Self-repairing polyurethane electromagnetic shielding material and preparation method thereof

By introducing a dynamic network of amide urea bonds and reversible disulfide bonds into the polyurethane molecular chain and modifying MXene with organic ammonium intercalation, the problems of easy damage and poor dispersibility of electromagnetic shielding materials during service are solved, achieving a balance between efficient self-repair and high electromagnetic shielding performance.

CN123131818APending Publication Date: 2026-11-20GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611639934.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing electromagnetic shielding materials are easily damaged during service, MXene has poor dispersion in polyurethane matrix, and it is difficult to achieve high mechanical properties, high self-healing efficiency and high electromagnetic shielding effectiveness.

Method used

A composite chain-extended system composed of hydrazide compounds and aromatic disulfides was constructed to form a dynamic network of multiple hydrogen bonds and reversible disulfide bonds. MXene was then modified by intercalation with organic ammonium compounds to enhance interfacial bonding and dispersibility, thereby preparing a self-healing polyurethane electromagnetic shielding material.

Benefits of technology

It enables structural reconstruction and performance recovery of materials after damage, improves the self-healing efficiency and electromagnetic shielding effectiveness of materials, while maintaining high tensile strength and elongation at break, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131818A_ABST
    Figure CN123131818A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of electromagnetic shielding materials, and discloses a self-repairing polyurethane electromagnetic shielding material and a preparation method thereof, the preparation method comprises the following steps: taking polyether polyol as a soft segment and aliphatic diisocyanate as a hard segment, adopting a first chain extender of a hydrazine type and a second chain extender of an aromatic disulfide type for composite chain extension to obtain a self-repairing polyurethane solution; etching a Ti3AlC2 MAX phase by using hydrofluoric acid to prepare MXene, and then carrying out intercalation modification and surface organic modification by using tetrabutylammonium hydroxide to obtain an organic ammonium intercalation modified MXene dispersion solution; after the two solutions are blended, casting forming and heating curing are carried out, and thus the material is obtained, wherein the content of the modified MXene is 5 wt%-20 wt%. The polyurethane electromagnetic shielding material prepared by the application is particularly prominent in flexible recovery capacity, can significantly prolong the service life of the electromagnetic shielding material, and has good self-repairing performance and electromagnetic shielding efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electromagnetic shielding materials technology, and in particular to a self-healing polyurethane electromagnetic shielding material and its preparation method. Background Technology

[0002] With the widespread adoption of 5G mobile communication technology and the increasing integration of electronic devices, electromagnetic interference has become a prominent issue, affecting not only the normal operation of precision instruments but also posing potential threats to communication security and human health. Developing shielding materials that combine high-efficiency electromagnetic shielding, lightweight flexibility, and long-term service stability has become a focus of attention for both academia and industry. Polyurethane, with its excellent mechanical properties, good processability, and resistance to chemical corrosion, is widely used as the matrix for electromagnetic shielding composite materials. Among these, aliphatic polyurethane prepared from isophorone diisocyanate (IPDI) and polytetrahydrofuran ether diol (PTMEG) exhibits significant advantages in flexible films, special encapsulation, and high-end coatings due to the anti-yellowing and light stability imparted by alicyclic isocyanates, and the low-temperature toughness and resilience provided by polyether soft segments.

[0003] Existing electromagnetic shielding materials generally suffer from the following three technical problems:

[0004] First, electromagnetic shielding materials inevitably suffer repeated bending, surface scratching, ultraviolet aging, or chemical corrosion during service. Once the conductive network inside the material is mechanically damaged, the electromagnetic shielding effectiveness will be greatly reduced or even fail, and the material's service life will be severely shortened.

[0005] Second, although two-dimensional transition metal carbides / nitrides (MXene) have high electrical conductivity, abundant surface functional groups and good electromagnetic wave attenuation capabilities, their nanosheets have strong van der Waals interactions, making them prone to aggregation and stacking. At the same time, the surface of MXene is rich in polar functional groups such as hydroxyl and fluorine, making it hydrophilic and having poor interfacial compatibility with the hydrophobic polyurethane matrix. This makes it difficult to disperse uniformly in the matrix and form an efficient conductive network, thus limiting its shielding effectiveness.

[0006] Third, existing self-healing electromagnetic shielding materials cannot simultaneously achieve high mechanical properties, high self-healing efficiency, and high electromagnetic shielding effectiveness: increasing the amount of filler can improve shielding effectiveness, but it often leads to filler agglomeration and a decrease in material strength and toughness; while introducing dynamic reversible bonds to achieve self-healing often comes at the cost of sacrificing the mechanical strength of the material, making it difficult to achieve the three in a coordinated manner.

[0007] Therefore, there is an urgent need to provide an electromagnetic shielding material and its preparation method that can take into account mechanical strength and toughness, high efficiency self-healing and high efficiency electromagnetic shielding, and is simple to process and suitable for mass production. Summary of the Invention

[0008] To overcome the above-mentioned shortcomings of the prior art, the present invention provides a self-healing polyurethane electromagnetic shielding material and its preparation method, so as to solve the technical problems of shielding performance decay and failure after the conductive network of electromagnetic shielding material is damaged, poor dispersion and weak interfacial bonding of MXene in polyurethane matrix, and difficulty in simultaneously achieving mechanical properties, self-healing properties and shielding effectiveness.

[0009] To achieve the above objectives, the present invention provides a method for preparing a self-healing polyurethane electromagnetic shielding material, comprising the following steps:

[0010] Step S1, Prepolymerization: After dehydration treatment of the soft segment monomer polyether polyol, it is dissolved in the first part of the polar aprotic solvent. Under nitrogen protection, the hard segment monomer aliphatic diisocyanate and catalyst are added. The mixture is stirred at 70-90℃ for 2-4 h and then cooled to 35-45℃ to obtain the isocyanate-terminated polyurethane prepolymer solution.

[0011] Step S2, chain extension: The first chain extender, an acylhydrazine compound, and the second chain extender, an aromatic disulfide, are dissolved in the second part of a polar aprotic solvent and then added dropwise to the prepolymer solution. The reaction is carried out at 35-45°C for 10-20 h to obtain a self-healing polyurethane solution. The molar ratio of the hard segment monomer aliphatic diisocyanate, the soft segment monomer polyether polyol, the first chain extender, and the second chain extender is (1.5-2.5):1:(0.6-0.9):(0.2-0.4).

[0012] Step S3: Preparation of organoammonium intercalation modified MXene dispersion: The Ti3AlC2MAX phase precursor is added to an aqueous hydrofluoric acid solution and stirred at 20–30 °C for 18–30 h. The mixture is washed with deionized water and centrifuged until the pH of the supernatant is 6–7. The precipitate is collected to obtain the etching filler. The etching filler is added to an organoammonium intercalating agent and stirred at room temperature for 3–6 h. The residual organoammonium intercalating agent is washed with ethanol to remove it. The resulting precipitate is then dispersed in the polar aprotic solvent and centrifuged. The supernatant is collected to obtain the organoammonium intercalation modified MXene dispersion. The molar ratio of the organoammonium intercalating agent to the Ti3AlC2MAX phase precursor is 0.6–1.2:1.

