A conductive porous material and a method for preparing and using the same
Large-sized monolayer Ti₃C₂TₓMXene was prepared by a mixed acid etching method and LiCl intercalation reaction and loaded onto porous foam. This method solves the problem of insufficient adsorption performance of existing adsorbent materials for nitroglycerin, and achieves efficient and safe adsorption of nitroglycerin. It is suitable for safe transportation and storage in military and mining blasting fields.
Patent Information
- Application Number
- CN202611219164.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-20
AI Technical Summary
Existing adsorption materials have insufficient adsorption performance for nitroglycerin and pose a risk of electrostatic sparks, leading to safety hazards and making it difficult to achieve efficient and safe adsorption of nitroglycerin.
Large-size monolayer Ti₃C₂TₓMXene was prepared by a mixed acid etching method and then loaded onto a polyurethane or polyvinyl alcohol porous foam matrix through multiple impregnations to form a conductive porous material. Combined with LiCl intercalation reaction, the conductivity and porosity of the material were enhanced to achieve efficient adsorption of nitroglycerin.
The prepared conductive porous material exhibits high adsorption capacity and rapid adsorption rate for nitroglycerin, moderate resistance, and excellent cyclic adsorption-desorption performance, significantly reducing the hazards of nitroglycerin and making it suitable for safe transportation and storage in military and mining blasting fields.
Smart Images

Figure CN123131815A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of safe adsorption technology of energetic materials, specifically relating to a conductive porous material, its preparation method and application. Background Technology
[0002] Nitroglycerin (NG, trinitroglycerin ester), as a high-energy material, is widely used in military blasting, mining, and other fields. However, it has extremely high mechanical sensitivity (explosion can be triggered by impact or friction) and thermal instability (it decomposes easily above 50°C), posing serious safety hazards during transportation, storage, and use. Furthermore, nitroglycerin leaks can cause groundwater pollution, threatening the ecological environment and human health.
[0003] Currently, diatomaceous earth, activated carbon, mesoporous silica, or metal oxides are mainly used in industry to adsorb nitroglycerin and reduce its sensitivity. However, existing materials have limitations in adsorption performance (such as low adsorption capacity and slow adsorption rate), and traditional adsorption materials are mostly poor conductors of electricity, easily generating static electricity due to friction during adsorption. Static sparks could ignite the nitroglycerin, further exacerbating safety risks. Therefore, it is essential to develop a material with high conductivity, high adsorption rate, and high adsorption capacity. Summary of the Invention
[0004] To address the problems mentioned in the background section, the present invention aims to provide a conductive porous material, its preparation method, and its applications. In terms of material design, the present invention utilizes the -F and -OH functional groups on the MXene surface to enhance oleophilicity, combined with the high porosity and interconnected pore structure of the matrix, to achieve synergistic adsorption of nitroglycerin through "surface adsorption-capillary condensation." The monolayer preparation process employs a mixed acid etching method combined with LiCl intercalation reaction to scalably prepare large-size monolayer Ti3C2T. x MXene is loaded through multiple impregnation processes, which are simple and controllable. In terms of performance, the material resistivity ranges from 0.1 to 1.5 MΩ, and the swelling rate is less than 3.0% when adsorbed at 5 times its own weight. After 10 cycles of adsorption-desorption, Ti3C2T... x @PU adsorption capacity remains above 90% of the initial value, Ti3C2T x The PVA adsorption capacity remains above 80% of its initial value. This conductive porous material can efficiently passivate the hazards of nitroglycerin, making it suitable for safe transportation and storage in military and mining blasting fields. It can also be extended to organic solvent recovery, demonstrating promising industrialization prospects.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: On the one hand, the present invention provides a conductive porous material, comprising a matrix and a functional modifier, wherein the functional modifier is loaded on the matrix; The matrix is polyurethane porous foam or polyvinyl alcohol porous foam; The functional modifier is a monolayer Ti3C2T x MXene, the monolayer Ti3C2T x The average lateral dimension of Mxene is 10–13 μm, and the monolayer Ti3C2T x The thickness of MXene is 0.98–1.8 nm. This invention uses polyurethane porous foam or polyvinyl alcohol porous foam as the matrix. Compared with polyurethane porous foam or polyvinyl alcohol porous foam, metal foam or ceramic foam has poorer adsorption compatibility and capillary coagulation effect for nitroglycerin, and cannot achieve efficient adsorption.
[0006] MXene is a novel two-dimensional (2D) material, T x These represent functional groups (-OH, -O, and -F) on the surface of the material. MXene materials possess excellent intrinsic electrical conductivity, outstanding mechanical properties, and a unique two-dimensional layered structure, while their surface is rich in a variety of tunable functional groups.
[0007] Furthermore, the porosity of the polyurethane porous foam is 85%–95%, and the pore size is 150–400 μm; The polyvinyl alcohol porous foam has a porosity of 80%–91% and a pore size of 150–500 μm.
[0008] Furthermore, the loading rate of the functional modifier is 4% to 9%, preferably 7% to 9%, and the formula for calculating the loading rate is as follows:
[0009] In the formula, The mass of the conductive porous material, The mass of the matrix is given.
[0010] Furthermore, the monolayer Ti3C2T x The preparation method of MXene includes the following steps: (1) Mix hydrofluoric acid and concentrated hydrochloric acid evenly to obtain an etching solution; (2) Slowly add Ti3AlC2-MAX powder to the etching solution. After the addition is complete, continue the etching reaction. After the etching reaction is completed, centrifuge the solution, discard the supernatant, and wash the precipitate until the pH of the supernatant after centrifugation is ≥6 to obtain the washed precipitate. (3) The washed precipitate was dispersed in LiCl solution for intercalation reaction. After the intercalation reaction was completed, the precipitate was centrifuged and the supernatant was discarded. The precipitate was washed until the supernatant showed no obvious stratification after centrifugation. After washing, water was added to the precipitate to obtain a dispersion. The dispersion was mechanically vibrated to remove the precipitate and obtain a monolayer Ti3C2T.x MXene colloidal suspension.
