A light-shielding protective film resistant to moist heat aging and a preparation method thereof
By coating the surface of carbon black with a silica-like shell and a phosphomolybdic acid-loaded layer, and chemically bonding it with PET oligomers, the problems of dispersion and interfacial bonding of carbon black light-shielding film in PET matrix are solved, achieving stable light-shielding properties and mechanical properties under humid and hot environments.
Patent Information
- Application Number
- CN202611585143.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-20
AI Technical Summary
Existing carbon black opaque films exhibit poor dispersion and weak interfacial bonding in PET matrices, resulting in a significant reduction in opacity and mechanical properties under humid and hot conditions. They cannot simultaneously achieve uniform dispersion, permanent antistatic properties, and chemically bonded interfaces.
Modified carbon black is used, and a silica-like shell and a phosphomolybdic acid-loaded layer are formed by coating the carbon black surface with a catechol coupling agent. These layers are then chemically bonded to PET oligomers through ester bonds and combined with electrostatic attraction to form a stable interfacial connection.
It significantly improves the dispersibility and moisture resistance of carbon black in PET matrix, maintains the stability of light-blocking and mechanical properties, has a low rate of change in light transmittance, and a high rate of retention of breaking strength, making it suitable for long-term working conditions of 85℃ and 85% relative humidity.
Smart Images

Figure CN123131801A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of PET protective film technology, and in particular relates to a light-shielding protective film resistant to damp heat aging and its preparation method. Background Technology
[0002] Light-shielding protective films are a type of functional film widely used in consumer electronics, displays, and photovoltaics. They typically use heat-resistant polymers such as PET, polyethylene naphthalate, or polyimide as the matrix, and carbon black, carbon black-based pigments, and organic light-absorbing dyes as light-shielding agents. Among these, carbon black has long been the most mainstream light-shielding filler due to its broad optical absorption spectrum, low cost, and good heat resistance.
[0003] In practical applications, especially inside display module backlight units and electronic tags, the light-shielding film needs to operate under humid and hot conditions such as 85℃ and 85% relative humidity for extended periods. Existing carbon black light-shielding films mainly suffer from the following problems: 1. Poor dispersion of carbon black in the PET matrix. Virgin carbon black has high surface energy and small particle size, making it extremely easy to form micron-sized aggregates through van der Waals forces and π-π interactions. When directly blended with PET chips using a twin-screw extruder, these aggregates are difficult to fully open under shear force, resulting in micron-sized particle defects in the film after casting. This leads to localized stress concentration, making the film prone to pinholes, silver streaks, and brittle fracture during biaxial stretching and humid aging. 2. The relationship between carbon black particles and the PET matrix is primarily a physical interface, lacking chemical bonding. In a humid and hot environment, water molecules diffuse and accumulate along the carbon black-polymer interface, gradually causing the interface to dehydrate and peel off. After the interface debonds, the carbon black particles lose the constraint of the matrix. On the one hand, they form new light scattering centers, which increases the light transmittance of the film and decreases the light blocking effect. On the other hand, they become crack sources during the stretching process, resulting in a significant reduction in elongation at break and tear strength.
[0004] To address the aforementioned issues, existing technologies have proposed surface treatment of carbon black using silane coupling agents, titanate coupling agents, or stearic acid, followed by blending with PET. While such approaches can improve carbon black dispersion to some extent, the coupling agents only bind to the carbon black surface through physical adsorption or weak hydrogen bonds, making them prone to desorption under high-temperature shearing in twin-screw extruders and prolonged humid and hot conditions. Furthermore, a single silane shell lacks permanent antistatic properties, necessitating the addition of small-molecule antistatic agents, thus failing to simultaneously solve the problems of dispersion, antistatic properties, and interfacial bonding.
[0005] Therefore, it is necessary to develop a new light-shielding protective film and its preparation method, so that carbon black can be uniformly dispersed, permanently antistatic and chemically bonded in the PET matrix at the same time, thereby maintaining stable light-shielding and mechanical properties under humid heat aging conditions. Summary of the Invention
[0006] To address the above problems, this application provides a light-shielding protective film resistant to damp heat aging and its preparation method.
