Environment-friendly fluorine-free flame-retardant polycarbonate insulation composite material and preparation method thereof
By introducing components such as hexaphenoxycyclotriphosphazene into the polycarbonate matrix, and combining high-speed mixing and twin-screw melt blending processes, the shortcomings of polycarbonate flame retardant materials in terms of flame retardancy, mechanical properties, light transmission, resistance to damp heat and processing stability are solved, forming a fluorine-free flame retardant polycarbonate composite material with excellent performance.
Patent Information
- Application Number
- CN202611436938.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-20
AI Technical Summary
Existing polycarbonate flame retardant materials have shortcomings in balancing flame retardancy, mechanical properties, light transmittance, insulation properties, resistance to damp heat, and processing stability. In particular, fluorinated flame retardant systems are prone to decomposition and volatilization during high-temperature processing, which affects the material's performance.
Using branched bisphenol A type polycarbonate as the matrix, combined with hexaphenoxycyclotriphosphazene, epoxy functional group acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone, a fluorine-free flame retardant system is formed through high-speed mixing and twin-screw melt blending processes, which improves the uniformity of component dispersion and interfacial compatibility.
This invention achieves a balance between flame retardant properties, mechanical properties, light transmittance, and resistance to damp heat in fluorine-free flame-retardant polycarbonate composite materials, improving the long-term stability and processing stability of the materials and meeting the application requirements of electronic appliances and insulating components.
Smart Images

Figure CN123131807A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, specifically to an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material and its preparation method. Background Technology
[0002] Polycarbonate possesses high impact strength, good light transmittance, dimensional stability, electrical insulation, and resistance to high and low temperatures, making it widely used in flame-retardant structural components, insulating accessories, and appearance parts in fields such as electronics, new energy, smart homes, and rail transportation. As the requirements for flame-retardant safety performance in related products continue to increase, polycarbonate materials often need to incorporate flame-retardant components to meet requirements such as UL94 V0 rating. Currently, some polycarbonate flame-retardant materials still employ fluorinated flame-retardant systems. While these systems can improve flame-retardant performance, they still have certain shortcomings in terms of environmental compliance, material compatibility, and processing stability.
[0003] Existing fluorinated flame retardants have relatively poor compatibility with polycarbonate matrices. At higher addition levels, they can easily cause decreased light transmittance, increased haze, and surface precipitation and whitening of the products. Furthermore, during high-temperature injection molding, they may decompose, volatilize, and experience a decline in mechanical properties. To mitigate the impact of fluorinated systems, existing technologies are increasingly adopting fluorine-free flame retardant systems such as phosphorus-based and silicon-based systems. However, single phosphorus-based flame retardants suffer from insufficient heat resistance and damp heat stability, while single silicon-based flame retardant systems have low flame retardant efficiency and face significant challenges in achieving thin-walled flame retardancy.
[0004] Therefore, existing fluorine-free flame-retardant polycarbonate materials still struggle to simultaneously achieve flame retardancy, mechanical properties, light transmittance, insulation properties, resistance to damp heat, and processing stability. They are prone to issues such as decreased impact resistance or light transmittance after improving flame retardancy, and performance degradation under long-term high-temperature and humid conditions. Thus, there is a need for a polycarbonate composite material and its preparation method that can achieve fluorine-free flame retardancy while maintaining the comprehensive performance of the polycarbonate substrate, while also ensuring processing stability and long-term service stability. Summary of the Invention
[0005] In view of the aforementioned existing problems, the present invention is proposed.
[0006] Therefore, this invention provides an environmentally friendly, fluorine-free flame-retardant polycarbonate insulating composite material and its preparation method, solving the common technical problems of existing polycarbonate flame-retardant materials, such as environmental limitations, insufficient flame-retardant efficiency, poor component compatibility, and difficulty in simultaneously achieving flame-retardant performance, mechanical properties, light transmittance, damp heat resistance, and processing stability.
[0007] To solve the above-mentioned technical problems, the present invention provides the following technical solution: This invention provides a method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material, comprising the following steps: S1. Raw material pretreatment: Branched bisphenol A type polycarbonate is dried at 80-100 ℃ for 3-4 h. Hexaphenoxycyclotriphosphazene, epoxy functional group acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone are passed through a 75-85 mesh sieve to improve the uniformity of subsequent mixing and dispersion. S2. Weigh out 85-95 parts by weight of pretreated branched bisphenol A type polycarbonate, 3.0-8.0 parts by weight of hexaphenoxycyclotriphosphazene, 0.5-2.5 parts by weight of epoxy functional group acrylic copolymer, 0.2-0.5 parts by weight of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, 0.2-0.5 parts by weight of polycarbodiimide, 0.1-0.5 parts by weight of pentaerythritol stearate and 1.0-3.0 parts by weight of 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone, put the above raw materials into a high-speed mixer, and mix at 800-1000 r / min for 5-8 min to obtain a homogeneous mixture. S3. The homogeneous mixture is fed into a twin-screw extruder for melt blending and extrusion. The temperature of the first zone of the twin-screw extruder is 220-240 ℃, the temperature of the second zone is 240-260 ℃, the temperature of the third zone is 260-280 ℃, the die head temperature is 270-290 ℃, the screw speed is 300-400 r / min, and the vacuum degree is -0.10--0.08 MPa. The extruded strip material is water-cooled, shaped, and pelletized to obtain fluorine-free flame-retardant polycarbonate granules. S4. The fluorine-free flame-retardant polycarbonate particles are dried at 90-100 ℃ for 2-3 h, cooled to room temperature, and then sealed and packaged to obtain an environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material.
[0008] As a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S1, the drying temperature is 90 ℃; the drying time is 3.5 h; and the sieve is an 80-mesh sieve.
[0009] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S2, the branched bisphenol A type polycarbonate is 90 parts; the hexaphenoxycyclotriphosphazene is 5.00 parts; the epoxy functional group acrylic copolymer is 1.50 parts; the tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant is 0.30 parts; the polycarbodiimide is 0.31 parts; the pentaerythritol stearate is 0.27 parts; and the 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone is 1.68 parts.
[0010] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S3, the feeding rate is 10 kg / h; the temperature of the first zone is 230 ℃; and the temperature of the second zone is 250 ℃.
[0011] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S4, the drying temperature is 95 ℃ and the drying time is 2.5 h.
[0012] As a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S2, the high-speed mixing speed is 900 r / min; and the high-speed mixing time is 7 min.
[0013] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S3, the temperature of the three zones is 270 ℃; and the temperature of the machine head is 280 ℃.
[0014] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S3, the screw speed is 350 r / min; and the vacuum degree is -0.09 MPa. The water-cooling and pelletizing process is as follows: the strip material with a diameter of 2-3 mm formed by extrusion is cooled and shaped by circulating water at 25±2 ℃ and then fed into a pelletizer. The pellets are pelletized at a speed of 300 r / min to obtain fluorine-free flame-retardant polycarbonate particles with a length of 3-4 mm and a diameter of 2-3 mm.
