Neutron shielding type nuclear grade firestop plug and preparation method thereof
By using a modified boron carbide and composite silicone rubber matrix as a sealing material, the problem of multifunctional integration of sealing materials for nuclear power plants has been solved. This material achieves comprehensive performance in terms of high-efficiency neutron shielding, gamma shielding, fire resistance, and radiation resistance, making it suitable for the rapid construction needs of nuclear power plants.
Patent Information
- Application Number
- CN202611447711.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-20
AI Technical Summary
Existing nuclear power plant sealing materials cannot simultaneously achieve the four functions of neutron shielding, gamma shielding, fire protection, and radiation resistance. Furthermore, the B₄C filler is not modified, resulting in poor dispersibility and unstable overall material performance. The simple process leads to numerous internal pores and a long curing cycle, which cannot meet the construction requirements for short maintenance windows in nuclear power plants.
A composite matrix of methyl vinyl silicone rubber and phenyl silicone rubber is used. Boron carbide and silica powder are modified by coating with silane coupling agent KH-550. Combined with fumed silica, carbon black and carboxyl-terminated polybutadiene liquid rubber, an addition-type silicone rubber system is formed. With the help of vacuum mixing and segmented plasticizing processes, the material achieves multifunctional integration.
It achieves a neutron shielding efficiency of over 80%, improves resistance to gamma-ray irradiation, and the material does not crack or pulverize under 10⁶ Gy gamma irradiation. It also has excellent fire resistance and rapid curing ability, meeting the requirements for rapid construction in nuclear power plants.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the technical field of special functional materials for nuclear power plants, and in particular to a neutron-shielded nuclear-grade fireproof sealant and its preparation method. Background Technology
[0002] Nuclear power plant reactors, spent fuel pools, and related irradiated areas contain significant amounts of neutron and gamma-ray radiation, and must meet stringent fire safety standards (such as a fire resistance rating of ≥2 hours). Sealing penetrations (such as pipes and cables) in these areas requires a special material that integrates fire resistance, radiation shielding, and resistance to long-term radiation.
[0003] Existing sealing materials for nuclear power plant operations fall into two categories, each with significant technical shortcomings: 1. Ordinary silicone fireproof materials: These only possess fireproof and sealing capabilities, lacking neutron shielding functionality and thus unsuitable for use in neutron radiation areas; 2. Conventional boron-containing neutron shielding materials: Borides (B4C) are prone to moisture absorption and aggregation, exhibiting poor compatibility with polymer matrices, and lacking sufficient fireproof and radiation resistance capabilities.
[0004] Summary of existing technical defects: ① Functional separation, unable to simultaneously achieve the four major functions of neutron shielding, gamma shielding, fire protection, and radiation resistance; ② B4C filler is not modified, resulting in poor dispersibility and unstable overall material performance; ③ The matrix formulation is simple, leading to material embrittlement and cracking after high-dose gamma irradiation; ④ The process is simple, with many internal pores and a long curing cycle, failing to meet the construction requirements for short maintenance windows in nuclear power plants.
[0005] In existing publicly available technologies, fireproof sealing and neutron shielding materials are independent of each other and lack integrated formulation design; most B4C-containing shielding materials have not undergone surface coating modification, resulting in poor interfacial bonding of fillers; at the same time, there is a lack of radiation-resistant formulation systems for phenyl silicone rubber and toughening agents. Summary of the Invention
[0006] To address the issue of poor interfacial bonding in B4C shielding materials due to lack of surface coating modification, this application provides a neutron-shielded nuclear-grade fireproof sealing material and its preparation method.
[0007] This application provides a neutron-shielded nuclear-grade fireproof sealing solution, employing the following technical solution: A neutron-shielded nuclear-grade fireproof sealing agent comprises, by weight, the following raw materials: 70-100 parts of methyl vinyl silicone rubber, 20-40 parts of phenyl silicone rubber, 40-70 parts of silane coupling agent KH-550 coated and modified boron carbide, 80-110 parts of silica powder, 15-30 parts of fumed silica, 3-5 parts of carbon black, 3-5 parts of carboxyl-terminated polybutadiene liquid rubber, 5-10 parts of hydrogen-containing silicone oil, and 0.5-2 parts of platinum catalyst.
[0008] By adopting the above technical solutions, methyl vinyl silicone rubber undergoes hydrosilylation crosslinking and curing with hydrogen-containing silicone oil, exhibiting excellent resistance to high and low temperatures, aging, water vapor, and insulation properties. It is also resistant to corrosion in nuclear power plant environments, making it the most commonly used silicone rubber substrate for fireproofing and sealing. Phenyl silicone rubber improves the interfacial wettability with boron carbide and silica micropowder inorganic fillers, reducing filler agglomeration; it enhances resistance to gamma rays and neutron radiation, inhibits molecular chain breakage and pulverization under long-term irradiation, and strengthens the fireproof and heat-insulating barrier.