[0013] Step S4, Composite: Add the organic ammonium intercalated modified MXene dispersion obtained in step S3 to the self-healing polyurethane solution obtained in step S2, and stir for 4-8 h to obtain a self-healing polyurethane / modified MXene composite dispersion.

[0014] Step S5, Molding and Curing: Pour the composite dispersion into a mold, heat at 70-90℃ for 3-6 h, and then vacuum dry at 70-90℃ for 40-60 h to obtain the self-healing polyurethane electromagnetic shielding material. The modified MXene accounts for 5%-20% of the total mass of the self-healing polyurethane electromagnetic shielding material.

[0015] In step S1 of this invention, the polyether polyol is first dehydrated and prepolymerized under nitrogen protection because polyether polyol is highly hygroscopic. If it is not dehydrated, the moisture will react with the isocyanate groups in the aliphatic diisocyanate to generate CO2, causing bubbles and defects in the material. Simultaneously, it consumes aliphatic diisocyanate, leading to an imbalance in the proportions. Nitrogen protection prevents moisture intrusion and high-temperature oxidation side reactions. Controlling the prepolymerization temperature at 70–90°C and the reaction time at 2–4 hours ensures sufficient reaction between the isocyanate groups in the aliphatic diisocyanate and the hydroxyl groups in the polyether polyol, while inhibiting secondary crosslinking reactions such as urea-formate and biuret, thus preventing a sudden increase in system viscosity or even gelation.

[0016] In step S2 of this invention, a composite chain extender system is constructed using a first chain extender, an acylhydrazine compound, and a second chain extender, an aromatic disulfide. The terminal hydrazine group of the acylhydrazine chain extender adds to the terminal isocyanate group of the prepolymer to form an amide urea bond, introducing dense hydrogen bond donors and acceptors into the hard segment, forming a multi-layered hydrogen bond physical cross-linking network, which significantly improves the tensile strength, heat resistance, and dimensional stability of the material. The aromatic primary amino groups at both ends of the aromatic disulfide add to the terminal isocyanate group of the prepolymer to form urea bonds, and simultaneously introduce the disulfide bonds (-SS-) in its molecule into the polyurethane backbone. The disulfide bonds can undergo a reversible exchange reaction under heating conditions, endowing the material with thermally driven self-healing properties. The synergistic effect of the two types of chain extenders enables the material to maintain high strength while possessing highly efficient self-healing capabilities.

[0017] In step S2 of this invention, the two types of chain extenders are dissolved and added dropwise, and reacted for a long time at a relatively low temperature of 35-45°C. Because aromatic disulfides and hydrazide compounds have significantly different reactivity, dissolving and adding them dropwise separately allows the two chain extenders to be orderly incorporated into the molecular chain in the designed ratio, avoiding excessively rapid local reactions and excessively wide molecular weight distribution caused by concentrated feeding. The lower reaction temperature can suppress the exchange side reactions of disulfide bonds during the chain extension stage, ensuring that the disulfide bonds are completely retained in the molecular chain, thereby enabling the material to exhibit stable thermally driven self-healing properties during subsequent service.

[0018] Meanwhile, the present invention limits the molar ratio of diisocyanate, polyether polyol, first chain extender and second chain extender to the above range, which has the following advantages: the excess of aliphatic diisocyanate relative to polyether polyol can ensure that the prepolymer is end-capped with isocyanate groups, avoiding premature termination of growth of the prepolymer due to excess hydroxyl groups; the total molar number of active hydrogens that can react with isocyanate groups in the two types of chain extenders should match the amount of remaining isocyanate groups in the prepolymer (molar ratio close to 1:1), which avoids both incomplete molecular chain growth, low molecular weight and insufficient mechanical properties caused by insufficient chain extender, and excessive residual chain extender causing small molecule migration and precipitation and material performance degradation.

[0019] In step S3 of this invention, MXene is prepared by selectively etching the Al atomic layer in the Ti3AlC2MAX phase precursor with hydrofluoric acid. The advantages are: hydrofluoric acid has a selective etching effect on the Al layer with little damage to the Ti-C framework, and can obtain MXene with complete layered structure and fluorine, hydroxyl and oxygen functional groups on the surface, retaining its high conductivity and abundant surface functional groups; after etching, washing and centrifugation until the pH of the supernatant is 6-7 can fully remove residual acid and by-product salts, avoiding residual acidic substances from corroding equipment, catalyzing the degradation of polyurethane or affecting the electrical properties of the material.

[0020] In step S3 of this invention, an organic ammonium intercalating agent (tetrabutylammonium hydroxide) is further used to intercalate and surface organically modify the etching product, thereby introducing tetrabutylammonium cations (TBA) into the product. + Insertion of TBA into the interlayer of MXene significantly increases the interlayer spacing and weakens the van der Waals interactions between the layers, making it easier to exfoliate multilayer MXene into few-layer or even single-layer nanosheets; simultaneously, TBA + By replacing some surface functional groups and arranging hydrophobic butyl chains outwards, MXene's surface changes from hydrophilic to organic solvent-philic, enabling long-term stable dispersion in polar aprotic solvents such as N,N-dimethylacetamide. This allows for homogeneous composite formation with polyurethane solutions, which are also DMAc systems, effectively suppressing MXene aggregation in the polyurethane matrix and facilitating the construction of continuous conductive networks with low filler content. Furthermore, the residual surface hydroxyl and oxygen functional groups after intercalation can still form hydrogen bonds with -NH- and C=O groups on the polyurethane molecular chains, enhancing the interfacial bonding between the two phases and improving stress transfer efficiency.

[0021] In step S4, the modified MXene dispersion is compounded with the self-healing polyurethane solution by solution blending, which can achieve uniform mixing of filler and matrix at the nanoscale. The process is simple and does not require additional dispersion equipment.

[0022] In step S5, a two-stage curing process of "atmospheric pressure pre-evaporation + vacuum drying" is employed. The advantages are: firstly, most of the solvent evaporates slowly under atmospheric pressure, avoiding the formation of pinholes and bubbles in the film due to violent boiling of the solvent caused by direct vacuuming; subsequently, prolonged vacuum drying thoroughly removes residual solvent, preventing plasticization by residual solvent that could lead to decreased strength or slow release during use. The curing temperature is controlled between 70 and 90°C, ensuring efficient solvent removal while avoiding premature disulfide bond exchange or thermo-oxidative aging of the polyurethane due to excessively high temperatures.

