 60℃, stir at 600r / min for 15min, and after stirring, cool the material to 35℃ under continuous stirring. Discharge the material, crush it using a pulverizing device and pass it through a vibrating screen with a pore size of 150μm. Collect the undersize material, seal and store it to obtain a new type of organophosphorus nitrogen flame retardant.

[0031] Preparation steps of triazine trihydroxyethylpiperazine phosphonate:

[0032] A1. Add 86.5g of anhydrous sodium carbonate to 346g of deionized water and stir at 300r / min for 20min at 25℃ to prepare a 20% sodium carbonate aqueous solution, which is then sealed and set aside. Add 100g of cyanuric chloride and 500g of acetone to a reactor equipped with a mechanical stirrer, temperature detection device, constant pressure dripping device, nitrogen introduction device, and reflux condenser. Stir at 300r / min to uniformly disperse the cyanuric chloride. Purge with nitrogen at a flow rate of 100mL / min for 20min to purge air from the reactor. Cool the material to 2.5℃ under continuous nitrogen purging to obtain a cyanuric chloride dispersion. Add 72g of 1-(2-hydroxyethyl)piperazine to 400g of deionized water and stir at 300r / min at 25℃ until completely dissolved. Add the sodium carbonate aqueous solution dropwise to adjust the pH to 7.75 to obtain the first piperazine solution. A constant-pressure dropping apparatus was installed, and under the conditions of maintaining the temperature of the cyanuric chloride dispersion at 2.5℃ and the stirring speed at 350 r / min, the first piperazine solution was added dropwise to the cyanuric chloride dispersion at a uniform rate over 60 min. During the dropwise addition, the sodium carbonate aqueous solution was added dropwise simultaneously to maintain the pH of the reaction system at 6.85. After the dropwise addition was completed, the first substitution reaction was carried out by stirring at 2.5℃ for 2.5 h. After the first substitution reaction was completed, the temperature of the reaction system was increased to 22.5℃ at a heating rate of 0.5℃ / min, and the system was stirred at 350 r / min at 22.5℃ for 1.5 h to mature. After the maturation was completed, the reaction system was transferred to a vacuum distillation apparatus, and vacuum distillation was carried out under the conditions of material temperature at 40℃ and vacuum degree at -0.085 MPa. Acetone was condensed and recovered until the outflow rate of the condensate was less than 1 g / min and there was no obvious acetone odor in the reaction system. Vacuum distillation was then stopped to obtain the first substitution reaction solution.

[0033] A2. Add 144g of 1-(2-hydroxyethyl)piperazine to 300g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a second piperazine solution. Heat the first substitution reaction solution to 40℃ and adjust the stirring speed to 350r / min. Add the second piperazine solution dropwise to the first substitution reaction solution at a uniform rate over 90min. Simultaneously add the sodium carbonate aqueous solution prepared in step A1, maintaining the pH of the reaction system at 7.5. After the addition is complete, continue stirring at 40℃ for 2.5h to carry out the second substitution reaction. After the second substitution reaction is complete, reduce the temperature at 1℃ / The reaction system was heated to 97.5°C at a heating rate of min, and the mixture was kept under reflux and stirred at 400 r / min for 5 h for the third substitution reaction. During the third substitution reaction, the sodium carbonate aqueous solution prepared in step A1 was added dropwise to maintain the pH of the reaction system at 7.5. The cumulative amount of sodium carbonate aqueous solution used in steps A1 and A2 was 432.5 g. After the third substitution reaction was completed, the reaction system was cooled to 40°C. 170 g of aminotrimethylenephosphonic acid was added to 170 g of deionized water, and the mixture was stirred at 300 r / min at 40°C until a homogeneous solution was formed. The solution was then processed within 60 min. The obtained solution was added to the reaction system at a uniform rate, with the stirring speed maintained at 350 r / min during the addition. After the addition was completed, stirring was continued at 40℃ for 2 h to stabilize the pH of the reaction system at 4.0, yielding a salt-forming reaction solution. The salt-forming reaction solution was concentrated to a solid content of 45% under a vacuum of 60℃ and -0.080 MPa. The concentrate was cooled to 10℃ and allowed to stand for 2 h to allow sodium chloride to precipitate. The solution was then filtered using a 20 μm filtration medium, and the filtrate was collected. Under stirring conditions of 25℃ and 300 r / min, 1300 g of mass fraction was added to the filtrate over 30 min. Add 95% ethanol, continue stirring for 30 minutes after the addition is complete, cool the material to 10℃ and let it stand for 3 hours, filter, and collect the precipitate; wash the precipitate twice with 400g of 95% ethanol, using 200g of 95% ethanol each time, filter, and place the precipitate in a vacuum drying device, dry it at 70℃ and a vacuum degree of -0.080-MPa until the difference between two consecutive weighings 1 hour apart is no greater than 0.1% of the precipitate mass, pulverize the dried product and pass it through a vibrating sieve with a pore size of 150μm to obtain triazine trihydroxyethylpiperazine phosphonate.

