Bamboo-based biodegradable bubble film and production process

By constructing a dual network mechanism of chemical bridging and physical springs in biodegradable bubble film, the problems of poor interfacial compatibility and low resin melt strength after the introduction of plant fiber filler are solved, realizing high-strength molding and high load-bearing capacity of bubble film, and improving the overall performance of materials and production efficiency.

CN123131802APending Publication Date: 2026-11-20FUJIAN YANGZHU NEW MATERIALS TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611628896.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing biodegradable bubble films suffer from problems such as decreased mechanical properties due to poor interfacial compatibility when plant fiber fillers are introduced, and high bubble breakage rate and insufficient bubble load-bearing capacity due to low resin melt strength during vacuum forming.

Method used

A chemical bridge is formed on the surface of modified bamboo powder using an ethylene-methyl acrylate-glycidyl methacrylate terpolymer. Covalent bonds are constructed through etherification and esterification reactions. A dynamic physical spring network is formed using zinc ion neutralization of the ethylene-methyl methacrylate copolymer, which enhances the deformation hardening characteristics of the melt. Combined with the pre-coating of modified bamboo powder and vacuum devolatilization in the process, the fluidity and formability of the material are improved.

Benefits of technology

It improves the interfacial compatibility between plant fiber filler and polyester resin, reduces the bubble breakage rate of bubble film, increases the static compression bearing capacity of bubbles, and inhibits the thermal degradation of polyester matrix, thereby improving the overall mechanical properties and molding quality of bubble film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131802A_ABST
    Figure CN123131802A_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of biodegradable packaging materials, and discloses a bamboo-based biodegradable bubble film and a production process, wherein the bubble film is made of polybutylene adipate terephthalate, levorotatory polylactic acid, ethylene-methyl acrylate-glycidyl methacrylate terpolymer, ethylene-methacrylic acid copolymer zinc ion neutralization and modified bamboo powder, and the production process comprises the following steps: preparing modified bamboo powder; feeding polyester resin and copolymer into melting through a main feeding port, adding modified bamboo powder through a side feeding port to perform reaction extrusion and devolatilization; preparing a blister layer and a flat bottom layer base film through casting, performing vacuum blister molding and hot pressing compounding, and improving the interface compatibility of fillers and resin matrix by constructing covalent bond crosslinking structure, improving the transient tensile viscosity of the melt by using a dynamic ion cluster network, and then reducing the blister breaking rate of the blister and improving the compression bearing capacity of the bubble.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biodegradable packaging materials technology, specifically bamboo-based biodegradable bubble wrap and its production process. Background Technology

[0002] Bubble wrap, as a commonly used cushioning packaging material, is widely used in logistics and product packaging. With the increasing environmental protection requirements, the use of biodegradable polyesters such as poly(butylene adipate / terephthalate) and polylactic acid to prepare biodegradable bubble wrap has become an industry trend. In order to further reduce the production cost of materials and improve the rigidity of bubble wrap, plant fibers such as bamboo powder are introduced into the polyester resin matrix as fillers.

[0003] In practical production applications, biodegradable bubble films with plant fiber fillers have limitations. Plant fibers such as bamboo powder contain a large number of free hydroxyl groups on their surface, exhibiting strong polarity and hydrophilicity. In contrast, conventional biodegradable polyester matrices are mostly non-polar or weakly polar materials. The difference in physicochemical properties between the two leads to poor interfacial compatibility between the filler and the resin matrix. Bamboo powder particles will agglomerate in the resin matrix and are difficult to disperse evenly. This separation at the phase interface disrupts the continuity of the material matrix. When subjected to external forces, stress concentration will occur at the interface between the filler and the resin, which in turn causes a decrease in the overall tensile strength and tear strength of the bubble film.

[0004] The processing rheological properties of conventional biodegradable polyester resins are also difficult to adapt to the forming requirements of bubble wrap. The production of bubble wrap requires a vacuum thermoforming process after casting. This process requires the resin melt to generate bidirectional stretching flow under negative pressure suction. The existing polyester resin melt strength is generally low, and the transient stretching viscosity is insufficient when subjected to tensile stress. Especially after mixing in bamboo powder filler, the continuity of the melt under stretching is further damaged. In the vacuum thermoforming stage, due to the lack of an effective deformation hardening mechanism, the melt cannot resist the local rapid stretching and thinning caused by negative pressure, which leads to the rupture of the top or sidewall of the formed bubble, resulting in a high overall bubble breakage rate. At the same time, due to the uneven stretching flow of the material during the forming process, the thickness distribution of the bubble wall after curing is inconsistent, which makes the bubble insufficient in terms of support force when subjected to external pressure. This manifests as the bubble wrap's static compression bearing capacity not meeting the actual use requirements of cushioning packaging. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides bamboo-based biodegradable bubble film and its production process, which solves the problems of decreased mechanical properties due to poor interfacial compatibility when introducing plant fiber fillers in existing biodegradable bubble films, as well as high bubble breakage rate and insufficient bubble load-bearing capacity due to low resin melt strength during vacuum forming.

[0006] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides a bamboo-based biodegradable bubble film, employing the following technical solution: Bamboo-based biodegradable bubble wrap is made from the following materials in parts by weight: 50-70 parts of poly(butylene adipate) / terephthalate; 10-25 parts of polylactic acid (L-L); 1.0-5.0 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer; 1.0-4.0 parts of zinc ion neutralizer of ethylene-methacrylic acid copolymer; 15.62-32.1 parts of modified bamboo powder.

[0007] By employing the above technical solution, this invention constructs a dual network mechanism of chemical bridging and physical springs at the microscopic level. The ethylene-methyl acrylate-glycidyl methacrylate terpolymer acts as a chemical bridge, with its epoxy groups undergoing ring-opening in a high-temperature molten state. One end engages with the exposed cellulose hydroxyl groups on the modified bamboo powder surface, undergoing etherification, while the other end reacts with the carboxyl or hydroxyl groups at the end groups of the matrix resin, resulting in esterification and etherification. This establishes covalent bonds between the incompatible inorganic bamboo powder and organic polyester, anchoring the filler within the resin matrix. The zinc ion neutralizer of the ethylene-methyl acrylate copolymer acts as... The dynamic physical spring, in which zinc ions coordinate with carboxylate groups of polymer chain segments to form reversible ion clusters, under the high shear force of the extruder, the ion clusters temporarily separate like unlocked locks, giving the material fluidity; when the melt flows out of the die and enters the vacuum forming stage, the shear force is unloaded and subjected to bidirectional stretching, the free zinc ions and carboxylate groups seek each other to reassociate and lock together, exhibiting deformation hardening characteristics. This transient stretch viscosity surge effect, which makes the bubble film more and more tough, is like an elastic net attached when it is formed by negative pressure suction, reducing the probability of the bubble wall being ruptured and giving the formed bubble a pressure-resistant load-bearing skeleton.