[0023] In this invention, the modified MXene content is controlled to be 5% to 20% of the total mass of the self-healing polyurethane electromagnetic shielding material. When the modified MXene content is below 5%, it is difficult to form a continuous conductive network, resulting in insufficient shielding effectiveness. When it is above 20%, the filler is prone to stacking and agglomeration, the system viscosity is too high, and the material strength decreases significantly. By controlling the modified MXene content within the range of 5% to 20%, the shielding effectiveness can reach above 18 dB while ensuring the material's mechanical properties and self-healing performance, thus meeting the requirements for electromagnetic shielding in civilian and some industrial applications.

[0024] Further, in step S1, the hard segment monomer aliphatic diisocyanate is one or both of isophorone diisocyanate and hexamethylene diisocyanate. The aliphatic diisocyanate molecule does not contain easily oxidized aromatic rings, and the resulting polyurethane is less prone to yellowing and aging degradation under ultraviolet irradiation and long-term use, thus ensuring that the electromagnetic shielding material maintains stable appearance and performance even after long-term service in outdoor or sunlight environments. In contrast, polyurethanes made from aromatic isocyanates (such as MDI and TDI) have strong cohesion and high strength in the hard segment, but poor weather resistance and are prone to yellowing.

[0025] Further, in step S1, the number average molecular weight of the soft segment monomer polyether polyol is 1000-3000, preferably 2000; and it is one or more of polytetrahydrofuran ether diol, polyethylene glycol, and polypropylene glycol, preferably polytetrahydrofuran ether diol.

[0026] When the molecular weight of the polyether soft segment monomer is too low, the relative content of the hard segment increases, the molecular chain flexibility is insufficient, and the chain segment mobility is weak. During self-repair, the molecular chain has difficulty migrating and diffusing to the damaged interface, resulting in reduced self-repair efficiency. When the molecular weight is too high, the tendency of soft segment crystallization increases, the mechanical strength decreases, and the compatibility with the hard segment deteriorates, leading to excessive microphase separation. This invention selects a polyether polyol with a number average molecular weight of around 2000, which enables the material to possess both high tensile strength (above 70 MPa) and large elongation at break (above 900%), and moderate molecular chain flexibility, which is beneficial to improving self-repair efficiency.

[0027] Further, in step S2, the first chain extender is one or more of adipate dihydrazide, sebacic dihydrazide, and terephthalic dihydrazide, preferably adipate dihydrazide; the second chain extender is one or two of 4,4′-dithiodiphenylamine and 2,2′-dithiodiphenylamine, preferably 4,4′-dithiodiphenylamine. When the first chain extender is adipate dihydrazide, its molecular chain is short and has good symmetry, resulting in a high density of amide bonds and strong hydrogen bonding. Furthermore, the raw materials are readily available, and the reactivity is moderate and easily controlled. When the second chain extender is 4,4′-dithiodiphenylamine, its two ends are aromatic primary amino groups, which have high reactivity with the isocyanate groups of the hard segment monomer aliphatic diisocyanate and complete chain extension. The generated urea bond can further enhance the cohesive force of the hard segment. At the same time, the rigidity of the benzene ring helps to improve the strength of the material, while the disulfide bond located in the middle of the molecule has a moderate bond energy and can undergo reversible exchange at 80-120℃, enabling the material to achieve self-repair under mild conditions.

[0028] Furthermore, the catalyst is dibutyltin dilaurate, and its dosage is 0.05% to 0.2% of the mass of the polyether polyol. The organotin active center of the catalyst dibutyltin dilaurate can coordinate with the isocyanate group of the hard segment monomer aliphatic diisocyanate to form an active intermediate, which significantly reduces the activation energy of the reaction between the isocyanate group and the hydroxyl and amine groups, so that prepolymerization and chain extension can be carried out rapidly at a lower temperature (≤90℃), with mild reaction conditions and low energy consumption.

[0029] Further, in step S1, the dehydration treatment of the soft segment monomer polyether polyol is as follows: the soft segment monomer polyether polyol is dried under reduced pressure and vacuum at 100-110°C for 1-2 h; the dissolution temperature of the polyether polyol in step S1 is 40-60°C, and the stirring speed is 150-300 rpm.

[0030] Further, in step S3, the mass concentration of the hydrofluoric acid aqueous solution is 30%–40%, and the mass ratio of the Ti3AlC2MAX phase precursor to the volume of the hydrofluoric acid aqueous solution is 1:10–25 g / mL; the organic ammonium intercalating agent is a tetrabutylammonium hydroxide aqueous solution; the centrifugation speed in step S3 is 8000–12000 rpm, and the number of centrifugation cycles is 6–8. If the hydrofluoric acid concentration is too low or the acid content is insufficient, it will lead to incomplete etching of the Al layer, residual MAX phase impurities in the product, and reduced MXene purity and conductivity; if the concentration is too high, the etching will be too intense, damaging the Ti-C framework and fragmenting the MXene sheets, which is also detrimental to the construction of the conductive network. Therefore, this invention selects a hydrofluoric acid aqueous solution with a mass concentration of 30%–40%.

[0031] Furthermore, in step S4, the stirring speed is 200-400 rpm.

[0032] This invention also discloses a self-healing polyurethane electromagnetic shielding material, comprising a polyurethane matrix and an organoammonium intercalated modified MXene dispersed in the polyurethane matrix; wherein the organoammonium intercalated modified MXene is a tetrabutylammonium intercalated modified Ti3C2T x MXene accounts for 5% to 20% of the total mass of the self-healing polyurethane electromagnetic shielding material; the polyurethane matrix is ​​a polyurethane with polyether polyol as the soft segment and aliphatic diisocyanate as the hard segment.

[0033] Furthermore, the self-healing polyurethane electromagnetic shielding material of the present invention is prepared by the above-described preparation method.

[0034] Compared with existing technologies, this invention uses aliphatic diisocyanates and polyether polyols as monomers to prepare isocyanate-terminated polyurethane prepolymers in polar aprotic solvents. A composite chain extender system is constructed using hydrazide compounds as the first chain extender and aromatic disulfides as the second chain extender. The former introduces amide bonds into the hard segments and forms a multi-hydrogen bond physical cross-linking network, while the latter introduces reversible disulfide bonds and generates urea bonds while introducing benzene ring rigidity. This constructs a dual dynamic network of "multi-hydrogen bonds-disulfide bonds" in the polyurethane molecular chain, eliminating the trade-off between strength and self-healing properties. Furthermore, before MXene is composited with polyurethane, this invention uses an organic ammonium intercalating agent to intercalate and surface-organize the MXene obtained by hydrofluoric acid etching, increasing the interlayer spacing and changing the surface from hydrophilic to organic solvent-philic. This allows for homogeneous composite formation with the polyurethane solution in a polar aprotic solvent, effectively inhibiting nanosheet aggregation and enhancing the interfacial bonding between the two phases. This allows the modified MXene to achieve a high strength within 5... An effective conductive network can be formed even at a low content of wt%.