[0011] The monolayer Ti3C2T x MXene exhibits low defect levels. SEM characterization shows no significant damage and intact lamellae. TEM characterization reveals straight edges without jaggedness. HRTEM characterization shows continuous and clear hexagonal lattice fringes without interruption. SAED characterization shows sharp six-fold symmetric diffraction points. This indicates a monolayer Ti3C2T. x The MXene surface is free of obvious damage, has a complete structure, straight edges without serrations, and a relatively complete crystal structure.
[0012] Further, the washing of the obtained precipitate in step (2) until the pH of the supernatant after centrifugation is ≥6 is specifically as follows: add water to the obtained precipitate and shake it thoroughly to disperse it evenly, then centrifuge and discard the supernatant, repeat the above "add water-centrifuge and discard supernatant" operation until the pH of the supernatant after centrifugation is ≥6.
[0013] Further, the washing of the obtained precipitate in step (3) until the supernatant after centrifugation has no obvious stratification is specifically as follows: add water to the obtained precipitate and shake it thoroughly to disperse it evenly, then centrifuge and discard the supernatant, repeat the above "add water-centrifuge and discard supernatant" operation until the supernatant after centrifugation has no obvious stratification.
[0014] Further, in step (1), the volume ratio of hydrofluoric acid to concentrated hydrochloric acid is (0.7-2.2):1, the concentration of hydrofluoric acid is 49 wt%, and the concentration of concentrated hydrochloric acid is 38 wt%. And / or, the volume ratio of the hydrofluoric acid in step (1) to the mass ratio of the Ti3AlC2-MAX powder in step (2) is (8-12 mL): 1 g, and the concentration of the hydrofluoric acid is 49 wt%; And / or, the Ti3AlC2-MAX powder described in step (2) has a mesh size of 300; And / or, the etching reaction temperature in step (2) is 25-30°C, and the etching reaction time is 10-14h; And / or, the volume ratio of the LiCl solution in step (3) to the mass ratio of the Ti3AlC2-MAX powder in step (2) is (8-12 mL): 1 g, and the concentration of the LiCl solution is 1.2 mol / L; And / or, the temperature of the intercalation reaction in step (3) is room temperature, and the time of the intercalation reaction is 8 to 12 hours; And / or, the power of the mechanical oscillation stripping in step (3) is 1000-1200W, and the time of the mechanical oscillation stripping is 30-40min; And / or, the monolayer Ti3C2T described in step (3) x The concentration of MXene colloidal suspension is 30–50 mg / mL.
[0015] Furthermore, the etching reaction process described in step (2) involves a rotation speed of 400–500 rpm. The rotation speed used during the etching reaction affects the progress of the etching reaction. While a rotation speed greater than 500 rpm will accelerate the reaction, it will also cause over-etching of Ti3AlC2-MAX, reducing the Ti3C2T... x The quality of MXene is affected, and liquid splashing also poses a significant chemical safety risk. A rotation speed below 400 rpm can lead to incomplete reactions, prolonging etching time and causing uneven etching of Ti3AlC2-MAX, which also affects the final Ti3C2T etching result. x The quality of MXene.
[0016] Further, the Ti3AlC2-MAX powder described in step (2) is added slowly in 5 to 8 portions. The purpose of adding it slowly in 5 to 8 portions is to ensure that the initial concentration of the etchant is excessive each time the Ti3AlC2-MAX powder is added, and that adding a small amount allows the Ti3AlC2-MAX powder to be evenly dispersed and avoids clumping, thus ensuring sufficient etching. The interval between two additions is 1 to 2 minutes. Stirring is performed while adding the powder.
[0017] Furthermore, the rotation speed during the intercalation reaction in step (3) is 800–900 rpm. A rotation speed greater than 900 rpm will shear and damage Ti3C2T. x The size of the MXene sheets; a rotation speed of less than 800 rpm will cause uneven intercalation, resulting in poor subsequent peeling effect.
[0018] Further, the solvent in the LiCl solution in step (3) is at least one of water, ethanol, and N,N-dimethylformamide, preferably water.
[0019] The mixed acid etching method used in this invention, combined with LiCl intercalation reaction, effectively reduces the Ti3C2T content while ensuring efficient etching and removal of the Al layer in Ti3AlC2-MAX powder. x The introduction of surface defects into MXene nanosheets effectively increased the interlayer spacing of MXene through the intercalation reaction, inhibiting the recombination of nanosheets during subsequent processing. Furthermore, mechanical oscillation exfoliation ensured the integrity of Ti3C2T. x MXene nanosheets have large lateral dimensions, enabling the successful fabrication of large-size, low-defect monolayer Ti3C2T. x MXene significantly improves its intrinsic conductivity.