[0008] Preferably, the modified bamboo powder is a liquid-solid phase pre-coated modified bamboo powder, made from the following materials in parts by weight: 15-30 parts of lignin-de-lignosed bamboo powder; 0.5-1.5 parts of magnesium aluminum hydrotalcite; 0.02-0.1 parts of zinc stearate; and 0.1-0.5 parts of epoxidized soybean oil.

[0009] By employing the above technical solution, bamboo powder undergoes delignin treatment, removing the inert lignin coating surrounding the cellulose and exposing the reactive cellulose skeleton and free hydroxyl groups. This opens up the binding sites for subsequent interfacial reactions. Epoxidized soybean oil, with the lubrication and dispersion synergistic effect of zinc stearate, transforms into an active and compatible coating that encapsulates the bamboo powder. Its inherent epoxy groups first bind with the hydroxyl groups of the bamboo powder, passivating the surface polarity of the bamboo powder and promoting its integration into the polyester matrix. Magnesium aluminum hydrotalcite, as a layered dihydroxy composite metal oxide, transforms into a microscopic acidic sponge during high-temperature processing, adsorbing and neutralizing the acidic free small molecules released from the thermal degradation of polyester resin, blocking the autocatalytic degradation cycle of the polyester matrix, and maintaining the molecular weight stability of the system.

[0010] Preferably, in the ethylene-methyl acrylate-glycidyl methacrylate terpolymer, the mass fraction of ethylene structural units is 65%–75%, the mass fraction of methyl acrylate structural units is 20%–28%, and the mass fraction of glycidyl methacrylate structural units is 5%–10%; in the ethylene-methacrylate copolymer zinc ion neutralizer, the mass fraction of methacrylate structural units is 10%–20%, and the degree of zinc ion neutralization of the carboxylic acid groups is 40%–60%.

[0011] By adopting the above technical solution, the mass fraction of glycidyl methacrylate is controlled within the crosslinking window of 5% to 10%, providing sufficient epoxy group anchor points in the system to hold bamboo powder and resin. At the same time, it avoids the risk of excessive crosslinking and locking of the resin matrix due to excessively dense reaction sites. The zinc ion neutralization degree is set between 40% and 60%, so that the dissociation and association of ion clusters in the system are in a balanced dynamic network. This prevents the network from being too sparse and losing the tear resistance brought by stretch hardening, and also avoids the melt from being too sluggish and difficult to flow due to excessive crosslinking, thus balancing the viscosity and strength required for vacuum forming.

[0012] Secondly, this invention provides a production process for bamboo-based biodegradable bubble film, employing the following technical solution: The production process of bamboo-based biodegradable bubble film includes: preparing modified bamboo powder by mixing delignified bamboo powder with magnesium aluminum hydrotalcite, zinc stearate and epoxidized soybean oil; drying poly(butylene adipate / terephthalate) and polylactic acid (PLA), and then feeding them into an extruder with ethylene-methyl acrylate-glycidyl methacrylate terpolymer and ethylene-methacrylate copolymer zinc ion neutralizer for melt plasticization; feeding modified bamboo powder into the side feed port of the extruder for reactive extrusion and devolatilization to obtain a homogeneous reactive melt; preparing a vacuum-formed base film and a flat base film from the homogeneous reactive melt through a casting process; vacuum forming the vacuum-formed base film and hot-pressing it with the flat base film.

[0013] By adopting the above technical solution, the process intertwines chemical reaction and physical molding. Polyester resin and compatibilizer are first fed into the main feed port to melt, and then modified bamboo powder is fed in through a side channel. This staggered entry strategy reduces the heating time of bamboo powder in the high-temperature environment of the extruder, reducing the risk of carbonization of plant fibers. The in-situ reaction extrusion operation allows the bridging of epoxy groups and the disassembly and recombination of ion clusters to occur simultaneously under the kneading of the twin screw. The devolatilization process is like a suction machine, removing reaction byproducts and water vapor, making the final cast base film clear and homogeneous, and reducing internal bubble defects.

[0014] Preferably, the steps for preparing modified bamboo powder include: drying the lignin-free bamboo powder at 100-110℃ for 6-10 hours, controlling the moisture content to ≤0.5%; adding the dried lignin-free bamboo powder, magnesium aluminum hydrotalcite, and zinc stearate into a high-speed mixer, controlling the rotation speed to 800-1200 r / min, and heating the material to raise the temperature to 50-70℃; adding liquid epoxidized soybean oil into the mixer through an atomizing nozzle, maintaining the corresponding rotation speed and material temperature for continuous mixing for 5-15 minutes before discharging.

[0015] By adopting the above technical solution, the liquid epoxidized soybean oil is torn into micron-sized liquid mist by means of the fragmentation effect of the atomizing nozzle, and penetrates into the deep pores of the lignin-free bamboo powder in the centrifugal vortex of the high-speed mixer. The 50-70°C thermal field is like a hotbed for catalytic penetration, giving the epoxidized soybean oil molecules peristaltic activity, allowing the pre-coated outer layer of the solid and liquid phases to penetrate into the fiber texture.

[0016] Preferably, the melt plasticizing step includes: drying poly(butylene adipate) / poly(terephthalate) and polylactic acid (PLA) at a vacuum of -0.08 to -0.10 MPa and a temperature of 70 to 90°C for 3 to 5 hours, controlling the moisture content to be less than 0.02%; and simultaneously feeding the dried resin mixture, ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and ethylene-methacrylate copolymer zinc ion neutralizer through the main feed port of a twin-screw extruder, controlling the rotation speed to be 200 to 300 r / min, and setting the temperature of zones 1 to 4 to be 155 to 175°C.

[0017] By adopting the above technical solution, vacuum drying is like a dehydration process, which removes free water molecules dormant in the resin and cuts off the path of chain scission caused by hydrolysis of polyester at high temperature. The material advances into the barrel at 155-175°C, the matrix resin melts into a melt, and the zinc ion clusters in the zinc ion neutralizer of ethylene-methacrylic acid copolymer are then decomposed by heat. The system loses its solid skeleton and becomes a fused fluid phase environment, which can accommodate the subsequent incorporation and interweaving of bamboo powder.

[0018] Preferably, the reactive extrusion and devolatilization steps include: forcibly feeding modified bamboo powder into the feed port of zone 5, setting the temperature of zones 5 to 7 to 160 to 180°C for reactive extrusion, opening a vacuum devolatilization of -0.08 to -0.098 MPa in zone 8, and the material continuing to pass through zones 9 to 10 at 165 to 175°C.