[0034] Preparation steps of phytic acid-melamine-piperazine complex salt:

[0035] B1. Add 100g of 70% phytic acid aqueous solution and 450g of deionized water to a reactor equipped with a mechanical stirrer, temperature detection device, dropping device, and reflux condenser. Stir at 300r / min for 30min at 25℃ to obtain a diluted phytic acid solution. Add 28g of melamine and 200g of deionized water to another container. Heat the material to 75℃ and stir at 500r / min for 30min to obtain a melamine aqueous dispersion. Heat the diluted phytic acid solution to 82.5℃ and adjust the stirring speed to 350r / min. Within 30min, uniformly add the melamine aqueous dispersion to the diluted phytic acid solution. After the addition is completed, continue stirring and reacting at 82.5℃ for 3h. Maintain reflux during the reaction to obtain a phytic acid-melamine reaction solution.

[0036] B2. Add 32g of anhydrous piperazine to 140g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a piperazine aqueous solution. Cool the phytic acid-melamine reaction solution to 45℃ and purge nitrogen gas into the reactor at a flow rate of 100mL / min for 20min. Under continuous nitrogen purging and stirring at 350r / min, add the piperazine aqueous solution dropwise to the phytic acid-melamine reaction solution at a uniform rate over 60min. By controlling the dropping rate of the piperazine aqueous solution, the pH of the reaction system is gradually increased to 5.15. After the addition is completed, continue the neutralization reaction at 45℃ for 1.5h, ensuring that the pH change is no greater than 0.1 within 30min. Concentrate the reaction solution under conditions of 60℃ and a vacuum of -0.080MPa. The solid content was reduced to 40%, and the concentrate was cooled to 25°C. 900g of 95% ethanol was added over 30 minutes with stirring at 300r / min. After addition, stirring continued for another 30 minutes. The material was then cooled to 10°C and allowed to stand for 3 hours. The mixture was filtered, and the precipitate was collected. The precipitate was washed twice with 150g of 95% ethanol each time. The washed precipitate was placed in a vacuum dryer and dried at 70°C and a vacuum of -0.080MPa until the difference between two consecutive weighings taken 1 hour apart was no more than 0.1% of the precipitate mass. The dried product was then pulverized and passed through a vibrating sieve with a pore size of 150μm to obtain phytic acid-melamine-piperazine composite salt.

[0037] Example 2

[0038] The difference between this embodiment and Embodiment 1 is that this embodiment provides a preparation process for a novel organophosphorus nitrogen flame retardant, the steps of which include:

[0039] S1. Weigh out 26g piperazine pyrophosphate, 12g melamine polyphosphate, 8g ammonium type II polyphosphate, 15g triazine trihydroxyethyl piperazine phosphonate, 9g phytic acid melamine piperazine complex salt, 5g dipentaerythritol, 1g zinc borate, 1g methylphenyl silicone resin, 0.5g hydrophilic fumed silica, 0.3g 3-aminopropyltriethoxysilane, and 0.3g ethylene bis-stearamide, wherein the zinc borate is type 2335 zinc borate; 26g piperazine pyrophosphate, 12g melamine polyphosphate, 8g... Type II ammonium polyphosphate, 1g zinc borate, and 0.5g hydrophilic fumed silica were dried at 80℃ and a vacuum of -0.080MPa for 4 hours, cooled to 25℃, and then added to a high-speed mixer. The mixture was mixed at 800r / min for 10 minutes to obtain a basic flame-retardant mixture. 0.3g of 3-aminopropyltriethoxysilane was added to a mixture of 2.43g ethanol and 0.27g deionized water, and stirred at 300r / min for 5 minutes at 25℃. 0.09g of... Acetic acid was added to 0.81 g of deionized water to obtain a 10% acetic acid aqueous solution. This acetic acid aqueous solution was then added dropwise to a mixture containing 3-aminopropyltriethoxysilane. The pH was adjusted to 4.0, and the mixture was hydrolyzed at 25°C with stirring at 300 rpm for 30 min to obtain a silane-treated solution. The base flame retardant mixture was heated to 55°C and stirred at 1000 rpm. Within 5 min, the silane-treated solution was uniformly sprayed onto the base flame retardant mixture using an atomizing method. The mixture was then subjected to further hydrolysis at 55°C. Continue stirring for 15 minutes, then continue stirring until there are no visible wet lumps in the material and the volatile matter mass fraction is no more than 0.5%, to obtain a surface-treated flame-retardant mixture; mix 15g of triazine trihydroxyethyl piperazine phosphonate, 9g of phytic acid melamine piperazine composite salt and 5g of dipentaerythritol at 500r / min for 10 minutes to obtain an organophosphorus nitrogen premix; add the organophosphorus nitrogen premix to the surface-treated flame-retardant mixture, and stir at 700r / min at 55℃ for 15 minutes to obtain a composite flame-retardant mixture;

[0040] S2. Add 1g of methylphenyl silicone resin and 0.3g of ethylene bis-stearamide to the composite flame retardant mixture, stir at 600r / min for 10min at 55℃, cool the material to 35℃ under continuous stirring, discharge the material, crush it and pass it through a vibrating screen with a pore size of 150μm, collect the undersize material, seal and store it to obtain a new type of organophosphorus nitrogen flame retardant.