[0015] In a preferred embodiment of the method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to the present invention, in step S4, the room temperature is 23±2 ℃.
[0016] The beneficial effects of this invention are as follows: In summary, by constructing a continuous matrix with branched bisphenol A type polycarbonate, introducing hexaphenoxycyclotriphosphazene to form a fluorine-free flame-retardant system, and combining it with epoxy functional group acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate, and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone pigment for synergistic modification, and combining high-speed mixing and twin-screw melt blending processes, the dispersion uniformity and interfacial compatibility of each functional component in the polycarbonate matrix are improved, thus improving the problem that traditional flame-retardant polycarbonate materials are difficult to balance in terms of flame retardant performance, mechanical properties, insulation properties, light transmittance, and hygrothermal stability.
[0017] Specifically, this invention improves the flame retardant properties of the material through hexaphenoxycyclotriphosphazene, enhances the compatibility between hexaphenoxycyclotriphosphazene and the branched bisphenol A type polycarbonate matrix through epoxy-functionalized acrylic copolymer, improves the thermal and oxygen stability and damp heat resistance of the material through a composite antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide, and improves the melt processing fluidity and extrusion stability through pentaerythritol stearate. Simultaneously, by synergistically controlling the high-speed mixing speed, mixing time, melt extrusion temperature, screw speed, and vacuum degree, hexaphenoxycyclotriphosphazene, epoxy-functionalized acrylic copolymer, and various additives are fully dispersed in the branched bisphenol A type polycarbonate matrix, reducing the risk of thermal degradation and performance fluctuations during processing. The resulting environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material possesses good flame retardant properties, notched impact resistance, insulation properties, light transmittance, and resistance to damp heat, thus improving the long-term stability of the material in electronic, electrical, and insulating component applications. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 The figure shows the experimental results of optimizing the amount of hexaphenoxycyclotriphosphazene added.
[0020] Figure 2 The figure shows the experimental results of optimizing the addition amount of epoxy functional group acrylic copolymer.
[0021] Figure 3Figure 1 shows the experimental results of high-speed mixing rotation speed and time.
[0022] Figure 4 Figure 2 shows the experimental results of high-speed mixing rotation speed and time.
[0023] Figure 5 The figure shows the experimental results of processing optimization for the combination of melt extrusion temperatures.
[0024] Figure 6 Figure 1 shows the experimental results of the machining optimization of screw speed and vacuum degree.
[0025] Figure 7 Figure 2 shows the experimental results of the machining optimization of screw speed and vacuum degree.
[0026] Figure 8 This is a schematic diagram of the microstructure of an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material.
[0027] Figure 9 This is a flowchart illustrating the preparation method of an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material. Detailed Implementation
[0028] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0029] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0030] Secondly, the term "one embodiment" or "example" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the invention. An embodiment appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that mutually excludes other embodiments. Example 1
[0031] This embodiment aims to explore a polycarbonate matrix system suitable for environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite materials, in order to solve the common technical problems of existing polycarbonate flame-retardant materials, such as environmental limitations, insufficient flame-retardant efficiency, poor component compatibility, and difficulty in simultaneously achieving flame-retardant performance, mechanical properties, light transmittance, damp heat resistance, and processing stability.
[0032] 1.1 Screening of substrate materials In the preparation of polycarbonate insulating composite materials, the substrate is not only the main material that carries the fluorine-free flame-retardant components and various additives, but also the core foundation that determines the melt strength, processing fluidity, mechanical properties, and combustion droplet behavior of the composite material. To meet the requirements of flame retardancy, insulation, and industrial processing stability in the fields of electronics, electrical appliances, and new energy, the selected substrate must have good thermal stability, melt strength, and mechanical properties; at the same time, it must maintain suitable melt fluidity so that the fluorine-free flame-retardant components can be uniformly dispersed, avoiding problems such as processing difficulties, obvious droplets, or performance degradation caused by matrix viscosity mismatch.
[0033] Six representative polycarbonates commonly used in the field of polycarbonate modified materials were selected as candidates. By testing their melt flow rate, volume resistivity, notched impact strength, and number of droplets within 60 seconds of combustion, a substrate material with processing fluidity, mechanical properties, and melt strength was screened.
[0034] Melt mass flow rate test: The test shall be conducted in accordance with GB / T 3682.1. The PC sample shall be thoroughly dried beforehand, and the mass of melt passing through a standard die within 10 min shall be measured under conditions of 300℃ and 1.2 kg load. The result shall be expressed as g / 10 min. Each group shall be tested 5 times, and the average value shall be taken.
[0035] Notched impact strength testing: The cantilever beam notched impact method is used according to GB / T 1843. The specimens are injection molded into standard specimens and the specified notches are processed. After conditioning at 23℃ and 50% relative humidity for 24 hours, the impact test is carried out. Five specimens are tested in each group, and the average value is taken.
[0036] Volume resistivity testing: The test shall be conducted according to GB / T 1410. The material shall be prepared into a flat plate sample of specified dimensions and conditioned for 24 hours at 23℃ and 50% relative humidity. The volume resistivity of the sample under a specified DC voltage shall be measured using a high-resistivity meter, and then calculated. Five samples shall be tested in each group, and the average value shall be taken.
[0037] Test for the number of molten droplets within 60 seconds of combustion: Prepare strip-shaped specimens of uniform size and thickness, fix them vertically, place the lower end above a specified flame, and continuously apply flame to the specimen for 60 seconds. Record the number of molten droplets that detach from the specimen body and completely separate during the flame application. Test 5 parallel specimens in each group and calculate the average number of molten droplets.
[0038] The test results are as follows:
[0039] Among them, polycarbonate-polysiloxane copolymers have high notched impact strength and fewer combustion dripping times, but their low volume resistivity can easily lead to a decrease in the insulation performance of the material, affecting the stable use of insulating components. High heat-resistant copolymer polycarbonate has high volume resistivity and good anti-dripping performance, but its low melt flow rate can easily lead to excessively high melt viscosity, resulting in uneven dispersion of flame-retardant components. Therefore, branched bisphenol A type polycarbonate with relatively balanced properties was selected as the base material for the insulating composite material of this invention.
[0040] 1.2 Screening of Fluorine-Free Flame Retardants Although branched bisphenol A polycarbonate exhibits good overall performance in terms of processing fluidity, mechanical properties, insulation properties, and anti-dripping ability, its inherent flame retardancy is limited, making it difficult to meet the high flame retardancy requirements of the electronics, electrical appliances, and new energy sectors. Therefore, the introduction of fluorine-free flame retardants aims to improve the flame retardancy of the material while maintaining the mechanical and insulation properties of the polycarbonate matrix as much as possible, and further screening of fluorine-free flame retardants with good compatibility with the matrix is necessary.
