High-toughness edible full-degradable functional tapioca-slag-based master batch and preparation process thereof

By adding specific components to potato residue-based materials and employing steam pressure holding and vacuum flash evaporation processes, a porous cross-linked network and a hydrophobic transition layer are formed, which solves the problems of material brittleness and processing instability, improves the mechanical properties and coating adhesion of the materials, and achieves a stable granulation process.

CN123131684APending Publication Date: 2026-11-20SHUWOHANG (HEBEI) ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611257286.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing fully biodegradable materials based on pure plant residue lack an internal flexible cross-linking network during hot pressing, resulting in high mechanical brittleness. At the same time, premature cross-linking reactions during conventional mixing processes can easily cause premature agglomeration of materials, disrupting the continuity of extrusion granulation. Furthermore, hot materials are prone to problems such as pressure roller slippage and equipment torque overload during extrusion granulation.

Method used

The formula uses water-containing potato residue, glycerin, sodium alginate, calcium citrate, sodium hexametaphosphate and soybean lecithin. Through specific process steps such as closed steam reactor pressure heat treatment and vacuum flash steam depressurization, a porous elastic hot dough is formed. Soybean lecithin is introduced during extrusion granulation to construct a hydrophobic transition layer to improve interfacial adhesion.

Benefits of technology

It improves the mechanical toughness of fully degradable materials and the interfacial adhesion of coatings, solves the problem of material brittleness, and alleviates the problems of equipment torque overload and pressure roller slippage during the granulation process, ensuring the continuity and stability of processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131684A_ABST
    Figure CN123131684A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of fully degradable biomass material processing technology, and discloses a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, aiming to solve the problems of early coagulation, poor granulation, and insufficient toughness and interfacial adhesion performance of potato residue-based materials. The masterbatch comprises, by weight, 100 parts of hydrated potato residue (dry basis), 15.0 to 20.0 parts of glycerol, 5.0 to 8.0 parts of sodium alginate, 2.0 to 4.0 parts of calcium citrate, 0.5 to 1.5 parts of sodium hexametaphosphate, and 1.5 to 3.0 parts of soybean lecithin. The preparation process includes pressing, crushing, physical mixing, steam pressure holding, vacuum flash evaporation, extrusion granulation, and drying. Sodium hexametaphosphate and calcium citrate work together to regulate the crosslinking of sodium alginate, vacuum flash evaporation forms a porous elastic material, and soybean lecithin helps improve interfacial adhesion performance. The obtained masterbatch can be used to prepare edible fully degradable molded products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fully degradable biomass material processing technology, specifically to a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process. Background Technology

[0002] Potato residue is a major byproduct of potato starch processing, containing large amounts of cellulose and residual starch. Developing fully biodegradable edible materials from potato residue is significant for reducing single-use plastics and enhancing the utilization value of agricultural byproducts. However, conventional potato residue-based materials still face limitations in performance and processing during actual molding and application.

[0003] Unmodified or physically mixed potato residue matrices rely primarily on hydrogen bonds and physical stacking to maintain their structure after molding. The lack of a flexible network to effectively transfer and disperse stress results in low tensile strength and impact toughness, exhibiting significant brittleness. To improve the mechanical strength of the material, existing technologies attempt to introduce alginate and metal ions to construct ionic cross-linked structures. However, during conventional mixing or extrusion processes, free metal ions readily combine with alginate, initiating early cross-linking. This causes material agglomeration and abnormally high viscosity in the mixing equipment, which not only disrupts the material's rheological properties but also easily leads to roller slippage and equipment torque overload during extrusion granulation, affecting the stability of continuous production.

[0004] Furthermore, potato residue substrate itself is highly hydrophilic, while the outer coating used to improve moisture barrier properties is typically composed of hydrophobic substances such as proteins and natural waxes. Due to the difference in interfacial tension between the hydrophilic substrate and the hydrophobic coating, the coating is difficult to form a tight bond with the substrate surface. When exposed to high humidity environments or immersed in boiling water, the outer coating is prone to peeling, allowing moisture to rapidly penetrate through the pores of the substrate, causing the material to absorb water, swell, and disintegrate, thus affecting the stability of its moisture barrier properties. Therefore, how to maintain processing continuity while simultaneously ensuring the mechanical toughness of the potato residue-based material and the interfacial adhesion of the coating is a problem that needs to be solved in this technical field. Summary of the Invention

[0005] The technical problem solved by this invention is that existing pure plant residue-based fully degradable materials lack an internal flexible cross-linking network during hot pressing, resulting in high mechanical brittleness. At the same time, premature cross-linking reactions during conventional mixing processes can easily cause premature agglomeration of materials, disrupting the continuity of extrusion granulation. In addition, hot materials are prone to problems such as pressure roller slippage and equipment torque overload during extrusion granulation.

[0006] To address the above problems, the present invention provides the following technical solution: The first aspect of this invention provides a high-toughness, potato residue-based, edible, fully biodegradable functional masterbatch, made from raw materials comprising the following parts by weight: Moist potato residue, 100 parts on a dry basis; Glycerin 15.0 to 20.0 parts; Sodium alginate 5.0 to 8.0 parts; Calcium citrate 2.0 to 4.0 parts; Sodium hexametaphosphate, 0.5 to 1.5 parts; 1.5 to 3.0 parts of soybean lecithin.

[0007] Furthermore, it is made from raw materials comprising the following parts by weight: Moist potato residue, 100 parts on a dry basis; 17.5 parts glycerin; 6.5 parts sodium alginate; Calcium citrate 3.0 parts; Sodium hexametaphosphate 1.0 part; 2.2 parts of soybean lecithin.

[0008] Furthermore, the water-containing potato residue is a water-containing material that has undergone mechanical pressing to remove some of the free water, and its moisture content is controlled to be between 45.0% and 55.0%.

[0009] Furthermore, the sodium alginate is a food-grade powder with a weight-average molecular weight of 100,000 g / mol to 150,000 g / mol, and a dynamic viscosity of 200 mPa·s to 500 mPa·s in a 1.0% aqueous solution at 20°C.

[0010] Furthermore, the sodium hexametaphosphate is food-grade sodium hexametaphosphate with an average degree of polymerization of 10 to 20; the soybean lecithin is a food-grade powder with an acetone-insoluble content of ≥60.0% by mass.

[0011] A second aspect of this invention provides a method for preparing a high-toughness, potato residue-based, edible, fully degradable functional masterbatch, comprising the following steps: The potato residue is mechanically pressed to remove some of the free water, resulting in the water-containing potato residue. The water-containing potato residue is then pulverized at high speed to obtain slightly moist initial powder. The slightly moist initial powder is physically mixed with the glycerol, sodium alginate, calcium citrate, sodium hexametaphosphate and soybean lecithin according to the weight ratio of the raw materials of the functional masterbatch to obtain loose and moist granular bulk material; The loose and moist granular material is fed into a closed steam reactor and steam is introduced for pressure heat treatment. Then, the vacuum system is turned on to perform vacuum flash steam depressurization. After the vacuum is broken and the material is discharged, a porous elastic hot dough is obtained. The porous elastic hot dough is continuously fed into a ring die granulator for extrusion and cutting to obtain primary masterbatch. The primary masterbatch is then dried to obtain the fully degradable functional masterbatch.