[0019] By adopting the above technical solution, after the modified bamboo powder is introduced, the material is placed in a reaction furnace at 160-180°C. The epoxy groups exhibit ring-opening and interlocking capabilities, grafting macromolecular chain segments onto the surface of the bamboo powder to complete microscopic rooting and sprouting. The vacuum devolatilization zone acts as a turbidity removal checkpoint, using negative pressure to remove the mixed water vapor and small volatile molecules generated by the reaction, eliminating the path of micropores and dark bubbles generated inside the melt due to gas expansion. In the homogenization zone, it is kneaded into a dense and stable high-pressure melt.

[0020] Preferably, the steps of preparing the base film and hot-pressing lamination include: preparing a vacuum-formed base film with a thickness of 60-80 μm and a flat base film with a thickness of 20-40 μm using a casting die at a temperature of 165-175°C and a water-cooled roller surface temperature of 20-30°C; introducing the vacuum-formed base film into a forming roller at 85-105°C, stretching it to form bubbles under a vacuum of -0.07 to -0.09 MPa, and simultaneously hot-pressing it with the flat base film at a temperature of 80-100°C and a pressure of 0.3-0.5 MPa.

[0021] By adopting the above technical solution, the thermoforming range of 85-105℃ is at the awakening critical point of zinc ion dynamic network reconstruction. When the negative pressure of -0.07 to -0.09MPa is applied downward to draw and pull, the deformation stress awakens the clustering and association of free zinc ions, and stimulates the deformation hardening effect. Just like pulling a rubber band that gets tighter and tighter, the surge in transient tensile viscosity supports the dome at the top of the bubble, maintaining uniform thickness. The flat base film is laminated under the catalysis of heat and extrusion at 80-100℃. The polymer molecular chains at the junction of the two films are like intertwined tendrils, which entangle and penetrate each other under the drive of heat energy, and bite together to complete the thermo-press sealing.

[0022] This invention provides bamboo-based biodegradable bubble film and its production process. It has the following beneficial effects: 1. This invention improves the interfacial compatibility between plant fiber fillers and polyester resins, ensuring the mechanical properties of the bubble film. By introducing an ethylene-methyl acrylate-glycidyl methacrylate terpolymer into the poly(dibutyl terephthalate) and polylactic acid (PLA) matrix, and utilizing the etherification and esterification reactions between the epoxy groups on the molecular chain and the cellulose hydroxyl groups of the modified bamboo powder and the polyester end groups, a covalent cross-linked structure is constructed between the resin matrix and the bamboo powder filler. This reduces interfacial defects and improves the dispersion state of bamboo powder in the system, enabling the bubble film to maintain good overall mechanical properties while increasing the amount of bamboo powder used to reduce costs.

[0023] 2. This invention effectively reduces the bubble breakage rate of bubble film during vacuum forming and improves the static compressive strength of the bubbles. The zinc ion neutralizer of ethylene-methacrylic acid copolymer added to the formula can form a dynamic and reversible ion cluster network in the system. Under the high shear of extrusion processing, the ion clusters dissociate to maintain the normal flowability of the material. When entering the vacuum forming stage, with the elimination of shear stress and the application of negative pressure stretching, zinc ions and carboxylate groups re-coordinate and associate, causing the melt to undergo deformation hardening. This mechanism improves the transient tensile viscosity and melt strength of the melt, ensuring that the bubble wall has sufficient resistance to deformation and will not break when subjected to negative pressure suction.

[0024] 3. This invention inhibits the thermal degradation of the polyester matrix during processing and improves the appearance quality of the cast film. In terms of process, epoxidized soybean oil is used to pre-coat the lignin-free bamboo powder, and the powder is fed through the side feed port of the extruder, which shortens the residence time of the bamboo powder in the high-temperature environment and reduces the risk of thermal carbonization of plant fibers. At the same time, the magnesium aluminum hydrotalcite in the formula can absorb the acidic free small molecules generated by the polyester when heated, blocking the autocatalytic degradation path of the matrix. Combined with the vacuum devolatilization operation in the later stage of the process, the moisture and volatiles in the system are concentrated and discharged, eliminating the potential factors that cause micropores and bubble defects inside the base film. Attached Figure Description

[0025] Figure 1 The samples of Example 2 and Comparative Examples 2 and 3 of the present invention were subjected to a temperature of 1575 cm⁻¹. -1 Infrared absorption spectrum of the characteristic absorption region of the nearby carboxylate; Figure 2 The samples of Example 2 and Comparative Examples 2 and 3 of the present invention were subjected to a temperature of 910 cm. -1 Infrared absorption spectrum of the characteristic absorption region of nearby epoxy groups; Figure 3 The graphs show the transient tensile viscosity of the samples from Example 2 and Comparative Examples 4 and 5 of this invention as a function of tensile time; wherein, Figure 3 (a) is a linear coordinate curve of transient tensile viscosity as a function of tensile time; Figure 3 (b) is a logarithmic graph showing the change of transient tensile viscosity with tensile time; Figure 4 The figures show the dynamic thermomechanical analysis test curves of the samples from Example 2 and Comparative Examples 1 and 3 of the present invention; wherein, Figure 4 (a) is a graph showing the change of the loss tangent of the sample with temperature; Figure 4 (b) is a graph showing the change of the storage modulus of the sample with temperature; Figure 5 This is a bar chart showing the molding quality test results of the embodiments and comparative samples of the present invention; wherein, Figure 5 (a) is a bar chart showing the vacuum forming bubble breaking rate test results of samples from Examples 1, 2, 4 and Comparative Examples 2, 3, and 4; Figure 5 (b) is a bar chart showing the test results of the average wall thickness at the top of the bubble for the samples of Examples 1, 2, 4 and Comparative Examples 2, 3, and 4; Figure 6 The figures show the static compression load-displacement test curves of bubbles for some embodiments and comparative samples of the present invention; wherein, Figure 6 (a) is a test curve showing the change of compressive load as a function of compressive displacement for the samples of Example 1, Example 2 and Comparative Example 1 and Comparative Example 3; Figure 6 (b) is a test curve showing the change of compressive load with compressive displacement for the samples of Example 2, Comparative Example 2, and Comparative Example 4; Figure 7 The figures show the basic mechanical property test results of the embodiments and comparative samples of the present invention; wherein, Figure 7 (a) is a test curve showing the longitudinal tensile stress as a function of strain for the samples of Example 2, Comparative Example 1, and Comparative Example 3. Figure 7 (b) Bar chart showing the dart impact damage quality test results of samples from Examples 2, 4, and Comparative Examples 1 to 4; Figure 8 The graphs shown are test curves illustrating the changes in biodegradability of the embodiments, comparative examples, and references of the present invention over composting time; wherein, Figure 8 (a) is a test curve showing the change in biodegradation rate of samples from Examples 1, 2, and 5 over composting time; Figure 8 (b) is a test curve showing the change in biodegradation rate of Example 2, Comparative Example 1 and standard reference as a function of composting time. Detailed Implementation

[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] The main raw materials and reagents used in the following examples and comparative examples and their specifications are as follows. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.