[0035] This invention replaces the aliphatic disulfide with an aromatic disulfide as the second chain extender. The aromatic primary amino groups at both ends react with isocyanate groups to form urea bonds, introducing rigidity to the benzene ring. This allows the material to achieve both thermally driven self-healing properties and higher tensile strength, reaching a tensile strength of 72.60 MPa. Simultaneously, this invention combines the dual-dynamic-bond polyurethane matrix with organic ammonium intercalation-modified MXene, expanding the material from a simple elastomer to a composite material with electromagnetic shielding capabilities. While maintaining high tensile strength (72.56–72.60 MPa) and high elongation at break (above 935%), the tensile strength self-healing efficiency reaches a maximum of 93.92%, and an electromagnetic shielding effectiveness of 32.88 dB is achieved with a modified MXene content of 10 wt%. This achieves a synergistic balance of mechanical properties, self-healing properties, and electromagnetic shielding effectiveness.

[0036] Furthermore, the present invention can be prepared by only prepolymerization, composite chain extension, intercalation modification, solution blending and two-stage curing, without the need for additional dispersion equipment or filler surface treatment process. The process is simple and suitable for large-scale production.

[0037] The above technical solution has the following advantages, unlike existing technologies:

[0038] (1) To address the technical problem of "defense performance degradation and short material lifespan after conductive network damage", this invention introduces a multi-hydrogen bond network formed by amide urea bonds and reversible disulfide bonds provided by aromatic disulfides into the polyurethane molecular chain, enabling the material to achieve structural reconstruction and performance recovery through heating after damage. Test data shows that after treatment at 120℃ for 0.5 h and placement at 60℃ for 24 h, the self-repair efficiency of the tensile strength of the material can reach 80.20% to 93.92%, with the modified MXene content reaching as high as 93.92% when the content is 10 wt%, which is significantly higher than that of pure polyurethane without filler (81.76%). The retention rate of elongation at break increases from 80.21% of pure polyurethane to 93.86% to 99.07%, indicating that the material's flexible recovery ability is particularly outstanding, thereby significantly extending the service life of electromagnetic shielding materials.

[0039] (2) To address the technical problems of "MXene's tendency to aggregate, poor compatibility with hydrophobic polyurethane interfaces, and difficulty in forming a highly efficient conductive network," this invention employs organic ammonium intercalation to modify the etched MXene through intercalation and surface organic modification. This increases the interlayer spacing of MXene and changes its surface from hydrophilic to organic solvent-philic, allowing it to be stably dispersed in polar aprotic solvents and homogeneously composited with the polyurethane solution. Infrared spectroscopy shows that after composite formation, the 3323 cm⁻¹... -1 The NH stretching vibration peak redshifted to 1660 cm⁻¹. -1 The weakening of the C=O peak indicates that hydrogen bonds have formed between the polyurethane and the modified MXene, demonstrating good interfacial compatibility. Therefore, the self-healing polyurethane electromagnetic shielding material prepared in this invention can form an effective conductive network even with low filler content: the electromagnetic shielding effectiveness reaches 18.65 dB at 5 wt% modified MXene, 32.88 dB at 10 wt%, and 39.20 dB at 20 wt%, while no shielding effectiveness was detected in pure polyurethane without filler.

[0040] (3) In response to the technical problem that "it is difficult to balance mechanical properties, self-healing properties and shielding effectiveness", this invention achieves a balance of the three through the synergistic design of hydrazide / aromatic disulfide composite chain extension system and organic ammonium intercalation modified MXene: when the modified MXene content is 5-10 wt%, the tensile strength of the material is 72.56-72.60 MPa, which is higher than the 69.33 MPa of pure polyurethane, and the elongation at break is still above 935%. At the same time, the self-healing efficiency reaches up to 93.92% and the electromagnetic shielding effectiveness reaches 18.65-32.88 dB. That is, without sacrificing (or even improving) mechanical properties, efficient self-healing and efficient electromagnetic shielding performance are obtained simultaneously.

[0041] (4) The present invention adopts a solution blending-cast molding process route. The reaction temperature of each step does not exceed 90°C, and there is no need for high temperature, high pressure and special equipment. The reaction conditions are mild, the operation is simple and the repeatability is good, making it suitable for large-scale production. Attached Figure Description

[0042] Figure 1 The Fourier transform infrared spectra of the materials prepared in Examples 2, 3, and Comparative Example 1 are shown below.

[0043] Figure 2 X-ray photoelectron spectra of the modified MXene powder (T-MXene) not dispersed in N,N-dimethylacetamide prepared in step 4 of Example 1, the self-healing polyurethane material prepared in Example 2, and the filler-free self-healing polyurethane material prepared in Comparative Example 1.

[0044] Figure 3 Here are scanning electron microscope (SEM) images of the self-healing polyurethane electromagnetic shielding material prepared in Example 2; wherein, Figure 3 (a) is a low-magnification scanning electron microscope (SEM) image of the self-healing polyurethane electromagnetic shielding material prepared in Example 2; Figure 3 (b) is a high-magnification scanning electron microscope (SEM) image of the self-healing polyurethane electromagnetic shielding material prepared in Example 2. Detailed Implementation

[0045] To explain in detail the technical content, structural features, objectives, and effects of the technical solution, the following description is provided in conjunction with specific embodiments and accompanying drawings.

[0046] Unless otherwise specified, all raw materials used in the following examples are commercially available analytical grade or industrial grade products: polytetrahydrofuran ether diol (PTMEG, number average molecular weight 2000), isophorone diisocyanate (IPDI), adipic acid dihydrazide (AD), 4,4′-dithiodiphenylamine (SS), dibutyltin dilaurate (DBTDL), Ti3AlC2MAX phase ceramic powder (400 mesh), hydrofluoric acid (40 wt% aqueous solution), tetrabutylammonium hydroxide (TBAOH, 25 wt% aqueous solution), and N,N-dimethylacetamide (DMAc).

[0047] Example 1

[0048] A self-healing polyurethane electromagnetic shielding material includes a polyurethane matrix and modified MXene (T-MXene) dispersed therein, wherein the modified MXene is a tetrabutylammonium intercalated modified Ti3C2T. x Its mass accounts for 5 wt% of the total mass of the material.

