High-elastic wear-resistant sports shoe material and preparation method thereof

The high-elasticity and abrasion-resistant sports shoe material prepared by specific components and processes solves the problem of insufficient elasticity and abrasion resistance in the existing technology, and achieves both high elasticity and abrasion resistance, thereby improving the efficiency of sports shoes.

CN123131784APending Publication Date: 2026-11-20MINGZHI SPORTS GOODS (CHINA) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611077911.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

While existing sports shoe materials improve elasticity, they have poor abrasion resistance, which affects their performance.

Method used

Highly elastic and wear-resistant sports shoe materials are prepared by using a specific ratio of epoxy resin, phenolic resin, nanocomposite emulsion, gel, zinc oxide, zinc stearate, diatomaceous earth, vinyl silicone oil and stearic acid through intensive mixing and open milling processes. This forms a reinforced organosilicon network structure, which enhances the elasticity and wear resistance of the material.

Benefits of technology

It achieves a combination of high elasticity and abrasion resistance in sports shoe materials, improves the abrasion resistance and rebound rate of the materials, and exhibits excellent tear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131784A_ABST
    Figure CN123131784A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of high elastic wear-resistant sports shoes materials, including the following weight parts of component: 50-60 weight parts of epoxy resin, 20-30 weight parts of phenolic resin, 20-30 weight parts of nano composite emulsion, 25-35 weight parts of gel, 3-5 weight parts of zinc oxide, 3-5 weight parts of zinc stearate, 1-3 weight parts of diatomite, 6-10 weight parts of vinyl silicone oil and 5-8 weight parts of stearic acid.A kind of high elastic wear-resistant sports shoes material preparation method, corresponding weight parts of material are mixed uniformly in internal mixer at 70-80 ℃, dense and knead 30-60 min, and continue to mix at 100-110 ℃ for 20-30 min, after opening and rolling granulation, cooling to room temperature, obtain high elastic wear-resistant sports shoes material.The present application relates to a kind of high elastic wear-resistant sports shoes materials and its preparation method, with good wear resistance and elastic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of footwear, specifically to a high-elasticity and abrasion-resistant sports shoe material and its preparation method. Background Technology

[0002] The design and manufacture of footwear and athletic equipment involves a wide range of factors, from aesthetics and comfort to performance and durability. While designs and fashion may change rapidly, the demand for enhanced performance in the footwear and athletic equipment market remains constant.

[0003] Existing sports shoe materials use EVA foam, which can improve the product's elasticity, but it can easily reduce the product's abrasion resistance, thus affecting the product's efficiency. Summary of the Invention

[0004] In view of this, the purpose of this invention is to provide a high-elasticity and wear-resistant sports shoe material and its preparation method, which has good wear resistance and elasticity.

[0005] To achieve the above objectives, the present invention provides the following technical solution: A highly elastic and abrasion-resistant sports shoe material, comprising the following components in parts by weight: 50-60 parts by weight of epoxy resin, 20-30 parts by weight of phenolic resin, 20-30 parts by weight of nanocomposite emulsion, 25-35 parts by weight of gel, 3-5 parts by weight of zinc oxide, 3-5 parts by weight of zinc stearate, 1-3 parts by weight of diatomaceous earth, 6-10 parts by weight of vinyl silicone oil and 5-8 parts by weight of stearic acid.

[0006] A method for preparing a high-elasticity and wear-resistant sports shoe material involves mixing 50-60 parts by weight of epoxy resin, 20-30 parts by weight of phenolic resin, 20-30 parts by weight of nanocomposite emulsion, 25-35 parts by weight of gel, 3-5 parts by weight of zinc oxide, 3-5 parts by weight of zinc stearate, 1-3 parts by weight of diatomaceous earth, 6-10 parts by weight of vinyl silicone oil, and 5-8 parts by weight of stearic acid in a mixer at 70-80°C for 30-60 minutes, followed by further mixing at 100-110°C for 20-30 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain the high-elasticity and wear-resistant sports shoe material.

[0007] Preferably, the preparation method of the nanocomposite emulsion is as follows: Methyl methacrylate, butyl acrylate, modified nano silica, sodium dodecyl sulfate, hexadecane and water are mixed and emulsified for 10-20 min, and sonicated for 10-20 min to obtain a fine emulsion. The mixture is then heated to 70-80℃, ammonium persulfate is added, and the mixture is stirred at 200-300 r / min for 2-4 h. After cooling to room temperature, a nanocomposite emulsion is obtained.