[0028] Poly(butylene adipate) terephthalate has a weight-average molecular weight of 80,000–120,000 g / mol and a melt flow rate of 2.0–5.0 g / 10 min at 190 °C and 2.16 kg.

[0029] The L-type polylactic acid has a mass fraction of less than 2% for the L-type and D-type lactic acid structural units, a weight-average molecular weight of 100,000–150,000 g / mol, and a melt flow rate of 3.0–8.0 g / 10 min at 190 °C and 2.16 kg.

[0030] Deligninated bamboo powder is a plant fiber material obtained by deligninating bamboo powder, wherein the residual lignin mass fraction is less than 5% and the particle size is 300-500 mesh.

[0031] The terpolymer of ethylene-methyl acrylate-glycidyl methacrylate has a mass fraction of 65%–75% for ethylene structural units, 20%–28% for methyl acrylate structural units, and 5%–10% for glycidyl methacrylate structural units. The melt flow rate at 190℃ and 2.16 kg is 4.0–8.0 g / 10 min.

[0032] The zinc ion neutralized ethylene-methacrylic acid copolymer has a methacrylic acid structural unit mass fraction of 10%–20% and a zinc ion neutralization degree of 40%–60% for the carboxylic acid groups. The melt flow rate at 190℃ and 2.16 kg is 1.0–3.0 g / 10 min.

[0033] Magnesium aluminum hydrotalcite has an interlayer spacing of 0.75–0.85 nm and an average particle size of 0.2–0.8 μm.

[0034] Epoxidized soybean oil has an epoxy value of 6.0%–6.5% and an iodine value of less than 3.0g / 100g.

[0035] Zinc stearate, purity ≥99.5%.

[0036] Preparation Example 1: This preparation example provides a method for preparing liquid-solid phase pre-coated modified bamboo powder, including the following steps: (1) Place the lignin-free bamboo powder in a forced-air drying oven and dry it at 110℃ for 10 hours, controlling the moisture content to be ≤0.5%; (2) Add 30 parts of dried lignin-free bamboo powder, 1.5 parts of magnesium aluminum hydrotalcite, and 0.1 parts of zinc stearate into a high-speed mixer; start the mixer and control the speed to 1200 r / min, and use the mixer jacket heating to raise the material temperature to 70℃; (3) Then, 0.5 parts of liquid epoxidized soybean oil were sprayed into the mixer through the atomizing nozzle. The mixture was continuously mixed for 15 minutes at a speed of 1200 r / min and a material temperature of 70°C to obtain modified bamboo powder A.

[0037] Preparation Example 2: This preparation example provides a method for preparing liquid-solid phase pre-coated modified bamboo powder, including the following steps: (1) Place the lignin-free bamboo powder in a forced-air drying oven and dry it at 105℃ for 8 hours, controlling the moisture content to be ≤0.5%; (2) Add 22.5 parts of dried lignin-free bamboo powder, 1.0 part of magnesium aluminum hydrotalcite, and 0.06 parts of zinc stearate into a high-speed mixer; start the mixer and control the speed to 1000 r / min, and use the mixer jacket heating to raise the material temperature to 60℃; (3) Then, 0.3 parts of liquid epoxidized soybean oil were sprayed into the mixer through the atomizing nozzle. The mixture was continuously mixed for 10 minutes at a speed of 1000 r / min and a material temperature of 60°C to obtain modified bamboo powder B.

[0038] Preparation Example 3: This preparation example provides a method for preparing liquid-solid phase pre-coated modified bamboo powder, including the following steps: (1) Place the lignin-free bamboo powder in a forced-air drying oven and dry it at 100℃ for 6 hours, controlling the moisture content to be ≤0.5%; (2) Add 15 parts of dried lignin-free bamboo powder, 0.5 parts of magnesium aluminum hydrotalcite, and 0.02 parts of zinc stearate into a high-speed mixer; start the mixer and control the speed to 800 r / min, and use the mixer jacket heating to raise the material temperature to 50℃; (3) Then, 0.1 parts of liquid epoxidized soybean oil were sprayed into the mixer through the atomizing nozzle. The mixture was continuously mixed for 5 minutes at a speed of 800 r / min and a material temperature of 50°C to obtain modified bamboo powder C.

[0039] Example 1: This embodiment provides a production process for bamboo-based biodegradable bubble film, including the following steps: (1) Place 70 parts of poly(dibutyl terephthalate) and 25 parts of poly(lactic acid) in a vacuum drying oven and dry for 5 hours at a vacuum of -0.09 MPa and 90°C, controlling the moisture content to be less than 0.02% to obtain a dried resin mixture. (2) The dry resin mixture, 5.0 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and 4.0 parts of ethylene-methacrylic acid copolymer zinc ion neutralizer are simultaneously fed into the main feed port of the twin-screw extruder. The speed of the twin-screw extruder is controlled at 300 r / min, and the temperature of the first to fourth zones of the extruder is set at 175°C to melt and plasticize the material. (3) 32.1 parts of modified bamboo powder A are forcibly fed into the feed port of the fifth zone of the extruder. The temperature of the fifth to seventh zones is set at 180°C for reactive extrusion. An exhaust port is set in the eighth zone and vacuum devolatilization is turned on. The vacuum degree is controlled at -0.098MPa. The material continues to pass through the ninth to tenth zones at a temperature of 175°C to obtain a homogeneous reactive melt. (4) Using homogeneous reactive melts of the same composition, vacuum forming base film and flat base film are prepared by independent casting process. The casting die head temperature is 175℃, the surface temperature of the water-cooled roller is 30℃, the traction speed is 15m / min, and the thickness of vacuum forming base film is controlled to 70μm and the thickness of flat base film is controlled to 30μm by adjusting the die head gap. (5) The thermoforming base film is introduced into the vacuum thermoforming roller at 105°C and stretched to form bubbles under a vacuum of -0.09MPa. At the same time, the flat bottom base film is introduced and hot-pressed with the thermoforming layer under a temperature of 100°C and a pressure of 0.5MPa. After traction, cooling and cutting, bamboo-based biodegradable bubble film is obtained.