[0049] Its preparation method includes the following steps:

[0050] 1) Material preparation: Weigh the raw materials according to the following quantities:

[0051] Polytetrahydrofuran ether diol (Mn=2000) 20.00 g (10 mmol); isophorone diisocyanate 4.45 g (20 mmol); dibutyltin dilaurate 0.020 g (0.0317 mmol); adipic acid dihydrazide 1.305 g (7.49 mmol); 4,4′-dithiodiphenylamine 0.621 g (2.5 mmol); Ti3AlC2MAX phase precursor (400 mesh) 0.631 g (3.24 mmol); tetrabutylammonium hydroxide (based on pure substance) 0.757 g (2.92 mmol, equivalent to 3.0 g of 25 wt% aqueous solution); hydrofluoric acid aqueous solution (40 wt%) 12.5 mL; N,N-dimethylacetamide 80 mL. The amount of Ti3AlC2 fed is calculated based on the target T-MXene accounting for 5wt% of the total mass of the material, and the molar ratio of tetrabutylammonium hydroxide to Ti3AlC2 is 0.9:1.

[0052] 2) Prepolymerization: Polytetrahydrofuran ether diol was dried under reduced pressure at 100℃ for 2 hours to remove moisture. 10 mL of N,N-dimethylacetamide was added to a four-necked flask. The dehydrated polytetrahydrofuran ether diol was stirred and dissolved at 50℃ and mixed evenly. Dibutyltin dilaurate was added. Isophorone diisocyanate was slowly added under a nitrogen atmosphere. The temperature was raised to 80℃ and stirred at 200 rpm for 3 hours. The mixture was then cooled to 40℃ to obtain a polyurethane prepolymer solution with isocyanate-terminated groups.

[0053] 3) Chain extension: Dissolve adipic dihydrazide in 60 mL of N,N-dimethylacetamide and 4,4′-dithiodiphenylamine in 10 mL of N,N-dimethylacetamide, and add them dropwise to the above prepolymer solution. React at 40 °C for 15 h to obtain a viscous and transparent self-healing polyurethane solution.

[0054] 4) Preparation of organoammonium intercalation modified MXene dispersion: Ti3AlC2MAX phase ceramic powder was slowly added to hydrofluoric acid aqueous solution and stirred at 25℃ for 24h; then washed with deionized water and centrifuged 7 times at 10000 rpm until the pH of the supernatant stabilized at 6-7, and the precipitate was collected to obtain the etching product; the etching product was added to tetrabutylammonium hydroxide aqueous solution and stirred at 25℃ for 4h; then washed with ethanol to remove residual intercalating agent, the precipitate was dispersed in N,N-dimethylacetamide, shaken to make it uniformly dispersed and centrifuged, and the upper liquid was collected to obtain modified T-MXene dispersion.

[0055] 5) Composite: Under stirring conditions of 25℃ and 200 rpm, the modified T-MXene dispersion obtained in step 4) is added to the self-healing polyurethane solution obtained in step 3), and stirred for 6 hours to obtain a self-healing polyurethane / T-MXene composite dispersion.

[0056] 6) Molding and curing: Pour the composite dispersion into a polytetrafluoroethylene mold, heat it on a heating table at 80°C for 4 hours, and then place it in a vacuum oven at 80°C for 48 hours to obtain the self-healing polyurethane electromagnetic shielding material.

[0057] Example 2

[0058] The difference from Example 1 is that: the Ti3AlC2MAX phase precursor is 1.337 g (6.87 mmol), tetrabutylammonium hydroxide (based on pure substance) is 1.602 g (6.17 mmol, equivalent to 6.40 g of 25 wt% aqueous solution), and hydrofluoric acid aqueous solution (40 wt%) is 25 mL, that is, the modified MXene accounts for 10 wt% of the total mass of the material; the remaining raw material amounts, steps and process parameters are the same as in Example 1.

[0059] Example 3

[0060] The difference from Example 1 is that: the Ti3AlC2MAX phase precursor is 3.012 g (15.48 mmol), tetrabutylammonium hydroxide (based on pure substance) is 3.607 g (13.90 mmol, equivalent to 14.43 g of 25 wt% aqueous solution), and hydrofluoric acid aqueous solution (40 wt%) is 56.25 mL, that is, the modified MXene accounts for 20 wt% of the total mass of the material; the amount of other raw materials, steps and process parameters are the same as in Example 1.

[0061] Example 4

[0062] A self-healing polyurethane electromagnetic shielding material includes a polyurethane matrix and modified MXene (T-MXene) dispersed therein, wherein the modified MXene is a tetrabutylammonium intercalated modified Ti3C2T. x Its mass accounts for 10 wt% of the total mass of the material.

[0063] Its preparation method includes the following steps:

[0064] 1) Material preparation: Weigh the raw materials according to the following quantities:

[0065] Polytetrahydrofuran ether diol (Mn=2000) 20.00 g (10 mmol); isophorone diisocyanate 4.45 g (20 mmol); dibutyltin dilaurate 0.040 g (0.0634 mmol); sebacic dihydrazide 1.725 g (7.49 mmol); 2,2′-dithiodiphenylamine 0.621 g (2.5 mmol); Ti3AlC2MAX phase precursor (400 mesh) 1.683 g (8.65 mmol); tetrabutylammonium hydroxide (based on pure substance) 1.357 g (5.23 mmol, equivalent to 4.45 g of 25 wt% aqueous solution); hydrofluoric acid aqueous solution (30 wt%) 25 mL; N,N-dimethylacetamide 80 mL. The amount of Ti3AlC2 fed is calculated based on a target T-MXene content of 10wt%, and the molar ratio of tetrabutylammonium hydroxide to Ti3AlC2 is 0.6:1.

[0066] 2) Prepolymerization: Polytetrahydrofuran ether diol was dried under reduced pressure at 100℃ for 2 hours to remove moisture. 10 mL of N,N-dimethylacetamide was added to a four-necked flask. The dehydrated polytetrahydrofuran ether diol was stirred and dissolved at 40℃ and mixed evenly. Dibutyltin dilaurate was added. Isophorone diisocyanate was slowly added under a nitrogen atmosphere. The temperature was raised to 70℃ and stirred at 300 rpm for 4 hours. The mixture was then cooled to 35℃ to obtain a polyurethane prepolymer solution with isocyanate-terminated groups.

[0067] 3) Chain extension: Dissolve sebacate dihydrazide in 60 mL of N,N-dimethylacetamide and 2,2′-dithiodiphenylamine in 10 mL of N,N-dimethylacetamide, and add them dropwise to the above prepolymer solution. React at 45 °C for 10 h to obtain a viscous and transparent self-healing polyurethane solution.

[0068] 4) Preparation of organoammonium intercalation modified MXene dispersion: Ti3AlC2MAX phase ceramic powder was slowly added to hydrofluoric acid aqueous solution and stirred at 20℃ for 30h; then washed with deionized water and centrifuged 8 times at 8000 rpm until the pH of the supernatant stabilized at 6-7, and the precipitate was collected to obtain the etching product; the etching product was added to tetrabutylammonium hydroxide aqueous solution and stirred at 25℃ for 6h; then washed with ethanol to remove residual intercalating agent, the precipitate was dispersed in N,N-dimethylacetamide, shaken to make it uniformly dispersed and centrifuged, and the upper liquid was collected to obtain modified T-MXene dispersion.