[0008] Preferably, the weight ratio of methyl methacrylate, butyl acrylate, modified nano silica, sodium dodecyl sulfate, hexadecane, water and ammonium persulfate is 3:3:2:1:2:5:1.

[0009] Preferably, the preparation method of the modified nano silica is as follows: nano silica, triethoxyvinylsilane and ethanol are mixed, stirred at room temperature for 24-36 hours at a speed of 200-300 r / min, and dried at 75°C for 24-36 hours to obtain modified nano silica.

[0010] Preferably, the weight ratio of the nano-silica, triethoxyvinylsilane and ethanol is 1:1:3.

[0011] Preferably, the method for preparing the gel is as follows: Urea, hexadecyltrimethylammonium bromide, water and o-xylene are mixed and stirred evenly. Acetic acid is added to adjust the pH value to 2-3. Then methyltrimethoxysilane, dimethyldimethoxysiloxane and perfluorooctyltrimethoxysilane are added, stirred and sonicated for 12-20 hours. Modified nanocellulose is then added and stirring is continued for 24-36 hours. The mixture is filtered and dried to obtain a gel.

[0012] Preferably, the weight ratio of urea, hexadecyltrimethylammonium bromide, water, o-xylene, methyltrimethoxysilane, dimethyldimethoxysiloxane, perfluorooctyltrimethoxysilane, and modified nanocellulose is 1:1:3:1:1:1:1:1.

[0013] Preferably, the preparation method of the modified nanocellulose is as follows: bamboo fiber flocs are soaked and swollen in deionized water, and urea, KH550 and diammonium hydrogen phosphate are added, stirred and dissolved, dried, and then heated to 120-150℃ for 30-40 minutes for curing treatment. After washing, drying and grinding, the modified nanocellulose is obtained.

[0014] Preferably, the weight ratio of the bamboo fiber fluff, urea, KH550 and diammonium hydrogen phosphate is 2:2:1:3.

[0015] This invention connects long alkyl chains to the surface of nano-silica particles, increasing steric hindrance between particles and preventing aggregation to some extent, thus enhancing their dispersibility. This increases the number of double bond sites on the acrylate matrix, further enhancing the cross-linking degree between acrylate chains and improving the material's compactness and wear resistance. The polymer chains in this invention intertwine with the modified nanocellulose, strengthening the interaction forces between the modified nanocellulose. The introduction of the co-solvents o-xylene and oxysilane promotes the hydrolysis and condensation of the silane precursor. The phosphorylation and silanization processes help reduce or destroy the fiber... The crystalline region of the cellulose is reduced, its crystallinity is decreased, and the degree of exfoliation is improved, thereby increasing the aspect ratio of the filaments and increasing the specific surface area. Due to the steric hindrance of the methyl group, the gel has enough space to withstand large deformation compression and deformation, which increases the elasticity of the material. Through hydrogen bonds, chemical covalent bonds and physical interactions, strong interactions are formed between the gel and the organosilicon backbone molecular chains, thereby enhancing the organosilicon network structure and forming a network structure. A reinforced organosilicon network structure is formed in the gel and nanosolution matrix, which improves the toughness and cohesiveness of the material, thereby enhancing the elasticity and wear resistance of the material. Attached Figure Description

[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a schematic diagram of the overall structure of the sole of a sports shoe. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In addition, it should be specifically noted that the raw materials and equipment of the present invention are all commercially available and will not be listed one by one. Among them, the raw materials of the present invention are all commercially available and well known to those skilled in the art, and will not be described in detail. Example 1:

[0019] To achieve the above objectives, the present invention provides the following technical solution: A highly elastic and abrasion-resistant sports shoe material, comprising the following components in parts by weight: 50 parts by weight of epoxy resin, 20 parts by weight of phenolic resin, 20 parts by weight of nanocomposite emulsion, 25 parts by weight of gel, 3 parts by weight of zinc oxide, 3 parts by weight of zinc stearate, 1 part by weight of diatomaceous earth, 6 parts by weight of vinyl silicone oil and 5 parts by weight of stearic acid.

[0020] A method for preparing a high-elasticity and wear-resistant sports shoe material involves mixing the above-mentioned parts by weight of the material evenly in a mixer at 70°C for 30 minutes, then continuing to mix at 100°C for 20 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain the high-elasticity and wear-resistant sports shoe material.