[0041] Six representative and commonly used fluorine-free flame retardants in polycarbonate materials were selected for screening: hexaphenoxycyclotriphosphazene (4.63 parts), resorcinol bis(diphenyl phosphate) (6.17 parts), bisphenol A bis(diphenyl phosphate) (6.54 parts), triphenyl phosphate (5.86 parts), melamine polyphosphate (7.23 parts), and phenyl silicone resin (3.79 parts). By testing the limiting oxygen index, average burning time, notched impact strength, and volume resistivity, fluorine-free flame retardants with flame retardant, mechanical, and insulating properties were selected.
[0042] Limiting oxygen index test: The limiting oxygen index is determined according to GB / T 2406.2. The sample is placed vertically in an oxygen-nitrogen mixed gas flow and ignited. By adjusting the oxygen concentration, the minimum volume fraction of oxygen required to maintain the specified combustion state is determined.
[0043] Average burning time test: The test was conducted according to the vertical burning method specified in GB / T 2408. The sample was prepared into a standard strip with a thickness of 1.5 mm, and vertically clamped after adjustment under specified environmental conditions. The lower end of the sample was ignited twice, and the afterburning time of the sample was recorded after the flame was removed each time. Five parallel samples were set up in each group, and the average of the two afterburning times of each sample was calculated as the average burning time.
[0044] The test results are as follows:
[0045] Among them, melamine polyphosphate has a high limiting oxygen index, but low notched impact strength and volume resistivity, which can easily lead to a decrease in material toughness and affect insulation performance; phenyl silicone resin has high notched impact strength and volume resistivity, but low limiting oxygen index, which can easily lead to insufficient flame retardant effect. Therefore, hexaphenoxycyclotriphosphazene, which has a more balanced performance, was selected as the fluorine-free flame retardant of this invention.
[0046] 1.3 Screening of compatibilizers In fluorine-free flame-retardant polycarbonate composites, compatibilizers are mainly used to improve the compatibility between the polycarbonate matrix and the fluorine-free flame-retardant components. Insufficient compatibility can easily lead to problems such as uneven dispersion, precipitation, and surface whitening of the flame-retardant components; conversely, an overly strong compatibilizer may affect melt flowability. Therefore, it is necessary to screen compatibilizers with good overall performance to improve the dispersion stability and processing properties of the material.
[0047] Six representative and commonly used compatibilizers in polycarbonate materials were selected for screening: epoxy functional group acrylic copolymer (1.08 parts), styrene-maleic anhydride copolymer (1.24 parts), ethylene-glycidyl methacrylate copolymer (1.37 parts), ethylene-methyl acrylate-glycidyl methacrylate terpolymer (1.56 parts), maleic anhydride-grafted SEBS (1.73 parts), and maleic anhydride-grafted POE (1.92 parts). Compatibilizers with compatibility, mechanical properties, processability, and insulation properties were selected by testing notched impact strength, melt flow rate, volume resistivity, and surface precipitation degree.
[0048] Surface precipitation area ratio detection: Each group of materials was injection molded into... The flat plate sample was conditioned at 23℃ and 50% relative humidity for 24 hours, then placed at 80℃ for 72 hours, removed, and cooled to room temperature. Images of the sample surface were acquired under the same illumination conditions, and the center of the sample was selected. The detection area is defined as the region where image analysis methods are used to identify and statistically analyze the areas of white spots, oily exudates, and other exudated areas. The total area of exudated areas within the detection region is used as the basis for the calculation. Total area of the detection area The ratio calculation of the surface precipitation area percentage ,Right now .
[0049] The test results are as follows:
[0050] Among them, the surface precipitation area of ethylene-glycidyl methacrylate copolymer is relatively low, but its volume resistivity is relatively low, which can easily affect the insulation performance of the material; styrene-maleic anhydride copolymer has a high volume resistivity, but its melt mass flow rate is low, which can easily lead to high melt viscosity. Therefore, epoxy functional group acrylic copolymer with relatively balanced properties was selected as the compatibilizer of this invention.
[0051] 1.4 Screening of Compound Antioxidants In fluorine-free flame-retardant polycarbonate composites, composite antioxidants are mainly used to inhibit thermo-oxidative aging during high-temperature processing and long-term use. Insufficient antioxidant effect can easily lead to polycarbonate degradation, discoloration, and a decline in mechanical properties; improper matching of the antioxidant system may also affect the processing stability of the material. Therefore, it is necessary to screen composite antioxidants with good overall performance to improve the thermo-oxidative stability and long-term performance of the material.
[0052] Six representative and commonly used composite antioxidants in polycarbonate materials were selected for screening: antioxidant 1010 / antioxidant 168 composite system (0.32 parts), antioxidant 1076 / antioxidant 168 composite system (0.36 parts), antioxidant 1010 / dilauryl thiodipropionate composite system (0.41 parts), antioxidant 1076 / dilauryl thiodipropionate composite system (0.38 parts), antioxidant 1010 / antioxidant 626 composite system (0.29 parts), and antioxidant 245 / antioxidant 168 composite system (0.34 parts). The composite antioxidants with resistance to thermo-oxidative aging, processing stability, appearance stability, and insulation properties were screened by testing the notched impact strength retention rate, melt flow rate change rate, yellowing index, and volume resistivity after thermal aging.
[0053] Thermal aging method: Each group of materials is prepared separately. Notched impact test specimens and Flat plate samples were conditioned at 23℃ and 50% relative humidity for 24 hours, then placed in a hot air aging chamber and aged continuously at 120℃ for 168 hours. After aging, the samples were removed, cooled to room temperature, and placed at 23℃ and 50% relative humidity for 24 hours before notched impact strength, yellowing index, and volume resistivity were tested. The melt flow rate was tested using materials from the same batch of aged materials.
[0054] Notched impact strength testing: The cantilever beam notched impact method is used according to GB / T 1843. Standard specimens of uniform size are injection molded from each group of materials, and notches are machined at specified locations. The specimens are then conditioned for 24 hours at 23℃ and 50% relative humidity. During testing, the specimens are fixed in the fixture of the impact testing machine, and the pendulum is released from a specified height to impact the specimen. The impact energy at specimen fracture is recorded, and the notched impact strength is calculated based on the remaining cross-sectional dimensions at the notch.
[0055] Melt mass flow rate change rate test: Each group of materials was aged in a 120℃ hot air aging chamber for 168 h, then dried. The melt mass flow rate after aging was measured according to the aforementioned melt mass flow rate test method, and the change rate was calculated based on the test results before and after aging.
[0056] Yellowing index testing: The test was conducted according to GB / T 39822-2021, and each group of materials was prepared... The flat plate samples were first conditioned at 23±2 ℃ and 50%±5% relative humidity for 24 h, and then aged in a 120 ℃ hot air aging chamber for 168 h. After aging, the samples were removed and conditioned again at 23±2 ℃ and 50%±5% relative humidity for 24 h, and the yellow index YI was measured using a colorimeter.