[0069] 5) Composite: Under the conditions of stirring at 25℃ and 300 rpm, the modified T-MXene dispersion obtained in step 4) is added to the self-healing polyurethane solution obtained in step 3), and stirred for 4 hours to obtain a self-healing polyurethane / T-MXene composite dispersion.

[0070] 6) Molding and curing: Pour the composite dispersion into a polytetrafluoroethylene mold, heat it on a heating table at 70°C for 6 hours, and then place it in a vacuum oven at 70°C for 60 hours to dry it, thereby obtaining the self-healing polyurethane electromagnetic shielding material.

[0071] Example 5

[0072] A self-healing polyurethane electromagnetic shielding material includes a polyurethane matrix and modified MXene (T-MXene) dispersed therein, wherein the modified MXene is a tetrabutylammonium intercalated modified Ti3C2T. x Its mass accounts for 10 wt% of the total mass of the material.

[0073] Its preparation method includes the following steps:

[0074] 1) Material preparation: Weigh the raw materials according to the following quantities:

[0075] Polyethylene glycol (Mn=3000) 30.00 g (10 mmol); hexamethylene diisocyanate 4.2 g (25 mmol); dibutyltin dilaurate 0.020 g (0.0317 mmol); adipic acid dihydrazide 1.57 g (9 mmol); 4,4′-dithiodiphenylamine 0.99 g (4 mmol); Ti3AlC2MAX phase precursor (400 mesh) 1.575 g (8.09 mmol); tetrabutylammonium hydroxide (based on pure substance) 2.507 g (9.66 mmol, equivalent to 10.03 g of 25 wt% aqueous solution); hydrofluoric acid aqueous solution (40 wt%) 35 mL; N,N-dimethylacetamide 80 mL. The amount of Ti3AlC2 fed is calculated based on a target T-MXene content of 10wt%, and the molar ratio of tetrabutylammonium hydroxide to Ti3AlC2 is 1.2:1.

[0076] 2) Prepolymerization: Polyethylene glycol was dried under reduced pressure at 110°C for 1 hour to remove moisture. 10 mL of N,N-dimethylacetamide was added to a four-necked flask. The dehydrated polyethylene glycol was stirred and dissolved at 60°C and mixed evenly. Dibutyltin dilaurate was added. Hexamethylene diisocyanate was slowly added under a nitrogen atmosphere. The temperature was raised to 90°C and stirred at 150 rpm for 2 hours. The mixture was then cooled to 45°C to obtain a polyurethane prepolymer solution with isocyanate-terminated groups.

[0077] 3) Chain extension: Dissolve adipic acid dihydrazide in 60 mL of N,N-dimethylacetamide and 4,4′-dithiodiphenylamine in 10 mL of N,N-dimethylacetamide, and add them dropwise to the above prepolymer solution. React at 35°C for 20 h to obtain a viscous and transparent self-healing polyurethane solution.

[0078] 4) Preparation of organoammonium intercalation modified MXene dispersion: Ti3AlC2MAX phase ceramic powder was slowly added to hydrofluoric acid aqueous solution and stirred at 30℃ for 18h; then washed with deionized water and centrifuged 6 times at 10000 rpm until the pH of the supernatant stabilized at 6-7, and the precipitate was collected to obtain the etching product; the etching product was added to tetrabutylammonium hydroxide aqueous solution and stirred at 25℃ for 3h; then washed with ethanol to remove residual intercalating agent, the precipitate was dispersed in N,N-dimethylacetamide, shaken to make it uniformly dispersed and centrifuged, and the upper liquid was collected to obtain modified T-MXene dispersion.

[0079] 5) Composite: Under the conditions of 25℃ and 400 rpm stirring, the modified T-MXene dispersion obtained in step 4) is added to the self-healing polyurethane solution obtained in step 3), and stirred for 8 hours to obtain the self-healing polyurethane / T-MXene composite dispersion.

[0080] 6) Molding and curing: Pour the composite dispersion into a polytetrafluoroethylene mold, heat it on a heating table at 90°C for 3 hours, and then place it in a vacuum oven at 90°C for 40 hours to obtain the self-healing polyurethane electromagnetic shielding material.

[0081] Comparative Example 1

[0082] The difference from Example 1 is that modified MXene is not added, that is, steps 4) and 5) are not performed. The self-healing polyurethane solution obtained in step 3) is directly molded and cured according to step 6) to obtain a filler-free self-healing polyurethane material; the remaining raw material dosage, steps and process parameters are the same as in Example 1.

[0083] Comparative Example 2

[0084] The difference from Example 1 is that in step 3), only the first chain extender, adipic acid dihydrazide, is added, and the second chain extender, 4,4′-dithiodiphenylamine, is not added. That is, the self-healing polyurethane solution obtained in step 3 is only chain extended once, and the remaining raw material dosages, steps and process parameters are the same as in Example 1.

[0085] Performance testing

[0086] (1) Tensile properties and self-healing efficiency: The specimens were cut into dumbbell-shaped strips according to GB / T 528-2009. The tensile strength and elongation at break were tested using a universal tensile testing machine at a rate of 100 mm / min. Each sample was tested 3 times and the average value was taken. Self-healing experiment: A 2 mm deep crack was cut into the middle of the dumbbell-shaped strip, and it was placed in a constant temperature chamber at 120℃ for 0.5 h, followed by 24 h at 60℃. The repaired strip was then subjected to tensile testing. The self-healing efficiency was calculated according to formula (1):

[0087] SE = σ² / σ¹ × 100% (1)

[0088] In the formula, σ2 is the tensile strength of the healed sample, and σ1 is the tensile strength of the original sample.

[0089] (2) Electromagnetic shielding effectiveness: The Agilent E5071C vector network analyzer was used to test the waveguide method. The test frequency range was 8.2 to 12.4 GHz (X-band), and the sample size was 22.9 mm × 10.2 mm × 1 mm.

[0090] The detection data of each embodiment and the comparative embodiment are shown in Table 1.

[0091] Table 1 Performance test data of materials prepared in each embodiment and comparative embodiment

[0092]

[0093] As can be seen from the data in Table 1:

[0094] First, the material exhibits significant electromagnetic shielding performance after the addition of modified MXene, and the shielding effectiveness increases with the increase of filler content: As shown in Example 1, the shielding effectiveness is 18.65 dB when the modified MXene content is 5 wt%, and as shown in Example 2, it is 32.88 dB when the content is 10 wt% and reaches 39.20 dB when the content is 20 wt%. In contrast, no shielding effectiveness was detected in Comparative Example 1 without filler. This indicates that the present invention enables MXene to be uniformly dispersed in the polyurethane matrix and form an effective conductive network through organic ammonium intercalation modification.