[0007] This application provides a light-shielding protective film resistant to damp heat aging, comprising a PET matrix and modified carbon black dispersed in the matrix. The modified carbon black has a carbon black core, and its surface is sequentially coated with a silica-like shell formed by the hydrolysis and condensation of a catechol coupling agent with silane, a phosphomolybdic acid layer supported on the shell, and end-carboxyl PET oligomer segments chemically bonded to the residual hydroxyl groups of the shell and / or the coordination sites of the phosphomolybdic acid through ester bonds.
[0008] The polyethylene terephthalate matrix is a film-grade PET homopolymer polyester; the catechol coupling agent is preferably a urea bond product formed by the addition reaction of the amino group of dopamine molecule and the isocyanate group of 3-isocyanopropyltriethoxysilane, and the molecular structure contains both catechol group and triethoxysilane group; the phosphomolybdic acid is preferably dodecamolybdic acid with a Keggin structure, and its loading is 5wt%~20wt% based on the mass of modified carbon black; the number average molecular weight of the carboxyl-terminated PET oligomer is preferably 1500~6000g / mol, and the carboxyl-terminated value is 30~120mgKOH / g; based on the total mass of the light-shielding protective film, the modified carbon black content is 1wt%~8wt%, the PET matrix content is 85wt%~98wt%, and the balance is additives. The adjuvants may include antioxidants, such as pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010), in an amount of 0.1wt% to 0.5wt%.
[0009] This application provides a method for preparing the aforementioned light-shielding protective film, comprising: pre-dispersing carbon black in an aqueous phase; preparing a catechol coupling agent by reacting dopamine hydrochloride, triethylamine, and propyltriethoxysilane 3-isocyanate under an inert atmosphere; mixing the carbon black dispersion with anhydrous ethanol and adjusting the pH to acidic, then adding the catechol coupling agent dropwise to perform silane hydrolysis and condensation to obtain CB@Cat-Si; and impregnating CB@Cat-Si with an aqueous solution of phosphomolybdic acid under acidic conditions to obtain PMA@CB-Cat- Si; PET chips are reacted with ethylene glycol under an inert atmosphere, and then desized under vacuum to obtain carboxyl-terminated PET oligomers; PMA@CB-Cat-Si, carboxyl-terminated PET oligomers and tetrabutyl titanate are premixed and then melt-grafted through a twin-screw extruder to obtain modified carbon black grafted PET oligomer masterbatch; the masterbatch is blended and granulated with PET chips and antioxidants to obtain light-shielding PET masterbatch; finally, light-shielding protective film is obtained by single-screw casting and simultaneous biaxial stretching, heat setting and cooling.
[0010] Compared with the prior art, this application has the following beneficial effects:
[0011] 1. This application utilizes the π-π stacking and hydrogen bonding between the catechol groups in the catechol coupling agent and the graphitized surface of carbon black, as well as the Si-O-Si network formed after the hydrolysis and condensation of triethoxysilyl groups. Compared with conventional coupling treatment that relies solely on the direct adsorption of silanols, this method is less prone to desorption under high-temperature shear and humid conditions, and can significantly improve the dispersibility of carbon black in the PET matrix.
[0012] 2. This application utilizes the electrostatic attraction and coordination between phosphomolybdic acid anions and the silanol and catechol residual phenolic hydroxyl groups on the shell surface to anchor phosphomolybdic acid on the shell at the nanoscale, rather than allowing it to remain free in the matrix as a small molecule. This inhibits the interfacial transfer of water molecules and further improves the dispersion uniformity and resistance to damp heat of carbon black.
[0013] 3. In this application, the terminal carboxyl groups of the PET oligomer undergo transesterification and condensation reactions with the residual silanol groups of the catechol coupling agent and the hydroxyl groups on the surface of phosphomolybdic acid under the catalysis of tetrabutyl titanate, chemically bonding the flexible PET segments to the surface of carbon black particles. During biaxial stretching, this structure can disperse stress through segment deformation and inhibit the diffusion and debonding of water molecules along the interface under humid and hot conditions. As a result, the film maintains a low rate of change in transmittance, stable surface resistance and high tensile strength retention rate even after being placed at 85°C and 85% relative humidity for 500 hours. Attached Figure Description
[0014] Figure 1 This is a schematic diagram of the manufacturing process of the moisture- and heat-resistant aging-resistant light-shielding protective film provided in the embodiments of this application.