[0009] Boron carbide effectively absorbs neutrons. Its high melting point, high temperature resistance, and high Mohs hardness enhance the high-temperature structural strength of the sealing material, preventing collapse during fire resistance. KH-550's surface modification properties significantly improve its compatibility and dispersibility with silicone rubber, preventing agglomeration and ensuring uniform shielding effectiveness. Silica micropowder increases the hardness and compression set of the compound, and during high-temperature combustion, it synergistically forms a continuous SiO2 ceramic layer, blocking the diffusion of flames, heat, smoke, and radioactive aerosols.
[0010] Fumed silica, produced through fumed silica production, significantly enhances tensile strength, tear strength, and abrasion resistance by adsorbing silicone rubber molecular chains onto its surface silanol groups. This compensates for the brittleness issues caused by excessive boron carbide and silica powder fillers. Simultaneously, it improves the thixotropic properties of the compound, preventing flow during pouring / packing and ensuring stable morphology after molding. Carbon black absorbs ultraviolet light and radiation, improving resistance to radiation aging and enhancing the uniformity of thermal conductivity to prevent localized overheating and ablation. It also imparts a degree of conductivity and antistatic properties to sealing materials, mitigating the risk of static electricity buildup in nuclear power plant areas.
[0011] Carboxyl-terminated liquid polybutadiene can weakly interact with the amino groups of KH-550, anchoring itself at the filler interface and alleviating stress concentration caused by inorganic fillers; flexible rubber segments are interspersed in the gaps of the silicone rubber network, improving the low-temperature toughness and vibration crack resistance of the sealing material, making it suitable for sealing integrity under thermal vibration and seismic conditions of nuclear power pipelines and cables; platinum catalyst enables addition vulcanization, with no byproducts, resulting in uniform deep curing and stable performance of the material.
[0012] Boron carbide neutron shielding combined with silicone rubber ceramic fireproofing simultaneously meets the dual requirements of nuclear radiation protection and fire-resistant sealing. The addition-type silicone rubber system is free of volatiles, low in toxicity and smoke, radiation resistant, and exhibits a low aging rate in nuclear power plant environments. Boron carbide modified with silane coupling agent KH-550 ensures shielding, solves the common interfacial compatibility problem in highly filled systems, and provides high sealing density, preventing radioactive dust leakage. The surface of the boron carbide is covalently modified with silane coupling agent, giving the material thermal neutron shielding, gamma-ray shielding, fire resistance ≥2h, and 10 6 The Gy / γ irradiation-resistant, non-cracking, and pulverizing integrated nuclear-grade function combines four key features: silica micropowder-controlled refractory structure, fumed silica reinforcement, liquid rubber toughening, and good system balance.
[0013] This application discloses a nuclear-grade multifunctional plugging material solution based on modified B4C, composite silicone rubber, and toughening system. Through triple optimization of the shielding filler modification formula, composite rubber matrix formula, and toughening system formula, combined with improvements in vacuum mixing and segmented plasticizing processes, it achieves multifunctional integration and solves problems such as filler agglomeration, irradiation embrittlement, single function, and slow construction.
[0014] Preferably, the silane coupling agent KH-550 is used to coat and modify boron carbide: boron carbide powder is mixed and stirred with silane coupling agent KH-550 to obtain silane coupling agent KH-550 coated and modified boron carbide.
[0015] By adopting the above technical solution, the silane coupling agent KH-550 forms an organic molecular layer on the surface of boron carbide, which acts as a molecular bridge, bonding boron carbide at one end and entangled with silicone rubber molecular chains at the other end, thereby greatly improving the compatibility between the two. After modification, boron carbide is more tightly bonded to the matrix, and when the material is subjected to external force, the stress can be effectively transferred, avoiding the crack source due to interface debonding, thereby maintaining the mechanical strength and elasticity of the material.
[0016] The organic amino outer layer and the silicone rubber matrix generate hydrogen bonding forces, which greatly improves the interfacial bonding strength between the inorganic filler and the silicone rubber; the filler is uniformly dispersed, and the rubber compound is free of pores and defects, ensuring the gas tightness of the sealing and the uniformity of neutron shielding; no large amount of free coupling agent enters the rubber compound, avoiding the amino complexation of platinum catalyst and preventing delayed vulcanization and incomplete curing; when the finished sealing material is subjected to stress and thermal expansion and contraction, the filler and the matrix are not prone to interfacial gaps, taking into account neutron shielding, fire resistance, and long-term sealing stability.
[0017] Preferably, the organic treatment of the silicon micropowder includes the following: mixing and stirring the silicon micropowder with the silane coupling agent KH-550, drying it, and then storing it for later use.
[0018] By adopting the above technical solution, KH-550 disperses agglomerated silicon micropowder particles, and relies on material flow to allow the liquid coupling agent to uniformly wet the surface of all silicon micropowder particles, forming a continuous thin liquid film. This eliminates the phenomenon of localized coupling agent enrichment and clumping, and the phenomenon of some particles being exposed without coating. This system shares the KH-550 modification system with boron carbide. After modification, both fillers have amino groups on their surfaces, resulting in better compatibility between the fillers. During mixing, boron carbide and silicon micropowder are less prone to segregation and stratification.