[0041] Preparation steps of triazine trihydroxyethylpiperazine phosphonate:

[0042] A1. Add 82g of anhydrous sodium carbonate to 328g of deionized water and stir at 300r / min for 20min at 25℃ to prepare a 20% sodium carbonate aqueous solution. Seal and set aside. Add 95g of cyanuric chloride and 450g of acetone to a reactor equipped with a mechanical stirrer, temperature detection device, constant pressure dripping device, nitrogen introduction device, and reflux condenser. Stir at 300r / min to uniformly disperse the cyanuric chloride. Purge with nitrogen at a flow rate of 100mL / min for 20min. Cool the material to 0℃ under continuous nitrogen purging to obtain a cyanuric chloride dispersion. Add 68g of 1-(2-hydroxyethyl)piperazine to 350g of deionized water and stir at 300r / min at 25℃ until completely dissolved. Add the sodium carbonate aqueous solution dropwise and adjust the pH. The solution was adjusted to pH 7.5 to obtain the first piperazine solution. While maintaining the cyanuric chloride dispersion at 0°C and stirring at 350 r / min, the first piperazine solution was added dropwise to the cyanuric chloride dispersion at a uniform rate over 60 min. Simultaneously, the sodium carbonate aqueous solution was added dropwise to maintain the pH of the reaction system at 6.5. After the addition was completed, stirring was continued at 0°C for 2 h to carry out the first substitution reaction. After the first substitution reaction was completed, the reaction system was heated to 20°C at a rate of 0.5°C / min and matured at 20°C with stirring at 350 r / min for 1 h. After maturation, vacuum distillation was carried out at a material temperature of 35°C and a vacuum degree of -0.075 MPa until the condensate outflow rate was less than 1 g / min and there was no obvious acetone odor in the reaction system, thus obtaining the first substitution reaction solution.

[0043] A2. Add 136g of 1-(2-hydroxyethyl)piperazine to 250g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a second piperazine solution. Heat the first substitution reaction solution to 35℃ and adjust the stirring speed to 350r / min. Add the second piperazine solution dropwise to the first substitution reaction solution at a uniform rate over 90min. Simultaneously add the sodium carbonate aqueous solution prepared in step A1, maintaining the pH of the reaction system at 7.0. After the addition is complete, continue stirring at 35℃ to proceed with the second substitution reaction. After the second substitution reaction, the reaction system was heated to 95°C at a rate of 1°C / min, kept under reflux, and stirred at 400 r / min for 4 hours for the third substitution reaction. During the third substitution reaction, the sodium carbonate aqueous solution prepared in step A1 was added dropwise to maintain the pH of the reaction system at 7.0. The cumulative amount of sodium carbonate aqueous solution used in steps A1 and A2 was 410 g. After the third substitution reaction, the reaction system was cooled to 35°C. 160 g of aminotrimethylenephosphonic acid was added to 160 g of deionized water. In a mixture, the solution was stirred at 300 rpm at 35°C until a homogeneous solution was formed. This solution was then added to the reaction system at a uniform rate over 60 minutes. After the addition was complete, stirring continued at 35°C for 2 hours to stabilize the pH of the reaction system at 3.5, yielding a salt-forming reaction solution. This solution was concentrated to a solid content of 45% at 60°C and a vacuum of -0.080 MPa. The concentrate was cooled to 10°C and allowed to stand for 2 hours. The solution was then filtered through a 20 μm filter medium, and the filtrate was collected. The solution was then stirred at 25°C and 300 rpm. Under the following conditions, 1200g of 95% ethanol was added to the filtrate within 30 minutes, and stirring was continued for another 30 minutes. The material was cooled to 10℃ and allowed to stand for 3 hours. After filtration, the precipitate was collected. The precipitate was washed twice with 350g of 95% ethanol. The precipitate was dried at 70℃ and a vacuum of -0.080MPa until the difference between two consecutive weighings taken 1 hour apart was no more than 0.1% of the precipitate mass. The precipitate was then pulverized and passed through a vibrating sieve with a pore size of 150μm to obtain triazine trihydroxyethylpiperazine phosphonate.

[0044] Preparation steps of phytic acid-melamine-piperazine complex salt:

[0045] B1. Add 95g of 68% phytic acid aqueous solution and 400g of deionized water to the reactor, and stir at 300r / min for 30min at 25℃ to obtain a diluted phytic acid solution; add 24g of melamine to 180g of deionized water, heat the material to 70℃ and stir at 500r / min for 30min to obtain a melamine aqueous dispersion; heat the diluted phytic acid solution to 80℃ and adjust the stirring speed to 350r / min, add the melamine aqueous dispersion to the diluted phytic acid solution within 30min, and continue stirring and reacting at 80℃ for 2h, maintaining reflux during the reaction to obtain a phytic acid-melamine reaction solution;

[0046] B2. Add 28g of anhydrous piperazine to 120g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a piperazine aqueous solution. Cool the phytic acid-melamine reaction solution to 40℃ and purge with nitrogen gas at a flow rate of 100mL / min for 20min. Under continuous nitrogen purging and stirring at 350r / min, add the piperazine aqueous solution dropwise to the phytic acid-melamine reaction solution at a uniform rate over 60min. By controlling the dropping rate of the piperazine aqueous solution, the pH of the reaction system is gradually increased to 4.8. After the addition is completed, continue the neutralization reaction at 40℃ for 1h, ensuring that the pH change is no greater than 0.1 within 30min. Heat the reaction solution at 60℃ under a vacuum... The product was concentrated to a solid content of 40% under a vacuum of -0.080 MPa. The concentrate was cooled to 25°C, and 800 g of 95% ethanol was added over 30 min while stirring at 300 r / min. The stirring was continued for another 30 min. The material was then cooled to 10°C and allowed to stand for 3 h. The product was filtered, and the precipitate was collected. The precipitate was washed twice with 250 g of 95% ethanol. The precipitate was dried at 70°C under a vacuum of -0.080 MPa until the difference between two consecutive weighings taken 1 h apart was no more than 0.1% of the precipitate mass. The product was then pulverized and passed through a vibrating sieve with a pore size of 150 μm to obtain phytic acid-melamine-piperazine composite salt.