[0095] Secondly, as shown in Examples 1 and 2, when the filler content is 5–10 wt%, the tensile strength of the material (72.56 MPa, 72.60 MPa) is higher than that of Comparative Example 1 (69.33 MPa), and the elongation at break remains above 935%. This indicates that the addition of an appropriate amount of modified MXene not only does not impair the mechanical properties of the material, but also produces a reinforcing effect due to the hydrogen bonding between the filler and the polyurethane molecular chains. When the filler content is increased to 20 wt%, the tensile strength decreases to 33.56 MPa and the elongation at break decreases to 790.71%, indicating that the filler agglomerates and becomes a stress concentration point under high filler content. Therefore, considering the shielding effectiveness, mechanical properties, and raw material cost, the preferred content of modified MXene is 5 wt%–10 wt%.

[0096] Third, the self-healing efficiencies of Examples 2 and 3 were 93.92% and 90.76%, respectively, which were significantly higher than the 81.76% of Comparative Example 1. At the same time, the retention rate of elongation at break (after healing / original) increased from 80.21% in Comparative Example 1 to 93.86%, 99.07%, and 98.24% in Examples 1-3, respectively. This indicates that the introduction of modified MXene is beneficial to the reconstruction and performance recovery of the damaged interface. This may be due to the reversible reconstruction of hydrogen bonds between the residual functional groups on the MXene surface and the polyurethane segments, as well as the high thermal conductivity of MXene promoting the disulfide bond exchange reaction.

[0097] Fourth, the self-healing efficiencies of Examples 2 and 3 were 93.92% and 90.76%, respectively, significantly higher than the 22.86% of Comparative Example 2. Simultaneously, the retention rate of elongation at break (after healing / original) increased from 46.35% in Comparative Example 2 to 93.86%, 99.07%, and 98.24% in Examples 1-3, respectively. Furthermore, the tensile strength of the materials prepared in Examples 1 and 2 (72.56 MPa, 72.60 MPa) was higher than that of Comparative Example 2 (65.75 MPa), and the elongation at break remained above 935%, indicating that the two chain extenders can produce a synergistic effect, enabling the material to maintain high strength while possessing efficient self-healing capabilities. This is because the terminal hydrazine group of the hydrazine chain extender adds to the terminal isocyanate group of the prepolymer to form an amide urea bond, introducing dense hydrogen bond donors and acceptors into the hard segment, forming a multi-hydrogen bond physical cross-linking network, which significantly improves the tensile strength, heat resistance and dimensional stability of the material; the aromatic primary amino groups at both ends of the aromatic disulfide add to the terminal isocyanate group of the prepolymer to form a urea bond, and at the same time introduce the disulfide bond (-SS-) in its molecule into the polyurethane backbone. The disulfide bond can undergo a reversible exchange reaction under heating conditions, giving the material thermally driven self-healing properties.

[0098] Fifth, the material of this invention can recover most of its electromagnetic shielding performance after damage, and the self-repair efficiency of electromagnetic shielding increases with the increase of modified MXene content. As shown in Example 1, the electromagnetic shielding self-repair efficiency is 83.38% when the modified MXene content is 5 wt%; in Example 2, it is 89.63% at 10 wt%; and in Example 3, it is 92.63% at 20 wt%. In contrast, the electromagnetic shielding self-repair efficiency of Comparative Example 2 without the addition of hydrazide chain extenders is only 32.17%, indicating that the multiple hydrogen bond network constructed by the hydrazide chain extenders effectively promotes the recovery of the modified MXene conductive network.

[0099] The materials prepared in Examples 2, 3, and Comparative Example 1 were characterized by scanning with Fourier transform infrared spectroscopy (FTIR): an attenuated total reflectance (ATR) attachment was used with air as the background, and the scanning range was 4000-400 cm⁻¹. -1 The resolution is 4 cm. -1 The scan was performed 32 times at a speed of 0.2 cm / s at a temperature of 25 °C. The resulting spectra were analyzed after baseline correction and normalization. The infrared spectra of the materials prepared in Examples 2, 3, and Comparative Example 1 are shown below. Figure 1 .Depend on Figure 1 It can be known that 2270 cm -1 No absorption peak was observed at 3323 cm⁻¹, indicating that the -NCO groups in the system have completely reacted; -1 and 1536 cm -1The absorption peaks at 2854 cm⁻¹ represent the stretching and bending vibrations of the NH bond in the carbamate, respectively. -1 and 2935 cm -1 The peaks at 1701 cm⁻¹ represent the symmetric and asymmetric stretching vibrations of the methylene group in the molecular chain, respectively. -1 The peak at 1101 cm⁻¹ represents the stretching vibration of C=O in carbamate. -1 The peak at [location] corresponds to the stretching vibration of the COC group in PTMEG. Compared to Comparative Example 1, the peak at 3323 cm⁻¹ after adding modified MXene [is observed]. -1 The NH stretching vibration peak redshifted to 1660 cm⁻¹. -1 The weakening of the C=O peak intensity indicates that hydrogen bonding has formed between the polyurethane and the modified MXene, and the two phases are well bonded at the interface, which is consistent with the improvement of the material's mechanical properties and shielding performance.

[0100] X-ray photoelectron spectroscopy (XPS) was used to characterize the self-healing polyurethane material prepared in Example 2, the filler-free self-healing polyurethane material prepared in Comparative Example 1, and the modified MXene powder (T-MXene) not dispersed in N,N-dimethylacetamide prepared in step 4 of Example 1. The testing instrument was an X-ray photoelectron spectrometer with a working voltage of 12 kV and a working current of 6 mA (pass energy 100 eV, step size 1.0 eV). High-resolution narrow-region scanning was then performed on the characteristic peaks of Ti 2p, C 1s, O 1s, N 1s, and F 1s (pass energy 20 eV, step size 0.05 eV).

[0101] The X-ray photoelectron spectroscopy (XPS) spectra of the self-healing polyurethane electromagnetic shielding material prepared in Example 2, the filler-free self-healing polyurethane material prepared in Comparative Example 1, and the modified MXene powder (T-MXene) not dispersed in N,N-dimethylacetamide prepared in step 4 of Example 1 are shown below. Figure 2 .Depend on Figure 2It can be seen that the spectrum of the filler-free self-healing polyurethane material prepared in Comparative Example 1 shows C 1s, O 1s and a weak N 1s peak, which is consistent with the elemental composition of urethane bonds, urea bonds and polyether segments in the polyurethane molecular chain; the spectrum of the modified MXene not dispersed in N,N-dimethylacetamide prepared in step 4 of Example 1 shows Ti 2p, C 1s, O 1s and F 1s peaks, which correspond to the Ti-C skeleton and surface -O, -OH and -F functional groups of MXene, respectively, indicating that the skeleton structure and surface functional groups of MXene are preserved after hydrofluoric acid etching and tetrabutylammonium hydroxide intercalation modification; the spectrum of the self-healing polyurethane electromagnetic shielding material prepared in Example 2 shows C 1s, N 1s and O 1s peaks from polyurethane and Ti 2p and F 1s peaks from modified MXene, indicating that the obtained material is indeed composed of two phases: polyurethane matrix and modified MXene, and the modified MXene has been successfully composited in the polyurethane matrix.