[0012] Furthermore, during the physical mixing process, the specific parameters of the mixing process are as follows: physical mixing is carried out at a temperature of 15 to 30°C and a stirring speed of 300 to 500 rpm for 15 to 20 minutes.

[0013] By adopting the above technical solution, the appropriate mixing temperature limits the early reaction rate of water-soluble components, and the specific stirring speed allows the powder particles to be fully mixed under the shear force field, promoting the uniform dispersion of trace additives on the potato residue carrier and avoiding uneven concentration of local cross-linking sites.

[0014] Furthermore, the specific implementation method of the pressure-holding heat treatment and vacuum flash evaporation depressurization is as follows: Steam at 110 to 120°C is introduced into the sealed steam reactor. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.15 to 0.20 MPa. The total treatment time inside the sealed steam reactor is 20 to 30 minutes. Three to five minutes before the planned discharge, close the steam inlet valve and turn on the vacuum system. Within 15 to 30 seconds, the absolute pressure inside the vessel will drop sharply to 0.02 to 0.04 MPa, and vacuum flash evaporation will be carried out within the absolute pressure range of 0.02 to 0.04 MPa for 2 to 4 minutes. Wherein, the sum of the pressure reduction time and the maintenance time within the absolute pressure range is less than the time from closing the steam inlet valve to the planned discharge.

[0015] Furthermore, during the extrusion cutting process, the ring die temperature of the ring die granulator is controlled at 85 to 95°C.

[0016] Furthermore, during the drying process, infrared low-temperature drying treatment with a core temperature set at 70 to 85°C is adopted, and the drying time is 20 to 40 minutes, controlling the moisture content of the obtained fully degradable functional masterbatch to be 8.0% to 12.0%.

[0017] This invention provides a high-toughness, potato residue-based, edible, fully biodegradable functional masterbatch and its preparation process. It has the following beneficial effects: 1. This invention, by adding sodium hexametaphosphate and calcium citrate to the raw materials, utilizes the coordination complexation between sodium hexametaphosphate and free calcium ions during the mixing stage to inhibit the early cross-linking of sodium alginate, thus preventing material agglomeration and maintaining processing rheological properties. In the subsequent vacuum flash depressurization process, changes in environmental pressure cause the complex to dissociate and release calcium ions, triggering the in-situ formation of an ionic cross-linking network of sodium alginate. This cross-linking network physically entangles with the potato residue matrix, improving the mechanical toughness of the fully degraded product.

[0018] 2. This invention employs a steam pressure holding and vacuum flash evaporation process. High-temperature steam permeates the material, causing the starch to initially swell. Subsequent rapid vacuum depressurization causes moisture to vaporize and escape, expanding the microporous structure within the material. This process transforms the originally loose material into a porous and compressible elastic hot dough, allowing it to pass smoothly through the die orifice during extrusion granulation and providing appropriate friction, thus mitigating the problems of roller slippage and equipment torque overload that often occur during granulation.

[0019] 3. This invention introduces soybean lecithin into the raw materials, utilizing its amphiphilic properties to induce thermal migration to the material surface during the thermoforming stage. The hydrophilic end of the soybean lecithin binds to the polar groups inside the potato residue matrix, while the hydrophobic end extends outward, constructing a hydrophobic transition layer on the substrate surface. This structure alleviates the interfacial tension difference between the polar substrate and the outer hydrophobic coating, providing physical bonding sites for the coating, improving the interfacial adhesion between the hydrophobic coating and the substrate, and enhancing the water resistance and moisture barrier properties of the finished product. Attached Figure Description

[0020] Figure 1 This is a graph showing the test results of free calcium ion release and pH changes in different experimental groups of the present invention. Among them, (a) shows the free calcium ion release of aqueous extracts from Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 4 at different processing stages. 2+ Concentration change curves, (b) is a graph showing the pH changes of the system before and after treatment in Example 1, Comparative Example 1 and Comparative Example 2; Figure 2 This is a graph showing the change in the main shaft torque of the reactor during the steam reaction process in Embodiment 1, Comparative Example 1, and Comparative Example 2 of the present invention; Figure 3 These are the results of the ring die granulation adaptability test of Examples 1 to 5 and Comparative Example 2 of the present invention; Figure 4 The graph shows the test results of the boiling water resistance and moisture barrier properties of Examples 1 to 5, Comparative Example 3 and Comparative Example 5 of the present invention. Detailed Implementation

[0021] To enable those skilled in the art to better understand the present invention, the present invention will be further described in detail below with reference to specific embodiments. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications: the raw materials, excipients and processing aids used in the preparation of functional masterbatches and finished products are all food-grade products; the reagents used only for analysis and detection are commercially available analytical grade or higher products.

[0023] Potato residue is a byproduct of potato starch processing. The original hydrated potato residue used in this invention mainly contains cellulose and residual potato starch on a dry basis, with an initial free water mass fraction of 80.0% to 90.0%.

[0024] Glycerin (CAS No.: 56-81-5), purity ≥99.5%, food grade.

[0025] Sodium alginate (CAS No.: 9005-38-3) is a linear polymer composed of block copolymers of β-D-mannuronic acid and α-L-guluronic acid. It is produced as a food-grade powder with a weight-average molecular weight between 100,000 g / mol and 150,000 g / mol. The dynamic viscosity of a 1.0% aqueous solution at 20°C is 200 mPa·s to 500 mPa·s.

[0026] Calcium citrate (CAS No.: 813-94-5), purity ≥98.0%, food grade.

[0027] Sodium hexametaphosphate (CAS No.: 10124-56-8), with an average degree of polymerization of 10 to 20, is food grade.

[0028] Soy lecithin (CAS No.: 8002-43-5) is a food-grade powder with an acetone-insoluble content of ≥60.0%.

[0029] Corn gluten (CAS No.: 9010-66-6), purity ≥90.0%, food-grade powder.

[0030] Natural beeswax (CAS No.: 8012-89-3), melting point range of 62℃ to 67℃, food grade refined.

[0031] Anhydrous ethanol (CAS No.: 64-17-5), purity ≥99.5%, food grade.

[0032] Preparation Example 1: This preparation example provides a method for preparing an impregnation coating liquid, including the following steps: (1) Weigh 10g of corn gluten powder and add it to 100g of 70% ethanol aqueous solution. Stir for 40min under a constant temperature closed water bath at 65℃ to completely dissolve it and obtain a clear corn gluten alcohol aqueous solution. Maintain the system temperature at 65℃. (2) Weigh 3g of natural refined beeswax and heat it separately to 68℃ to melt it into a liquid state; (3) The above-mentioned molten beeswax was slowly added dropwise to a 65°C zeatin alcohol aqueous solution under high shear homogenization conditions of 6500 rpm. The homogenization was continued for 12 min while maintaining the temperature at 65°C. Then, the temperature was naturally cooled down to 45°C to obtain a stable zeatin-beeswax double hydrophobic emulsion, which was kept warm for later use.