[0057] The test results are as follows:
[0058] Among them, the antioxidant 1010 / antioxidant 626 composite system has a lower melt flow rate change rate and yellowing index, but its notched impact strength retention rate and volume resistivity after thermal aging are relatively low, which easily affects the mechanical and insulation properties of the material. The antioxidant 245 / antioxidant 168 composite system has a higher notched impact strength retention rate and volume resistivity, but its melt flow rate change rate and yellowing index are relatively high, and the processing stability and color stability of the material after thermal aging are slightly poor. Therefore, the antioxidant 1010 / antioxidant 168 composite system (a composite antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite) with relatively balanced properties was selected as the composite antioxidant of this invention.
[0059] 1.5 Screening of Heat Stabilizing Agents In fluorine-free flame-retardant polycarbonate composites, heat stabilizers are primarily used to inhibit molecular chain degradation of polycarbonate under high-temperature processing and humid conditions. Polycarbonate is prone to hydrolysis under the combined influence of moisture and heat, leading to a decrease in molecular weight and further reducing the material's impact resistance, melt stability, and insulation properties. Insufficient compatibility between the heat stabilizer and the polycarbonate matrix can also cause yellowing or fluctuations in processing performance. Therefore, it is necessary to screen for heat stabilizers with good overall performance to improve the material's ability to retain performance under high-temperature and humid conditions.
[0060] Six representative and commonly used heat-stabilizing additives in polycarbonate materials were selected for screening: polycarbodiimide (0.31 parts), N,N′-bis(2,6-diisopropylphenyl)carbodiimide (0.25 parts), 2,2′-(1,3-phenylene)dioxazoline (0.37 parts), epoxy styrene-acrylic acid oligomer (0.43 parts), hydrotalcite (0.44 parts), and calcium stearate (0.28 parts). Heat-stabilizing additives with combined properties of damp heat stability, processing stability, appearance stability, and insulation performance were screened by testing the notched impact strength retention rate, melt flow rate change rate, yellowing index, and volume resistivity after damp heat aging.
[0061] Damp heat aging treatment: Each group of materials is prepared separately. Notched impact test specimens and Flat plate samples were conditioned at 23℃ and 50% relative humidity for 24 hours, then placed in a constant temperature and humidity test chamber and aged continuously at 85℃ and 85% relative humidity for 168 hours. After aging, the samples were removed, surface moisture was wiped off, and the samples were placed at 23℃ and 50% relative humidity for 24 hours. Subsequently, notched impact strength, yellowing index, and volume resistivity were tested. The melt flow rate was tested using materials from the same batch that had undergone wet heat aging treatment and were fully dried.
[0062] The test results are as follows:
[0063] Among them, N,N′-bis(2,6-diisopropylphenyl)carbodiimide exhibits a high notched impact strength retention rate after damp heat aging, but it also has a high melt flow rate change rate and low volume resistivity, which can easily affect the processing stability and insulation properties of the material. Epoxy styrene-acrylic acid oligomers have a low yellowing index, but their notched impact strength retention rate and volume resistivity are relatively low, which can easily affect the mechanical and insulation properties of the material. Therefore, polycarbodiimide, with its relatively balanced properties, was selected as the heat-stabilizing additive in this invention.
[0064] 1.6 Screening of machining lubricants In polycarbonate fluorine-free flame-retardant composites, processing lubricants are mainly used to reduce friction between the material and equipment during melting, mixing, and extrusion, thereby improving melt flow stability and product surface quality. Insufficient processing lubrication can easily lead to unstable melt flow, increased extrusion load, and rough product surface. Furthermore, mismatched amounts or types of lubricants can easily cause migration and precipitation, affecting the material's mechanical and insulation properties. Therefore, it is necessary to screen processing lubricants with good overall performance to balance the material's processing performance, surface stability, mechanical properties, and insulation properties.
[0065] Six representative and commonly used processing lubricants for polycarbonate materials were selected for screening: pentaerythritol stearate (0.27 parts), ethylene bis-stearamide (0.23 parts), polyethylene wax (0.32 parts), oxidized polyethylene wax (0.36 parts), zinc stearate (0.18 parts), and silicone masterbatch (0.42 parts). The processing lubricants with processing fluidity, surface precipitation area ratio, notched impact strength, and volume resistivity were screened by testing the melt mass flow rate, surface precipitation area ratio, notched impact strength, and volume resistivity.
[0066] Surface precipitation area ratio detection: Each group of materials was injection molded into... The flat plate sample was conditioned at 23℃ and 50% relative humidity for 24 hours, then placed at 80℃ for 72 hours, removed, and cooled to room temperature. Images of the sample surface were acquired under the same illumination conditions, and the center of the sample was selected. The detection area is defined as the region where image analysis methods are used to identify and statistically analyze the areas of white spots, oily exudates, and other exudated areas. The total area of exudated areas within the detection region is used as the basis for the calculation. Total area of the detection area The ratio calculation of the surface precipitation area percentage ,Right now .
[0067] The test results are as follows:
[0068] Among them, silicone masterbatch has a high melt flow rate and notched impact strength, but a high surface precipitation area ratio and relatively low volume resistivity, which can easily affect the surface stability and insulation properties of the material; ethylene bis-stearamide has a low surface precipitation area ratio, but a relatively low melt flow rate and notched impact strength, which can easily affect the processing fluidity and mechanical properties of the material. Therefore, pentaerythritol stearate, which has a more balanced range of properties, was selected as the processing lubricant of this invention.
[0069] 1.7 Screening of Pigment Powder In fluorine-free flame-retardant polycarbonate composites, colorants are primarily used to adjust the material's appearance and color, while maintaining the original light transmittance and processing stability of the polycarbonate matrix. Different colorants vary in tinting strength, heat resistance, and compatibility with the polycarbonate matrix. Inappropriate selection can easily lead to decreased light transmittance, color changes after high-temperature processing, and negatively impact the material's overall performance. Therefore, it is necessary to select colorants that have minimal impact on the polycarbonate's light transmittance and offer superior overall performance, while still meeting aesthetic requirements.
[0070] Six representative and commonly used colorants in polycarbonate materials were selected for screening: 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone (1.68 parts), phthalocyanine blue (1.84 parts), ultramarine blue (2.16 parts), cobalt blue (2.37 parts), rutile titanium dioxide white (1.53 parts), and carbon black (1.26 parts). The colorants with good light transmittance, color difference after heat treatment, notched impact strength, and volume resistivity were selected by testing their visible light transmittance, color stability, mechanical properties, and insulation properties.