[0021] The specific preparation method of the nanocomposite emulsion is as follows: Nano-silica, triethoxyvinylsilane and ethanol were mixed in a weight ratio of 1:1:3, stirred at room temperature for 24 hours at a speed of 200 r / min, and dried at 75°C for 24 hours to obtain modified nano-silica. Methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, and water were mixed and emulsified for 10 min, followed by sonication for 10 min to obtain a fine emulsion. The mixture was then heated to 70°C, and ammonium persulfate was added. The weight ratio of methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, water, and ammonium persulfate was 3:3:2:1:2:5:1. The mixture was stirred at 200 r / min for 2 h and then cooled to room temperature to obtain a nanocomposite emulsion.

[0022] The specific method for preparing the gel is as follows: Bamboo fiber flocs were soaked and swollen in deionized water, and urea, KH550 and diammonium hydrogen phosphate were added. The weight ratio of bamboo fiber flocs, urea, KH550 and diammonium hydrogen phosphate was 2:2:1:3. The mixture was stirred and dissolved, dried, and then heated to 120℃ for 30 minutes to solidify. After washing, drying and grinding, modified nanocellulose was obtained. Urea, hexadecyltrimethylammonium bromide, water, and o-xylene were mixed and stirred evenly. Acetic acid was added to adjust the pH to 2. Then, methyltrimethoxysilane, dimethyldimethoxysiloxane, and perfluorooctyltrimethoxysilane were added. The mixture was stirred and sonicated for 12 hours. Modified nanocellulose was then added and stirring was continued for 24 hours. The weight ratio of urea, hexadecyltrimethylammonium bromide, water, o-xylene, methyltrimethoxysilane, dimethyldimethoxysiloxane, perfluorooctyltrimethoxysilane, and modified nanocellulose was 1:1:3:1:1:1:1:1. The mixture was filtered and dried to obtain a gel. Example 2:

[0023] A highly elastic and abrasion-resistant sports shoe material, comprising the following components in parts by weight: 55 parts by weight of epoxy resin, 25 parts by weight of phenolic resin, 25 parts by weight of nanocomposite emulsion, 30 parts by weight of gel, 4 parts by weight of zinc oxide, 4 parts by weight of zinc stearate, 2 parts by weight of diatomaceous earth, 8 parts by weight of vinyl silicone oil and 6 parts by weight of stearic acid.

[0024] A method for preparing a high-elasticity and wear-resistant sports shoe material involves mixing the above-mentioned parts by weight of the material evenly in a mixer at 75°C for 45 minutes, then continuing to mix at 105°C for 25 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain the high-elasticity and wear-resistant sports shoe material.

[0025] The specific preparation method of the nanocomposite emulsion is as follows: Nano-silica, triethoxyvinylsilane and ethanol were mixed in a weight ratio of 1:1:3, stirred at room temperature for 30 h at a speed of 250 r / min, and dried at 75 °C for 30 h to obtain modified nano-silica. Methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, and water were mixed and emulsified for 15 min, followed by sonication for 15 min to obtain a fine emulsion. The mixture was then heated to 75°C, and ammonium persulfate was added. The weight ratio of methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, water, and ammonium persulfate was 3:3:2:1:2:5:1. The mixture was stirred at 250 r / min for 3 h and then cooled to room temperature to obtain a nanocomposite emulsion.

[0026] The specific method for preparing the gel is as follows: Bamboo fiber flocs were soaked and swollen in deionized water, and urea, KH550 and diammonium hydrogen phosphate were added. The weight ratio of bamboo fiber flocs, urea, KH550 and diammonium hydrogen phosphate was 2:2:1:3. The mixture was stirred and dissolved, dried, and then heated to 130℃ for 35 minutes to solidify. After washing, drying and grinding, modified nanocellulose was obtained. Urea, hexadecyltrimethylammonium bromide, water, and o-xylene were mixed and stirred until homogeneous. Acetic acid was added to adjust the pH to 3. Then, methyltrimethoxysilane, dimethyldimethoxysiloxane, and perfluorooctyltrimethoxysilane were added. The mixture was stirred and sonicated for 18 hours. Modified nanocellulose was then added and the mixture was stirred for another 30 hours. The weight ratio of urea, hexadecyltrimethylammonium bromide, water, o-xylene, methyltrimethoxysilane, dimethyldimethoxysiloxane, perfluorooctyltrimethoxysilane, and modified nanocellulose was 1:1:3:1:1:1:1:1. The mixture was filtered and dried to obtain a gel. Example 3:

[0027] A highly elastic and abrasion-resistant sports shoe material, comprising the following components in parts by weight: 60 parts by weight of epoxy resin, 30 parts by weight of phenolic resin, 30 parts by weight of nanocomposite emulsion, 35 parts by weight of gel, 5 parts by weight of zinc oxide, 5 parts by weight of zinc stearate, 3 parts by weight of diatomaceous earth, 10 parts by weight of vinyl silicone oil and 8 parts by weight of stearic acid.