[0019] After grafting amino organic segments onto the surface of silica micropowder, hydrogen bonds and molecular entanglement are formed with the silicone rubber molecular chains, enhancing interfacial adhesion and improving the tensile and tear strength of the material, preventing brittleness under high filling conditions. After molding, the interior is free of voids and defects, effectively blocking the penetration of flames, smoke, and radioactive aerosols, and can also achieve a uniform neutron shielding effect when combined with boron carbide. Modified silica micropowder reduces the oil absorption value of the powder, resulting in better flowability of the compound, reducing the likelihood of material blockage and internal air bubble formation during pouring; it also reduces the permanent compression set of the compound, ensuring that pores remain sealed under long-term pressure. During high-temperature combustion, modified silica micropowder, in conjunction with the pyrolysis products of silicone rubber, forms a continuous and dense silica ceramic layer, blocking heat transfer and improving the overall fire resistance limit.
[0020] Preferably, the raw materials also include 10-15 parts of composite kaolin, which is composed of kaolin, quartz sand, and sodium lignosulfonate.
[0021] By adopting the above technical solutions, kaolin is incorporated into the silicone rubber system, improving the material's hardness and compressive strength. This mitigates the problems of excessive rigidity and brittleness caused by high-hardness fillers such as boron carbide and silica powder, optimizing the resilience of the sealing body and adapting to the sealing requirements of pore deformation. Kaolin can absorb heat from the fire; at high temperatures, it forms a mullite phase, which, together with silica powder and boron carbide, constructs a stable high-temperature resistant ceramic skeleton. After combustion, the solidified layer is less prone to collapse and detachment, extending the fire resistance time. Kaolin significantly extends the penetration path of flames, smoke, and radioactive aerosols, strengthening the airtightness and smoke tightness of the sealing layer and meeting the radioactive dust barrier requirements of nuclear sites.
[0022] Quartz sand can be uniformly dispersed in the material, forming a micron-sized rigid skeleton, significantly improving the mechanical strength, rigidity, and dimensional stability of the sealing material. Its structure remains stable under high-temperature open flame conditions, compensating for the porous structure of dehydrated kaolin, and enhancing the high-temperature residual strength of the fireproof sealing material. It will not collapse or break under heat and pressure. The thermal expansion rate of the overall filler system is coordinated with the silica powder within the system, preventing internal microcracks from forming due to thermal expansion and contraction during high-temperature-to-room-temperature cycles, ensuring a continuous and uninterrupted neutron shielding layer.
[0023] Sodium lignosulfonate adsorbs onto the surface of kaolin and quartz sand particles, relying on electrostatic repulsion and steric hindrance to disperse agglomerated particles, allowing the composite kaolin to be uniformly dispersed in the silicone rubber matrix without forming localized agglomeration defects. Combined with KH-550, sodium lignosulfonate optimizes the wetting effect between inorganic powders and organic rubber, reduces the viscosity of the compound, and improves processing fluidity. Sodium lignosulfonate slowly decomposes in the initial stage of heating, releasing inert gases to dilute combustible fumes, while simultaneously decomposing and carbonizing to form a char layer, assisting in the initial flame retardancy and smoke suppression of the matrix, reducing combustion smoke production, and meeting the low smoke toxicity standards for nuclear-grade materials.
[0024] The rigid framework of quartz sand provides the basic strength of the material, while the ceramic protective layer formed by the high-temperature transformation of kaolin adheres to this framework. The combination of the two forms a reinforced structure that is both strong and heat-resistant. The dispersing and binding effect of sodium lignosulfonate allows the former two (kaolin and quartz sand) and other fillers in the formulation (such as boron carbide and silica powder) to be uniformly dispersed and firmly bonded to the rubber matrix.
[0025] Preferably, the composite kaolin is prepared by dispersing sodium lignosulfonate in deionized water, adding kaolin and quartz sand, stirring at 60-62℃ for 1-2 hours, and drying to obtain composite kaolin.
[0026] By employing the above technical solution, sodium lignosulfonate is pre-dispersed in deionized water. The aqueous solution system can uniformly encapsulate kaolin sheets and quartz sand particles in a molecular state, weakening the hydrogen bond adsorption force between kaolin sheets and pre-exfoliating the original kaolin aggregates. The dissolved sodium lignosulfonate is rapidly adsorbed onto the surface of kaolin and quartz sand particles, relying on electrostatic repulsion and steric hindrance of polymers to break up the powder aggregates, avoiding localized filler aggregation and microporous defects inside the material after the addition of silicone rubber. By having both powders coated with the same dispersant layer, the kaolin and quartz sand are more tightly bonded, forming a two-dimensional gradation structure of the composite powder. Subsequent filling into the silicone rubber results in a denser buildup, improving the sealing airtightness and the density of the high-temperature carbon layer.