[0071] Visible light transmittance testing: Each group of materials was injection molded into... The flat plate samples were conditioned at 23℃ and 50% relative humidity for 24 h. The transmittance of the samples in the visible light range was measured using a spectrophotometer. Five samples were tested in each group, and the average value was taken.
[0072] Color difference detection after heat treatment: Prepare each group of materials... The color parameters of the flat plate sample before heat treatment were measured. The sample was then placed in a 120℃ hot air aging chamber for 168 h, removed, and cooled to room temperature before the color parameters were measured again. The overall color difference before and after heat treatment was used as the basis for the determination. Indicates the degree of color change.
[0073] The test results are as follows:
[0074] Phthalocyanine blue pigment has high visible light transmittance, but its notched impact strength is relatively low, which can easily affect the mechanical properties of the material. Rutile titanium dioxide white pigment has low color difference after heat treatment, but its visible light transmittance is low, which can easily affect the original light transmittance of the polycarbonate matrix. Therefore, 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone, which has better overall performance, is used as the pigment of this invention. Example 2
[0075] Reference Figures 1 to 2This is the second embodiment of the present invention. Based on determining the types of each functional component, this embodiment further optimizes the amount of the main components added to determine a more suitable ratio, so that the material has flame retardant properties, mechanical properties, insulation properties, processing stability and light transmittance.
[0076] 2.1 Optimization of the amount of hexaphenoxycyclotriphosphazene added Based on 90 parts of branched bisphenol A type polycarbonate, the following amounts were fixed: 1.08 parts of epoxy functional group acrylic copolymer, 0.30 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, 0.31 parts of polycarbodiimide, 0.27 parts of pentaerythritol stearate, and 1.68 parts of 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone. The amount of hexaphenoxycyclotriphosphazene added was used as a single variable.
[0077] The results are as follows Figure 1 As shown, with the increase of hexaphenoxycyclotriphosphazene addition, the flame retardant component content increases, and the flame retardant performance of the system gradually improves. However, the introduction of excessive flame retardant components reduces the matrix continuity, causing a decrease in notched impact strength and volume resistivity. When the hexaphenoxycyclotriphosphazene addition is 4.0–6.0 parts, the overall performance is at a relatively good level, and this range is defined as the effective addition range of hexaphenoxycyclotriphosphazene. Further normalized comprehensive evaluation was performed on the limiting oxygen index, mean burning time, notched impact strength, and volume resistivity under each addition gradient. Among them, the limiting oxygen index, notched impact strength, and volume resistivity were used as positive indicators. Normalization is performed, with average combustion time used as an inverse indicator, according to Normalization is performed, where, This corresponds to the actual detection value of this indicator at the corresponding hexaphenoxycyclotriphosphazene addition level. and These represent the maximum and minimum detection values for this detection index across all addition amounts. These are the normalized index values. And according to... Calculate the comprehensive evaluation value, where, and These are the normalized values of limiting oxygen index, mean combustion time, notched impact strength, and volume resistivity, respectively.
[0078] With the amount of hexaphenoxycyclotriphosphazene added The horizontal axis represents the overall evaluation value. A quadratic curve is fitted to the ordinate to obtain the fitting equation. And based on the extreme points The theoretically optimal addition amount was determined to be approximately 5.46 parts. Considering the accuracy of material weighing and the convenience of formula control in industrial production, the final addition amount of hexaphenoxycyclotriphosphazene was determined to be 5.0 parts.
[0079] 2.2 Optimization of the amount of epoxy functional group acrylic copolymer added Based on 90 parts of branched bisphenol A type polycarbonate, with fixed addition amounts of 5.0 parts hexaphenoxycyclotriphosphazene, 0.30 parts pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]triamethylenetetramine ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, 0.31 parts polycarbodiimide, 0.27 parts pentaerythritol stearate, and 1.68 parts 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone, the addition amount of epoxy-functionalized acrylic copolymer was used as the single variable. Considering the effective addition range of epoxy-functionalized acrylic copolymer in the polycarbonate system, five addition amount gradients were set with a lower limit of 0.5 parts, an upper limit of 2.5 parts, and a gradient step size of 0.5 parts. The melt flow rate, notched impact strength, volume resistivity, and surface precipitation area ratio of each group of samples were measured to determine the appropriate amount of epoxy functional group acrylic copolymer to be added.
[0080] The results are as follows Figure 2 As shown, with the increase of epoxy-functionalized acrylic copolymer addition, the melt flow rate of the system gradually decreases, the notched impact strength and volume resistivity show a trend of first increasing and then decreasing, and the surface precipitation area ratio shows a trend of first decreasing and then increasing. When the epoxy-functionalized acrylic copolymer addition is 1.0 to 2.0 parts, the overall performance is at a relatively good level, and this range is determined to be the effective addition range of epoxy-functionalized acrylic copolymer.
[0081] Following the same normalized comprehensive evaluation method described above, the melt flow rate, notched impact strength, volume resistivity, and surface precipitation area ratio under each addition gradient were processed. Melt flow rate, notched impact strength, and volume resistivity were used as positive indicators, while the surface precipitation area ratio was used as a negative indicator. The comprehensive evaluation value S corresponding to each addition amount was calculated. Subsequently, a quadratic curve was fitted with the epoxy-functionalized acrylic copolymer addition amount x as the abscissa and the comprehensive evaluation value S as the ordinate to obtain the fitting equation. Based on the fitting results, the theoretically optimal addition amount was approximately 1.54 parts. Considering the material weighing accuracy and ease of formulation control in industrial production, the final addition amount of the epoxy functional group acrylic copolymer was determined to be 1.50 parts. Example 3
[0082] Reference Figures 3 to 8This is the third embodiment of the present invention. Based on the aforementioned preferred formulation, this embodiment further investigates the processing adaptability of the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material during melt blending and extrusion granulation. By adjusting key process parameters, the influence of different process conditions on the dispersion state of each component, material processing stability, and overall performance is analyzed, thereby determining the suitable process conditions for stable processing and large-scale production of this polycarbonate insulating composite material.
[0083] 3.1 Optimization of high-speed mixing speed and time A fixed formulation was prepared using 90 parts of branched bisphenol A polycarbonate, 5.00 parts of hexaphenoxycyclotriphosphazene, 1.50 parts of epoxy-functionalized acrylic copolymer, 0.30 parts of a composite antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite, 0.31 parts of polycarbodiimide, 0.27 parts of pentaerythritol stearate, and 1.68 parts of 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone. The branched bisphenol A polycarbonate was dried at 90°C for 3.5 h. The hexaphenoxycyclotriphosphazene and other additives were passed through an 80-mesh sieve and then weighed according to the above-mentioned amounts and added to a high-speed mixer in one go. The high-speed mixing speed was set to 500–1000 r / min with a gradient step of 100 r / min; the high-speed mixing time was set to 5–10 min with a gradient step of 1 min. Experimental groups were set up by combining the speed and mixing time in different ways. The melt mass flow rate, notch impact strength and surface precipitation area ratio were detected to determine the appropriate high-speed mixing speed and mixing time.