[0040] Example 2: This embodiment provides a production process for bamboo-based biodegradable bubble film, including the following steps: (1) Place 60 parts of poly(dibutyl terephthalate) and 17.5 parts of poly(lactic acid) in a vacuum drying oven and dry at -0.10 MPa vacuum and 80°C for 4 h, controlling the moisture content to be less than 0.02% to obtain a dried resin mixture. (2) The dried resin mixture, 3.0 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and 2.5 parts of ethylene-methacrylic acid copolymer zinc ion neutralizer are simultaneously fed into the main feed port of the twin-screw extruder. The speed of the twin-screw extruder is controlled at 250 r / min, and the temperature of the first to fourth zones of the extruder is set at 165°C to melt and plasticize the material. (3) 23.86 parts of modified bamboo powder B are forcibly fed into the feed port of the 5th zone of the extruder. The temperature of the 5th to 7th zones is set at 170°C for reactive extrusion. An exhaust port is set in the 8th zone and vacuum devolatilization is turned on. The vacuum degree is controlled at -0.089MPa. The material continues to pass through the 9th to 10th zones at a temperature of 170°C to obtain a homogeneous reactive melt. (4) Using homogeneous reactive melts of the same composition, vacuum forming base film and flat base film are prepared by independent casting process. The casting die temperature is 170℃, the surface temperature of the water-cooled roller is 25℃, the traction speed is 12m / min, and the thickness of vacuum forming base film is controlled to 80μm and the thickness of flat base film is controlled to 40μm by adjusting the die gap. (5) The thermoforming base film is introduced into the vacuum thermoforming roller at 95°C and stretched to form bubbles under a vacuum of -0.08MPa. At the same time, the flat bottom base film is introduced and hot-pressed with the thermoforming layer under a temperature of 90°C and a pressure of 0.4MPa. After traction, cooling and cutting, bamboo-based biodegradable bubble film is obtained.

[0041] Example 3: This embodiment provides a production process for bamboo-based biodegradable bubble film, including the following steps: (1) Place 50 parts of poly(dibutyl terephthalate) and 10 parts of poly(lactic acid) in a vacuum drying oven and dry at -0.08 MPa vacuum and 70°C for 3 h, controlling the moisture content to be less than 0.02% to obtain a dried resin mixture. (2) The dry resin mixture, 1.0 part of ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and 1.0 part of ethylene-methacrylic acid copolymer zinc ion neutralizer are simultaneously fed into the main feed port of the twin-screw extruder. The speed of the twin-screw extruder is controlled at 200 r / min, and the temperature of the first to fourth zones of the extruder is set at 155°C to melt and plasticize the material. (3) 15.62 parts of modified bamboo powder C were forcibly fed into the feed port of the fifth zone of the extruder. The temperature of the fifth to seventh zones was set at 160°C for reactive extrusion. An exhaust port was set in the eighth zone and vacuum devolatilization was turned on. The vacuum degree was controlled at -0.08MPa. The material continued to pass through the ninth to tenth zones at a temperature of 165°C to obtain a homogeneous reactive melt. (4) Using homogeneous reactive melts of the same composition, vacuum forming base film and flat base film are prepared by independent casting process. The casting die head temperature is 165℃, the surface temperature of the water-cooled roller is 20℃, the traction speed is 10m / min, and the thickness of vacuum forming base film is controlled to 60μm and the thickness of flat base film is controlled to 20μm by adjusting the die head gap. (5) The thermoforming base film is introduced into the vacuum thermoforming roller at 85°C and stretched to form bubbles under a vacuum of -0.07MPa. At the same time, the flat bottom base film is introduced and hot-pressed with the thermoforming layer under a temperature of 80°C and a pressure of 0.3MPa. After traction, cooling and cutting, bamboo-based biodegradable bubble film is obtained.

[0042] Example 4: This embodiment provides a production process for bamboo-based biodegradable bubble film, including the following steps: (1) Place 55 parts of poly(dibutyl terephthalate) and 22.5 parts of poly(lactic acid) in a vacuum drying oven and dry for 4 hours at a vacuum of -0.085 MPa and 80°C, controlling the moisture content to be less than 0.02% to obtain a dried resin mixture. (2) The dried resin mixture, 3.0 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and 2.5 parts of ethylene-methacrylic acid copolymer zinc ion neutralizer are simultaneously fed into the main feed port of the twin-screw extruder. The speed of the twin-screw extruder is controlled at 250 r / min, and the temperature of the first to fourth zones of the extruder is set at 165°C to melt and plasticize the material. (3) 23.86 parts of modified bamboo powder B are forcibly fed into the feed port of the 5th zone of the extruder. The temperature of the 5th to 7th zones is set at 170°C for reactive extrusion. An exhaust port is set in the 8th zone and vacuum devolatilization is turned on. The vacuum degree is controlled at -0.089MPa. The material continues to pass through the 9th to 10th zones at a temperature of 170°C to obtain a homogeneous reactive melt. (4) Using homogeneous reactive melts of the same composition, vacuum forming base film and flat base film are prepared by independent casting process. The casting die head temperature is 170℃, the surface temperature of the water-cooled roller is 25℃, the traction speed is 12m / min, and the thickness of vacuum forming base film is controlled to 75μm and the thickness of flat base film is controlled to 35μm by adjusting the die head gap. (5) The thermoforming base film is introduced into the vacuum thermoforming roller at 95°C and stretched to form bubbles under a vacuum of -0.08MPa. At the same time, the flat bottom base film is introduced and hot-pressed with the thermoforming layer under a temperature of 90°C and a pressure of 0.4MPa. After traction, cooling and cutting, bamboo-based biodegradable bubble film is obtained.

[0043] Example 5: This embodiment provides a production process for bamboo-based biodegradable bubble film, including the following steps: (1) Place 60 parts of poly(dibutyl terephthalate) and 17.5 parts of poly(lactic acid) in a vacuum drying oven and dry for 4 hours at a vacuum of -0.095 MPa and 80°C, controlling the moisture content to be less than 0.02% to obtain a dried resin mixture. (2) The dry resin mixture, 4.5 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and 3.5 parts of ethylene-methacrylic acid copolymer zinc ion neutralizer are simultaneously fed into the main feed port of the twin-screw extruder. The speed of the twin-screw extruder is controlled at 250 r / min, and the temperature of the first to fourth zones of the extruder is set at 165°C to melt and plasticize the material. (3) 32.1 parts of modified bamboo powder A are forcibly fed into the feed port of the fifth zone of the extruder. The temperature of the fifth to seventh zones is set at 170°C for reactive extrusion. An exhaust port is set in the eighth zone and vacuum devolatilization is turned on. The vacuum degree is controlled at -0.089MPa. The material continues to pass through the ninth to tenth zones at a temperature of 170°C to obtain a homogeneous reactive melt. (4) Using homogeneous reactive melts of the same composition, the thermoforming base film and the flat base film are prepared by independent casting processes. The casting die head temperature is 170℃, the surface temperature of the water-cooled roller is 25℃, and the traction speed is 12m / min. The thickness of the thermoforming base film is controlled to 65μm and the thickness of the flat base film is controlled to 25μm by adjusting the die head gap. (5) The thermoforming base film is introduced into the vacuum thermoforming roller at 95°C and stretched to form bubbles under a vacuum of -0.08MPa. At the same time, the flat bottom base film is introduced and hot-pressed with the thermoforming layer under a temperature of 90°C and a pressure of 0.4MPa. After traction, cooling and cutting, bamboo-based biodegradable bubble film is obtained.