[0047] Example 3

[0048] The difference between this embodiment and Embodiment 1 is that this embodiment provides a preparation process for a novel organophosphorus nitrogen flame retardant, the steps of which include:

[0049] S1. Weigh out 34g piperazine pyrophosphate, 18g melamine polyphosphate, 14g ammonium type II polyphosphate, 21g triazine trihydroxyethyl piperazine phosphonate, 15g phytic acid melamine piperazine complex salt, 9g dipentaerythritol, 3g zinc borate, 3g methylphenyl silicone resin, 1.5g hydrophilic fumed silica, 0.8g 3-aminopropyltriethoxysilane, and 0.8g ethylene bis-stearamide, wherein the zinc borate is type 2335 zinc borate; 34g piperazine pyrophosphate, 18g melamine polyphosphate, 1... 4g of type II ammonium polyphosphate, 3g of zinc borate, and 1.5g of hydrophilic fumed silica were dried at 80℃ and a vacuum of -0.080MPa for 4 hours, cooled to 25℃, and then added to a high-speed mixer. The mixture was stirred at 800r / min for 10 minutes to obtain a basic flame-retardant mixture. 0.8g of 3-aminopropyltriethoxysilane was added to a mixture of 6.48g of ethanol and 0.72g of deionized water, and stirred at 300r / min for 5 minutes at 25℃. 0.2g of... 2g of acetic acid was added to 1.98g of deionized water to obtain a 10% (w / w) acetic acid aqueous solution. This acetic acid aqueous solution was then added dropwise to a mixture containing 3-aminopropyltriethoxysilane. The pH was adjusted to 5.0, and the mixture was hydrolyzed at 25°C with stirring at 300 rpm for 30 minutes to obtain a silane-treated solution. The base flame-retardant mixture was heated to 70°C and stirred at 1000 rpm. Within 5 minutes, the silane-treated solution was uniformly sprayed onto the base flame-retardant mixture using an atomization method. The mixture was then subjected to further hydrolysis at 70°C. Continue stirring for 25 minutes, then continue stirring until there are no visible wet lumps in the material and the volatile matter mass fraction is no more than 0.5%, to obtain a surface-treated flame-retardant mixture; mix 21g of triazine trihydroxyethyl piperazine phosphonate, 15g of phytic acid melamine piperazine composite salt and 9g of dipentaerythritol at 500r / min for 10 minutes to obtain an organophosphorus nitrogen premix; add the organophosphorus nitrogen premix to the surface-treated flame-retardant mixture, and stir at 700℃ and 700r / min for 15 minutes to obtain a composite flame-retardant mixture;

[0050] S2. Add 3g of methylphenyl silicone resin and 0.8g of ethylene bis-stearamide to the composite flame retardant mixture, stir at 600r / min for 20min at 65℃, cool the material to 35℃ under continuous stirring, discharge the material, crush it and pass it through a vibrating screen with a pore size of 150μm, collect the undersize material, seal and store it to obtain a new type of organophosphorus nitrogen flame retardant.

[0051] Preparation steps of triazine trihydroxyethylpiperazine phosphonate:

[0052] A1. Add 91g of anhydrous sodium carbonate to 364g of deionized water and stir at 300r / min for 20min at 25℃ to prepare a 20% sodium carbonate aqueous solution. Seal and set aside. Add 105g of cyanuric chloride and 550g of acetone to a reactor equipped with a mechanical stirrer, temperature detection device, constant pressure dripping device, nitrogen introduction device, and reflux condenser. Stir at 300r / min to uniformly disperse the cyanuric chloride. Purge with nitrogen at a flow rate of 100mL / min for 20min. Cool the material to 5℃ under continuous nitrogen purging to obtain a cyanuric chloride dispersion. Add 76g of 1-(2-hydroxyethyl)piperazine to 450g of deionized water and stir at 300r / min at 25℃ until completely dissolved. Add the sodium carbonate aqueous solution dropwise to adjust the pH. The solution was adjusted to 8.0 to obtain the first piperazine solution. While maintaining the temperature of the cyanuric chloride dispersion at 5°C and the stirring speed at 350 r / min, the first piperazine solution was added dropwise to the cyanuric chloride dispersion at a uniform rate over 60 min. Simultaneously, the sodium carbonate aqueous solution was added dropwise to maintain the pH of the reaction system at 7.2. After the addition was completed, the system was stirred at 5°C for 3 h to carry out the first substitution reaction. After the first substitution reaction was completed, the reaction system was heated to 25°C at a heating rate of 0.5°C / min and then stirred at 350 r / min for 2 h to mature. After maturation, the system was subjected to vacuum distillation at a material temperature of 40°C and a vacuum degree of -0.075 MPa until the condensate outflow rate was less than 1 g / min and there was no obvious acetone odor in the reaction system, thus obtaining the first substitution reaction solution.