[0027] Sodium lignosulfonate, combined with KH-550-modified boron carbide and silica powder, significantly improves the dispersibility of the entire inorganic filler system. Under high filler conditions, the compound exhibits better processing fluidity, reducing the likelihood of voids during casting. Kaolin, with its tortuous structure, extends the penetration path of flue gas and radioactive dust, while quartz sand enhances the strength of the high-temperature ceramic layer, preventing the sealing structure from collapsing after combustion and improving refractory integrity. The mineral lattice, combined with hydrogen, slows down fast neutrons, while boron carbide absorbs thermal neutrons, forming a synergistic shielding system that improves overall neutron shielding efficiency. Kaolin imparts excellent thixotropy to the compound, preventing flow and promoting rapid setting after on-site pore filling.
[0028] Preferably, the pretreatment of the quartz sand includes the following steps: calcining the quartz sand at 300-310℃ under a nitrogen atmosphere for 1-2 hours, dispersing it in an ethanol solution of polyvinyl alcohol, adding graphene, sonicating for 2-3 hours, and drying to obtain pretreated quartz sand.
[0029] By employing the above technical solution, calcination removes adsorbed water, free crystal water, dust, oil, and residual organic impurities from the surface of quartz sand, purifying the particle surface and exposing fresh, highly active silanol sites, facilitating the subsequent strong adhesion of polyvinyl alcohol. Polyvinyl alcohol molecules possess numerous hydroxyl groups, with one end bonded to the activated quartz sand surface via hydrogen bonds, coating the quartz particles with a flexible organic polymer film. The outer organic segments can achieve compatibility with the silicone rubber matrix and sodium lignosulfonate, improving the interfacial bonding force between the rigid quartz particles and the rubber matrix and reducing interfacial defects. The polyvinyl alcohol film also serves as a load-bearing and bonding carrier for graphene, allowing graphene to be stably fixed on the quartz surface, preventing it from detaching or agglomerating during the mixing and shearing process.
[0030] Graphene loaded onto the surface of quartz sand improves the poor thermal conductivity and localized concentrated ablation problems of highly filled inorganic filler systems, enhancing the overall uniformity of heat conduction in the fireproof layer. The graphene fills the tiny voids created by the accumulation of fillers, further improving the airtightness of the sealing material, preventing the leakage of radioactive aerosols, and enhancing the material's mechanical strength, wear resistance, and erosion resistance. It can also capture free radicals generated by irradiation, delaying the irradiation aging and breakage of silicone rubber molecular chains, and improving the long-term service stability of the sealing material.
[0031] Quartz sand, after being modified by coating with polyvinyl alcohol and graphene, becomes a functional filler with thermal conductivity, radiation resistance, and airtightness. Graphene is uniformly dispersed on the support of quartz particles, preventing it from being directly mixed into the rubber matrix and causing localized abnormal conductivity or a surge in system viscosity. Combined with a dispersion system of kaolin and sodium lignosulfonate, the filler is multi-stage compounded and stacked more densely, simultaneously improving neutron shielding uniformity, fire resistance integrity, and radiation resistance life. The polyvinyl alcohol organic transition layer connects the inorganic quartz and the organic silicone rubber matrix, reducing interfacial stress and making the sealing material less prone to cracking and failure during thermal cycling.
[0032] Preferably, the carbon black is pretreated with nano-cerium oxide and gypsum.
[0033] By adopting the above technical solutions, carbon black exhibits improved radiation resistance, homogenized thermal conductivity, antistatic properties, UV radiation absorption, and auxiliary light-shielding to delay the aging of silicone rubber. After gypsum coating modification, the carbon black dispersion is significantly improved, eliminating localized conductive points, uneven color of the rubber compound, and mechanical defects caused by carbon black aggregation. Gypsum microparticles and nano-cerium oxide are uniformly attached to and embedded on the surface of carbon black particles, constructing a composite particle structure with a carbon black core, a gypsum intermediate coating layer, and a nano-cerium oxide surface layer.
[0034] Rare earth cerium oxide possesses variable valence states, enabling it to capture a large number of free radicals generated by gamma rays and neutron irradiation. This blocks the irradiation degradation and chain breakage of silicone rubber molecular chains, significantly improving the long-term radiation resistance of materials under nuclear conditions. At high temperatures, cerium oxide can catalyze the pyrolysis of silicone rubber to generate a denser and more continuous SiO2 ceramic carbon layer, improving the density of the refractory layer and blocking the penetration of heat, flue gas, and radioactive aerosols. The gypsum inorganic coating isolates carbon black from direct contact with the platinum catalyst, ensuring the normal progress of the hydrosilylation reaction; the gypsum layer connects the hydrophobic carbon black to the silicone rubber matrix, improving the wetting and dispersion of carbon black in the rubber compound.