[0020] On the other hand, the present invention provides a method for preparing any of the above-described conductive porous materials, comprising the following steps: (1) The substrate is cleaned and dried to obtain the pretreated substrate; (2) The above-mentioned single-layer Ti3C2T x MXene colloidal suspension was diluted to 5–8 mg / mL (when the concentration was less than 5 mg / mL, the increase in matrix loading rate after impregnation was not significant, and the increase in conductivity was low; when the concentration was greater than 8 mg / mL, Ti3C2T…). x MXene colloidal suspension has a high viscosity, and Ti3C2T is present during matrix impregnation. x MXene colloidal suspensions do not easily penetrate into the matrix and may clog pores. This results in a 5–8 mg / mL monolayer of Ti3C2T. x MXene colloidal suspension; the pretreated matrix is immersed in 5-8 mg / mL Ti3C2T monolayer. x The material is immersed in an MXene colloidal suspension, then removed, and its surface is dried after being blotted with filter paper. The immersion-drying process is repeated to obtain the conductive porous material.
[0021] Further, step (1) specifically involves: ultrasonically cleaning the substrate with water 3-4 times and ultrasonically cleaning it with anhydrous ethanol 2-3 times in sequence, and then drying it at 75-85℃ for 1-1.5h to obtain the pretreated substrate.
[0022] Furthermore, the ultrasonic cleaning frequency is 40–60 kHz, the ultrasonic cleaning power is 80–120 W, and the ultrasonic cleaning time is 3–5 min.
[0023] Furthermore, the immersion time in step (2) is 3 to 5 minutes; And / or, the drying temperature in step (2) is 75-85°C, and the drying time is 30-40 min; And / or, when the matrix is polyurethane porous foam, the number of repetitions in step (2) is 2 to 3 times; when the matrix is polyvinyl alcohol porous foam, the number of repetitions in step (2) is 1 to 2 times.
[0024] On the other hand, the present invention provides an application of any of the above-described conductive porous materials or conductive porous materials prepared by any of the above-described preparation methods in the efficient adsorption, safe handling, transportation, and storage of nitroglycerin.
[0025] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention uses a mixed acid etching method, by adjusting the H of the etching solution + / F- By adjusting the proportions, reaction temperature, and stirring rate, and combining this with the LiCl intercalation reaction, a low-defect monolayer Ti3C2T with an average lateral dimension of 10–13 μm was prepared. x MXene, with functional groups such as -F and -OH on its surface, has excellent electrical conductivity and provides a high-quality modifier for the modification of porous materials.
[0026] (2) This invention employs a multiple impregnation method, controlling the number of impregnations, suspension concentration, and drying conditions to achieve uniform loading (loading rate 4~9%) of MXene on the surface of porous materials. This forms a continuous conductive network (resistance value between 0.1 and 1.5 MΩ) without clogging the pores, preserving the high porosity of the material and significantly improving the adsorption efficiency of nitroglycerin. This design is for regulating Ti3C2T x The uniform composite of MXene with porous materials and the problem of conductivity provide an effective solution for achieving efficient adsorption and safe passivation of nitroglycerin.
[0027] (3) The saturated adsorption capacity of the conductive porous material of the present invention for nitroglycerin: Ti3C2T x @PU>15.0g / g, Ti3C2T x @PVA > 24.0 g / g; swelling ratio < 3.0% when adsorbed at 5 times its own weight, and < 4.5% when adsorbed at 8 times its own weight; resistivity between 0.1 and 1.5 MΩ; after 10 cycles of adsorption-desorption, Ti3C2T x The saturated adsorption capacity of @PU remains above 90% of its initial value, Ti3C2T x The saturated adsorption capacity of @PVA remained above 80% of its initial value. After 1 minute of adsorption, Ti3C2T... x @PU adsorption rate > 8.0 g / g, Ti3C2T x @PVA adsorption rate >12.0g / g. Attached Figure Description
[0028] Figure 1 In this context, 'a' refers to the monolayer Ti3C2T prepared in Example 1 of this invention. x SEM images of MXene, Figure 1 In this context, 'b' represents the monolayer Ti3C2T prepared in Example 1 of this invention. x TEM images of MXene Figure 1 In this context, 'c' represents the monolayer Ti3C2T prepared in Example 1 of this invention. x AFM images of MXene Figure 1 In this paper, d and e refer to the monolayer Ti3C2T prepared in Example 1 of this invention. x HRTEM images of MXene at different magnifications, Figure 1In this context, f represents the monolayer Ti3C2T prepared in Example 1 of this invention. x SAED spectrum of MXene; Figure 2 In this paper, 'a' and 'd' represent the monolayer Ti3C2T prepared in Example 1 of this invention, respectively. x SEM images and size distribution statistics of MXene, Figure 2 In the figure, b and e represent the monolayer Ti3C2T prepared in Comparative Example 4 of this invention, respectively. x SEM images and size distribution statistics of MXene, Figure 2 In the figure, c and f are the monolayer Ti3C2T prepared in Comparative Example 5 of this invention, respectively. x SEM images and size distribution statistics of MXene; Figure 3 a, b, and c in the figure are SEM images of commercially available polyurethane porous foam used in this invention at different resolutions. Figure 3 In the figure, d, e, and f represent Ti3C2T prepared in Comparative Example 1 of this invention at different resolutions. x SEM image of @PU; Figure 4 In this context, 'a' refers to the Ti3AlC2-MAX powder used in Example 1 of this invention and the monolayer Ti3C2T prepared in Example 1. x XRD images of MXene Figure 4 In this paper, b represents the commercially available polyurethane porous foam used in this invention and the Ti3C2T prepared in Comparative Example 1. x FTIR image of @PU, Figure 4 In this paper, c represents the Ti3C2T prepared in Comparative Example 1 of this invention. x @PU's XPS full spectrum image Figure 4 In this paper, d represents the Ti3C2T prepared in Comparative Example 1 of this invention. x Narrow scan image of Ti element in @PU; Figure 5 In this context, 'a' refers to the Ti3C2T prepared in Examples 2-3 and Comparative Examples 1-2 of this invention. x @PU's MXene loading rate versus resistance value graph Figure 5 In this context, 'b' refers to the Ti3C2T prepared in Examples 4-5 and Comparative Example 3 of this invention. x MXene loading rate versus resistance value graph for @PVA; Figure 6 In this invention, 'a' refers to the commercially available polyurethane porous foam used in this invention, and the Ti3C2T prepared in Examples 2-3. x @PU and Ti3C2T prepared in Comparative Examples 1-2 x@PU adsorption rate at 1 min, adsorption rate at 5 min, and saturation adsorption rate. Figure 6 In this invention, b represents the commercially available polyvinyl alcohol porous foam used in this invention, and the Ti3C2T prepared in Examples 4 and 5. x @Ti3C2T prepared in PVA and Comparative Example 3 x @PVA adsorption rate at 1 min, adsorption rate at 5 min, and saturation adsorption rate; Figure 7 In this context, 'a' refers to the Ti3C2T prepared in Example 3 of this invention. x @PU and Ti3C2T prepared in Example 5 x @Swelling rate images of PVA at 5 and 8 times its own weight when adsorbed. Figure 7 In this context, b represents the Ti3C2T prepared in Example 3 of this invention. x @PU and Ti3C2T prepared in Example 5 x @Adsorption rate image of PVA cycle "adsorption-desorption" process 10 times. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be noted that the specific embodiments described herein are only for explaining and illustrating the technical solutions of this invention and do not constitute a limitation on the scope of protection of this invention.