[0044] Comparative Example 1: Compared with Example 2, the difference is that modified bamboo powder B was not added and the side feeding operation in step (3) was not performed, but the rest are the same.

[0045] Comparative Example 2: Compared with Example 2, the difference is that the modified bamboo powder B was not prepared in advance. Instead, 22.5 parts of lignin-de-lignosed bamboo powder, 1.0 parts of magnesium aluminum hydrotalcite, 0.3 parts of epoxidized soybean oil, 0.06 parts of zinc stearate and the dried resin mixture obtained in step (1) were fed into the main feed port in step (2) at the same time. The side feeding operation in step (3) was not performed. All other steps were the same.

[0046] Comparative Example 3: Compared with Example 2, the difference is that the ethylene-methyl acrylate-glycidyl methacrylate terpolymer was not added in step (2), but all other steps are the same.

[0047] Comparative Example 4: Compared with Example 2, the difference is that no zinc ion neutralizer of ethylene-methacrylic acid copolymer was added in step (2), otherwise the same.

[0048] Comparative Example 5: Compared with Example 2, the difference is that the material forcibly fed in step (3) is modified bamboo powder without magnesium aluminum hydrotalcite, that is, magnesium aluminum hydrotalcite was not added when the modified bamboo powder was prepared, and the rest are the same.

[0049] Comparative Example 6: Compared with Example 2, the difference is that the material forcibly fed in step (3) is modified bamboo powder without epoxidized soybean oil, that is, no epoxidized soybean oil was added when preparing the modified bamboo powder, and the rest are the same.

[0050] Test Example 1: (1) Take 5g of each of the biodegradable bubble film samples prepared in Example 2, Comparative Example 2 and Comparative Example 3, and freeze them in liquid nitrogen environment for 15min. After the samples become brittle, use a micro pulverizer to pulverize them at low temperature and collect the powder that passes through a 200-mesh standard sieve as the original test sample.

[0051] (2) The obtained test sample was placed in a vacuum drying oven and dried at 40°C for 24 hours to remove surface adsorbed moisture. Then, the test sample was mixed with spectral grade potassium bromide powder at a mass ratio of 1:150 and ground in an agate mortar in a single direction for 5 minutes.

[0052] (3) Take 200mg of the ground mixed powder and fill it into the tableting mold. Apply a pressure of 15MPa on the hydraulic press and hold for 2min to press it into potassium bromide tablets of uniform thickness.

[0053] (4) Place the pressed slice in the sample chamber of the Fourier transform infrared spectrometer, collect the background spectrum using blank potassium bromide pellets, and set the scanning wavenumber range to 4000 to 400 cm⁻¹. -1 The spectral resolution was set to 4cm. -1 A total of 32 scans were performed in a single test to obtain the infrared absorbance spectrum curves of each sample.

[0054] (5) Baseline correction was performed on the collected raw data using spectral analysis software, and the baseline was adjusted to 1750 cm⁻¹. -1 The carbonyl stretching vibration peak of the polyester matrix was normalized using the internal standard, and the characteristic absorption peak intensity data of a specific wavenumber range were extracted.

[0055] Table 1. Normalized absorbance data of characteristic infrared absorption peaks of Example 2 and Comparative Examples 2 and 3:

[0056] From Table 1 and Figure 1 and Figure 2 Therefore, 1575cm -1 The nearby absorption band characterizes the carboxylate structure in the system, 910 cm⁻¹ -1The absorption bands near the system characterize the epoxy groups in the system. Example 2 shows the absorption band at 1575 cm⁻¹. -1 The absorbance at 910 cm⁻¹ was 0.814, higher than that of Comparative Example 2 (0.263) and Comparative Example 3 (0.914). -1 The normalized absorbance of the sample was 0.046; the normalized absorbance of Example 2 was 0.127; and the normalized absorbance of Comparative Example 2 was 0.408.

[0057] Test Example 2: (1) Homogeneous reaction materials were extracted from the reaction extrusion process of Example 2, Comparative Example 4 and Comparative Example 5 respectively, and the sheets with a thickness of 0.7 mm were prepared by pressing under pressure of 170°C and 10 MPa for 3 min and then placed at room temperature for natural cooling.

[0058] (2) Use a standard cutter to cut the cooled sheet into rectangular samples with a length of 18 mm and a width of 10 mm.

[0059] (3) Install the tensile rheological fixture on the rotational rheometer, set the test environment temperature and keep it constant to 170°C.

[0060] (4) Clamp the sample between the two drums of the tensile rheological fixture, close the heating environment box, and keep it warm for 3 minutes.

[0061] (5) Set a constant Hench tensile strain rate of 1.0 s. -1 The test is started, and the rheometer records the torque and rotor displacement data during the stretching process. The transient tensile viscosity changes over time, and the data is collected until the sample undergoes melt fracture or tensile yielding.

[0062] Table 2 Transient tensile viscosity test data of Example 2 and Comparative Examples 4 and 5:

[0063] From Table 2 and Figure 3 It can be seen that: the tensile viscosity of Example 2 showed an increasing trend throughout the entire test time, reaching 142055.4 Pa·s at 3.0s; the tensile viscosity of Comparative Example 4 showed a decreasing trend after reaching 20145.8 Pa·s at 2.0s; and the tensile viscosity of Comparative Example 5 showed a decreasing trend after reaching 26850.7 Pa·s at 2.5s. In the larger Hench strain region, the transient tensile viscosity value of Example 2 was higher than that of Comparative Example 4 and Comparative Example 5.

[0064] Test Example 3: (1) From the production casting process of Example 2, Comparative Example 1 and Comparative Example 3, the flat bottom base film that has not been thermoformed was extracted and placed in an environment with a temperature of 23°C and a relative humidity of 50% for 48 hours.

[0065] (2) Use a punch along the longitudinal direction of the base film to cut out a rectangular strip with a length of 30 mm and a width of 5 mm, and the thickness of the strip is 30 μm.

[0066] (3) Clamp the rectangular strip in the film stretching fixture of the dynamic thermomechanical analyzer, set the initial spacing of the clamps to 15 mm, and apply an initial static pre-stretching force of 0.05 N to the strip.

[0067] (4) The test was conducted under a high-purity nitrogen protective atmosphere, with the dynamic strain amplitude set to 0.1% and the vibration frequency set to 1Hz.

[0068] (5) Set the temperature scanning program, with the starting temperature at -60℃ and the temperature rising linearly to 80℃ at a rate of 3℃ / min. The instrument records the energy storage modulus and loss tangent data of the sample during the heating process and calculates the half-peak width of the characteristic loss tangent peak.