[0102] The microstructure and structural order of the self-healing polyurethane electromagnetic shielding material prepared in Example 2 were characterized using scanning electron microscopy (SEM). The accelerating voltage was set to 5-10 kV, and the sample surface was sputter-coated with gold before testing. SEM images of the self-healing polyurethane electromagnetic shielding material prepared in Example 2 are shown below. Figure 3 .in, Figure 3 (a) is a low-magnification scanning electron microscope (SEM) image. Figure 3 (b) is a high-magnification scanning electron microscope (SEM) image. (From...) Figure 3 (a) It can be seen that the modified MXene is uniformly dispersed in the polyurethane matrix in a layered morphology; from Figure 3 (b) It can be seen that most of the sheets are tightly covered by the polyurethane matrix, and some sheets overlap or are stacked. No obvious large-sized agglomerates or obvious interfacial voids and pores are observed. This uniformly dispersed sheet structure is conducive to the construction of a continuous conductive network with a low filler content and provides abundant interfacial polarization and multiple electromagnetic wave reflection sites. This is consistent with the good interfacial bonding between the two phases demonstrated by infrared spectroscopy and X-ray photoelectron spectroscopy, as well as the improved mechanical properties and electromagnetic shielding effectiveness of the material shown in Table 1.

[0103] It should be noted that although the above embodiments have been described herein, this does not limit the scope of patent protection of the present invention. Therefore, any changes and modifications made to the embodiments described herein based on the innovative concept of the present invention, or equivalent structural or procedural transformations made using the content of the present invention's specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields, are all included within the scope of patent protection of the present invention.

Claims

1. A method for preparing a self-healing polyurethane electromagnetic shielding material, characterized in that, It includes the following steps: Step S1, Prepolymerization: After dehydration treatment of the soft segment monomer polyether polyol, it is dissolved in the first part of the polar aprotic solvent. Under nitrogen protection, the hard segment monomer aliphatic diisocyanate and catalyst are added. The mixture is stirred at 70-90℃ for 2-4 h and then cooled to 35-45℃ to obtain the isocyanate-terminated polyurethane prepolymer solution. Step S2, chain extension: The first chain extender, an acylhydrazine compound, and the second chain extender, an aromatic disulfide, are dissolved in the second part of a polar aprotic solvent and then added dropwise to the prepolymer solution. The reaction is carried out at 35-45°C for 10-20 h to obtain a self-healing polyurethane solution. The molar ratio of the hard segment monomer aliphatic diisocyanate, the soft segment monomer polyether polyol, the first chain extender, and the second chain extender is (1.5-2.5):1:(0.6-0.9):(0.2-0.4). Step S3: Preparation of organoammonium intercalation modified MXene dispersion: The Ti3AlC2 MAX phase precursor is added to an aqueous hydrofluoric acid solution and stirred at 20–30 °C for 18–30 h. The mixture is washed with deionized water and centrifuged until the pH of the supernatant is 6–7. The precipitate is collected to obtain the etching filler. The etching filler is added to an organoammonium intercalating agent and stirred at room temperature for 3–6 h. The residual organoammonium intercalating agent is washed with ethanol to remove it. The resulting precipitate is then dispersed in the polar aprotic solvent and centrifuged. The supernatant is collected to obtain the organoammonium intercalation modified MXene dispersion. The molar ratio of the organoammonium intercalating agent to the Ti3AlC2 MAX phase precursor is 0.6–1.2:

1. Step S4, Composite: Add the organic ammonium intercalated modified MXene dispersion obtained in step S3 to the self-healing polyurethane solution obtained in step S2, and stir for 4-8 h to obtain a self-healing polyurethane / modified MXene composite dispersion. Step S5, Molding and Curing: Pour the composite dispersion into a mold, heat at 70-90℃ for 3-6 h, and then vacuum dry at 70-90℃ for 40-60 h to obtain the self-healing polyurethane electromagnetic shielding material. The mass of the organic ammonium intercalated modified MXene accounts for 5%-20% of the total mass of the self-healing polyurethane electromagnetic shielding material.

2. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S1, the hard segment monomer aliphatic diisocyanate is one or both of isophorone diisocyanate and hexamethylene diisocyanate.

3. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S1, the number average molecular weight of the soft segment monomer polyether polyol is 1000-3000, and it is one or more of polytetrahydrofuran ether diol, polyethylene glycol, and polypropylene glycol.

4. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S2, the first chain extender is one or more of adipic acid dihydrazide, sebacic acid dihydrazide, and terephthalic acid dihydrazide; the second chain extender is one or two of 4,4′-dithiodiphenylamine and 2,2′-dithiodiphenylamine.

5. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, The catalyst is dibutyltin dilaurate, and its amount is 0.05% to 0.2% of the mass of the polyether polyol.

6. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S1, the dehydration treatment of the soft segment monomer polyether polyol is as follows: the soft segment monomer polyether polyol is dried under reduced pressure and vacuum at 100-110°C for 1-2 h; the dissolution temperature of the polyether polyol in step S1 is 40-60°C, and the stirring speed is 150-300 rpm.

7. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S3, the mass concentration of the hydrofluoric acid aqueous solution is 30%–40%, and the mass ratio of the Ti3AlC2 MAX phase precursor to the volume of the hydrofluoric acid aqueous solution is 1:10–25 g / mL; the organic ammonium intercalating agent is a tetrabutylammonium hydroxide aqueous solution; the centrifugation speed in step S3 is 8000–12000 rpm, and the number of centrifugations is 6–8.

8. The method for preparing the self-healing polyurethane electromagnetic shielding material according to claim 1, characterized in that, In step S4, the stirring speed is 200-400 rpm.

9. A self-healing polyurethane electromagnetic shielding material, characterized in that, It comprises a polyurethane matrix and an organoammonium intercalated modified MXene dispersed in the polyurethane matrix; the organoammonium intercalated modified MXene is a tetrabutylammonium intercalated modified Ti3C2T x MXene accounts for 5% to 20% of the total mass of the self-healing polyurethane electromagnetic shielding material; the polyurethane matrix is ​​a polyurethane with polyether polyol as the soft segment and aliphatic diisocyanate as the hard segment.

10. The self-healing polyurethane electromagnetic shielding material according to claim 9, characterized in that, It is prepared by any one of claims 1 to 8.