[0015] Figure 2 The transmittance curves of Examples 1-3 and Comparative Examples 1-3 in the visible light range of 380nm-780nm are shown.
[0016] Figure 3 Typical tensile stress-strain curves for Examples 1-3 and Comparative Examples 1-3 are shown. Detailed Implementation
[0017] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the embodiments of this application. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0019] When using “including,” “having,” and “contains” as described herein, the intention is to cover non-exclusive inclusion, unless an explicit qualifying term such as “only,” “consisting of,” etc., is used, in which case another component may be added.
[0020] The terms "preferred," "more preferably," "better," and "even better" used in this application refer to embodiments of this application that provide certain beneficial effects under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the description of one or more preferred embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of this application. That is, in this application, "preferred," "more preferably," "better," and "even better" are merely descriptions of implementations or embodiments with better effects, but do not constitute a limitation on the scope of protection of this application.
[0021] In this application, terms such as "further," "even more," and "particularly" are used for descriptive purposes and to indicate differences in content, but should not be construed as limiting the scope of protection of this application.
[0022] In this application, "at least one" means one or more, such as one, two, or more. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layered" means at least two layers, such as two layers, three layers, etc., unless otherwise explicitly specified. In the description of this application, "several" means at least one, such as one, two, etc., unless otherwise explicitly specified.
[0023] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0024] Unless otherwise specified, all steps in this application may be performed sequentially or randomly. For example, the method comprising steps (a) and (b) indicates that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc. Unless otherwise stated, singular terms may include plural forms and should not be construed as having a quantity of one.
[0025] The present application will be further illustrated by the following examples, but these examples do not limit the scope of the present application.
[0026] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in this application, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. All reagents or instruments whose manufacturers are not specified are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description in this application, any prior art methods, equipment, and materials similar to or equivalent to those described, used, or made by the methods, equipment, and materials in the embodiments of this application may be used to implement this application.
[0027] Unless otherwise specified, all raw materials used in the embodiments and comparative examples of this application are commercially available raw materials. Carbon black, BP200. PET chips, intrinsic viscosity 0.64 dL / g. Dopamine hydrochloride, triethylamine, propyltriethoxysilane 3-isocyanate (IPTS), anhydrous N,N-dimethylformamide (DMF), anhydrous diethyl ether, anhydrous ethanol, glacial acetic acid, phosphomolybdic acid (dodecyl molybdate phosphate hydrate), tetrabutyl titanate, and antioxidant 1010 are all commercially available analytical grade or industrial grade reagents; the experimental water is deionized water.
[0028] Example 1
[0029] The method for preparing the light-shielding protective film resistant to damp heat aging in this embodiment includes the following steps:
[0030] Purification and pre-dispersion of carbon black: Add 10.0g of carbon black to 500mL of deionized water and disperse it at 8000rpm for 30min using a high-speed disperser. Then, use an ultrasonic homogenizer at 400W for 60min, sonicating for 3s and pausing for 2s to prevent overheating. After treatment, centrifuge at 3000rpm for 5min to remove a small amount of undispersed large agglomerates and collect the upper carbon black dispersion for later use.
[0031] Preparation of CB@Cat-Si: 1.90 g of dopamine hydrochloride and 30 mL of anhydrous DMF were added to a 500 mL three-necked flask and magnetically stirred under nitrogen protection until completely dissolved; then 1.40 mL of triethylamine was added and stirred at room temperature for 10 min to neutralize the hydrochloric acid; 2.47 g of propyltriethoxysilane 3-isocyanate was slowly added dropwise using a constant pressure dropping funnel, and the addition was completed in about 30 min, while keeping the reaction temperature below 30 °C during the addition; after the addition was completed, the reaction was continued to be stirred at room temperature under nitrogen protection for 12 h; after the reaction was completed, the reaction solution was slowly poured into 500 mL of vigorously stirred anhydrous diethyl ether, and a white to off-white precipitate was precipitated; the precipitate was filtered, the filter cake was washed three times with anhydrous diethyl ether, and dried under vacuum at room temperature for 24 h to obtain the catechol coupling agent;
[0032] The carbon black dispersion was transferred to a 1000 mL three-necked flask, and 200 mL of anhydrous ethanol was added to make a water / ethanol mixture with a water / ethanol volume ratio of approximately 5:3. The pH of the system was slowly adjusted to 4.5 with glacial acetic acid. Then, 1.5 g of catechol coupling agent was dissolved in 50 mL of anhydrous ethanol and slowly added dropwise to the carbon black dispersion over approximately 20 min, with stirring at 300 rpm during the addition. After the addition was complete, the system was heated to 60 °C and reacted for 8 h with stirring at 400 rpm. After the reaction was completed, the mixture was centrifuged at 8000 rpm for 10 min, and the supernatant was discarded. The resulting solid was washed three times with a deionized water / ethanol (1:1) mixed solvent to remove unreacted Cat-Si and hydrolysis byproducts. The washed solid was dried in a vacuum drying oven at 60 °C for 12 h to obtain CB@Cat-Si.