[0028] A method for preparing a high-elasticity and wear-resistant sports shoe material involves mixing the above-mentioned parts by weight of the material evenly in a mixer at 80°C for 60 minutes, then continuing to mix at 110°C for 30 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain the high-elasticity and wear-resistant sports shoe material.

[0029] The specific preparation method of the nanocomposite emulsion is as follows: Nano-silica, triethoxyvinylsilane and ethanol were mixed in a weight ratio of 1:1:3, stirred at room temperature for 36 h at a speed of 300 r / min, and dried at 75 °C for 36 h to obtain modified nano-silica. Methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, and water were mixed and emulsified for 20 min, followed by sonication for 20 min to obtain a fine emulsion. The mixture was then heated to 80 °C, and ammonium persulfate was added. The weight ratio of methyl methacrylate, butyl acrylate, modified nano-silica, sodium dodecyl sulfate, hexadecane, water, and ammonium persulfate was 3:3:2:1:2:5:1. The mixture was stirred at 300 r / min for 4 h and then cooled to room temperature to obtain a nanocomposite emulsion.

[0030] The specific method for preparing the gel is as follows: Bamboo fiber flocs were soaked and swollen in deionized water, and urea, KH550 and diammonium hydrogen phosphate were added. The weight ratio of bamboo fiber flocs, urea, KH550 and diammonium hydrogen phosphate was 2:2:1:3. The mixture was stirred and dissolved, dried, and then heated to 150℃ for 40 minutes to solidify. After washing, drying and grinding, modified nanocellulose was obtained. Urea, hexadecyltrimethylammonium bromide, water, and o-xylene were mixed and stirred until homogeneous. Acetic acid was added to adjust the pH to 3. Then, methyltrimethoxysilane, dimethyldimethoxysiloxane, and perfluorooctyltrimethoxysilane were added. The mixture was stirred and sonicated for 20 hours. Modified nanocellulose was then added and the mixture was stirred for another 36 hours. The weight ratio of urea, hexadecyltrimethylammonium bromide, water, o-xylene, methyltrimethoxysilane, dimethyldimethoxysiloxane, perfluorooctyltrimethoxysilane, and modified nanocellulose was 1:1:3:1:1:1:1:1. The mixture was filtered and dried to obtain a gel. Comparative Example 1:

[0031] The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that nanocomposite emulsions and gels are not used. Specifically: A highly elastic and abrasion-resistant sports shoe material, comprising the following components in parts by weight: 50 parts by weight of epoxy resin, 20 parts by weight of phenolic resin, 3 parts by weight of zinc oxide, 3 parts by weight of zinc stearate, 1 part by weight of diatomaceous earth, 6 parts by weight of vinyl silicone oil and 5 parts by weight of stearic acid.

[0032] A method for preparing a high-elasticity and wear-resistant sports shoe material involves mixing the above-mentioned parts by weight of the material evenly in a mixer at 70°C for 30 minutes, then continuing to mix at 100°C for 20 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain the high-elasticity and wear-resistant sports shoe material.

[0033] The athletic shoe materials obtained in Examples 1-3 and Comparative Example 1 were placed in a foaming mold and molded under a closing pressure of 15 MPa. Then, the mold and material were heated to 180°C and vulcanized for 8 minutes. After cooling, the mixture was allowed to stand at room temperature for 20 hours to obtain the desired product. Figure 1 The abrasion resistance and rebound rate of the shoe soles shown are tested below for the soles of Examples 1-3, the soles sold by Jinjiang Datian Sports Goods Co., Ltd., and the soles obtained in Comparative Example 1.

[0034] Rebound rate: Tested in accordance with HG / T3869-2006 "Determination of compression or shear properties of rubber".

[0035] Abrasion resistance: Tested according to the method specified in national standard GB / T 9867-2008.