[0030] Based on the embodiments disclosed in this invention, all other embodiments obtained by those skilled in the art through direct application or simple adjustment without creative effort are within the protection scope of the claims of this invention.
[0031] It should be understood that the terminology used in this invention is for describing specific embodiments only and does not constitute a limitation on the scope of the invention. Furthermore, regarding the numerical ranges involved in this invention, it should be explicitly understood that all intermediate values between the upper and lower limits of the range are specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and every other stated value or intermediate value within a stated range, is included within the scope of protection of this invention. The upper and lower limits of these smaller ranges can be independently selected to include or exclude from the range.
[0032] Unless otherwise stated, the methods used in the following embodiments are conventional methods in the art; the reagents and materials used are commercially available unless otherwise specified.
[0033] Example 1 Single-layer Ti3C2T xPreparation of MXene colloidal suspension: (1) In a polytetrafluoroethylene reactor, 40 mL of 49 wt% hydrofluoric acid (Sinopharm Chemical Reagent Shaanxi Co., Ltd., AR grade) and 40 mL of 38 wt% concentrated hydrochloric acid (Sinopharm Chemical Reagent Shaanxi Co., Ltd., AR grade) were mixed and stirred at 300 rpm for 10 min to obtain etching solution; (2) 4 g Ti3AlC2-MAX powder (300 mesh, Foshan Xinxi Technology Co., Ltd.) was slowly added to the etching solution in 6 portions while stirring. The interval between the two additions was 2 minutes. After the addition was completed, the rotation speed was increased to 500 rpm and the etching reaction was carried out at 25°C for 12 hours. After the etching reaction was completed, the reaction solution was centrifuged at 3500 rpm for 1 minute and the supernatant was discarded. Then, deionized water was added to the precipitate and the precipitate was shaken thoroughly to redisperse the precipitate. Then, the supernatant was discarded by centrifugation. The above operation of "adding deionized water - centrifugation and discarding supernatant" was repeated until the pH test paper of the supernatant showed that the pH was ≥6, and the washed precipitate was obtained. (3) The washed precipitate was added to 40 mL of 1.2 mol / L LiCl solution and the intercalation reaction was carried out at 900 rpm at room temperature for 10 hours. After the intercalation reaction was completed, the reaction mixture was centrifuged at 5000 rpm for 1 min, and the supernatant was discarded. Then, deionized water was added to the obtained precipitate, and the mixture was shaken thoroughly to disperse it evenly. The mixture was then centrifuged again, and the supernatant was discarded. The above operation of "adding deionized water - centrifuging and discarding supernatant" was repeated until there was no obvious stratification of the supernatant after centrifugation. After washing, deionized water was added to the obtained precipitate to obtain a dispersion. The dispersion was placed on a mechanical oscillator and mechanically oscillated (1200W) for 30 min to obtain a monolayer Ti3C2T with a concentration of 36.9 mg / mL. x MXene colloidal suspension.
[0034] Single-layer Ti3C2T x Preparation of Mxene: A monolayer of Ti3C2T x The MXene colloidal suspension was vacuum filtered and dried at 50°C for 2 hours to obtain a monolayer of Ti3C2T. x MXene (denoted as MA-Ti3C2T) x ).
[0035] Example 2 Preparation of conductive porous materials: (1) Commercial polyurethane porous foam (Foshan Bomei Packaging Materials Products Co., Ltd., porosity 94.1%, pore size 150~400μm, denoted as PU) was selected and cut into 5×5×5cm cubic samples. The samples were ultrasonically cleaned 3 times with deionized water (5min each time, ultrasonic cleaning frequency 40kHz, power 120W) and ultrasonically cleaned 2 times with anhydrous ethanol (5min each time, ultrasonic cleaning frequency 40kHz, power 120W) to remove surface impurities. Then, it was placed in an 80℃ forced-air drying oven (Shanghai Yiheng Scientific Instrument Co., Ltd., DHG-9140A) and dried for 1h to obtain pretreated polyurethane porous foam; (2) The single-layer Ti3C2T with a concentration of 36.9mg / mL in Example 1 was used. x MXene colloidal suspension was mixed with deionized water and sonicated (frequency 40kHz, power 120W, time 5min) to ensure uniform dispersion of MXene sheets without aggregation, thus preparing a monolayer Ti3C2T with a concentration of 6mg / mL. x MXene colloidal suspension; pretreated polyurethane porous foam was immersed in 6 mg / mL monolayer Ti3C2T x In MXene colloidal suspension for 3 minutes, ensure monolayer Ti3C2T x The MXene colloidal suspension was allowed to fully penetrate the pores of the sample. The sample was then removed, excess liquid was absorbed with filter paper, and the sample was dried at 80°C for 30 minutes. This immersion-drying process was repeated twice to obtain a conductive porous material, denoted as Ti3C2T. x @PU.