[0035] Cerium oxide endows the material with excellent resistance to radiation and heat-oxidative aging, matching the long-term radiation service environment of nuclear power plants; gypsum serves as both a coating carrier and a refractory filler, optimizing fire resistance; uniformly dispersed modified carbon black can evenly conduct internal heat, ensuring a uniform temperature field when the sealing body is heated, preventing localized overheating and burn-through. This solves two major problems of ordinary carbon black: difficulty in dispersion due to agglomeration and interference with sulfidation due to platinum catalyst adsorption.
[0036] Secondly, this application also provides a method for preparing a neutron-shielded nuclear-grade fireproof seal, comprising the following steps: Methyl vinyl silicone rubber, phenyl silicone rubber, and carboxyl-terminated polybutadiene are mixed and plasticized. Silane coupling agent KH-550 is added in three batches to coat and modify boron carbide, silica powder, fumed silica, and carbon black. After each addition, the mixture is kneaded and continuously degassed under vacuum. The above-mentioned well-mixed base rubber compound is divided into two components, A and B. Platinum catalyst is added to component A and hydrogen-containing silicone oil is added to component B. The mixture is stirred under vacuum conditions. Mix the two-component materials A and B, inject them into the mold of the hole to be sealed, and let it stand at room temperature to cure for no more than 12 hours to obtain the final product.
[0037] By adopting the above technical solution, boron carbide (neutron shielding) is coated and modified using the silane coupling agent KH-550, and a composite shielding filler of silica powder is used. Simultaneously, KH-550 is used as a coating agent to chemically bond and modify boron carbide. This solves the industry problems of boron carbide's moisture absorption, agglomeration, and weak bonding with the matrix, achieving dual shielding against neutrons and gamma rays. Instead of using single silicone rubber, a composite matrix of methyl vinyl silicone rubber and phenyl silicone rubber is adopted. The phenyl structure enhances the material's resistance to gamma radiation, preventing brittleness after long-term irradiation. A carboxyl-terminated polybutadiene toughening agent is added, combined with hydrogen-containing silicone oil and a platinum catalytic system, forming a synergistic system of matrix, toughening, and catalysis, improving material toughness and molding efficiency, and shortening curing time.
[0038] In summary, this application has the following beneficial effects: 1. The B4C-specific coating process in this application achieves chemical bonding coating of the silane coupling agent, unlike conventional simple mixing; the fireproof + shielding composite filler system simultaneously adds modified B4C (neutron shielding), silica powder (gamma shielding), and fumed silica (reinforcing / charring), achieving a three-in-one combination of fireproofing, neutron shielding, and gamma shielding. The synergistic design of radiation resistance and anti-embrittlement utilizes a methyl vinyl silicone rubber and phenyl silicone rubber composite matrix, with the addition of carboxyl-terminated polybutadiene toughening agent, to withstand 10... 6 Gy γ irradiation does not cause cracking or pulverization, solving the problem of "embrittlement after irradiation" in boron-containing polymer materials.
[0039] 2. The stepwise vacuum mixing process in this application: The rubber matrix is first plasticized separately, and then the filler is added in three stages for gradual mixing, which significantly improves the uniformity of filler dispersion. The entire mixing process is carried out in a vacuum environment to eliminate internal pores in the material and improve the sealing tightness and protective performance. Room temperature rapid curing process: The catalytic system ratio is optimized to achieve complete curing within 12 hours at room temperature, meeting the rapid construction requirements of nuclear power plants.
[0040] 3. This application integrates four major functions—neutron shielding, gamma-ray shielding, nuclear-grade fire resistance, and resistance to long-term radiation—into a single material system, exhibiting excellent neutron / gamma-ray shielding performance: By chemically modifying the surface of B4C, its dispersion problem in silicone rubber is solved, achieving a thermal neutron shielding efficiency of over 80%. Furthermore, the synergistic design of phenyl silicone rubber and carboxyl-terminated polybutadiene toughening agent overcomes the industry challenge of traditional boron-containing polymers becoming brittle and cracking under long-term high-dose radiation. Detailed Implementation
[0041] The present application will be further described in detail below with reference to the embodiments.
[0042] The raw materials used in the examples and comparative examples are all commercially available.
[0043] Example 1 A neutron-shielded nuclear-grade fireproof sealing agent, by weight, comprises the following raw materials: 85 parts of methyl vinyl silicone rubber, 30 parts of phenyl silicone rubber, 55 parts of silane coupling agent KH-550 coated and modified boron carbide, 100 parts of silica powder, 22 parts of fumed silica, 4 parts of carbon black, 4 parts of carboxyl-terminated polybutadiene liquid rubber, 8 parts of hydrogen-containing silicone oil, and 1.5 parts of platinum catalyst.
[0044] Methyl vinyl silicone rubber was purchased from Shandong Dayi Chemical Co., Ltd., phenyl silicone rubber was purchased from Shandong Dayi Chemical Co., Ltd., carboxyl-terminated polybutadiene liquid rubber was purchased from Shandong Dayi Chemical Co., Ltd., hydrogen-containing silicone oil was purchased from Shandong Dayi Chemical Co., Ltd., and platinum catalyst was purchased from Shanghai Silicon Power Advanced Materials Co., Ltd.