[0033] Preparation Example 2: This preparation example provides a method for preparing an impregnation coating liquid, including the following steps: (1) Weigh 8g of corn gluten powder and add it to 100g of 70% ethanol aqueous solution. Stir for 30min under a constant temperature closed water bath at 65℃ to completely dissolve it and obtain a clear corn gluten alcohol aqueous solution. Maintain the system temperature at 65℃. (2) Weigh 2g of natural refined beeswax and heat it separately to 68℃ until it is completely melted into a liquid state; (3) The above molten beeswax was slowly added dropwise to a 65°C zeatin alcohol aqueous solution under high shear homogenization conditions of 5000 rpm. The homogenization was continued for 10 min while maintaining the 65°C condition. Then, the solution was naturally cooled down to 45°C to obtain a stable zeatin-beeswax double hydrophobic emulsion, which was kept warm for later use.

[0034] Preparation Example 3: This preparation example provides a method for preparing an impregnation coating liquid, including the following steps: (1) Weigh 12g of corn gluten powder and add it to 100g of 70% ethanol aqueous solution. Stir for 45min under a constant temperature closed water bath at 68℃ to completely dissolve it and obtain a clear corn gluten alcohol aqueous solution. Maintain the system temperature at 68℃. (2) Weigh 4g of natural refined beeswax and heat it separately to 70℃ to melt it into a liquid state; (3) The above molten beeswax was slowly added dropwise to a 68°C zeatin alcohol aqueous solution under high shear homogenization conditions of 8000 rpm. The homogenization was continued for 15 min while maintaining the temperature at 68°C. Then, the solution was naturally cooled down to 45°C to obtain a stable zeatin-beeswax double hydrophobic emulsion, which was kept warm for later use.

[0035] Example 1: This embodiment provides a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, including the following steps: (1) The original water-containing potato residue that has passed the test is sent to the high-frequency filter through the elevator and screw conveyor to remove some of the free water by applying a mechanical pressing pressure of 0.5MPa. The moisture content of the discharged material is controlled to be 50.0%. 100kg of the water-containing material is weighed and sent to the meshless wet high-speed grinder through the conveyor to be crushed at 3000rpm. The slightly moist initial powder is collected. (2) The above slightly moist initial powder is fed into a mixer, and 17.5 kg of glycerol, 6.5 kg of sodium alginate, 3.0 kg of calcium citrate, 1.0 kg of sodium hexametaphosphate and 2.2 kg of soybean lecithin are added sequentially at 25°C under a stirring speed of 400 rpm. The mixture is continuously physically mixed for 18 min to obtain loose and moist granular bulk material. (3) The bulk material is fed into a sealed steam reactor with a twin-shaft kneading and stirring device. 115°C steam is introduced into the reactor at a stirring speed of 50 rpm. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.18 MPa. The total treatment time for this step is controlled at 25 min. 4 min before the planned discharge, the steam inlet valve is closed and the vacuum system connected to the reactor body is turned on. The absolute pressure inside the reactor is suddenly reduced to 0.03 MPa within 20 s and the vacuum is maintained for 3 min for flash steaming. Then the vacuum is broken and the material is discharged to obtain a porous elastic hot dough.

[0036] During the mixing stage, sodium hexametaphosphate competitively complexes and masks the free calcium ions generated by the dissociation of calcium citrate to inhibit premature cross-linking of sodium alginate. In the subsequent vacuum flash evaporation and depressurization process, the complexation state changes, causing the masked calcium ions to transform into a free state that can participate in cross-linking, thereby triggering the formation of an ionic cross-linking network by sodium alginate. (4) The hot dough discharged from the reactor is continuously fed into the ring die granulator by the extrusion mechanism. The primary masterbatch is obtained by extrusion and cutting at a ring die temperature of 90°C. The primary masterbatch is spread on the mesh belt and passed through the infrared low temperature drying tunnel with a core temperature set at 78°C. After drying for 30 minutes, the final moisture content is reduced to 10.0%, and the fully degradable functional masterbatch is obtained. (5) The masterbatch is sent to a high-speed pulverizer and crushed into molding powder that passes through an 80-mesh sieve at 5000 rpm. The powder is then fed into the mold cavity by an automatic feeder and held at a molding temperature of 140℃ and a molding pressure of 15.0MPa for 45s. The blank is then removed by a vacuum suction cup combined with a robotic arm after the mold is opened.

[0037] During the above-mentioned high-temperature molding process, soybean lecithin migrates and accumulates to the surface area of ​​the material when heated. Its hydrophilic end anchors with the polar groups in the potato residue matrix, while its hydrophobic end extends toward the outer surface of the material, thereby forming a hydrophobic transition interface on the substrate surface and providing physical anchor points for subsequent impregnation coating. (6) Immerse the blank with residual heat into the 45°C impregnation coating liquid prepared in Preparation Example 1 for 3.5s, pull it up at a uniform speed to drain the liquid, and then send it into an infrared low temperature drying tunnel with the core temperature set at 68°C for 12min. The finished product is obtained by discharging the material.

[0038] Example 2: This embodiment provides a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, including the following steps: (1) The original water-containing potato residue that has passed the test is subjected to a mechanical pressing pressure of 0.8MPa through a high-frequency filter to remove free water, and the output moisture content is controlled to be 55.0%. Weigh 100kg of the water-containing material with dry basis and feed it into a meshless wet high-speed grinder and grind it at 3500rpm to obtain slightly moist initial powder. (2) The slightly moist initial powder is fed into the mixer, and 20.0 kg of glycerol, 8.0 kg of sodium alginate, 4.0 kg of calcium citrate, 1.5 kg of sodium hexametaphosphate and 3.0 kg of soybean lecithin are added sequentially at 30°C and stirred at 500 rpm. The mixture is mixed for 20 min to obtain loose and moist granular bulk material. (3) The bulk material is fed into a closed steam reactor and steam at 120°C is introduced at a stirring speed of 60 rpm. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.20 MPa. The total processing time for this step is controlled at 30 min. Five minutes before the planned discharge, the steam valve is closed and the vacuum system is turned on to make the absolute pressure inside the reactor drop to 0.02 MPa within 15 seconds and maintain this vacuum for 4 minutes for flash steaming. The discharge yields a porous elastic hot dough. (4) The hot dough is fed into the ring die granulator and extruded and cut at a ring die temperature of 95°C to obtain primary masterbatch. It is then dried in an infrared drying tunnel at a core temperature of 85°C for 20 minutes to reduce the final moisture content to 8.0%, thus obtaining fully degradable functional masterbatch. (5) The masterbatch is fed to a high-speed pulverizer and crushed at 6000 rpm and passed through an 80-mesh sieve. It is then fed into the mold cavity and held under pressure for 60 seconds at a molding temperature of 150℃ and a molding pressure of 20.0 MPa. The mold is then opened and the blank is removed. (6) Immerse the blank in the 45°C impregnation coating liquid prepared in Preparation Example 3 for 5.0s, drain the liquid and send it into the infrared drying tunnel with a core temperature of 75°C for 15min, and the finished product is obtained by discharging the material.