[0036] Example 3 Preparation of conductive porous material: Compared with Example 2, the only difference is that the immersion in the drying process is repeated 3 times.
[0037] Example 4 Preparation of conductive porous material: Compared with Example 2, the only difference is that the commercial polyurethane porous foam in Example 2 is replaced with commercial polyvinyl alcohol porous foam (Foshan Bomei Packaging Materials Products Co., Ltd., porosity 90.5%, pore size 150~500μm, denoted as PVA), and the immersion and drying process is repeated once. The resulting conductive porous material is denoted as Ti3C2T. x @PVA.
[0038] Example 5 Preparation of conductive porous material: Compared with Example 2, the only difference is that the commercial polyurethane porous foam in Example 2 is replaced with commercial polyvinyl alcohol porous foam (Foshan Bomei Packaging Materials Products Co., Ltd., porosity 90.5%, pore size 150~500μm, denoted as PVA). The resulting conductive porous material is denoted as Ti3C2T. x@PVA.
[0039] Comparative Example 1 Preparation of conductive porous material: Compared with Example 2, the only difference is that the immersion in the drying process was repeated 0 times.
[0040] Comparative Example 2 Preparation of conductive porous material: Compared with Example 2, the only difference is that the immersion in the drying process is repeated once.
[0041] Comparative Example 3 Preparation of conductive porous material: Compared with Comparative Example 1, the only difference is that the commercial polyurethane porous foam in Comparative Example 1 is replaced with commercial polyvinyl alcohol porous foam (Foshan Bomei Packaging Materials Products Co., Ltd., porosity 90.5%, pore size 150~500μm, denoted as PVA). The resulting conductive porous material is denoted as Ti3C2T. x @PVA.
[0042] Comparative Example 4 Monolayer Ti3C2T was prepared using the conventional hydrofluoric acid (HF) etching method. x MXene (denoted as HF-Ti3C2T) x ): First, 40 mL of 49 wt% HF and 10 mL of deionized water were weighed and placed together in a polytetrafluoroethylene (PTFE) reactor. The reactor was then placed in an ice-water bath and stirred for 30 min to ensure thorough mixing. Next, 2 g of Ti3AlC2-MAX powder (300 mesh, Foshan Xinxi Technology Co., Ltd.) was weighed and slowly added to the reactor along its inner wall. The reactor was then covered and reacted at a constant temperature of 40°C for 48 h. After the reaction was complete, the reaction product was washed multiple times with deionized water until the pH of the supernatant was ≥6. The MXene precipitate at the bottom of the reactor was then thoroughly mixed with 40 mL of a 5 wt% tetrabutylammonium hydroxide (TBAOH) aqueous solution and stirred continuously at room temperature for 24 h to complete the intercalation reaction. After the intercalation reaction, the reaction system was centrifuged to collect the precipitate. The precipitate was washed to completely remove any residual intercalating agent, and deionized water was added to the washed precipitate to obtain a dispersion.
[0043] Finally, the intercalated Ti3C2T xMXene was subjected to ultrasonic exfoliation. The specific exfoliation method was as follows: First, the dispersion was ultrasonically treated in an ice-water bath for 30 min. After ultrasonication, it was transferred to a centrifuge tube and centrifuged at 3500 r / min for 1 min. The supernatant was collected and ultrasonically treated again in an ice-water bath for 30 min. After ultrasonication, centrifugation was performed (the centrifugation speed was increased to 5000 r / min and the centrifugation time was maintained at 1 min). The ice-water bath ultrasonic exfoliation and centrifugation were repeated. The initial centrifugation parameters were set at 3500 r / min for 1 min. As the number of treatments increased, the centrifugation parameters were gradually increased to 9000 r / min for 10 min. The supernatant was collected after each centrifugation. The above ultrasonic exfoliation-centrifugation collection operation was repeated until no obvious precipitate was formed at the bottom of the centrifuge tube after centrifugation. The monolayer Ti3C2T was thus prepared. x MXene solution.
[0044] Comparative Example 5 Monolayer Ti3C2T was prepared using in-situ HF etching. x MXene (denoted as is -Ti3C2T x ): 40 mL of 38 wt% concentrated hydrochloric acid, 10 mL of deionized water, and 2 g of lithium fluoride (LiF) were added to a tetrafluoroethylene reactor and stirred for 30 min to completely dissolve the LiF, obtaining an etching solution. Then, 2 g of Ti3AlC2-MAX powder (300 mesh, Foshan Xinxi Technology Co., Ltd.) was gradually added to the etching solution over 10 min, and the reaction was carried out at 40 °C for 48 h. After the reaction, the mixture was centrifuged, and the resulting precipitate was washed with 1 mol / L HCl solution to remove residual LiF, followed by washing with deionized water until the pH of the supernatant was ≥6. The washed precipitate was then thoroughly mixed with 40 mL of 5 wt% tetrabutylammonium hydroxide (TBAOH) aqueous solution and stirred for 24 h to complete the intercalation reaction. After the intercalation reaction was complete, the reaction system was centrifuged to collect the precipitate. The precipitate was washed until the supernatant was colorless and transparent after centrifugation, and deionized water was added to the washed precipitate to obtain a dispersion.