[0084] The results are as follows Figures 3 to 4 As shown, with the cross-variation of high-speed mixing speed and mixing time, the melt mass flow rate of the system generally shows a trend of first increasing and then stabilizing, the notched impact strength shows a trend of first increasing and then decreasing, and the surface precipitation area ratio shows a trend of first decreasing and then increasing. When the high-speed mixing speed is 800–1000 r / min and the mixing time is 5–8 min, the following performance parameters are evaluated. Within this range, the high-speed mixing speed x and mixing time y are used as independent variables, and the melt mass flow rate, notched impact strength, and surface precipitation area ratio are used as evaluation indicators for comprehensive evaluation. All test results are normalized, with the melt mass flow rate and notched impact strength using a forward normalization method. The surface precipitation area ratio was determined using a reverse normalization method. ,in, For the first Normalized values of the corresponding indicators in the group experiments. These are the actual test values for the corresponding experimental group. and These are the maximum and minimum values of the evaluation index across all experimental groups, and the comprehensive evaluation value is calculated for each evaluation index using an equal-weighted approach. .in, These are the normalized values corresponding to melt mass flow rate, notched impact strength, and surface precipitation area percentage, respectively. Then, a comprehensive evaluation value is used. As the response value, a quadratic response surface model is used for fitting: Perform fitting. Among them, For comprehensive evaluation, For high-speed mixing, For mixed time, For constant terms, , respectively, are the first-order fitting coefficients for high-speed mixing speed and mixing time. These are the quadratic fitting coefficients for the high-speed mixing speed and mixing time, respectively. The coefficients are the interaction terms between high-speed mixing speed and mixing time.
[0085] Based on response surface model fitting analysis, the model determination coefficients are... The coefficient of determination is 0.96, adjusted accordingly. The value of 0.93 indicates that the model has a good fit. Based on the model calculation results, the optimal point for comprehensive evaluation is located at a high-speed mixing speed of approximately 891.96 r / min and a mixing time of approximately 7.12 min. Considering the actual equipment adjustment accuracy and process control convenience, the final high-speed mixing speed was determined to be 900 r / min and the mixing time to be 7 min.
[0086] 3.2 Optimization of Melt Extrusion Temperature Combinations Under the aforementioned formulation, a homogeneous mixture was obtained by high-speed mixing at 900 r / min for 7 min. Based on this, while maintaining constant screw speed and vacuum, the temperatures of zones one, two, and three of the twin-screw extruder, along with the die head temperature, were adjusted as a whole. Zone one primarily handles initial heating and conveying of the material; zone two promotes further melting; zone three enhances plasticization, dispersion, and homogenization of the molten material; and the die head temperature maintains the flow stability of the melt before extrusion. The temperatures were set as follows: zone one: 210–250 °C; zone two: 230–270 °C; zone three: 250–290 °C; and die head temperature: 260–300 °C. Each zone was set with a 10 °C gradient, and the temperature increased synchronously across zones to form corresponding temperature gradient combinations. The effects of different melt extrusion temperature combinations on the material's processing properties, mechanical properties, and thermal stability were analyzed by measuring melt mass flow rate, notched impact strength, and yellowing index, thus determining the optimal melt extrusion temperature combination.
[0087] The results are as follows Figure 5As shown, with the overall increase in melt extrusion temperature, the melt mass flow rate continuously increases, the notched impact strength shows a trend of first increasing and then decreasing, and the yellowing index shows a trend of first decreasing and then increasing. When the temperature of Zone 1 is 220–240 ℃, Zone 2 is 240–260 ℃, Zone 3 is 260–280 ℃, and the die head temperature is 270–290 ℃, the overall performance is at a relatively good level. Based on this, the above range is determined as the suitable melt extrusion temperature range.
[0088] Further, following the aforementioned normalized comprehensive evaluation method, the melt mass flow rate, notched impact strength, and yellowing index corresponding to each temperature combination were processed. Melt mass flow rate and notched impact strength were used as positive indicators, while the yellowing index was used as a negative indicator. The comprehensive evaluation value S was then calculated. A quadratic curve was fitted using the zone I temperature x as the independent variable and the comprehensive evaluation value S as the dependent variable to obtain... Where S is the comprehensive evaluation value, x is the temperature of zone one, a is a constant term, and b1 and b2 are the fitting coefficients for the linear and quadratic terms, respectively; the temperatures of zone two, zone three, and the die head are increased by 20 ℃, 40 ℃, and 50 ℃ respectively, based on the temperature of zone one. Through model fitting analysis, the theoretical optimal value of the zone one temperature is approximately 232.47 ℃, corresponding to approximately 252.47 ℃ for zone two, approximately 272.47 ℃ for zone three, and approximately 282.47 ℃ for the die head. Considering the temperature adjustment precision of the twin-screw extruder and the convenience of parameter control in industrial production, the final melt extrusion temperatures are determined to be: 230 ℃ for zone one, 250 ℃ for zone two, 270 ℃ for zone three, and 280 ℃ for the die head.
[0089] 3.3 Optimization of screw speed and vacuum The mixture was fed into a twin-screw extruder. The melt extrusion temperatures were set to 230 °C in zone one, 250 °C in zone two, and 270 °C in zone three, with a die temperature of 280 °C. The feed rate was fixed at 10 kg / h. The screw speed was set to 250–450 r / min in 50 r / min increments, and the vacuum was set to -0.10–-0.06 MPa in 0.01 MPa increments. Experimental groups were established by combining screw speed and vacuum in various ways. The melt flow rate, notched impact strength, and yellowing index of each experimental group were measured to determine the appropriate screw speed and vacuum.
[0090] The results are as follows Figures 6 to 7As shown, with the cross-change of screw speed and vacuum level, the melt mass flow rate of the system generally shows an increasing trend, the notched impact strength shows a trend of first increasing and then decreasing, and the yellowing index shows a trend of first decreasing and then increasing. When the screw speed is 300~400 r / min and the vacuum level is -0.10~-0.08 MPa, the overall performance is at a relatively good level, and this range is determined as the suitable process range. Further, according to the aforementioned normalized comprehensive evaluation method, the melt mass flow rate, notched impact strength, and yellowing index of each experimental group are processed. The melt mass flow rate and notched impact strength are used as positive evaluation indicators, and the yellowing index is used as a negative evaluation indicator. The comprehensive evaluation value S is calculated according to the aforementioned equal weighting method. With screw speed x and vacuum level y as independent variables and the comprehensive evaluation value S as the response value, a quadratic response surface model is used for fitting: Where S is the comprehensive evaluation value, x is the screw speed, y is the vacuum degree, a is a constant term, b1 and b2 are the first-order fitting coefficients of screw speed and vacuum degree, b3 and b4 are the second-order fitting coefficients of screw speed and vacuum degree, and b5 is the fitting coefficient of the interaction term of screw speed and vacuum degree.