[0039] Example 3: This embodiment provides a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, including the following steps: (1) The original water-containing potato residue that has passed the test is subjected to a high-frequency filter and a mechanical pressing pressure of 0.3 MPa is applied to remove free water. The output moisture content is controlled to be 45.0%. 100 kg of the water-containing material with dry basis is weighed and fed into a meshless wet high-speed grinder and pulverized at 2800 rpm to obtain slightly moist initial powder. (2) The slightly moist initial powder is fed into the mixer, and 15.0 kg of glycerol, 5.0 kg of sodium alginate, 2.0 kg of calcium citrate, 0.5 kg of sodium hexametaphosphate and 1.5 kg of soybean lecithin are added sequentially at 15°C and stirred at 300 rpm. The mixture is mixed for 15 min to obtain loose and moist granular bulk material. (3) The bulk material is fed into a closed steam reactor and steam at 110°C is introduced at a stirring speed of 40 rpm. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.15 MPa. The total processing time for this step is controlled at 20 min. Three minutes before the planned discharge, the steam valve is closed and the vacuum system is turned on to make the absolute pressure inside the reactor drop sharply to 0.04 MPa within 30 seconds and maintain this vacuum for 2 minutes for flash steaming. The material is discharged to obtain a porous elastic hot dough. (4) The hot dough is fed into the ring die granulator and extruded and cut at a ring die temperature of 85°C to obtain primary masterbatch. It is then dried in an infrared drying tunnel at a core temperature of 70°C for 40 minutes to reduce the final moisture content to 12.0%, thus obtaining fully degradable functional masterbatch. (5) The masterbatch is sent to a high-speed pulverizer and crushed at 4000 rpm and passed through an 80-mesh sieve. It is then fed into the mold cavity and held under pressure for 30 seconds at a molding temperature of 130℃ and a molding pressure of 10.0 MPa. The blank is then opened and removed. (6) Immerse the blank in the 45°C impregnation coating liquid prepared in Preparation Example 2 for 2.0s, drain the liquid and send it into the infrared drying tunnel with a core temperature of 60°C for 10min, and the finished product is obtained by discharging the material.

[0040] Example 4: This embodiment provides a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, including the following steps: (1) Press the original water-containing potato residue to control the output moisture content to 48.0%, weigh 100 kg of water-containing material with dry basis and crush it at 3200 rpm to obtain slightly moist initial powder; (2) Feed the initial powder into the mixer, and add 18.0 kg of glycerol, 7.0 kg of sodium alginate, 3.5 kg of calcium citrate, 0.8 kg of sodium hexametaphosphate and 2.5 kg of soybean lecithin in sequence at 22°C and 450 rpm. Mix for 16 min to obtain loose bulk material. (3) The bulk material is fed into the steam reactor and steam at 118°C is introduced. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.19MPa. The total processing time for this step is controlled at 28min. 4min before the planned discharge, the steam valve is closed and the vacuum is turned on. The pressure is reduced to 0.025MPa within 25s and maintained for 3.5min for flash steaming. The dough is then discharged. (4) The dough is fed into a ring die granulator and granulated at 92°C. The dough is then dried at 80°C for 25 minutes until the moisture content is 9.0% to obtain the masterbatch. (5) Crush the masterbatch at 4500 rpm and mold it at 145℃ and 18.0 MPa for 50 seconds to remove the blank; (6) Immerse the blank in the coating liquid prepared in Preparation Example 1 for 4.0s, and then dry it in infrared at 70°C for 13min to obtain the finished product.

[0041] Example 5: This embodiment provides a high-toughness potato residue-based edible fully degradable functional masterbatch and its preparation process, including the following steps: (1) Press the original water-containing potato residue to control the output moisture content to 52.0%, weigh 100 kg of water-containing material with dry basis and crush it at 2900 rpm to obtain slightly moist initial powder; (2) Feed the initial powder into the mixer, and add 16.0 kg of glycerol, 6.0 kg of sodium alginate, 2.5 kg of calcium citrate, 1.2 kg of sodium hexametaphosphate and 1.8 kg of soybean lecithin in sequence at 28°C and 350 rpm. Mix for 19 min to obtain loose bulk material. (3) The bulk material is fed into the steam reactor and steam at 112°C is introduced. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.16MPa. The total processing time for this step is controlled at 22min. 3.5min before the planned discharge, the steam valve is closed and the vacuum is turned on. The pressure is reduced to 0.035MPa within 25s and maintained for 2.5min for flash steaming. The dough is then discharged. (4) The dough is fed into a ring die granulator and granulated at 88°C. The dough is then dried at 75°C for 35 minutes until the moisture content is 11.0% to obtain the masterbatch. (5) Crush the masterbatch at 5500 rpm and mold it at 135℃ and 12.0 MPa for 40s to remove the blank; (6) Immerse the blank in the coating liquid prepared in Preparation Example 2 for 3.0s, and then dry it at 65°C for 11min to obtain the finished product.

[0042] Comparative Example 1: Compared with Example 1, the difference is that sodium hexametaphosphate was not added to the mixture formulation in step (2), but the rest are the same.

[0043] Comparative Example 2: Compared with Example 1, the difference is that in step (3), the operation of opening the vacuum system for flash evaporation is not performed. Instead, the material is discharged directly under normal pressure and cooled down. The rest are the same.

[0044] Comparative Example 3: Compared with Example 1, the difference is that soybean lecithin was not added to the mixture formula in step (2), but the rest are the same.

[0045] Comparative Example 4: Compared with Example 1, the difference is that in step (2), calcium citrate is prepared according to the formula Ca... 2+ The amount of substance was replaced with food-grade anhydrous calcium chloride, and everything else remained the same.

[0046] Comparative Example 5: Compared with Example 1, the difference is that only glycerol is added in step (2), and sodium alginate, calcium citrate, sodium hexametaphosphate and soybean lecithin are not added, and the coating impregnation process in step (6) is omitted, while the rest are the same.

[0047] Test Example 1: (1) Using the materials of Examples 1 to 5 and Comparative Examples 1, 2 and 4 as test objects, process node monitoring of free calcium ion concentration and pH value was carried out.