[0045] Boron carbide coated with silane coupling agent KH-550: Boron carbide powder was added to a high-speed mixer, and 5% of the mass of silane coupling agent KH-550 was added while stirring. The mixture was stirred at 80℃ and 400r / min for 60min to obtain silane coupling agent KH-550 coated with boron carbide.
[0046] The silicon micro powder was purchased from Yongshun Mineral Products Processing Plant in Lingshou County.
[0047] Methyl vinyl silicone rubber, phenyl silicone rubber, and carboxyl-terminated polybutadiene were put into a kneader and plasticized at 50°C for 10 minutes. Boron carbide coated with silane coupling agent KH-550, silica powder, fumed silica, and carbon black were added in three equal portions. After each addition, the mixture was kneaded at 80°C and 1000 r / min for 30 minutes and continuously degassed under a vacuum of -0.08 MPa. The above-mentioned well-mixed base rubber compound was divided into two components, A and B. Platinum catalyst was added to component A and hydrogen-containing silicone oil was added to component B. The mixture was stirred for 30 minutes at 30°C, 800 r / min and vacuum. Mix the two-component materials A and B for 3 minutes, then inject them into the mold of the hole to be sealed. Allow it to stand at room temperature for 11 hours to cure and solidify.
[0048] Example 2: A neutron-shielded nuclear-grade fireproof sealing method, which differs from Example 1 in that it includes the following raw materials: 70 parts of methyl vinyl silicone rubber, 40 parts of phenyl silicone rubber, 40 parts of silane coupling agent KH-550 coated and modified boron carbide, 80 parts of silica powder, 15 parts of fumed silica, 3 parts of carbon black, 3 parts of carboxyl-terminated polybutadiene liquid rubber, 5 parts of hydrogen-containing silicone oil, and 0.5 parts of platinum catalyst.
[0049] Boron carbide coated with silane coupling agent KH-550: Boron carbide powder was added to a high-speed mixer, and 6% of the mass of silane coupling agent KH-550 was added while stirring. The mixture was stirred at 80℃ and 400r / min for 60min to obtain silane coupling agent KH-550 coated with boron carbide.
[0050] Example 3: A neutron-shielded nuclear-grade fireproof sealing method, which differs from Example 1 in that it includes the following raw materials: 100 parts of methyl vinyl silicone rubber, 20 parts of phenyl silicone rubber, 70 parts of silane coupling agent KH-550 coated and modified boron carbide, 110 parts of silica powder, 30 parts of fumed silica, 5 parts of carbon black, 5 parts of carboxyl-terminated polybutadiene liquid rubber, 10 parts of hydrogen-containing silicone oil, and 2 parts of platinum catalyst.
[0051] Boron carbide coated with silane coupling agent KH-550: Boron carbide powder was added to a high-speed mixer, and 4% of the mass of silane coupling agent KH-550 was added while stirring. The mixture was stirred at 80℃ and 400r / min for 60min to obtain silane coupling agent KH-550 coated with boron carbide.
[0052] Example 4: A neutron-shielded nuclear-grade fireproof sealing method, which differs from Example 1 in that the silicon micropowder undergoes organic treatment, including the following: mixing silicon micropowder with 6% by weight of silane coupling agent KH-550, stirring at 80°C for 30 minutes, and drying for later use.
[0053] Example 5: A neutron-shielded nuclear-grade fireproof sealing method, which differs from Example 4 in that the silicon micropowder undergoes organic treatment, including the following: mixing silicon micropowder with 4% by weight of silane coupling agent KH-550, stirring at 80°C for 30 minutes, and drying for later use.
[0054] Example 6: A neutron-shielded nuclear-grade fireproof sealant, which differs from Example 4 in that the raw materials also include 15 kg of composite kaolin, which is composed of kaolin, quartz sand, and sodium lignosulfonate.
[0055] Preparation of composite kaolin: Disperse 1 kg of sodium lignosulfonate in 30 L of deionized water, add 13 kg of kaolin and 3 kg of quartz sand, stir at 60 °C for 2 h, dry to obtain composite kaolin, and use the required amount.
[0056] A method for preparing a neutron-shielded nuclear-grade fireproof sealant involves adding methyl vinyl silicone rubber, phenyl silicone rubber, and carboxyl-terminated polybutadiene into a kneader and plasticizing at 50°C for 10 minutes. Then, in three equal portions, silane coupling agent KH-550-coated modified boron carbide, silica powder, fumed silica, carbon black, and composite kaolin are added. After each addition, the mixture is kneaded at 80°C and 1000 r / min for 30 minutes, and degassing is continuously performed under a vacuum of -0.08 MPa. Subsequent steps are the same as those described above.
[0057] Example 7: A neutron-shielded nuclear-grade fireproof sealant, which differs from Example 6 in that the raw materials also include 10 kg of composite kaolin.