[0036] Tear strength: Tested according to national standard GB / T 10808-2006.

[0037] Table 1: Test data of Examples 1-3, commercially available shoe soles, and the shoe sole of Comparative Example 1

[0038] As can be seen from the table above, the outsoles made from the athletic shoe materials of Examples 1-3 have lower wear volume, better wear resistance, higher rebound rate, and excellent tear resistance compared to Comparative Example 1 and commercially available outsoles.

[0039] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A high-elasticity, wear-resistant sports shoe material, characterized in that, Includes the following components in parts by weight: 50-60 parts by weight of epoxy resin, 20-30 parts by weight of phenolic resin, 20-30 parts by weight of nanocomposite emulsion, 25-35 parts by weight of gel, 3-5 parts by weight of zinc oxide, 3-5 parts by weight of zinc stearate, 1-3 parts by weight of diatomaceous earth, 6-10 parts by weight of vinyl silicone oil and 5-8 parts by weight of stearic acid.

2. A method for preparing a high-elasticity, abrasion-resistant sports shoe material, characterized in that, 50-60 parts by weight of epoxy resin, 20-30 parts by weight of phenolic resin, 20-30 parts by weight of nanocomposite emulsion, 25-35 parts by weight of gel, 3-5 parts by weight of zinc oxide, 3-5 parts by weight of zinc stearate, 1-3 parts by weight of diatomaceous earth, 6-10 parts by weight of vinyl silicone oil and 5-8 parts by weight of stearic acid are mixed evenly in an internal mixer at 70-80°C for 30-60 minutes, and then mixed again at 100-110°C for 20-30 minutes. After open milling, the mixture is granulated and cooled to room temperature to obtain a high-elasticity and wear-resistant sports shoe material.

3. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 2, characterized in that: The specific preparation method of the nanocomposite emulsion is as follows: Methyl methacrylate, butyl acrylate, modified nano silica, sodium dodecyl sulfate, hexadecane and water are mixed and emulsified for 10-20 min, and sonicated for 10-20 min to obtain a fine emulsion. The mixture is then heated to 70-80℃, ammonium persulfate is added, and the mixture is stirred at 200-300 r / min for 2-4 h. After cooling to room temperature, a nanocomposite emulsion is obtained.

4. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 3, characterized in that: The weight ratio of methyl methacrylate, butyl acrylate, modified nano silica, sodium dodecyl sulfate, hexadecane, water and ammonium persulfate is 3:3:2:1:2:5:

1.

5. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 4, characterized in that: The modified nano-silica is prepared by mixing nano-silica, triethoxyvinylsilane and ethanol, stirring at room temperature for 24-36 hours at a speed of 200-300 r / min, and drying at 75°C for 24-36 hours to obtain modified nano-silica.

6. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 5, characterized in that: The weight ratio of the nano-silica, triethoxyvinylsilane and ethanol is 1:1:

3.

7. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 2, characterized in that: The specific method for preparing the gel is as follows: Urea, hexadecyltrimethylammonium bromide, water and o-xylene are mixed and stirred evenly. Acetic acid is added to adjust the pH value to 2-3. Then methyltrimethoxysilane, dimethyldimethoxysiloxane and perfluorooctyltrimethoxysilane are added, stirred and sonicated for 12-20 hours. Modified nanocellulose is then added and stirring is continued for 24-36 hours. The mixture is filtered and dried to obtain a gel.

8. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 7, characterized in that, The weight ratio of urea, hexadecyltrimethylammonium bromide, water, o-xylene, methyltrimethoxysilane, dimethyldimethoxysiloxane, perfluorooctyltrimethoxysilane, and modified nanocellulose is 1:1:3:1:1:1:1:

1.

9. The method for preparing the high-elasticity, abrasion-resistant sports shoe material as described in claim 8, characterized in that, The specific preparation method of the modified nanocellulose is as follows: bamboo fiber flocs are soaked and swollen in deionized water, and urea, KH550 and diammonium hydrogen phosphate are added, stirred and dissolved, dried, and then heated to 120-150℃ for 30-40 minutes for curing treatment. After washing, drying and grinding, the modified nanocellulose is obtained.

10. The method for preparing the high-elasticity and abrasion-resistant sports shoe material as described in claim 9, characterized in that: The weight ratio of bamboo fiber fluff, urea, KH550 and diammonium hydrogen phosphate is 2:2:1:3.