[0048] (2) The concentration of free calcium ions was determined using the calcium ion selective electrode method. Sampling was performed at four pre-set points in the preparation process: Node A is when loose and moist granular bulk material is obtained after mixing in step (2); Node B is where, in step (3), steam is introduced and treated for 15 minutes. The sample is then taken under pressure using the high-temperature sampling valve on the side wall of the reactor and quickly cooled and quenched. Node C is the instant when the vacuum flashing ends in step (3). Before the vacuum is broken, the sampling time point is locked by the online signal, and the sample is taken immediately after the vacuum is broken. Node D is the point at which porous, elastic, hot dough is collected after discharge in step (3). For Comparative Example 2, which does not perform vacuum flash steaming, the time elapsed after the start of natural ventilation and cooling at atmospheric pressure is the same as that at node C in Example 1, which is taken as the corresponding node C.

[0049] Samples obtained at each node were homogenized and extracted with deionized water at a mass-to-volume ratio of 1:10. After centrifugation, the supernatant was collected, and the potential was read using a calibrated calcium ion selective electrode and converted into the free Ca2+ of the water extract. 2+ Concentration, expressed in mmol / L.

[0050] (3) The pH value of the system was determined using an industrial-grade puncture pH meter. The initial pH value of the original water-containing potato residue obtained after pressing in step (1) and the average pH value of the hot dough surface and internal core obtained after discharge in step (3) were recorded respectively. The arithmetic mean of the three measurements was taken as the final recorded value.

[0051] Table 1. Test data of free calcium ion concentration and pH value for each example and comparative example Test object <![CDATA[Free Ca in aqueous extract 2+ Concentration - Node A (mmol / L)]]> <![CDATA[Free Ca in water extract 2+ concentration - Node B (mmol / L)]]> <![CDATA[Free Ca in aqueous extract 2+ Concentration - Node C (mmol / L)]]> <![CDATA[Free Ca in aqueous extract 2+ concentration - Node D (mmol / L)]]> pH value of raw potato residue pH value after discharge Example 1 0.17 1.14 19.82 18.65 4.61 6.88 Example 2 0.22 1.36 23.11 21.94 4.58 7.04 Example 3 0.12 0.89 15.63 14.88 4.64 6.75 Example 4 0.19 1.21 20.45 19.21 4.60 6.91 Example 5 0.14 1.05 17.89 16.73 4.65 6.82 Comparative Example 1 3.52 14.78 — — 4.62 — Comparative Example 2 0.18 1.17 5.34 7.21 4.59 5.12 Comparative Example 4 18.96 21.05 21.58 — 4.61 —

[0052] In Table 1, “—” indicates that the group failed to obtain valid samples or test data for the corresponding process node.

[0053] To further visualize the changes in free Ca²⁺ concentration and pH value of the system before and after treatment at different processing stages for each test object, result curves were plotted based on the test data in Table 1, as shown below. Figure 1 As shown. Among them, Figure 1 (a) shows the free Ca²⁺ concentration changes of the water extracts of Examples 1, 1, 2, and 4 at different processing stages. Figure 1 (b) is a graph showing the pH changes of the systems before and after treatment in Example 1, Comparative Example 1 and Comparative Example 2.

[0054] Based on the data in Table 1, the free Ca in the aqueous extracts of Examples 1 to 5 at stages A and B were analyzed. 2+ The concentrations remained at low levels, not exceeding 1.5 mmol / L. This result indicates that the competitive complexation of sodium hexametaphosphate is beneficial in reducing detectable free Ca in the early stages. 2+ The horizontal structure effectively masks the trace calcium ions dissociated from slightly soluble calcium citrate, preventing sodium alginate from undergoing cross-linking reactions at this stage and maintaining the rheological processability of the system.

[0055] When the vacuum flash evaporation operation was performed at node C, the calcium ion concentration in each embodiment showed a step increase, reaching above 15.0 mmol / L. This change indicates that free Ca can be detected in the system before and after vacuum flash evaporation. 2+ The level changed significantly, which is consistent with the redistribution of complex states caused by changes in water content, ionic environment and acid-base balance during flash evaporation, and provides experimental support for subsequent ionic crosslinking.

[0056] The data from the comparative tests reveal the impact of a single variable change on the reaction pathway. In Comparative Example 1, the absence of sodium hexametaphosphate resulted in the release of 14.78 mmol / L of free calcium at node B, leading to uncontrolled early cross-linking before the system even entered vacuum flash evaporation. In Comparative Example 4, which replaced calcium citrate with readily soluble calcium chloride, even with the presence of sodium hexametaphosphate, the free calcium concentration at node A remained as high as 18.96 mmol / L, indicating that conventional readily soluble calcium sources cannot achieve blockade through this complexation system.

[0057] Comparative Example 2 did not introduce a vacuum flash evaporation operation, and the calcium ion release at nodes C and D was suppressed to below 7.21 mmol / L. This indicates that in an atmospheric pressure cooling environment lacking sudden boiling and pressure reduction disturbances, the chelation equilibrium is difficult to be broken, and the cross-linked network construction is insufficient.

[0058] Regarding the deacidification effect, the original hydrated potato residue exhibited a weakly acidic pH, ranging from 4.58 to 4.65. After flash evaporation in Examples 1 to 5, the pH value returned to the neutral range of 6.75 to 7.04. This result indicates that the pH of the system significantly increased after vacuum flash evaporation, suggesting that the flash evaporation process is beneficial for the removal of acidic volatile components and the adjustment of the system's acid-base balance. In contrast, Comparative Example 2, which used natural venting at atmospheric pressure, only saw its pH value rise to 5.12 after evaporation, with a significant amount of acidic substances remaining inside the matrix. This indicates that under the experimental conditions, vacuum flash evaporation is beneficial for improving the removal of residual acid.

[0059] Test Example 2: (1) Rheological phase monitoring and interfacial molecular spectroscopic characterization were carried out using the process materials and final products generated during the preparation of Examples 1 to 5, Comparative Examples 1, 2 and 3 as test objects.

[0060] (2) In-situ recording of reactor spindle torque. Using a high-precision torque sensor coupled to the drive motor of the sealed steam reactor spindle and a connected data acquisition platform, the torque values ​​of the entire process cycle (3) are collected in real time. Torque characteristic data of four key nodes are extracted: Node T1 is the 5th minute of steam introduction treatment; Node T2 is the 15th minute of steam introduction treatment; Node T3 is 30 seconds after the vacuum system is turned on; Node T4 is the instant before the vacuum flash evaporation ends and the material is discharged after the vacuum is broken. For Comparative Example 2, which does not perform vacuum flash evaporation, T3 and T4 are the same elapsed times as the corresponding nodes in Example 1 after the natural exhaust cooling at atmospheric pressure begins. Torque data is expressed in N·m.

[0061] (3) Attenuation of interface anchoring effect by total reflection Fourier transform infrared spectroscopy test. At room temperature, the outer surface of the uncoated blank obtained by step (5) and the coated surface of the finished product obtained by step (6) were cut off respectively.

[0062] The sample surface was tightly bonded to the diamond ATR crystal of the ATR-FTIR spectrometer for in-situ scanning, with a scanning wavenumber range of 4000 cm⁻¹. -1 Up to 400cm -1 The resolution is set to 4cm. -1 Infrared spectra were acquired and the center wavenumber position of the characteristic absorption peak of amide I band was extracted. The data unit is cm. -1 .

