Preparation method of chemically modified mica powder and UV three-proof paint
By modifying and dispersing mica powder with silane coupling agents, the incompatibility problem between mica powder and resin matrix was solved, achieving uniform dispersion and improved high-efficiency insulation performance of mica powder in UV conformal coatings.
Patent Information
- Application Number
- CN202611324379.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
In the existing technology, there is interfacial incompatibility between mica powder and organic UV resin matrix, which leads to poor uniform dispersion of filler, easy agglomeration and sedimentation, and weakens the insulation performance and density of coating.
By modifying mica powder with silane coupling agents to form Si-O-Si or Si-O-Al covalent chemical bonds, the interfacial bonding strength between the modified mica powder and the resin matrix is improved. High-speed dispersion and vacuum degassing technology are used to ensure that the mica powder is uniformly dispersed in the resin.
The interfacial bonding strength between modified mica powder and resin matrix is improved, the dispersion stability is increased by 134%, the electrical insulation performance of the coating is significantly improved, the breakdown field strength and volume resistivity are increased, the coating density is enhanced, and the protective performance is improved.
Smart Images

Figure CN123131850A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic protective coating technology, specifically a method for preparing chemically modified mica powder and UV conformal coating. Background Technology
[0002] Mica powder, with its unique layered structure and excellent insulation properties, is a core inorganic functional filler for improving the breakdown strength and volume resistivity of UV conformal coatings. However, the strong hydrophilicity of the large number of silanol and aluminol hydroxyl groups on the surface of mica powder makes it naturally incompatible with the organic UV resin matrix. The uniform dispersion and interfacial bonding strength of the filler directly determine the insulation performance and density of the coating.
[0003] Currently, the industry generally adopts a simple physical blending process with the addition of conventional dispersants for the mixing of mica powder fillers. This process relies solely on physical disturbance to achieve temporary dispersion and mixing of mica powder in UV resins, without any chemical bonding modification treatment on the filler surface.
[0004] Existing physical dispersion processes have inherent technical defects due to the lack of interfacial bonding mechanisms, making it impossible to build a stable chemical bond structure between mica powder and organic resin. During static storage and curing, filler agglomeration, sedimentation, and stratification are prone to occur, which destroys the continuous labyrinth barrier structure of the lamellar mica in the coating, significantly weakens the insulation and reinforcement effect, and forms micro-pores and mechanical weaknesses in the coating. This fundamentally limits the upper limit of improving the insulation performance, density, and long-term protective stability of UV conformal coatings.
[0005] Therefore, the present invention provides a method for preparing chemically modified mica powder and UV conformal coating. Summary of the Invention
[0006] In order to overcome the shortcomings of the prior art, at least one technical problem raised in the background art is solved.
[0007] The technical solution adopted by the present invention to solve its technical problem is as follows: In the first aspect, the present invention provides a method for preparing chemically modified mica powder, comprising the following steps: Step 1: Pre-treat the mica powder raw material to activate the surface hydroxyl groups. Place micron-sized mica powder with a particle size range of 300 to 800 mesh in a vacuum drying environment and continue drying at a temperature of 70 to 90°C for 1 to 3 hours to completely remove the water molecules physically adsorbed on the surface of the mica powder. At the same time, the silanol and aluminol hydroxyl groups on the surface of the mica powder are fully exposed and activated to provide sufficient active sites for the subsequent coupling reaction. Step 2: Prepare a hydrolyzed solution of silane coupling agent. Mix the selected silane coupling agent with deionized water and anhydrous ethanol at a mass ratio of 5 to 10 to 10 to 20 to 70 to 85. Add glacial acetic acid dropwise to adjust the pH of the system to a weakly acidic range of 4 to 5. Continue the hydrolysis reaction at room temperature with mechanical stirring for 0.5 to 1.5 hours to fully hydrolyze the alkoxy groups in the silane coupling agent molecules to generate silanol groups, and obtain a uniform and transparent hydrolyzed solution of silane coupling agent. Step 3: Perform surface modification grafting reaction. Add the dried and activated mica powder and the silane hydrolysate prepared in Step 2 into a reaction vessel at a mass ratio of 1:2 to 5. Stir continuously at a certain speed for 1 to 3 hours under constant temperature oil bath or water bath conditions of 60 to 90°C. During this process, the silanol functional groups generated by silane hydrolysis undergo dehydration condensation reaction with the hydroxyl groups on the surface of mica powder to form strong Si-O-Si or Si-O-Al covalent chemical bonds, which firmly anchor the silane coupling agent molecules to the surface of mica powder, thereby achieving a fundamental change in its surface hydrophilic properties. Step 4: Post-process the modified product to obtain the final product. Vacuum filter the reaction mixture to achieve solid-liquid separation. The resulting filter cake is repeatedly washed with anhydrous ethanol to completely remove the physically adsorbed, unreacted silane coupling agent and its oligomers. The washed mica powder is continuously dried in an oven at 80 to 100°C for 3 to 5 hours to remove residual solvent. After drying, it is ground, pulverized, and sieved to obtain a chemically modified mica powder product with a silane coupling agent coating, excellent hydrophobicity, and dispersibility.