[0033] Preparation of PMA@CB-Cat-Si: 10.0 g of CB@Cat-Si was added to 300 mL of deionized water and dispersed at 5000 rpm for 15 min using a high-speed disperser. The dispersion was then sonicated for 20 min at 300 W for 3 s followed by a 2 s pause to obtain a homogeneous CB@Cat-Si dispersion. The pH of the dispersion was adjusted to 3.5 with 0.1 mol / L dilute hydrochloric acid. 2.0 g of phosphomolybdic acid was dissolved in 50 mL of deionized water to prepare a phosphomolybdic acid aqueous solution. The phosphomolybdic acid aqueous solution was slowly added dropwise to the CB@Cat-Si dispersion under magnetic stirring at 300 rpm, completing the addition in approximately 15 min. After the addition was complete, the mixture was stirred and impregnated for 4 h at room temperature and in the dark. After impregnation, the mixture was centrifuged at 8000 rpm for 10 min, the supernatant was discarded, and the resulting solid was washed twice with deionized water. The washed solid was then dried in a vacuum drying oven at 80℃ for 12 h to obtain PMA@CB-Cat-Si.
[0034] Preparation of modified carbon black grafted PET oligomer masterbatch: 100g of PET chips and 20g of ethylene glycol were added to a reaction vessel. Under nitrogen protection, the system was heated to 220°C and stirred for 3 hours. Then the temperature was raised to 260°C and the system pressure was gradually reduced to below 100Pa. The reaction was carried out for 2 hours to remove excess EG and small molecule byproducts, and carboxyl-terminated PET oligomers were obtained.
[0035] 2 kg of PMA@CB-Cat-Si, 8 kg of PET oligomer, and 50 g of tetrabutyl titanate were mixed in a high-speed mixer for 5 min to obtain a homogeneous premix. The premix was then added to the hopper of a twin-screw extruder for melt grafting reaction. The temperature profile of the twin-screw extruder was set as follows: feeding section 140℃, plasticizing section 180℃ / 210℃, reaction section 235℃ / 240℃ / 235℃, venting section 230℃, homogenizing section 225℃, and die head 220℃. The screw speed was set to 200 rpm, the feeding rate was 5 kg / h, the residence time of the material in the reaction section was approximately 3 min, and the die head pelletizing water temperature was 20°C. After water cooling and pelletizing, the extrudate was dried in a vacuum drying oven at 80°C for 12 h to obtain modified carbon black grafted PET oligomer masterbatch.
[0036] Blending and granulation: Modified carbon black-grafted PET oligomer masterbatch and PET chips were mixed at a mass ratio of 1:4, with 0.2wt% antioxidant 1010 added. The mixture was stirred in a high-speed mixer for 3 minutes to obtain a homogeneous blend. The blend was then added to a twin-screw extruder for melt blending and granulation. Extrusion temperature profile: feeding section 240℃, plasticizing section 260℃ / 270℃, reaction section 275℃ / 280℃ / 275℃, venting section 270℃, homogenization section 265℃, die head 260℃ / 260℃. Screw speed 250 rpm, feed rate 8 kg / h, residence time approximately 3 minutes. The extrudate was water-cooled, granulated, and then vacuum-dried at 120℃ for 12 hours, with a moisture content ≤50 ppm, to obtain light-shielding PET masterbatch.