[0063] Table 2. Test data of spindle torque and surface feature absorption peak wavenumber for each embodiment and comparative example Test object Torque-node T1 (N·m) Torque-node T2 (N·m) Torque-node T3 (N·m) Torque-node T4 (N·m) <![CDATA[Surface absorption peak of blank part (cm -1 )]]> <![CDATA[Absorption peak on finished product surface (cm -1 )]]> Example 1 185.3 211.6 547.8 582.1 1658.2 1641.5 Example 2 192.7 224.3 563.2 605.4 1657.9 1640.8 Example 3 178.5 198.1 512.6 541.9 1659.1 1643.2 Example 4 181.2 215.8 536.4 577.3 1658.4 1642.1 Example 5 188.9 207.4 551.7 590.8 1658.6 1641.9 Comparative Example 1 395.4 1342.7 Shutdown and overload Shutdown and overload — — Comparative Example 2 183.1 209.5 228.4 243.6 1658.5 1657.1 Comparative Example 3 186.2 212.8 545.1 580.4 1658.2 1656.8

[0064] In Table 2, “—” indicates that no blank or finished product was obtained for corresponding characterization due to the termination of the upstream process. According to the data in Table 2, in Examples 1 to 5, the spindle torque remained at a low and stable level below 225.0 N·m in the early stages of the process, at nodes T1 and T2, and the material exhibited low-viscosity paste-like rheological characteristics.

[0065] To further visualize the effects of the vacuum flash evaporation process and different treatment methods on the rheological state of the material, torque variation curves were plotted based on the reactor spindle torque test data in Table 2, as shown below. Figure 2 As shown.

[0066] When entering the vacuum flash evaporation stages T3 and T4, the torque value rapidly increases and stabilizes in the range of 500.0 N·m to 610.0 N·m. This torque change is related to the rapid change in the moisture content of the material during flash evaporation and the Ca... 2+ Consistent with the structural enhancement resulting from the cross-linking of sodium alginate, the material is transformed from an amorphous bulk into a porous, hot dough with macroscopic elasticity, thereby increasing the shear resistance to the reactor wall scraper and stirring shaft.

[0067] The test data from the comparative examples, from the opposite perspective, confirmed the correlation between the processes. In Comparative Example 1, due to the lack of early free calcium complexation masking effect from sodium hexametaphosphate in the system, calcium citrate dissolved rapidly and underwent uncontrolled early cross-linking in the initial stage of high-temperature steam introduction. This caused the material to instantly clump together and harden, and the spindle torque distortedly surged from 395.4 N·m to 1342.7 N·m, triggering the mechanical overload shutdown protection of the equipment. Comparative Example 2 used atmospheric pressure natural exhaust, without flash evaporation pressure reduction induction. The torque at nodes T3 and T4 only showed slight fluctuations caused by heat transfer, without any increase, confirming that it failed to complete the phase transformation from a viscous paste to an elastic dough within the reactor.

[0068] In terms of spectral characterization, the characteristic absorption peak of amide I band on the surface of the uncoated blanks in each embodiment was concentrated at 1658.0 cm⁻¹. -1 Nearby. After impregnation coating, the absorption peak on the surface of the finished products of Examples 1 to 5 all showed a red shift, shifting to 1641.0 cm⁻¹. -1 The redshift is approximately 17.0 cm. -1 The wavenumber change indicates that the chemical environment of the relevant functional groups at the interface changed after the coating was formed, consistent with the enhanced intermolecular interactions such as hydrogen bonding. Combined with the significantly weakened peak position change in Comparative Example 3 after the absence of soybean lecithin, it can be concluded that the presence of soybean lecithin is beneficial to enhancing the interfacial interaction between the substrate and the corn gluten-beeswax coating. In Comparative Example 3, because soybean lecithin was removed from the formulation, the surface absorption peak after coating was located at 1656.8 cm⁻¹. -1 The absorption peak of the coating showed no significant shift compared to the background absorption peak of the blank, indicating that the interfacial interaction between the coating and the substrate was significantly weaker than that of the example group.

[0069] The specific experimental description and results of Test Example 3 are as follows: (1) The materials discharged after the steam reactor process in Examples 1 to 5 and Comparative Example 2 were used as test objects to carry out tests on the mechanical suitability of ring die granulation and the yield of masterbatch. Comparative Example 1 and Comparative Example 4 were not included in the test of this section because severe premature agglomeration had occurred in the steam reactor and normal mechanical discharge could not be achieved.

[0070] (2) Adjust the feeding temperature of each test object to 85℃ and keep it stable. Feed it continuously into the ring die pellet mill at a constant dry basis set rate of 100kg / h using a loss-in-weight feeder. Use the PLC control system and high-precision current transmitter of the pellet mill to record the current change curve during the operation of the main motor. Select the 10-minute steady-state operation interval from 5min to 15min after the start of feeding, and record the average current and current fluctuation range during the steady-state period. The data unit is A. Record the initial no-load current of the equipment before the test.

[0071] (3) During the 30-minute cycle after the start of feeding, collect the material that has been cut by the ring die granulator and fallen into the receiving trough. Manually sieve out unformed debris, powder, and pasty agglomerates, weigh the well-formed, dense columnar masterbatch, and convert it to dry basis weight. Calculate the ratio of this weight to the total dry basis weight of the material actually fed into the granulator during the same time period to obtain the masterbatch yield, expressed as a percentage by mass.

[0072] Table 3. Operating parameters of the ring die granulator and test data of masterbatch yield for each embodiment and comparative example. Test object Initial no-load current (A) Average current during the steady-state period (A) The range of current fluctuations during the steady-state period (A) Masterbatch yield (%) Example 1 32.4 88.5 4.2 96.3 Example 2 32.1 91.2 5.1 94.8 Example 3 32.6 85.6 3.8 97.1 Example 4 32.3 89.1 4.5 95.5 Example 5 32.5 87.4 4.1 96.8 Comparative Example 2 32.4 145.8 68.3 21.5 Comparative Example 1 — Not yet entered the granulation process — — Comparative Example 4 — Not yet entered the granulation process — —

[0073] In Table 3, “—” indicates that the group failed to obtain valid test data.

[0074] To further visually compare the equipment operating status and masterbatch yield of each test object during the ring die granulation process, test result graphs were plotted based on the average current during the stabilization period, current fluctuation range, and masterbatch yield data in Table 3, as shown in the figure below. Figure 3 As shown According to the data in Table 3, Examples 1 to 5 all showed good equipment operation stability in the ring die granulation process, with the average operating current maintained between 85.6A and 91.2A, and the current fluctuation range during the stable period not exceeding 5.1A, and the masterbatch yield reaching over 94.8%.

[0075] As can be seen from the results of Comparative Example 2, under the formulation and processing conditions adopted in this invention, vacuum flash evaporation treatment is beneficial to improving the operational stability and masterbatch yield in the subsequent ring die granulation stage. This improvement is related to the changes in the pore structure, surface condition, and compressibility of the material after flash evaporation, thereby improving the gripping effect of the pressure rollers on the material and the material's deformation capacity as it passes through the die orifice.