[0045] Finally, the intercalated Ti3C2T xMXene was subjected to ultrasonic exfoliation. The specific exfoliation method was as follows: First, the dispersion was ultrasonically treated in an ice-water bath for 30 min. After ultrasonication, it was transferred to a centrifuge tube and centrifuged at 3500 r / min for 1 min. The supernatant was collected and ultrasonically treated again in an ice-water bath for 30 min. After ultrasonication, centrifugation was performed (the centrifugation speed was increased to 5000 r / min and the centrifugation time was maintained at 1 min). The ice-water bath ultrasonic exfoliation and centrifugation were repeated. The initial centrifugation parameters were set at 3500 r / min for 1 min. As the number of treatments increased, the centrifugation parameters were gradually increased to 9000 r / min for 10 min. The supernatant was collected after each centrifugation. The above ultrasonic exfoliation-centrifugation collection operation was repeated until no obvious precipitate was formed at the bottom of the centrifuge tube after centrifugation. The monolayer Ti3C2T was thus prepared. x MXene solution.
[0046] The monolayer Ti3C2T prepared in Example 1 x MXene was tested using a scanning electron microscope (SEM), and the results are as follows: Figure 1 As shown in a, from Figure 1 As can be seen from 'a' in the figure, monolayer Ti3C2T x The MXene surface is smooth and clean, with no obvious structural defects such as fractures, breaks, or pores observed. Furthermore, it perfectly conforms to the contours of the substrate pores, indicating that it possesses both excellent structural integrity and interface compatibility. The monolayer Ti3C2T prepared in Example 1... x MXene was tested using transmission electron microscopy (TEM), and the results are as follows: Figure 1 As shown in b, from Figure 1 As can be seen from b in the figure, a single layer of Ti3C2T x MXene exhibits a uniform light gray translucent morphology, and no alternating light and dark stripes caused by multi-layer stacking were observed in the field of view. Meanwhile, a single layer of Ti3C2T... x The MXene surface was clean, free of obvious impurities, and the edges of the sheets were straight and without serrations. The monolayer Ti3C2T prepared in Example 1... x MXene was tested using atomic force microscopy (AFM), and the results are as follows: Figure 1 As shown in c, from Figure 1 As can be seen from 'c', the AFM image shows a single layer of Ti3C2T. x The thickness of the MXene nanosheets is 1.2 nm. This is in contrast to the monolayer Ti3C2T prepared in Example 1. x MXene was tested using high-resolution transmission electron microscopy (HRTEM), and the results are as follows: Figure 1 As shown in d and e. The monolayer Ti3C2T prepared in Example 1. xMXene performed selected area electron diffraction (SAED) tests, and the results are as follows: Figure 1 As shown in f in the figure. From Figure 1 As can be seen from d, e, and f in the image, the HRTEM image shows clear, continuous lattice fringes, and the SAED pattern exhibits typical hexagonal symmetric diffraction spots, indicating that the monolayer Ti3C2T prepared in Example 1 is... x MXene has a complete hexagonal crystal structure, high crystallinity, low defect density, and retains the intrinsic lattice characteristics of two-dimensional materials well.
[0047] The monolayer Ti3C2T prepared in Example 1, Comparative Example 4, and Comparative Example 5 x Mxene performed scanning electron microscopy tests and ImageJ software statistical analysis, and the results are as follows: Figure 2 As shown in the figures a, b, c, d, e, and f. From Figure 2 As can be seen from a, b, and c in the figures, the monolayer Ti3C2T prepared in Example 1, Comparative Example 4, and Comparative Example 5... x MXene exhibits significant differences in lateral dimensions and structural integrity, with the monolayer Ti3C2T prepared in Example 1 showing the most significant differences. x MXene exhibits superior quality, larger lateral dimensions, and virtually no obvious pores or defects on its surface, while the monolayer Ti3C2T prepared in Comparative Example 4... x Mxene not only has a small lateral dimension, but also exhibits obvious monolayer fragments. Figure 2 (b below). Meanwhile, the monolayer Ti3C2T prepared in Comparative Example 5... x The Mxene exhibits noticeable voids at its edges, resulting in poor lamellar integrity. Figure 2 As can be seen from d, e, and f in Example 1, the monolayer Ti3C2T prepared... x The size distribution of MXene ranges from 9.4 to 13.6 µm (average 12.5 µm). Comparative Examples 4 and 5 show monolayer Ti3C2T... x The size distributions of Mxene are 3.8–6.7 µm (average 5.6 µm) and 3.5–7.8 µm (average 4.3 µm), respectively, indicating that the monolayer Ti3C2T prepared in Example 1 has the desired size distribution. x MXene is much larger than the monolayer Ti3C2T prepared in Comparative Examples 4 and 5. x MXene.
[0048] The commercially available polyurethane porous foam used and the Ti3C2T prepared in Comparative Example 1 were compared. x @PU underwent scanning electron microscopy testing, and the results are as follows: Figure 3 As shown. From Figure 3As can be seen from the preparation process of impregnation and drying, the monolayer Ti3C2T x MXene is uniformly distributed on the porous polyurethane foam, and the porous polyurethane foam is loaded with a single layer of Ti3C2T. x The MXene hole structure was completely preserved, and the shape and size of the hole did not change significantly.