[0037] Casting and biaxially stretched film formation: Light-shielding PET masterbatch is added to a single-screw extruder with a screw diameter of 3 mm and an L / D ratio of 30. The extrusion is equipped with a metering pump and a T-die with a die width of 200 mm. The extrusion temperatures are: feeding section 250℃, plasticizing section 270℃ / 280℃, metering section 285℃, and die 280℃. The melt is extruded from the T-die via the metering pump and cast onto a chrome-plated cold roller. Electrostatic adhesion ensures the melt adheres tightly to the surface of the cold roller for rapid cooling, resulting in a cast sheet with a thickness of approximately 300 μm.
[0038] The cast sheet was cut into 100mm × 100mm square specimens and subjected to simultaneous biaxial tensile testing on a biaxial tensile testing machine. The process flow and parameters are as follows:
[0039] Preheating: Preheat the sample at 85°C for 30 seconds;
[0040] Longitudinal stretching: stretching temperature 90℃, stretching ratio 3.2 times, stretching speed 10% / s;
[0041] Transverse stretching: stretching temperature 100℃, stretching ratio 3.2 times, stretching speed 10% / s;
[0042] Heat setting: Immediately after stretching, heat set at 210℃ for 15s, while simultaneously applying 2% relaxation in the transverse direction, so that the stretched molecular chains crystallize under tension and release some internal stress.
[0043] Cooling: After heat setting, the crystals are rapidly cooled to room temperature at a rate of 30℃ / s to fix the crystal structure and orientation.
[0044] The thickness of the stretched film is approximately 29 μm, resulting in a light-shielding PET protective film that is resistant to damp heat aging.
[0045] Example 2
[0046] The only difference between Example 2 and Example 1 is that in step S4, the amount of phosphomolybdic acid was adjusted to 1.5 g (i.e., the mass ratio of phosphomolybdic acid to CB@Cat-Si was adjusted from 0.20 to 0.15), the impregnation pH was adjusted to 3.8, and the impregnation time was maintained at 4 h; the remaining steps, raw material amounts, and process parameters were the same as in Example 1, and the resulting film thickness was about 29 μm, which is referred to as Example 2.
[0047] Example 3
[0048] The only difference between Example 3 and Example 1 is that in step S8, the longitudinal and transverse stretching ratios are both adjusted to 3.0 times, the heat setting temperature is adjusted to 215℃, the heat setting time is adjusted to 12 s, and the transverse relaxation amount is maintained at 2%; the remaining steps, raw material amounts, and process parameters are the same as in Example 1, and the resulting film thickness is about 39.5 μm, which is referred to as Example 3.
[0049] Comparative Example 1
[0050] Comparative Example 1 did not undergo any surface modification treatment as described in steps S1-S6. Virgin carbon black was directly mixed with PET chips and 0.2 wt% antioxidant 1010 at the same ratio (approximately 4 wt%) as the final film in Example 1. The mixture was then granulated using a twin-screw extruder and followed by casting and biaxial stretching processes as described in steps S7 and S8 to form a film with a thickness of approximately 30 μm. Comparative Example 1 was used to investigate the dispersion and interfacial state of unmodified carbon black in the PET matrix.
[0051] Comparative Example 2
[0052] Comparative Example 2 underwent the same carbon black purification and pre-dispersion, catechol coupling agent synthesis, and CB@Cat-Si preparation as steps S1-S3, but without the phosphomolybdic acid impregnation in step S4. Subsequently, the same process as steps S5-S8 was followed for the synthesis of carboxyl-terminated PET oligomers, melt grafting, blending and granulation, casting, and biaxial stretching to form a film, resulting in a film thickness of approximately 29 μm. Comparative Example 2 was used to investigate the effect of only a catechol silane shell without the introduction of phosphomolybdic acid on damp heat resistance.
[0053] Comparative Example 3
[0054] Comparative Example 3 underwent the same carbon black purification and pre-dispersion, catechol coupling agent synthesis, CB@Cat-Si preparation, and PMA@CB-Cat-Si preparation as steps S1-S4. However, the synthesis and melt grafting of end-carboxyl PET oligomers described in steps S5 and S6 were omitted. Instead, the obtained PMA@CB-Cat-Si was directly mixed and granulated with PET chips and 0.2 wt% antioxidant 1010 in the same proportion as the final film in Example 1 using a twin-screw extruder. The resulting film was then formed using the same casting and biaxial stretching process as in step S8, yielding a film with a thickness of approximately 28.5 μm. Comparative Example 3 was used to investigate the effect of the carbon black-PET interface on moisture and heat resistance without introducing chemical bonds.