[0058] Example 8 A neutron-shielded nuclear-grade fireproof sealing method differs from Example 6 in that the quartz sand is pretreated, including the following: quartz sand is calcined at 300°C under a nitrogen atmosphere for 2 hours, dispersed in 15L of a 3% polyvinyl alcohol ethanol solution, 0.9kg of graphene is added, ultrasonicated for 3 hours, and dried to obtain pretreated quartz sand.
[0059] Example 9 A neutron-shielded nuclear-grade fireproof sealing method differs from Example 8 in that the quartz sand is pretreated, including the following: quartz sand is calcined at 300°C in a nitrogen atmosphere for 2 hours, mixed with 0.9 kg of graphene, stirred for 3 hours, and dried to obtain pretreated quartz sand.
[0060] Example 10: A neutron-shielded nuclear-grade fireproof sealing method, which differs from Example 8 in that the quartz sand is pretreated as follows: the quartz sand is calcined at 300°C in a nitrogen atmosphere for 2 hours, dispersed in 15L of a 3% polyvinyl alcohol ethanol solution, sonicated for 3 hours, and dried to obtain pretreated quartz sand.
[0061] Example 11: A neutron-shielded nuclear-grade fireproof sealant, which differs from Example 8 in that the carbon black is pretreated with nano-cerium oxide and gypsum.
[0062] 0.6 kg of gypsum was dispersed in 24 L of ethanol / deionized water solution (ethanol / deionized water volume ratio of 3:7), stirred for 25 min, carbon black and 1.5 kg of nano-cerium oxide were added, and ball milling was performed to obtain pretreated carbon black.
[0063] Example 12: A neutron-shielded nuclear-grade fireproof sealant, which differs from Example 11 in that the carbon black is pretreated with gypsum.
[0064] Example 13: A neutron-shielded nuclear-grade fireproof sealant, which differs from Example 11 in that the carbon black is pretreated with nano-cerium oxide.
[0065] Comparative Example 1 A neutron-shielded nuclear-grade fireproof sealing method differs from Example 1 in that the silane coupling agent KH-550 coating modified boron carbide is replaced by an equal amount of boron carbide.
[0066] The performance of a neutron-shielded nuclear-grade fireproof seal prepared in Examples 1-13 and Comparative Example 1 was tested. Test vertical fire resistance rating according to GB / T2408-2008.
[0067] Tensile strength: The test was conducted in accordance with GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", using dumbbell-shaped specimens.
[0068] After 5×10 6 After Gy γ irradiation, LOCA simulation tests were conducted according to ASTM D3911-2008, "Standard Test Method for Coatings for Light Water-Coated Nuclear Power Plants to Withstand Loss of Water Accident (LOCA) Simulation Environment." The following tests were performed: Tensile strength retention rate: The tensile strength of the irradiated samples was tested according to GB / T 528-2009, and the percentage of its tensile strength before irradiation was calculated. The test results are shown in Table 1.
[0069] Table 1 Test data for the examples and comparative examples
[0070] As shown in Table 1, the neutron-shielded nuclear-grade fireproof sealing materials prepared in Examples 1-3 of this application exhibit good comprehensive performance. Specifically, Example 1 shows a tensile strength of 6.5 MPa, a tensile strength retention rate of 85% after irradiation, and a flame retardant rating of V-0. It is evident that the nuclear-grade multifunctional sealing material scheme based on modified B4C, composite silicone rubber, and a toughening system of this application achieves multifunctional integration and solves problems such as filler agglomeration and irradiation embrittlement through triple optimization of the shielding filler modification formula, composite rubber matrix formula, and toughening system formula, combined with improvements in vacuum mixing and segmented plasticizing processes.
[0071] Examples 4-5 involved organic treatment of silica powder. As shown in Table 1, the tensile strength and tensile strength retention rate after irradiation of Examples 4-5 were better than those of Examples 1-3. This indicates that after grafting amino organic segments onto the surface of silica powder, hydrogen bonds and molecular entanglement are formed with the silicone rubber molecular chains, improving interfacial adhesion, enhancing the tensile and tear strength of the material, and forming a continuous and dense silica ceramic layer in conjunction with the pyrolysis products of silicone rubber, which blocks heat transfer and improves the overall fire resistance limit.
[0072] The raw materials of Examples 6-7 also include composite kaolin. As shown in Table 1, the tensile strength and tensile strength retention rate after irradiation of Examples 6-7 are better than those of Examples 4-5. This indicates that the rigid skeleton of quartz sand provides the basic strength of the material, and the ceramic protective layer formed by the high temperature transformation of kaolin adheres to this skeleton. The combination of the two forms a reinforced structure. The dispersing and binding effect of sodium lignosulfonate enables kaolin, quartz sand and other fillers in the formulation to be uniformly dispersed and firmly bonded to the rubber matrix.