[0049] The Ti3AlC2-MAX powder used in Example 1 and the monolayer Ti3C2T prepared in Example 1 x MXene was used for XRD characterization, and the results are as follows: Figure 4 As shown in Figure a, the disappearance of peak (104) indicates that the Al layer has been completely etched, and the shift of peak (002) to a lower angle indicates that Ti3C2T has been etched. x The interlayer spacing of MXene nanosheets increased. This was compared to the commercially available polyurethane porous foam (PU) used and the Ti3C2T prepared in Comparative Example 1. x @PU was characterized by FTIR, and the results are as follows Figure 4 As shown in b in the diagram. From Figure 4 As can be seen from b in the figure, PU is at 1095cm -1 An absorption peak for CO bonds appeared nearby; when a monolayer of Ti3C2T was loaded onto PU... x The peak of the CO bond after MXene shows a blue shift, which may be due to monolayer Ti3C2T. x The reaction of MXene with PU forms Ti-OC bonds, and the vibrations of the Ti-O bonds couple with the vibrations of the OC bonds, causing the peak position to shift towards higher wavenumbers. This is compared to the Ti3C2T prepared in Comparative Example 1. x XPS characterization was performed on the @PU, and the results are as follows: Figure 4 As shown in c and d. Figure 4 The 'c' indicates that a single layer of Ti3C2T is loaded on the PU. x Following MXene, Ti3C2T appeared on its surface. x The characteristic peaks of Ti 2p further confirm that monolayer Ti3C2T x MXene has been successfully loaded onto PU surfaces. Figure 4 The d in the figure indicates that in Ti3C2T x After being bonded to PU, Ti-OC- chemical bonds appear on the surface of the material.
[0050] The Ti3C2T prepared in Examples 2-3 and Comparative Examples 1-2 x @PU conducted MXene loading rate and resistance value tests. The resistance value test method involved taking a 5cm×5cm×5cm cube of Ti3C2T. X@PU, clamp both ends of the carbon rod tightly, and connect the two ends of the carbon rod to the Keithley 2400 digital source meter using wires. Set the Keithley 2400 digital source meter to resistance measurement mode. Record the resistance value every 30 seconds. A difference of ≤5% between two consecutive resistance values is considered valid data. The results are as follows... Figure 5 As shown in a. From Figure 5 As can be seen from 'a', the MXene loading rate increases with the number of immersion-drying processes, reaching a maximum of 8.3% as in Example 3. With the increase in loading rate, Ti3C2T... x The resistance value of @PU continuously decreased, reaching a minimum of 0.3801 × 10⁻⁶ in Example 3. 6 Ω. The Ti3C2T prepared in Examples 4-5 and Comparative Example 3... x @PVA performed MXene loading rate and resistance value tests. The resistance value test method involved taking a 5cm×5cm×5cm cube of Ti3C2T. X @PVA, clamp both ends of the carbon rod tightly, and connect the two ends of the carbon rod to a Keithley 2400 digital source meter using wires. Set the Keithley 2400 digital source meter to resistance measurement mode, and record the resistance value every 30 seconds. Data with a difference of ≤5% between two consecutive resistance values is considered valid. The results are as follows. Figure 5 As shown in b in the diagram. From Figure 5 As can be seen from b, with the increase of the number of "immersion-drying" processes, the MXene loading rate increases, with the highest loading rate being 8.4% of that in Example 5. As the loading rate increases, Ti3C2T... x The resistance of the PVA decreased continuously, reaching a minimum of 0.1673 × 10⁻⁶ in Example 5. 6 Ω. Figure 5 The test results show that the Ti3C2T prepared in Example 3 x The resistance value of @PU is the optimal result. The Ti3C2T prepared in Example 5... x The PVA resistance value is the optimal result.
[0051] Commercial polyurethane porous foam (PU) and Ti3C2T prepared in Examples 2-3 x @PU and Ti3C2T prepared from Comparative Examples 1-2 x The adsorption rate of @PU was tested at different times, and the results are as follows: Figure 6 As shown in a. From Figure 6 As can be seen from 'a' in the figure, as the MXene loading rate increases, Ti3C2T xThe adsorption rates of @PU increased rapidly at 1 min and 5 min, reaching a maximum of 8.6 g / g and 10.6 g / g in Example 3, respectively, representing increases of 83% and 24.7% compared to unmodified PU. The saturated adsorption rate remained relatively stable before and after modification. This was observed in commercial polyvinyl alcohol porous foam (PVA) and the Ti3C2T prepared in Examples 4-5. x @Ti3C2T prepared by PVA and Comparative Example 3 x The adsorption rate of PVA at different times was tested, and the results are as follows: Figure 6 As shown in b in the diagram. From Figure 6 As can be seen from b in the figure, as the MXene loading rate increases, Ti3C2T x The 1-minute adsorption rate of @PVA steadily increased, reaching a maximum of 12.5 g / g in Example 5, which is 10.6% higher than that of unmodified PVA. The 5-minute adsorption rate and saturated adsorption rate remained basically stable before and after modification. Figure 6 The test results show that the Ti3C2T prepared in Example 3 x The adsorption capacity and adsorption rate of PU were the optimal results. Example 5 prepared Ti3C2T x The adsorption capacity and adsorption rate of PVA are the optimal results.