[0055] Performance testing
[0056] 1. The following performance tests were performed on the samples from Examples 1-3 and Comparative Examples 1-3:
[0057] Transmittance: The total transmittance T(λ) was measured by scanning in the visible light range of 380nm to 780nm using an ultraviolet-visible spectrophotometer with air as a reference, and the average transmittance in this range was calculated.
[0058] High-temperature aging: The sample was placed in a 150℃ forced-air oven for 72 h. After being taken out, the transmittance was measured and the transmittance change rate ΔT_high was calculated. At the same time, the CIE Lab* color difference ΔE was measured using a colorimeter.
[0059] Mechanical properties under damp heat aging: The sample was placed under the above damp heat conditions for 500 h. After being taken out, the breaking strength was measured on a tensile testing machine according to the plastic tensile test method. The breaking strength was compared with the initial breaking strength, and the breaking strength retention rate was calculated.
[0060] Mechanical properties: Refer to GB / T 1040.3-2006, measure the stress-strain curve of the sample under the conditions of 23℃ and 50% relative humidity, and record the fracture strength and elongation at break.
[0061] The main performance test results of Examples 1-3 and Comparative Examples 1-3 are summarized in Table 1.
[0062] Table 1. Overall Performance Comparison of Examples and Comparative Examples
[0063] serial number Initial average transmittance (%) Average transmittance (%) after 500 hours at 85℃ / 85%RH Transmittance change rate (%) Color difference ΔE at 150℃ for 72 hours Fracture strength retention rate after damp heat (%) Initial fracture strength (MPa) Initial elongation at break (%) Example 1 0.85 0.92 8.2 1.8 92.4 215 55 Example 2 0.98 1.10 12.2 2.1 89.7 206 52 Example 3 1.12 1.26 12.5 2.0 88.1 198 49 Comparative Example 1 2.15 3.62 68.4 4.6 58.3 145 22 Comparative Example 2 1.45 1.78 22.8 2.9 76.5 168 30 Comparative Example 3 1.28 1.95 52.3 3.4 65.2 175 28
[0064] The changes in transmittance and color difference after high-temperature aging (150℃×72 h) are listed in Table 2.
[0065] Table 2 High-temperature aging performance data (150℃×72h)
[0066] serial number Initial average transmittance (%) Average transmittance (%) after high temperature Transmittance change rate (%) Color difference ΔE Example 1 0.85 0.90 5.9 1.8 Example 2 0.98 1.05 7.1 2.1 Example 3 1.12 1.20 7.1 2.0 Comparative Example 1 2.15 2.85 32.6 4.6 Comparative Example 2 1.45 1.68 15.9 2.9 Comparative Example 3 1.28 1.55 21.1 3.4
[0067] The data on light transmittance and tensile strength retention after damp heat aging (85℃, 85% relative humidity × 500 h) are listed in Table 3.
[0068] Table 3. Damp heat aging performance data (85℃ / 85%RH×500h)
[0069] serial number Light transmittance before humid heat (%) Light transmittance (%) after humid heat Transmittance change rate (%) Surface resistivity drift (orders of magnitude) Tensile strength before damp heat (MPa) Fracture strength (MPa) after damp heat Fracture strength retention rate (%) Example 1 0.85 0.92 8.2 0.43 215 198.7 92.4 Example 2 0.98 1.10 12.2 0.47 206 184.8 89.7 Example 3 1.12 1.26 12.5 0.44 198 174.4 88.1 Comparative Example 1 2.15 3.62 68.4 >1.0 145 84.5 58.3 Comparative Example 2 1.45 1.78 22.8 >1.0 168 128.5 76.5 Comparative Example 3 1.28 1.95 52.3 1.94 175 114.1 65.2
[0070] The transmittance data of each sample at key wavelengths in the visible light region are listed in Table 4.