[0091] The model fitting results show that the determination coefficient of the established response surface model is... The coefficient of determination is 0.95, adjusted accordingly. The value of 0.92 indicates that the model has good fitting reliability. Based on the response surface methodology, the theoretical optimal point is located at approximately 336.13 r / min screw speed and -0.092 MPa vacuum. Considering the accuracy of screw speed adjustment and the convenience of vacuum control in a twin-screw extruder, the final screw speed and vacuum level were determined to be 350 r / min and -0.09 MPa.
[0092] 3.4 Finished Product Preparation and Post-processing The resulting molten blend is continuously extruded through a die head to form strips with a diameter of 2–3 mm. These strips are then cooled and shaped in circulating cooling water at 25±2℃. After removing surface moisture, they are continuously fed into a pelletizer and pelletized at a roller speed of 300 r / min to obtain fluorine-free flame-retardant PC granules with a length of 3–4 mm and a diameter of 2–3 mm. The resulting granules are dried at 95℃ for 2.5 h, cooled to 23±2℃, and then sealed and packaged to obtain the environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material.
[0093] 3.5 Verification of Process Effect To verify the comprehensive improvement effect of the formulation and preparation process of this invention on the flame retardant properties, mechanical properties, insulation properties, optical properties, and damp heat resistance of the material, a halogen-free flame-retardant polycarbonate composite material disclosed in existing patent CN112538252A was selected as a control sample. The control sample was prepared according to its disclosed formulation. The performance of the sample of this invention and the control sample was tested under the same conditions, and their limiting oxygen index, UL94 vertical burning rating, average burning time, notched impact strength, volume resistivity, dielectric strength, light transmittance, haze, and yellowing index were compared. Furthermore, the notched impact strength retention rate, melt flow rate change rate, and volume resistivity after damp heat aging were compared. This was to evaluate the comprehensive improvement effect of the material of this invention on flame retardant properties, mechanical properties, insulation properties, optical properties, and damp heat resistance.
[0094] UL94 Vertical Flammability Rating Test: Tested according to GB / T 2408-2021, each group of materials was prepared... The strip-shaped sample was tested at 23±2 ℃ and relative humidity. The sample was conditioned for 48 hours under the specified conditions. The sample was held vertically, and a flame was applied to the lower end of the sample for 10 seconds. The flame was then removed and the first afterflame time was recorded. After the flame was extinguished, the flame was applied again for 10 seconds, and the second afterflame time and afterglow time were recorded. At the same time, it was observed whether burning drips appeared and whether the cotton pad below was ignited. The grade was determined based on the test results.
[0095] Dielectric strength testing: The test was conducted according to GB / T 1408.1-2016, and each group of materials was prepared... The flat plate sample was conditioned for 24 h at 23±2 ℃ and 50%±5% relative humidity. The sample was placed in transformer oil at 23±2 ℃, and cylindrical electrodes with diameters of 25 mm and 75 mm were used. The voltage was continuously increased at a rate of 1000 V / s under 50Hz AC conditions until the sample broke down, and the breakdown voltage was recorded. The ratio of breakdown voltage to sample thickness was used as the dielectric strength. Five parallel samples were tested in each group and the average value was taken. The unit is kV / mm.
[0096] Transmittance testing: The test was conducted according to GB / T 2410-2008, and each group of materials was prepared... The flat plate samples were conditioned for 40 h at 23±2 ℃ and 50%±10% relative humidity. Before testing, the sample surface was cleaned to ensure it was free of dust, oil, and obvious scratches. The visible light transmittance of the samples was measured using a transmittance haze meter. Three parallel samples were set up for each group, and three positions were selected for testing on each sample. The average value was taken as the transmittance.
[0097] Haze detection: The haze meter method was used to test the haze according to GB / T 2410-2008. Each group of materials was prepared... Flat samples of uniform thickness were conditioned at 23±2 ℃ and 50%±10% relative humidity for no less than 40 h. Before testing, the sample surface was kept clean, flat and free of scratches. The sample was placed in the test port of the haze meter, and the proportion of scattered light transmitted through the sample was measured and the haze was recorded.
[0098] The test results are as follows:
[0099] The test results show that both the sample of this invention and the existing patent control sample achieve a UL94V-0 rating at a thickness of 1.5 mm. However, the sample of this invention exhibits a higher limiting oxygen index and a shorter average burning time, indicating better flame retardant stability. Simultaneously, the notched impact strength, volume resistivity, and dielectric strength of the sample of this invention are higher than those of the control sample, demonstrating that the material maintains good mechanical and insulating properties while achieving fluorine-free flame retardancy. Regarding optical properties, the sample of this invention exhibits high light transmittance and low haze and yellowing index, indicating that the introduction of functional components did not significantly affect the optical properties and color stability of the polycarbonate matrix. After 168 h of humid heat aging at 85 °C and 85% RH, the sample of this invention still maintains a high notched impact strength retention rate and volume resistivity, while exhibiting a low melt flow rate change rate, indicating that the formulation and preparation process of this invention can improve the material's performance retention under humid heat conditions. Example 4
[0100] Reference Figure 9 This is the fourth embodiment of the present invention. This embodiment provides a method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material, specifically including the following steps: S1. Raw material pretreatment Branched bisphenol A type polycarbonate was dried at 90 °C for 3.5 h; hexaphenoxycyclotriphosphazene, epoxy functional group acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone were passed through an 80-mesh sieve to improve the uniformity of raw material particle size and enhance the subsequent mixing and dispersion effect.
[0101] S2. Raw material mixing By weight, 90 parts of pretreated branched bisphenol A type polycarbonate, 5.00 parts of hexaphenoxycyclotriphosphazene, 1.50 parts of epoxy functional group acrylic copolymer, 0.30 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, 0.31 parts of polycarbodiimide, 0.27 parts of pentaerythritol stearate, and 1.68 parts of 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone were weighed and added into a high-speed mixer at 900 r / min for 7 min to obtain a homogeneous mixture.
[0102] S3. Melt extrusion The resulting homogeneous mixture was fed into a twin-screw extruder at a feed rate of 10 kg / h for melt blending and extrusion. The twin-screw extruder was set with zone 1 temperature of 230 ℃, zone 2 temperature of 250 ℃, zone 3 temperature of 270 ℃, and die head temperature of 280 ℃. The screw speed was 350 r / min, and the vacuum degree was -0.09 MPa. The melt blend was continuously extruded through the die head to form strips with a diameter of 2–3 mm. These strips were then cooled and shaped in circulating cooling water at 25±2 ℃. After removing surface moisture, the strips were continuously fed into a pelletizer and pelletized at a cutter roller speed of 300 r / min to obtain fluorine-free flame-retardant polycarbonate granules with a length of 3–4 mm and a diameter of 2–3 mm.