[0052] The Ti3C2T prepared in Example 3 x @PU, Ti3C2T prepared in Example 5 x @PVA was tested for adsorption swelling rate at 5 times its own weight and 8 times its own weight, and the results are as follows: Figure 7 As shown in a. From Figure 7 As can be seen from 'a' in Ti3C2T x The swelling rates of @PU at 5 times and 8 times its own weight were 2.6% and 4.2%, respectively, and the swelling rates of Ti3C2T were also observed. x The swelling rates of the Ti3C2T prepared in Example 3 were 2.5% and 4.1% when adsorbed at 5 and 8 times its own weight of PVA, respectively. x @PU, Ti3C2T prepared in Example 5 x @PVA was subjected to cyclic adsorption performance testing, and the results are as follows: Figure 7 As shown in b in the diagram. From Figure 7 As can be seen from b in Ti3C2T x After 10 cycles of the @PU "adsorption-desorption" process, the saturated adsorption rate was 14.66 g / g, maintaining 96.4% of the initial adsorption rate (the initial value used was the adsorption rate after one cycle of adsorption). Ti3C2T x After 10 cycles of the PVA "adsorption-desorption" process, the saturated adsorption rate was 21.71 g / g, maintaining 88% of the initial adsorption rate (the initial value was the adsorption rate after 1 cycle of adsorption).
[0053] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A conductive porous material, characterized in that, It includes a matrix and a functional modifier, wherein the functional modifier is loaded on the matrix; The matrix is polyurethane porous foam or polyvinyl alcohol porous foam; The functional modifier is a monolayer Ti3C2T x MXene, the monolayer Ti3C2T x The average lateral dimension of MXene is 10–13 μm, and the monolayer Ti3C2T x The thickness of MXene is 0.98–1.8 nm.
2. The conductive porous material according to claim 1, characterized in that, The polyurethane porous foam has a porosity of 85%–95% and a pore size of 150–400 μm; The polyvinyl alcohol porous foam has a porosity of 80%–91% and a pore size of 150–500 μm.
3. The conductive porous material according to claim 1, characterized in that, The loading rate of the functional modifier is 4% to 9%, and the formula for calculating the loading rate is as follows:
4. In the formula, The mass of the conductive porous material, The mass of the matrix is given.
5. The conductive porous material according to claim 1, characterized in that, The monolayer Ti3C2T x The preparation method of MXene includes the following steps: (1) Mix hydrofluoric acid and concentrated hydrochloric acid evenly to obtain an etching solution; (2) Slowly add Ti3AlC2-MAX powder to the etching solution. After the addition is complete, continue the etching reaction. After the etching reaction is completed, centrifuge the solution, discard the supernatant, and wash the precipitate until the pH of the supernatant after centrifugation is ≥6 to obtain the washed precipitate. (3) The washed precipitate was dispersed in LiCl solution for intercalation reaction. After the intercalation reaction was completed, the precipitate was centrifuged and the supernatant was discarded. The precipitate was washed until the supernatant showed no obvious stratification after centrifugation. After washing, water was added to the precipitate to obtain a dispersion. The dispersion was mechanically vibrated to remove the precipitate and obtain a monolayer Ti3C2T. x MXene colloidal suspension.
6. The conductive porous material according to claim 4, characterized in that, In step (1), the volume ratio of hydrofluoric acid to concentrated hydrochloric acid is (0.7-2.2):1, the concentration of hydrofluoric acid is 49 wt%, and the concentration of concentrated hydrochloric acid is 38 wt%. And / or, the volume ratio of the hydrofluoric acid in step (1) to the mass ratio of the Ti3AlC2-MAX powder in step (2) is (8-12 mL): 1 g, and the concentration of the hydrofluoric acid is 49 wt%; And / or, the etching reaction temperature in step (2) is 25-30°C, and the etching reaction time is 10-14h; And / or, the volume ratio of the LiCl solution in step (3) to the mass ratio of the Ti3AlC2-MAX powder in step (2) is (8-12 mL): 1 g, and the concentration of the LiCl solution is 1.2 mol / L; And / or, the temperature of the intercalation reaction in step (3) is room temperature, and the time of the intercalation reaction is 8 to 12 hours; And / or, the power of the mechanical oscillation stripping in step (3) is 1000-1200W, and the time of the mechanical oscillation stripping is 30-40min; And / or, the monolayer Ti3C2T described in step (3) x The concentration of MXene colloidal suspension is 30–50 mg / mL.
7. The method for preparing the conductive porous material according to any one of claims 1 to 5, characterized in that, Includes the following steps: (1) The substrate is cleaned and dried to obtain the pretreated substrate; (2) The monolayer Ti3C2T described in claim 4 or 5 x MXene colloidal suspension was diluted to 5–8 mg / mL to obtain a 5–8 mg / mL Ti3C2T monolayer. x MXene colloidal suspension; the pretreated matrix is immersed in 5-8 mg / mL Ti3C2T monolayer. x The material is immersed in an MXene colloidal suspension, then removed, and its surface is dried after being blotted with filter paper. The immersion-drying process is repeated to obtain the conductive porous material.
8. The preparation method according to claim 6, characterized in that, Step (1) specifically involves ultrasonically cleaning the substrate with water 3-4 times and with anhydrous ethanol 2-3 times, followed by drying at 75-85℃ for 1-1.5 hours to obtain the pretreated substrate.
9. The preparation method according to claim 6, characterized in that, The immersion time in step (2) is 3 to 5 minutes; And / or, the drying temperature in step (2) is 75-85°C, and the drying time is 30-40 min; And / or, when the matrix is polyurethane porous foam, the number of repetitions in step (2) is 2 to 3 times; when the matrix is polyvinyl alcohol porous foam, the number of repetitions in step (2) is 1 to 2 times.
10. The application of the conductive porous material according to any one of claims 1 to 5 or the conductive porous material prepared by the preparation method according to any one of claims 6 to 8 in the efficient adsorption, safe handling, transportation, and storage of nitroglycerin.