[0071] Table 4. Transmittance of key wavelengths in the visible light region (unit: %)
[0072] serial number 450 nm 550 nm 650 nm 780 nm Average (380~780 nm) Example 1 0.68 0.78 0.92 1.18 0.85 Example 2 0.82 0.92 1.08 1.38 0.98 Example 3 0.95 1.08 1.25 1.58 1.12 Comparative Example 1 2.05 2.32 2.68 3.05 2.15 Comparative Example 2 1.32 1.48 1.68 1.95 1.45 Comparative Example 3 1.15 1.30 1.50 1.78 1.28
[0073] The mechanical properties of each sample are listed in Table 5.
[0074] Table 5 Mechanical properties of samples from the examples and comparative examples
[0075] serial number Initial fracture strength (MPa) Initial elongation at break (%) Initial Young's modulus (MPa) Fracture strength (MPa) after damp heat Fracture strength retention rate after damp heat (%) Example 1 215 55 2850 198.7 92.4 Example 2 206 52 2780 184.8 89.7 Example 3 198 49 2720 174.4 88.1 Comparative Example 1 145 22 2350 84.5 58.3 Comparative Example 2 168 30 2520 128.5 76.5 Comparative Example 3 175 28 2580 114.1 65.2
[0076] Analyze Tables 1 to 5 and Figure 2 , Figure 3 The following points can be observed:
[0077] First, in Comparative Example 1, which directly blends unmodified carbon black, the initial average transmittance reached 2.15%, which increased to 3.62% after hygrothermal aging, with a change rate as high as 68.4%. The fracture strength retention rate after hygrothermal aging was only 58.3%, and the elongation at break was only 22%. This indicates that unmodified carbon black is poorly dispersed in the PET matrix, and the interface is mainly physically bonded. Under hygrothermal conditions, it rapidly undergoes interfacial debonding and agglomerate light scattering, resulting in a significant decrease in both light-blocking and mechanical properties.
[0078] Second, in Comparative Example 2, which only had Cat-Si coating and no PMA loading, the initial transmittance decreased to 1.45%, indicating that the catechol silane shell effectively improved the carbon black dispersion; however, due to the lack of phosphomolybdic acid, the resistance to damp heat decreased; the transmittance change rate after damp heat was 22.8%, and the fracture strength retention rate was 76.5%, which was better than Comparative Example 1, but still significantly worse than Example 1, indicating that the long-term stability of the interface is still limited when only a silane shell is used and no chemical bonding bridges are introduced.
[0079] Third, in Comparative Example 3, which loads PMA but does not graft PET oligomers, the carbon black-PET interface is still mainly physically bonded because the terminal carboxyl PET oligomers do not form chemical bridges on the carbon black surface. The transmittance change rate is as high as 52.3%, and the tensile strength retention rate is only 65.2%.
[0080] Fourth, Examples 1-3, which simultaneously underwent three-stage modification and PET oligomer grafting, showed initial average transmittance between 0.85% and 1.12%, with transmittance changes after damp heat not exceeding 13%, and tensile strength retention rates all above 88%. Among them, Example 1 exhibited the best overall performance under the conditions of 2.0g PMA, pH 3.5, 4h impregnation, and 3.2× biaxial stretching.
[0081] Depend on Figure 2 As can be seen, the transmittance of all samples increases slowly with increasing wavelength; the entire curve of Example 1 is at the bottom, with the lowest average transmittance of visible light; the curve of Comparative Example 1 is at the top, and the slope is the largest with increasing wavelength, reflecting the light scattering caused by a large number of micron-sized carbon black agglomerates inside.
[0082] Depend on Figure 3 As can be seen, the fracture strength of Examples 1-3 is between 198 and 215 MPa, and the elongation at break is between 49% and 55%. The curves still have a relatively long plastic extension segment after yielding. The fracture strength of Comparative Examples 1-3 is between 145 and 175 MPa, and the elongation at break is between 22% and 30%. The curves show strain softening earlier after yielding, reflecting the early crack propagation caused by carbon black agglomerates and interface defects.