[0053] A2. Add 152g of 1-(2-hydroxyethyl)piperazine to 350g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a second piperazine solution. Heat the first substitution reaction solution to 45℃ and adjust the stirring speed to 350r / min. Add the second piperazine solution dropwise to the first substitution reaction solution at a uniform rate over 90min. Simultaneously add the sodium carbonate aqueous solution prepared in step A1, maintaining the pH of the reaction system at 8.0. After the addition is complete, continue stirring at 45℃ to proceed with the second substitution reaction. After the second substitution reaction, the reaction system was heated to 100°C at a rate of 1°C / min, kept under reflux, and stirred at 400 r / min for 6 hours for the third substitution reaction. During the third substitution reaction, the sodium carbonate aqueous solution prepared in step A1 was added dropwise to maintain the pH of the reaction system at 8.0. The cumulative amount of sodium carbonate aqueous solution used in steps A1 and A2 was 455 g. After the third substitution reaction, the reaction system was cooled to 45°C. 180 g of aminotrimethylenephosphonic acid was added to 180 g of deionized sodium carbonate. In water, the mixture was stirred at 300 rpm at 45°C until a homogeneous solution was formed. This solution was then added uniformly to the reaction system over 60 minutes. After the addition was complete, stirring continued at 45°C for 2 hours to stabilize the pH of the reaction system at 4.5, yielding a salt-forming reaction solution. This solution was concentrated to a solid content of 45% at 60°C and a vacuum of -0.080 MPa. The concentrate was cooled to 10°C and allowed to stand for 2 hours. The solution was then filtered through a 20 μm filter medium, and the filtrate was collected. The solution was then stirred at 25°C and 300 rpm. Under the following conditions, 1400g of 95% ethanol was added to the filtrate within 30 minutes, and stirring was continued for another 30 minutes. The material was cooled to 10℃ and allowed to stand for 3 hours. After filtration, the precipitate was collected. The precipitate was washed twice with 450g of 95% ethanol. The precipitate was dried at 70℃ and a vacuum of -0.080MPa until the difference between two consecutive weighings taken 1 hour apart was no more than 0.1% of the precipitate mass. The precipitate was then pulverized and passed through a vibrating sieve with a pore size of 150μm to obtain triazine trihydroxyethylpiperazine phosphonate.

[0054] Preparation steps of phytic acid-melamine-piperazine complex salt:

[0055] B1. Add 105g of 72% phytic acid aqueous solution and 500g of deionized water to the reactor, and stir at 300r / min for 30min at 25℃ to obtain a diluted phytic acid solution; add 32g of melamine to 220g of deionized water, heat the material to 80℃ and stir at 500r / min for 30min to obtain a melamine aqueous dispersion; heat the diluted phytic acid solution to 85℃ and adjust the stirring speed to 350r / min, add the melamine aqueous dispersion to the diluted phytic acid solution within 30min, and continue stirring and reacting at 85℃ for 4h, maintaining reflux during the reaction to obtain a phytic acid-melamine reaction solution;

[0056] B2. Add 36g of anhydrous piperazine to 160g of deionized water and stir at 300r / min at 25℃ until completely dissolved to obtain a piperazine aqueous solution. Cool the phytic acid-melamine reaction solution to 50℃ and purge with nitrogen gas at a flow rate of 100mL / min for 20min. Under continuous nitrogen purging and stirring at 350r / min, add the piperazine aqueous solution dropwise to the phytic acid-melamine reaction solution at a uniform rate over 60min. By controlling the dropping rate of the piperazine aqueous solution, the pH of the reaction system is gradually increased to 5.5. After the addition is completed, continue the neutralization reaction at 50℃ for 2h, ensuring that the pH change is no greater than 0.1 within 30min. Heat the reaction solution at 60℃ under a vacuum... The product was concentrated to a solid content of 40% under a vacuum of -0.080 MPa. The concentrate was cooled to 25°C, and 1000 g of 95% ethanol was added over 30 min while stirring at 300 r / min. The stirring was continued for another 30 min. The material was then cooled to 10°C and allowed to stand for 3 h. The product was filtered and the precipitate was collected. The precipitate was washed twice with 350 g of 95% ethanol. The precipitate was dried at 70°C under a vacuum of -0.080 MPa until the difference between two consecutive weighings taken 1 h apart was no more than 0.1% of the precipitate mass. The product was then pulverized and passed through a vibrating sieve with a pore size of 150 μm to obtain phytic acid-melamine-piperazine composite salt.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is that 18g of triazine trihydroxyethyl piperazine phosphonate and 12g of phytic acid melamine piperazine complex salt are not prepared and added. Instead, 18g of piperazine pyrophosphate is used to replace 18g of triazine trihydroxyethyl piperazine phosphonate, and 12g of melamine polyphosphate is used to replace 12g of phytic acid melamine piperazine complex salt. The rest is the same as in Example 1.

[0059] Comparative Example 2

[0060] The difference between this comparative example and Example 1 is that 18g of triazine trihydroxyethyl piperazine phosphonate is not prepared or added; instead, 18g of piperazine pyrophosphate is used in place of 18g of triazine trihydroxyethyl piperazine phosphonate. The rest is the same as in Example 1.