[0073] Example 8 involved pretreatment of quartz sand, while Examples 9-10 involved pretreatment of quartz sand without the addition of polyvinyl alcohol or graphene. Table 1 shows that Example 8 exhibited better tensile strength and post-irradiation tensile strength retention rates than Examples 6-7, while Examples 9-10 showed worse results than Example 8, but better than Examples 6-7. This indicates that after polyvinyl alcohol and graphene coating modification, quartz sand becomes a thermally conductive, radiation-resistant, and airtight reinforced functional filler. The multi-level compound packing of the filler results in a denser structure, simultaneously improving neutron shielding uniformity, fire resistance integrity, and radiation resistance lifespan. The sealing material is also less prone to cracking and failure during thermal cycling.
[0074] In Example 11, the carbon black underwent pretreatment with nano-cerium oxide and gypsum. In Examples 12-13, the carbon black pretreatment did not include nano-cerium oxide or gypsum. Table 1 shows that the tensile strength and tensile strength retention rate after irradiation in Example 11 were superior to those in Example 8. The corresponding test results in Examples 12-13 were inferior to those in Example 11, but superior to those in Example 8. This indicates that cerium oxide imparts excellent resistance to radiation and thermo-oxidative aging, matching the long-term irradiation environment of nuclear power plants; gypsum serves as both a coating carrier and a refractory filler, optimizing fire resistance; and the uniformly dispersed modified carbon black can evenly conduct internal heat, resulting in a uniform temperature field when the sealing body is heated, preventing localized overheating and burn-through.
[0075] In Comparative Example 1, the silane coupling agent KH-550 coated and modified boron carbide was replaced by boron carbide in equal amounts. As shown in Table 1, the tensile strength and tensile strength retention rate after irradiation of Comparative Example 1 were worse than those of Example 1. This indicates that the silane coupling agent KH-550 coated and modified boron carbide ensures shielding, solves the common problem of interfacial compatibility in high-filling systems, has high sealing density, and can block the leakage of radioactive dust.
[0076] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A neutron-shielded nuclear-grade fireproof sealing method, characterized in that, By weight, it includes the following raw materials: 70-100 parts of methyl vinyl silicone rubber, 20-40 parts of phenyl silicone rubber, 40-70 parts of silane coupling agent KH-550 coated and modified boron carbide, 80-110 parts of silica powder, 15-30 parts of fumed silica, 3-5 parts of carbon black, 3-5 parts of carboxyl-terminated polybutadiene liquid rubber, 5-10 parts of hydrogen-containing silicone oil, and 0.5-2 parts of platinum catalyst.
2. The neutron-shielded nuclear-grade fireproof sealing method according to claim 1, characterized in that, The silane coupling agent KH-550 coated and modified boron carbide: Boron carbide powder is mixed and stirred with silane coupling agent KH-550 to obtain silane coupling agent KH-550 coated and modified boron carbide.
3. The neutron-shielded nuclear-grade fireproof sealing method according to claim 1, characterized in that, The organic treatment of the silicon micropowder includes the following steps: mixing and stirring the silicon micropowder with the silane coupling agent KH-550, drying it, and then storing it for later use.
4. A neutron-shielded nuclear-grade fireproof sealing method according to claim 1, characterized in that, The raw materials also include 10-15 parts of composite kaolin, which is composed of kaolin, quartz sand, and sodium lignosulfonate.
5. A neutron-shielded nuclear-grade fireproof sealing method according to claim 4, characterized in that, The composite kaolin is prepared by dispersing sodium lignosulfonate in deionized water, adding kaolin and quartz sand, stirring at 60-62℃ for 1-2 hours, and drying to obtain composite kaolin.
6. A neutron-shielded nuclear-grade fireproof sealing method according to claim 5, characterized in that, The pretreatment of the quartz sand includes the following steps: calcining the quartz sand at 300-310℃ under a nitrogen atmosphere for 1-2 hours, dispersing it in an ethanol solution of polyvinyl alcohol, adding graphene, sonicating for 2-3 hours, and drying to obtain pretreated quartz sand.
7. A neutron-shielded nuclear-grade fireproof sealing method according to claim 1, characterized in that, The carbon black is pretreated with nano-cerium oxide and gypsum.
8. The method for preparing a neutron-shielded nuclear-grade fireproof seal according to claim 1, characterized in that, Includes the following steps: Methyl vinyl silicone rubber, phenyl silicone rubber, and carboxyl-terminated polybutadiene are mixed and plasticized. Silane coupling agent KH-550 is added in three batches to coat and modify boron carbide, silica powder, fumed silica, and carbon black. After each addition, the mixture is kneaded and continuously degassed under vacuum. The above-mentioned well-mixed base rubber compound is divided into two components, A and B. Platinum catalyst is added to component A and hydrogen-containing silicone oil is added to component B. The mixture is stirred under vacuum conditions. Mix the two-component materials A and B, inject them into the mold of the hole to be sealed, and let it stand at room temperature to cure for no more than 12 hours to obtain the final product.