[0069] Table 3. Dynamic thermomechanical analysis characteristic data of Example 2 and Comparative Examples 1 and 3:

[0070] From Table 3 and Figure 4 It can be seen that: the temperature corresponding to the low-temperature loss tangent peak of Comparative Example 1 is -31.2℃, the half-width of the loss tangent peak is 10.4℃, and the energy storage modulus at 25℃ is 285.3MPa; the temperature corresponding to the low-temperature loss tangent peak of Comparative Example 3 is -29.8℃, the half-width of the peak is 11.2℃, and the energy storage modulus at 25℃ is 645.8MPa; and the temperature corresponding to the low-temperature loss tangent peak of Example 2 is -24.3℃, the half-width of the peak is 18.7℃, and the energy storage modulus at 25℃ is 412.5MPa.

[0071] Test Example 4: (1) After the production lines of Examples 1 to 5 and Comparative Examples 1 to 6 have been running continuously and stably for 30 minutes, biodegradable bubble film with a length of 10m and a width of standard production width is cut from the winding section as test samples. The bubble diameter of the bubble forming mold is set to 10mm, the bubble height is set to 4mm, and the center distance between adjacent bubbles is set to 12mm.

[0072] (2) Lay the obtained test sample flat on the backlight detection stage, and mark 3 areas with a size of 1m² in the center of the sample. 2 The detection array.

[0073] (3) Count the total number of bubble units in each detection array, count the number of bubble units with top rupture, root unclosed leakage and pressure collapse to calculate the bubble breaking rate, and take the arithmetic mean of the three arrays as the vacuum forming bubble breaking rate of the sample.

[0074] (4) Randomly select 20 bubbles from the complete bubble unit of each sample and cut them along the central axis where the highest point of the bubble is located.

[0075] (5) Use a mechanical thin film thickness gauge to measure the solid wall thickness of the top of the bubble after it has been cut, record and calculate the average value as the average wall thickness of the top of the bubble.

[0076] Table 4 Molding quality test data of Examples 1 to 5 and Comparative Examples 1 to 6:

[0077] From Table 4 and Figure 5 It can be seen that the vacuum forming bubble breaking rate of Examples 1 to 5 is in the range of 1.1% to 2.3%, and the average wall thickness of the bubble top is in the range of 26.8 to 32.4 μm. The vacuum forming bubble breaking rate of Comparative Example 4 is 34.5%, and the average wall thickness of the bubble top is 7.2 μm. The vacuum forming bubble breaking rate of Comparative Examples 2, 5, and 6 is higher than that of Example 2, and the average wall thickness of the bubble top is lower than that of Example 2. The vacuum forming bubble breaking rate of Comparative Example 3 is 18.2%, and the average wall thickness of the bubble top is 13.5 μm.

[0078] Test Example 5: (1) Under the conditions of temperature 23℃ and relative humidity 50%, each sample was laid flat and left to stand for 48 hours.

[0079] (2) Cut out a square test block with a side length of 100mm in the center area at least 50mm from the edge of each bubble film, ensuring that the block contains complete and consistent bubble units.

[0080] (3) Place the test sample flat on the center of the lower platen of the universal testing machine, adjust the height of the upper platen so that it just touches but does not squeeze the highest point of the bubble film, and set the displacement to zero at this time.

[0081] (4) Set the downward compression rate of the upper pressure plate to 10 mm / min and start the test to apply a static compression load to the bubble film.

[0082] (5) Continuously collect load and displacement data during the compression process until the bubble ruptures irreversibly or the base film yields and collapses. Record the maximum compression load as the maximum static compression bearing capacity of the sample block. Repeat the test 5 times for each group of samples and calculate the average value.

[0083] Table 5. Test data of static compressive strength of bubbles in Examples 1 to 5 and Comparative Examples 1 to 6:

[0084] From Table 5 and Figure 6It can be seen that: the maximum static compression bearing capacity of Comparative Example 1 is 142.3 N, and the instantaneous displacement upon crushing is 2.6 mm; the maximum static compression bearing capacity of Comparative Example 3 is 112.8 N, and the instantaneous displacement upon crushing is 1.4 mm; the maximum static compression bearing capacity of Example 2 is 212.7 N, and the instantaneous displacement upon crushing is 3.6 mm; the maximum static compression bearing capacity of Comparative Example 4 is 91.2 N, and the instantaneous displacement upon crushing is 2.3 mm; the maximum static compression bearing capacity and instantaneous displacement of Comparative Examples 2, 5, and 6 are all lower than those of Example 2.

[0085] Test Example 6: (1) Extract the flat bottom base film from each production line that has not undergone vacuum forming process, and place it in an environment of 23°C and 50% relative humidity for 24 hours to adjust to a static state.

[0086] (2) A dumbbell-shaped tensile test strip with a length of 150 mm and a width of 10 mm is punched out along the extrusion traction direction of the base film.

[0087] (3) Clamp the specimen in the universal testing machine with a gauge length of 50 mm and perform tensile testing at a tensile rate of 500 mm / min. Record the stress and strain data, extract the longitudinal tensile strength and longitudinal elongation at break, test 5 specimens in each group and calculate the average value.

[0088] (4) Cut out square samples with a side length of 200 mm from the remaining base film after adjustment, and control the film thickness to 30 μm.

[0089] (5) Fix the sample to the dart impact tester and, referring to Method A in GB / T9639.1-2008, use a hemispherical dart with a diameter of 38mm to drop from a height of 0.66m to conduct the impact test.

[0090] (6) Record the test results of 20 consecutive samples and calculate the dart impact damage mass when 50% of the samples are damaged.

[0091] Table 6. Basic mechanical property test data of Examples 1 to 5 and Comparative Examples 1 to 6:

[0092] From Table 6 and Figure 7 It can be seen that: the elongation at break of Comparative Example 1 was 585.1%, the tensile strength of Comparative Example 3 was 30.1 MPa, the elongation at break was 43.6%, and the dart impact breakage mass was 61.5 g, the elongation at break of Example 2 was 482.4%, the tensile strength was 36.5 MPa, and the dart impact breakage mass was 215.7 g. The longitudinal tensile strength, longitudinal elongation at break, and dart impact breakage mass values ​​of Comparative Examples 2, 5, and 6 were all lower than those of Example 2.

[0093] Test Example 7: (1) The biodegradable bubble film sample was crushed into fragments with a size of less than 2 mm as the test sample, and microcrystalline cellulose powder with the same particle size was prepared as the standard reference. The mass fraction of carbon element was determined and the theoretical carbon dioxide release was calculated.

[0094] (2) Take fully decomposed industrial compost inoculum and adjust its moisture content to 50%.

[0095] (3) Mix the test sample and reference material with the inoculum at a ratio of 1:6, and put them into an independent sealed compost container. Set up a blank control group.

[0096] (4) Place the container in a 58°C incubator, introduce humid air to remove carbon dioxide, maintain an aerobic composting environment, and regularly turn and add water.