[0061] Comparative Example 3

[0062] The difference between this comparative example and Example 1 is that 12g of phytic acid melamine piperazine complex salt is not prepared and is not added. Instead, 12g of melamine polyphosphate is used to replace 12g of phytic acid melamine piperazine complex salt by the same mass. The rest is the same as in Example 1.

[0063] The performance of the novel organophosphorus nitrogen flame retardants provided in the above embodiments and comparative examples was tested using the following methods:

[0064] The novel organophosphorus nitrogen flame retardants prepared in Examples 1-3 and Comparative Examples 1-3 were mixed with polypropylene at a mass ratio of 25:75. Both polypropylene and novel organophosphorus nitrogen flame retardants were pre-dried at 80±2℃ for 4 hours. The mixture was added to a twin-screw extruder for melt blending. The temperatures of each zone of the extruder were set to 170℃, 175℃, 180℃, 185℃ and 180℃ respectively, and the screw speed was 60 r / min. After extrusion, the mixture was water-cooled and pelletized. The resulting pellets were dried at 80±2℃ for 4 hours and then injection molded at 190±5℃ into samples required for different test items. All samples were conditioned for 88 hours in an environment of 23±2℃ and 50±10% relative humidity before testing.

[0065] Limiting oxygen index test: The test shall be conducted in accordance with the method for testing the room temperature oxygen index of plastics. The test specimen shall be made into a strip with a size of 80mm×10mm×4mm. Each group shall prepare no less than 15 specimens. The specimen shall be installed vertically in the center of a transparent combustion tube, with the upper end of the specimen at least 100mm away from the top of the combustion tube. A mixture of oxygen and nitrogen shall be introduced into the combustion tube. After the gas flow stabilizes, the specimen shall be ignited from the top. The ignition time shall not exceed 30s. The oxygen volume fraction shall be adjusted step by step according to whether the previous specimen continues to burn. The test shall be judged when the burning time of the specimen reaches 180s or the flame propagation length reaches 50mm. The limiting oxygen index shall be calculated according to the volume fraction of oxygen flow rate to the total flow rate of oxygen and nitrogen. The result shall be accurate to 0.1%.

[0066] Vertical burning performance test: The test was conducted according to the plastic vertical burning test method. The sample was made into a strip with a size of 125mm×13mm×1.6mm. Five samples were tested in each group. The long axis of the sample was kept vertical and the upper end was clamped. Degreased cotton was placed under the sample. The flame height was adjusted to 20±1mm. The flame was applied to the center position of the lower end of the sample for 10±0.5s and then removed. The first afterflame time was recorded. After the afterflame was extinguished, the flame was immediately applied again for 10±0.5s and the second afterflame time and afterglow time were recorded. At the same time, it was observed whether the burning drips ignited the degreased cotton. The vertical burning level was determined based on the afterflame time of a single sample, the total afterflame time of each group of samples, the afterglow time, whether the burning reached the clamping position, and whether the degreased cotton was ignited.

[0067] Peak heat release rate test: The test was conducted using the cone calorimetry method. The samples were prepared as flat plates measuring 100mm × 100mm × 3mm, with three samples tested per group. The sides and bottom of the samples, except for the heated surface, were covered with aluminum foil. The samples were placed horizontally in a sample holder, with the effective exposed area controlled to be 0.0088m². 2 The external thermal radiation intensity is set to 35 kW / m². 2 The sample was ignited using an electric spark igniter, and data on the oxygen concentration, exhaust flow rate, and mass change of the combustion products were continuously collected. The heat release rate was calculated based on the oxygen consumption principle, and the maximum value in the heat release rate curve was taken as the peak heat release rate. The arithmetic mean of the test results of 3 samples was taken.

[0068] Maximum specific optical density test: The test was conducted according to the single-chamber method for plastic smoke density testing. The samples were prepared as flat plates measuring 75mm × 75mm × 3mm, with three samples tested per group. The samples were horizontally installed in a sealed smoke chamber, with the heated surface facing the radiation cone. The thermal radiation intensity was set to 25kW / m². 2 The test was conducted using an ignition flame. Before the test, the optical system of the smoke box was calibrated at zero point and full scale. After ignition, the test was conducted continuously for 20 minutes. The specific optical density was calculated by the change in beam transmittance. The maximum specific optical density that occurred during the test was taken as the maximum specific optical density. The arithmetic mean of the test results of 3 samples was taken.

[0069] Tensile strength test: The test shall be conducted in accordance with the tensile property test method for molded and extruded plastics. The specimen shall be made into a dumbbell-shaped specimen of type 1A, with a total length of 170 mm, a width of 10 mm for the narrow parallel section, and a thickness of 4 mm. Each test group shall have no less than 5 specimens. The actual width and thickness of the narrow parallel section of each specimen shall be measured. The specimen shall be clamped longitudinally between the upper and lower clamps of the universal testing machine, keeping the center line of the specimen aligned with the direction of force. The specimen shall be stretched at a test speed of 50 mm / min until it breaks. The tensile strength shall be calculated by dividing the maximum tensile force during the test by the original cross-sectional area of ​​the specimen. Specimens that break at the clamps or have obvious sample preparation defects shall be discarded. The arithmetic mean of the test results of the valid specimens shall be taken.