[0076] Comparative Example 2, due to the use of atmospheric pressure natural venting in the reactor section, did not exhibit the significant flash evaporation and pore expansion and free Ca concentrations seen in Example Group. 2+ The material discharged during the rapid rise in temperature is a high-density, wet, viscous paste lacking pores. When entering the ring die granulation stage, the high-density wet paste forms a liquid film lubrication effect on the surface of the metal die. The pressure rollers are unable to grip the material and generate effective positive pressure, resulting in severe pressure roller slippage. This causes a sharp drop in the actual extrusion volume into the die, resulting in most of the material being ineffectively agitated within the ring die cavity or even agglomerating and clogging the die holes.

[0077] The data shows that the operating current of the main unit in Comparative Example 2 reached as high as 145.8A, with a range increasing dramatically to 68.3A, accompanied by frequent overload alarms. The yield of qualified masterbatch collected was only 21.5%. This comparative result indicates that under the experimental formulation and equipment conditions, the vacuum flash evaporation process has a significant impact on the suitability of subsequent ring die granulation.

[0078] The specific experimental description and results of Test Example 4 are as follows: (1) The final products prepared in Examples 1 to 5, Comparative Examples 3 and 5 were used as test objects to determine the coating interface adhesion and boiling water resistance performance.

[0079] (2) The coating interface adhesion test was conducted according to the standard cross-cut test. Orthogonal grids with a spacing of 1 mm were cut on the surface of the finished product. Standard test tape was then applied tightly to the grid area and peeled off quickly and uniformly. The coating peeling at the grid intersections and edges was observed using a magnifying glass and graded from 0 to 5. Grade 0 indicates smooth grid edges with no peeling, while grade 5 indicates large areas of coating peeling with a peeling area exceeding 65%. Comparative Example 5 was not impregnated with a coating, so this test was recorded as no coating.

[0080] (3) In the boiling water moisture barrier performance test, each component was cut into 50mm×50mm square samples, and the initial thickness of the sample at the geometric center was measured using a digital thickness gauge. Then the sample was immersed in deionized water that was kept boiling, and the critical time required from the time of immersion until the sample underwent macroscopic disintegration or complete collapse and softening, thus losing its structural support, was recorded as the disintegration and softening time, in min.

[0081] Additionally, after 15 minutes of boiling water immersion, the sample that has not yet disintegrated is removed, the surface moisture is wiped dry, and the center thickness is measured again. The water absorption thickness swelling rate is calculated as follows: Water absorption thickness swelling rate = [(thickness after 15 minutes of immersion - initial thickness) / initial thickness] × 100%, and the result is expressed as a percentage. If the sample has disintegrated within 15 minutes, the swelling rate cannot be determined.

[0082] Table 4. Test data on coating adhesion and boiling water resistance of each embodiment and comparative example. Test object Coating interface adhesion level Boiling water disintegration and softening time (min) Soaking for 15 minutes, water absorption thickness expansion rate (%) Example 1 Level 0 124.6 15.24 Example 2 Level 0 137.2 13.58 Example 3 Level 1 119.5 18.06 Example 4 Level 0 129.8 14.73 Example 5 Level 0 122.4 16.11 Comparative Example 3 Level 4 17.8 81.35 Comparative Example 5 Uncoated 1.5 Unable to determine

[0083] To further compare the boiling water resistance and moisture barrier properties of each test object, a graph of the test results was plotted based on the boiling water disintegration and softening time and the water absorption thickness expansion rate after immersion for 15 minutes in Table 4. (See figure below.) Figure 4 As shown.

[0084] According to the data in Table 4, the finished products of Examples 1 to 5 all achieved a grade 0 or 1 standard in the coating interface adhesion test, demonstrating excellent bonding strength between the coating and the substrate. In the extreme boiling water immersion environment, the macroscopic structure maintenance time of Examples 1 to 5 all exceeded 119.5 min, and the water absorption thickness expansion rate at the 15-minute mark was controlled within 18.06%. This verifies that the synergistic effect of the polymer crosslinking network and the hydrophobic coating can effectively resist the penetration and damage of high-temperature water molecules.

[0085] The test results of Comparative Example 3 showed that the addition of soybean lecithin was significantly associated with improved coating adhesion and water resistance. Due to the removal of soybean lecithin from the formulation, the interfacial adhesion of the coating in Comparative Example 3 dropped to level 4, exhibiting severe peeling. Without soybean lecithin, the hydrophobic coating composed of corn gluten and beeswax could not stably adhere to the highly hydrophilic, hydroxyl-rich substrate surface. In boiling water, the coating rapidly peeled off and dissipated, with moisture quickly penetrating along the substrate pores, resulting in a water absorption thickness swelling rate of up to 81.35% in Comparative Example 3 at 15 min, a shortened disintegration and softening time to 17.8 min, and a precipitous drop in water resistance.

[0086] Comparative Example 5, serving as the baseline control group without ionic crosslinking or coating treatment, showed matrix disintegration and complete disintegration within just 1.5 minutes after contact with boiling water. This indicates that the control substrate, primarily composed of starch and cellulose from potato residue and only plasticized with glycerol without ionic crosslinking or surface coating, lacks an effective hot water-resistant structural barrier. Combining the results of the examples with those of Comparative Examples 3 and 5, it is evident that the addition of soybean lecithin and subsequent corn gluten-beeswax coating treatment improve the interfacial bonding stability between the substrate and the coating, and enhance the moisture barrier and boiling water resistance of the finished product.

[0087] The specific experimental description and results of Test Example 5 are as follows: (1) Using the functional masterbatches prepared in Examples 1 to 5 and Comparative Example 5 as raw materials, standard mechanical test strips were prepared according to the molding parameters of each group to evaluate the macroscopic mechanical properties of the masterbatch molding substrate.

[0088] (2) The masterbatch corresponding to each test object was molded into mechanical test specimens of standard size according to the preset molding parameters; the tensile test used a standard dumbbell-shaped specimen, and the impact test used a standard long strip specimen with a V-shaped notch. All samples were placed in a constant temperature and humidity environment of 23℃ and 50% for 48 hours to adjust.

[0089] (3) Tensile properties were tested using a universal testing machine. The dumbbell-shaped specimen was clamped in the upper and lower fixtures, and the tensile rate was set to 50 mm / min. The machine was run until the specimen broke. The tensile yield strength during the test was recorded and extracted in MPa. At the same time, the change in the distance between the gauge marks when the specimen broke was measured, and the elongation at break was calculated as a percentage.

[0090] (4) Notched impact strength test was performed using a cantilever beam impact testing machine. The specimen with a V-notch was vertically clamped to the base of the machine, and a pendulum with known initial potential energy was released to perform a single impact. The remaining potential energy after the pendulum broke the specimen was recorded, the energy absorbed by the specimen during the fracture process was calculated, and the result was divided by the cross-sectional area at the notch to obtain the notched impact strength, in kJ / m².2 .