[0083] Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A light-shielding protective film resistant to damp heat aging, characterized in that: It includes a polyethylene terephthalate matrix and modified carbon black dispersed in the matrix; the modified carbon black has a carbon black core and is sequentially coated with a silica shell formed by the hydrolysis and condensation of a catechol coupling agent with silane, a phosphomolybdic acid layer supported on the shell, and carboxyl-terminated polyethylene terephthalate oligomer segments.
2. The light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: The catechol coupling agent is prepared by an addition reaction of dopamine molecules with propyltriethoxysilane 3-isocyanate.
3. The light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: Based on the mass of modified carbon black, the loading of phosphomolybdic acid is 5wt%~20wt%; the phosphomolybdic acid is dodecamolybdic acid with a Keggin structure.
4. The light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: The number-average molecular weight of the terminal carboxyl polyethylene terephthalate oligomer is 1500~6000 g / mol, and the terminal carboxyl value is 30~120 mgKOH / g.
5. The light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: Based on the total mass of the light-shielding protective film, the content of the modified carbon black is 1wt%~8wt%, the content of the polyethylene terephthalate matrix is 85wt%~98wt%, and the balance is additives.
6. The light-shielding protective film resistant to damp heat aging according to claim 5, characterized in that: The adjuvant includes an antioxidant, which is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] in a content of 0.1wt% to 0.5wt%.
7. A method for preparing a light-shielding protective film resistant to damp heat aging as described in any one of claims 1 to 6, characterized in that: Includes the following steps: S1. Carbon black is dispersed in an aqueous phase at high speed and then ultrasonically crushed, followed by centrifugation to obtain the upper dispersion. S2. Under an inert atmosphere, dopamine hydrochloride and triethylamine were neutralized in N,N-dimethylformamide, and then 3-propyltriethoxysilane was added dropwise to carry out an addition reaction, and the catechol coupling agent was separated. S3. Mix the carbon black dispersion obtained in step S1 with anhydrous ethanol, adjust the pH to acidic, add the catechol coupling agent dissolved in anhydrous ethanol dropwise, heat the reaction, centrifuge, wash, and dry to obtain CB@Cat-Si. S4. Disperse CB@Cat-Si in deionized water, adjust the pH to acidic, add phosphomolybdic acid aqueous solution dropwise, impregnate at room temperature in the dark, centrifuge, wash, and dry to obtain PMA@CB-Cat-Si; S5. Polyethylene terephthalate chips were transesterified with ethylene glycol under an inert atmosphere, and then small molecules were removed under vacuum to obtain carboxyl-terminated polyethylene terephthalate oligomers. S6. PMA@CB-Cat-Si, carboxyl-terminated polyethylene terephthalate oligomer and tetrabutyl titanate are premixed and then melt-grafted in a twin-screw extruder, water-cooled pelletized and dried to obtain modified carbon black grafted polyethylene terephthalate oligomer masterbatch. S7. The masterbatch is mixed with polyethylene terephthalate chips and antioxidants in a certain proportion, melt-blended by a twin-screw extruder, water-cooled pelletized, and dried to a moisture content of no more than 50 ppm to obtain light-shielding PET masterbatch. S8. The light-shielding PET masterbatch is extruded and cast into sheets, and then preheated, stretched longitudinally, stretched laterally, heat-set and cooled to obtain the light-shielding protective film resistant to damp heat aging.
8. The method for preparing the light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: In step S2, the addition reaction is carried out at a temperature not exceeding 30°C for a reaction time of 8-16 hours. After the reaction is completed, the reaction solution is poured into anhydrous diethyl ether to precipitate the precipitate, which is then filtered, washed with anhydrous diethyl ether, and dried under vacuum at room temperature.
9. The method for preparing the light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: In step S4, the pH of the dispersion is adjusted to 3.0~4.0, the mass ratio of phosphomolybdic acid to CB@Cat-Si is (0.15~0.30):1, and the impregnation time at room temperature in the dark is 3h~6h.
10. The method for preparing the light-shielding protective film resistant to damp heat aging according to claim 1, characterized in that: The longitudinal stretching temperature is 85℃~95℃ and the stretching ratio is 2.8~3.5; the transverse stretching temperature is 95℃~105℃ and the stretching ratio is 2.8~3.5; the heat setting temperature is 200℃~220℃ and the heat setting time is 10s~20s; and a relaxation of 1%~3% is applied in the transverse direction during heat setting.