[0070] 24-hour water absorption rate test: The test was conducted according to the plastic water absorption test method. The sample was made into a flat sample with a size of 50mm×50mm×3.2mm. Three samples were tested in each group. The sample was dried in an oven at 50±2℃ for 24 hours. After being transferred to a desiccator and cooled to 23±2℃, the initial mass was weighed to an accuracy of 0.001g. Then, the sample was completely immersed in distilled water at 23±1℃ for 24±1 hours. A gap was maintained between the samples and between the samples and the container wall. After the immersion was completed, the sample was removed and the surface moisture was quickly absorbed with clean filter paper. The mass after immersion was weighed within 1 minute. The 24-hour water absorption rate was calculated by dividing the difference between the mass after immersion and the initial mass by the initial mass and then multiplying by 100%. The arithmetic mean of the test results of the three samples was taken.

[0071] The performance test data above are shown in Table 1.

[0072] Table 1: Performance Test Results

[0073]

[0074] As can be seen from the above, the limiting oxygen index of Examples 1-3 is 31.8-33.1%, which is higher than that of Comparative Examples 1-3 (28.5-30.3%). Examples 1-3 all reach V-0 level with a thickness of 1.6 mm, while Comparative Example 1 is V-2 level, and Comparative Examples 2 and 3 only reach V-1 level. This indicates that the addition of triazine trihydroxyethyl piperazine phosphonate and phytic acid melamine piperazine composite salt can better match the acid source, gas source and char source during heating, promote the formation of a continuous, stable and non-crackable expanded char layer, and solve the problems of the incoordination between the char formation rate and the gas release rate, the easy cracking of the char layer and the insufficient flame retardant level of traditional physical compound phosphorus and nitrogen flame retardants.

[0075] The peak heat release rates of Examples 1-3 are 210-232 kW / m². 2 It is significantly lower than the 258-315 kW / m² of the comparative examples 1-3. 2In Example 1, the temperature drop was approximately 33.3% lower than that of Comparative Example 1, which did not contain either triazine trihydroxyethyl piperazine phosphonate or phytic acid melamine piperazine composite salt. This indicates that there is a significant synergistic effect between triazine trihydroxyethyl piperazine phosphonate and phytic acid melamine piperazine composite salt, which can effectively inhibit the thermal decomposition of polymer materials and the release of flammable products, thereby reducing the combustion intensity.

[0076] The maximum specific optical density of Examples 1-3 was 155-171, lower than that of Comparative Examples 1-3 (190-232), indicating that the formed phosphorus-, nitrogen-, boron-, and silicon-containing composite carbon layer can reduce the emission of combustible pyrolysis products and soot, thus improving the problem of high smoke release in traditional intumescent flame retardant systems. In Comparative Example 2, lacking triazine trihydroxyethylpiperazine phosphonate, the limiting oxygen index decreased to 29.8%, and the peak heat release rate increased to 275 kW / m³. 2 The results indicate that triazine trihydroxyethylpiperazine phosphonate plays an important role in improving the thermal stability of phosphorus- and nitrogen-containing structures, promoting cross-linking to char, and reducing heat release. In Comparative Example 3, lacking the phytic acid-melamine-piperazine composite salt, the maximum specific optical density increased to 206, and the 24-hour water absorption rate increased to 0.54%, indicating that the phytic acid-melamine-piperazine composite salt can not only supplement phosphorus and nitrogen sources but also improve the density of the char layer and reduce the migration of flame-retardant components in water. The tensile strength of Examples 1-3 was 26.0-27.2 MPa, higher than the 24.4-25.7 MPa of Comparative Examples 1-3, indicating that the two modified compounds have good interfacial compatibility with the basic flame-retardant components treated with 3-aminopropyltriethoxysilane, which can reduce powder agglomeration and mechanical property loss caused by interfacial defects.

[0077] The 24-hour water absorption rate of Examples 1-3 was only 0.28-0.36%, significantly lower than that of Comparative Examples 1-3 (0.47-0.72%). Among them, Example 1 showed a reduction of approximately 61.1% compared to Comparative Example 1. This indicates that the composite system formed by triazine trihydroxyethyl piperazine phosphonate, phytic acid melamine piperazine composite salt, methyl phenyl silicone resin, hydrophilic fumed silica, and 3-aminopropyltriethoxysilane can improve the problems of strong hygroscopicity, easy migration, and insufficient water resistance of traditional polyphosphate flame retardants.

[0078] In summary, Examples 1-3 are superior to Comparative Examples 1-3 in terms of flame retardancy rating, suppression of heat release, reduction of smoke density, maintenance of mechanical properties, and improvement of water resistance. This demonstrates that the triazine trihydroxyethyl piperazine phosphonate and phytic acid melamine piperazine composite salt do not merely replace conventional flame retardant components in equal amounts, but rather improve flame retardancy efficiency, char layer quality, interfacial compatibility, and service stability through structural complementarity and phosphorus-nitrogen synergistic effects.