[0103] S4. Finished Product Post-Processing The fluorine-free flame-retardant polycarbonate particles were dried at 95 °C for 2.5 h, cooled to 23±2 °C, and then sealed and packaged to obtain an environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material.
[0104] The finished fluorine-free flame-retardant polycarbonate insulating composite material has a limiting oxygen index of 32.36% and a volume resistivity of [missing information]. The dielectric strength is 28.74 kV / mm, the light transmittance is 78.62%, the notched impact strength is 68.57 kJ / m², the change rate of melt mass flow rate after wet heat aging is 4.18%, and the average burning time is 3.86 s.
[0105] In summary, by constructing a continuous matrix using branched bisphenol A type polycarbonate, introducing hexaphenoxycyclotriphosphazene to form a fluorine-free flame-retardant system, and combining it with epoxy-functionalized acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate, and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone pigment for synergistic modification, and combining high-speed mixing and twin-screw melt blending processes, the dispersion uniformity and interfacial compatibility of each functional component in the polycarbonate matrix are improved. This addresses the problem of traditional flame-retardant polycarbonate materials struggling to balance flame retardancy, mechanical properties, insulation properties, light transmittance, and hygrothermal stability.
[0106] Specifically, this invention improves the flame retardant properties of the material through hexaphenoxycyclotriphosphazene, enhances the compatibility between hexaphenoxycyclotriphosphazene and the branched bisphenol A type polycarbonate matrix through epoxy-functionalized acrylic copolymer, improves the thermal and oxygen stability and damp heat resistance of the material through a composite antioxidant of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]tris(2,4-di-tert-butylphenyl) phosphite and polycarbodiimide, and improves the melt processing fluidity and extrusion stability through pentaerythritol stearate. Simultaneously, by synergistically controlling the high-speed mixing speed, mixing time, melt extrusion temperature, screw speed, and vacuum degree, hexaphenoxycyclotriphosphazene, epoxy-functionalized acrylic copolymer, and various additives are fully dispersed in the branched bisphenol A type polycarbonate matrix, reducing the risk of thermal degradation and performance fluctuations during processing. The resulting environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material possesses good flame retardant properties, notched impact resistance, insulation properties, light transmittance, and resistance to damp heat, thus improving the long-term stability of the material in electronic, electrical, and insulating component applications.
[0107] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing an environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material, characterized in that, Includes the following steps: S1. Raw material pretreatment: Branched bisphenol A type polycarbonate is dried at 80-100 ℃ for 3-4 h. Hexaphenoxycyclotriphosphazene, epoxy functional group acrylic copolymer, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, polycarbodiimide, pentaerythritol stearate and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone are passed through a 75-85 mesh sieve to improve the uniformity of subsequent mixing and dispersion. S2. Weigh out 85-95 parts by weight of the pretreated branched bisphenol A type polycarbonate, 3.0-8.0 parts by weight of hexaphenoxycyclotriphosphazene, 0.5-2.5 parts by weight of epoxy functional group acrylic copolymer, 0.2-0.5 parts by weight of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant, 0.2-0.5 parts by weight of polycarbodiimide, 0.1-0.5 parts by weight of pentaerythritol stearate and 1.0-3.0 parts by weight of 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone, and put the above raw materials into a high-speed mixer and mix at 800-1000 r / min for 5-8 min to obtain a homogeneous mixture. S3. The homogeneous mixture is fed into a twin-screw extruder for melt blending and extrusion. The temperature of the first zone of the twin-screw extruder is 220-240 ℃, the temperature of the second zone is 240-260 ℃, the temperature of the third zone is 260-280 ℃, the die head temperature is 270-290 ℃, the screw speed is 300-400 r / min, and the vacuum degree is -0.10--0.08 MPa. The extruded strip material is water-cooled, shaped, and pelletized to obtain fluorine-free flame-retardant polycarbonate granules. S4. The fluorine-free flame-retardant polycarbonate particles are dried at 90-100 ℃ for 2-3 h, cooled to room temperature, and then sealed and packaged to obtain an environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material.
2. The method for preparing the environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S1, the drying temperature is 90 ℃; the drying time is 3.5 h; and the sieve is an 80 mesh sieve.
3. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S2, the branched bisphenol A type polycarbonate is 90 parts; the hexaphenoxycyclotriphosphazene is 5.00 parts; the epoxy functional group acrylic copolymer is 1.50 parts; the tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester and tris(2,4-di-tert-butylphenyl) phosphite composite antioxidant is 0.30 parts; the polycarbodiimide is 0.31 parts; the pentaerythritol stearate is 0.27 parts; and the 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone is 1.68 parts.
4. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S3, the feeding rate is 10 kg / h; the temperature of zone one is 230 ℃; and the temperature of zone two is 250 ℃.
5. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S4, the drying temperature is 95 ℃ and the drying time is 2.5 h.
6. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S2, the high-speed mixing speed is 900 r / min; the high-speed mixing time is 7 min.
7. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S3, the temperature of the three zones is 270 ℃; the temperature of the machine head is 280 ℃.
8. The method for preparing the environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S3, the screw rotation speed is 350 r / min; the vacuum degree is -0.09 MPa. The water-cooling and pelletizing process is as follows: the strip material with a diameter of 2-3 mm formed by extrusion is cooled and shaped by circulating water at 25±2℃ and then fed into a pelletizer. The pellets are pelletized at a speed of 300 r / min to obtain fluorine-free flame-retardant polycarbonate particles with a length of 3-4 mm and a diameter of 2-3 mm.
9. The method for preparing the environmentally friendly fluorine-free flame-retardant polycarbonate insulating composite material according to claim 1, characterized in that, In step S4, the room temperature is 23±2 ℃.
10. An environmentally friendly, fluorine-free, flame-retardant polycarbonate insulating composite material, characterized in that, The composite material exhibits a continuous matrix-dispersion-interface-regulated three-dimensional physical structure at the microscopic level. The branched bisphenol A type polycarbonate constructs the continuous matrix phase; the hexaphenoxycyclotriphosphazene is distributed in the continuous matrix phase in the form of a dispersed phase; the epoxy functional group acrylic copolymer is distributed in the interfacial region between the branched bisphenol A type polycarbonate and the hexaphenoxycyclotriphosphazene, forming an interface-regulated layer; the composite antioxidant composed of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite, polycarbodiimide, pentaerythritol stearate, and 1,4-bis[(2,4,6-trimethylphenyl)amino]-9,10-anthradinone are uniformly distributed in the continuous matrix phase and its microscopic gaps, forming a stable composite dispersion structure.
Citation Information
Patent Citations
Transparent hydrolysis-resistant weather-resistant halogen-free flame-retardant polycarbonate composite material
CN112538252A