[0091] Each group must obtain test results of at least 5 valid parallel samples; only when there is a clear sample preparation defect, clamping abnormality or equipment abnormality and there is a corresponding record, the test shall be deemed invalid and supplemented for testing, so that the final valid data shall not be less than 5, and the arithmetic mean of all valid test results shall be used as the final recorded data.

[0092] Table 5. Test data of macroscopic mechanical properties of molded specimens of masterbatch from each embodiment and comparative example. Test object Tensile yield strength (MPa) Elongation at break (%) <![CDATA[Notched impact strength (kJ / m 2 )]]> Example 1 18.45 145.2 28.6 Example 2 21.12 122.8 25.4 Example 3 16.89 168.5 32.1 Example 4 19.34 139.6 27.8 Example 5 17.76 154.3 30.2 Comparative Example 5 6.54 21.4 4.2

[0093] According to the data in Table 5, the tensile yield strength of the molded specimens in Examples 1 to 5 ranged from 16.89 MPa to 21.12 MPa, the elongation at break all exceeded 122.8%, and the notched impact strength remained at 25.4 kJ / m. 2 Up to 32.1 kJ / m 2 Interval. Combined with the aforementioned free Ca... 2+ The mechanical properties shown in Table 5, based on the changes and rheological test results, indicate that the introduction of the sodium alginate-calcium ion crosslinking system is beneficial to improving the load-bearing capacity, ductility, and impact resistance of the potato residue-based molding material. The aforementioned performance improvements are consistent with the mechanism by which ionic cross-linking networks participate in the construction of the matrix structure. During the high-temperature molding stage, the cross-linked structure, together with the cellulose skeleton and starch segments in potato residue, forms a composite matrix, which is beneficial for the material to dissipate energy through molecular chain movement and phase deformation under external tensile and impact loads.

[0094] Comparative Example 5, serving as a baseline control group without the addition of functional components such as sodium alginate and calcium citrate, exhibited significantly lower mechanical properties than the Example Group. Its tensile yield strength was 6.54 MPa, elongation at break was 21.4%, and notched impact strength was 4.2 kJ / m². 2 .

[0095] The results indicate that the load-bearing, elongation, and impact resistance of potato residue matrix plasticized only with glycerol and without the construction of an ionic cross-linking network are significantly limited after hot pressing. These data demonstrate that the composite modification and controlled cross-linking system employed in this invention not only improves processing rheology but also enhances the mechanical load-bearing capacity and impact toughness of potato residue-based materials that do not contain traditional plastic resins.

Claims

1. A high-toughness, potato residue-based, edible, fully biodegradable functional masterbatch, characterized in that, Made from the following ingredients in parts by weight: Moist potato residue, 100 parts on a dry basis; Glycerin 15.0 to 20.0 parts; Sodium alginate 5.0 to 8.0 parts; Calcium citrate 2.0 to 4.0 parts; Sodium hexametaphosphate, 0.5 to 1.5 parts; 1.5 to 3.0 parts of soybean lecithin.

2. The high-toughness potato residue-based edible fully degradable functional masterbatch according to claim 1, characterized in that, Made from the following ingredients in parts by weight: Moist potato residue, 100 parts on a dry basis; 17.5 parts glycerin; 6.5 parts sodium alginate; Calcium citrate 3.0 parts; Sodium hexametaphosphate 1.0 part; 2.2 parts of soybean lecithin.

3. The high-toughness potato residue-based edible fully degradable functional masterbatch according to claim 1, characterized in that, The water-containing potato residue is a water-containing material that has been mechanically pressed to remove some of the free water, and its moisture content is controlled to be between 45.0% and 55.0%.

4. The high-toughness potato residue-based edible fully degradable functional masterbatch according to claim 1, characterized in that, The sodium alginate is a food-grade powder with a weight-average molecular weight of 100,000 g / mol to 150,000 g / mol, and a dynamic viscosity of 200 mPa·s to 500 mPa·s in a 1.0% aqueous solution at 20°C.

5. The high-toughness potato residue-based edible fully degradable functional masterbatch according to claim 1, characterized in that, The sodium hexametaphosphate is food-grade sodium hexametaphosphate with an average degree of polymerization of 10 to 20. The soybean lecithin is a food-grade powder with an acetone-insoluble content of ≥60.0% by mass.

6. A method for preparing the high-toughness potato residue-based edible fully degradable functional masterbatch according to any one of claims 1 to 5, characterized in that, Includes the following steps: The potato residue is mechanically pressed to remove some of the free water, resulting in the water-containing potato residue. The water-containing potato residue is then pulverized at high speed to obtain slightly moist initial powder. The slightly moist initial powder is physically mixed with the glycerol, sodium alginate, calcium citrate, sodium hexametaphosphate and soybean lecithin according to the weight ratio of the raw materials of the functional masterbatch to obtain loose and moist granular bulk material; The loose and moist granular material is fed into a closed steam reactor and steam is introduced for pressure heat treatment. Then, the vacuum system is turned on to perform vacuum flash steam depressurization. After the vacuum is broken and the material is discharged, a porous elastic hot dough is obtained. The porous elastic hot dough is continuously fed into a ring die granulator for extrusion and cutting to obtain primary masterbatch. The primary masterbatch is then dried to obtain the fully degradable functional masterbatch.

7. The preparation method according to claim 6, characterized in that, During the physical mixing process, the specific parameters of the mixing process are as follows: physical mixing is carried out at a temperature of 15 to 30°C and a stirring speed of 300 to 500 rpm for 15 to 20 minutes.

8. The preparation method according to claim 6, characterized in that, The specific implementation method of the pressure-holding heat treatment and vacuum flash evaporation depressurization is as follows: Steam at 110 to 120°C is introduced into the sealed steam reactor. During the steam treatment stage, the absolute pressure inside the reactor is maintained at 0.15 to 0.20 MPa. The total treatment time inside the sealed steam reactor is 20 to 30 minutes. Three to five minutes before the planned discharge, close the steam inlet valve and turn on the vacuum system. Within 15 to 30 seconds, the absolute pressure inside the vessel will drop sharply to 0.02 to 0.04 MPa, and vacuum flash evaporation will be carried out within the absolute pressure range of 0.02 to 0.04 MPa for 2 to 4 minutes. Wherein, the sum of the pressure reduction time and the maintenance time within the absolute pressure range is less than the time from closing the steam inlet valve to the planned discharge.

9. The preparation method according to claim 6, characterized in that, During the extrusion cutting process, the ring die temperature of the ring die granulator is controlled at 85 to 95°C.

10. The preparation method according to claim 6, characterized in that, During the drying process, infrared low-temperature drying treatment with a core temperature set at 70 to 85°C is used, and the drying time is 20 to 40 minutes, controlling the moisture content of the obtained fully degradable functional masterbatch to be 8.0% to 12.0%.