Claims

1. A novel organophosphorus-nitrogen flame retardant, characterized in that, Includes the following components in parts by weight: Piperazine pyrophosphate 26-34 parts, melamine polyphosphate 12-18 parts, ammonium type II polyphosphate 8-14 parts, triazine trihydroxyethyl piperazine phosphonate 15-21 parts, phytic acid melamine piperazine complex salt 9-15 parts, dipentaerythritol 5-9 parts, zinc borate 1-3 parts, methylphenyl silicone resin 1-3 parts, hydrophilic fumed silica 0.5-1.5 parts, 3-aminopropyltriethoxysilane 0.3-0.8 parts, and ethylene bis-stearamide 0.3-0.8 parts.

2. The novel organophosphorus nitrogen flame retardant according to claim 1, characterized in that, The preparation method of the triazine trihydroxyethylpiperazine phosphonate includes: A1. By weight, add 95-105 parts of cyanuric chloride to 450-550 parts of acetone, and cool under nitrogen protection to obtain a cyanuric chloride dispersion; add 68-76 parts of 1-(2-hydroxyethyl)piperazine to 350-450 parts of deionized water, and adjust the pH to 7.5-8.0 with sodium carbonate aqueous solution to obtain a first piperazine solution; under stirring, add the first piperazine solution dropwise to the cyanuric chloride dispersion, and carry out the first substitution reaction at 0-5℃. During the reaction, adjust the pH to 6.5-7.2 with sodium carbonate aqueous solution; after the reaction is completed, heat for aging, and distill under reduced pressure to obtain the first substitution reaction solution; A2. Mix 136-152 parts of 1-(2-hydroxyethyl)piperazine with 250-350 parts of deionized water to obtain a second piperazine solution; add the second piperazine solution dropwise to the first substitution reaction solution and carry out the second substitution reaction at 35-45℃; after the addition is complete, raise the temperature to 95-100℃ to carry out the third substitution reaction; after the reaction is complete, cool down to 35-45℃, add 160-180 parts of aminotrimethylenephosphonic acid, and stir until the pH is 3.5-4.5; concentrate, filter, and obtain the filtrate; add ethanol to the filtrate to precipitate, filter, wash with ethanol, dry, pulverize, and vibrate sieve.

3. The novel organophosphorus nitrogen flame retardant according to claim 2, characterized in that, In step A1, the first substitution reaction is carried out at 0-5℃ for 2-3 hours, and the aging temperature is 20-25℃ for 1-2 hours.

4. The novel organophosphorus nitrogen flame retardant according to claim 2, characterized in that, In step A2, during both the second and third substitution reactions, sodium carbonate aqueous solution is added to adjust the pH to 7.0-8.0; the second substitution reaction is carried out at 35-45℃ for 2-3 hours, and the third substitution reaction is carried out at 95-100℃ for 4-6 hours.

5. The novel organophosphorus nitrogen flame retardant according to claim 1, characterized in that, The preparation method of the phytic acid-melamine-piperazine composite salt includes: B1. By weight, add 95-105 parts of a phytic acid aqueous solution with a mass fraction of 68-72% to 400-500 parts of deionized water and stir to obtain a diluted phytic acid solution; add 24-32 parts of melamine to 180-220 parts of deionized water and stir to disperse at 70-80℃ to obtain a melamine aqueous dispersion; add the melamine aqueous dispersion to the diluted phytic acid solution and stir to react at 80-85℃ to obtain a phytic acid-melamine reaction solution; B2. Dissolve 28-36 parts of anhydrous piperazine in 120-160 parts of deionized water to obtain a piperazine aqueous solution; under nitrogen protection, add the piperazine aqueous solution dropwise to the phytic acid melamine reaction solution, adjust the pH to 4.8-5.5, and carry out the neutralization reaction at 40-50℃; after the reaction is completed, concentrate, add ethanol for precipitation, filter, wash, dry, pulverize and vibrate sieve.

6. The novel organophosphorus nitrogen flame retardant according to claim 5, characterized in that, In step B1, the reaction is stirred at 80-85℃ for 2-4 hours.

7. The novel organophosphorus nitrogen flame retardant according to claim 5, characterized in that, In step B2, the neutralization reaction is carried out at 40-50℃ for 1-2 hours.

8. A method for preparing a novel organophosphorus nitrogen flame retardant according to any one of claims 1-7, characterized in that, step include: S1. Piperazine pyrophosphate, melamine polyphosphate, ammonium type II polyphosphate, zinc borate, and hydrophilic fumed silica are dried and mixed to obtain a basic flame retardant mixture. 3-Aminopropyltriethoxysilane is added to a mixture of ethanol and deionized water, and the pH is adjusted to 4.0-5.0 with acetic acid. After stirring and hydrolysis, a silane treatment solution is obtained. The silane treatment solution is sprayed into the basic flame retardant mixture and stirred at 55-70℃ to obtain a surface-treated flame retardant mixture. Triazine trihydroxyethylpiperazine phosphonate, phytic acid melamine piperazine composite salt, and dipentaerythritol are mixed to obtain an organophosphorus nitrogen premix. The organophosphorus nitrogen premix is ​​added to the surface-treated flame retardant mixture and stirred to obtain a composite flame retardant mixture. S2. Add methylphenyl silicone resin and ethylene bis-stearamide to the composite flame retardant mixture, stir, cool, crush and vibrate screen.

9. The preparation method of the novel organophosphorus nitrogen flame retardant according to claim 8, characterized in that, In step S1, the zinc borate is type 2335 zinc borate; the stirring time at 55-70℃ is 15-25 minutes.