[0097] (5) Refer to GB / T19277.1-2025 standard, continuously monitor the cumulative release of carbon dioxide in the exhaust gas, test for 90 days, and calculate the biodegradation rate of each sample after deducting the blank release.

[0098] Table 7 Biodegradation rate test data of Examples 1 to 5, Comparative Example 1, and the reference:

[0099] From Table 7 and Figure 8 It was found that the biodegradation rates of the standard reference microcrystalline cellulose were 73.5% and 98.6% on day 45 and day 90, respectively; the biodegradation rates of Comparative Example 1 were 58.6% and 90.2% on day 45 and day 90, respectively; and the biodegradation rates of Examples 1 to 5 were 61.2% to 65.7% on day 45 and 90.5% to 94.2% on day 90. The biodegradation rate of the test samples showed an increasing trend with the extension of the test time.

[0100] While specific embodiments of the present invention have been described above, those skilled in the art should understand that these specific embodiments are merely illustrative. Those skilled in the art can omit, substitute, and modify the details of the above methods and systems in various ways without departing from the principles and essence of the present invention. For example, combining the above method steps to perform substantially the same function and achieve substantially the same result using substantially the same method falls within the scope of the present invention.

Claims

1. A bamboo-based biodegradable bubble film, characterized in that, The bamboo-based biodegradable bubble membrane is made from the following materials in parts by weight: 50-70 parts of poly(butylene adipate / terephthalate); 10-25 parts of polylactic acid (L-lactic acid); 1.0 to 5.0 parts of ethylene-methyl acrylate-glycidyl methacrylate terpolymer; 1.0–4.0 parts of zinc ion neutralization product of ethylene-methacrylic acid copolymer; Modified bamboo powder, 15.62–32.1 parts; The modified bamboo powder is a liquid-solid phase pre-coated modified bamboo powder, and the modified bamboo powder is made from the following materials in parts by weight: 15-30 parts of deligninized bamboo powder; 0.5–1.5 parts of magnesium aluminum hydrotalcite; 0.02–0.1 parts of zinc stearate; 0.1 to 0.5 parts of epoxidized soybean oil.

2. The bamboo-based biodegradable bubble membrane according to claim 1, characterized in that, In the ethylene-methyl acrylate-glycidyl methacrylate terpolymer, the mass fraction of ethylene structural units is 65%–75%, the mass fraction of methyl acrylate structural units is 20%–28%, and the mass fraction of glycidyl methacrylate structural units is 5%–10%.

3. The bamboo-based biodegradable bubble film according to claim 1, characterized in that, In the zinc ion neutralized ethylene-methacrylic acid copolymer, the mass fraction of methacrylic acid structural units is 10% to 20%, and the degree of zinc ion neutralization of carboxylic acid groups is 40% to 60%.

4. The production process of bamboo-based biodegradable bubble film, characterized in that, The process of using the bamboo-based biodegradable bubble film according to any one of claims 1-3 includes the following steps: Modified bamboo powder was prepared by mixing delignified bamboo powder with magnesium aluminum hydrotalcite, zinc stearate and epoxidized soybean oil. After drying, poly(butylene adipate) and polylactic acid (PLA) are fed into an extruder for melt plasticization with ethylene-methyl acrylate-glycidyl methacrylate terpolymer and ethylene-methacrylate copolymer zinc ion neutralizer. The modified bamboo powder is fed into the feed port on the side of the extruder for reactive extrusion and devolatilization to obtain a homogeneous reactive melt; The homogeneous reactive melt is used to prepare a thermoforming base film and a flat base film through a casting process. The vacuum-formed base film is vacuum-formed and then hot-pressed together with the flat base film to obtain a bamboo-based biodegradable bubble film.

5. The production process of bamboo-based biodegradable bubble film according to claim 4, characterized in that, The steps for preparing modified bamboo powder include: The lignin-treated bamboo powder was placed in a forced-air drying oven and dried at 100–110℃ for 6–10 hours, with the moisture content controlled to be ≤0.5%. The dried lignin-free bamboo powder, magnesium aluminum hydrotalcite, and zinc stearate are put into a high-speed mixer, and the speed is controlled at 800-1200 r / min. The material temperature is heated to 50-70℃. Liquid epoxidized soybean oil is injected into the mixer through an atomizing nozzle. After mixing for 5 to 15 minutes at the corresponding rotation speed and material temperature, the material is discharged to obtain modified bamboo powder.

6. The production process of bamboo-based biodegradable bubble film according to claim 4, characterized in that, The melt plasticizing step includes: Poly(butylene adipate) / terephthalate and polylactic acid (PLA) were placed in a vacuum drying oven and dried at a vacuum of -0.08 to -0.10 MPa and a temperature of 70 to 90°C for 3 to 5 hours, with the moisture content controlled to be less than 0.02%, to obtain a dried resin mixture. The dried resin mixture, ethylene-methyl acrylate-glycidyl methacrylate terpolymer, and ethylene-methacrylate copolymer zinc ion neutralizer are simultaneously fed into the main feed port of a twin-screw extruder. The speed of the twin-screw extruder is controlled at 200-300 r / min, and the temperature of the first to fourth zones of the extruder is set at 155-175°C to melt and plasticize the material.

7. The production process of bamboo-based biodegradable bubble film according to claim 4, characterized in that, The reactive extrusion and devolatilization steps include: The modified bamboo powder is forcibly fed into the feed port of zone 5 of the twin-screw extruder. The temperature of zones 5 to 7 is set at 160 to 180°C for reactive extrusion. An exhaust port is set in zone 8 and vacuum devolatilization is started. The vacuum degree is controlled at -0.08 to -0.098 MPa. The material continues to pass through zones 9 to 10 at a temperature of 165 to 175°C to obtain a homogeneous reactive melt.

8. The production process of bamboo-based biodegradable bubble film according to claim 4, characterized in that, The steps for preparing the thermoforming layer base film and the flat bottom layer base film include: The thermoforming base film and the flat base film are prepared by independent casting processes using homogeneous reactive melts of the same composition. The casting die temperature is 165-175℃, the surface temperature of the water-cooled roller is 20-30℃, and the traction speed is 10-15m / min. The thickness of the thermoforming base film is controlled to be 60-80μm and the thickness of the flat base film is controlled to be 20-40μm by adjusting the die gap.

9. The production process of bamboo-based biodegradable bubble film according to claim 4, characterized in that, The hot-pressing composite step includes: The thermoforming base film is introduced into a vacuum thermoforming roller at 85–105°C and stretched to form bubbles under a vacuum of -0.07–-0.09 MPa. At the same time, the flat bottom base film is introduced and hot-pressed together with the thermoforming layer under a temperature of 80–100°C and a pressure of 0.3–0.5 MPa. After traction, cooling and slitting, bamboo-based biodegradable bubble film is obtained.