[0008] According to the present invention, a method for preparing chemically modified mica powder is provided. The selection of mica powder raw materials has certain technical requirements. It is preferred to use muscovite powder or sericite powder as the base raw materials. Muscovite powder has excellent electrical insulation properties and chemical stability, while sericite powder has a finer particle size and a higher aspect ratio. Both types of mica powder belong to the layered silicate mineral structure. Their lamellar morphology plays an important role in forming a maze effect in the coating. The mesh size of the mica powder is controlled in the range of 300 to 800 mesh, which is a technical parameter that has been comprehensively considered. If the mesh size is too low, the specific surface area will be insufficient, the modification and grafting efficiency will be reduced, and the lamellar structure will be too thick and difficult to be oriented and arranged in the coating. If the mesh size is too high, the specific gravity of the powder will increase, the sedimentation tendency in the resin system will be enhanced, and it will not be conducive to long-term dispersion stability.
[0009] According to the method for preparing chemically modified mica powder provided by the present invention, the selection of the type of silane coupling agent has a decisive influence on the modification effect. Preferably, one or a combination of two of γ-aminopropyltriethoxysilane or γ-methacryloxypropyltrimethoxysilane is used as the modifying agent. The amino functional group in the γ-aminopropyltriethoxysilane molecule can react chemically with the epoxy group in the epoxy acrylate resin to form a stronger interfacial bonding force. The methacryloxy functional group in the γ-methacryloxypropyltrimethoxysilane molecule can participate in the free radical polymerization reaction under UV light irradiation to form a covalent cross-linked network with the resin matrix. The amount of silane coupling agent is strictly controlled within the range of 0.5% to 2.5% of the mica powder mass. When the amount is 1% to 1.5% of the mica powder mass, the dispersion effect of the modified mica powder reaches the optimal state, and the 24-hour sedimentation volume test shows that the dispersion system is most stable at this time.
[0010] According to the preparation method of chemically modified mica powder provided by the present invention, the process parameters of the surface modification reaction stage need to be precisely controlled. The reaction temperature is set in the range of 60 to 90°C, which is the optimal temperature range for the reaction system. If the temperature is too low, the silanol condensation reaction rate will be slow, resulting in insufficient grafting efficiency; if the temperature is too high, the hydrolysis and condensation side reaction of the silane coupling agent will be accelerated, generating a large amount of homopolymer and reducing the grafting rate. The reaction time is controlled in the range of 1 to 3 hours, preferably 1.5 to 2.5 hours. Under these conditions, the turbidity index of KH-570 modified sericite is increased by more than 115%, the activation index is increased by more than 134%, the contact angle is increased by more than 190%, and the hydrophobicity and dispersibility are significantly improved. The stirring speed during the reaction process needs to be sufficient to keep the mica powder particles in a suspended state to prevent uneven reaction due to gravity sedimentation.
[0011] Secondly, the present invention provides a method for preparing a modified UV conformal coating, comprising the following steps: Step 1: Prepare the raw materials according to the preset ratio. Using the mass parts as the measurement standard, accurately weigh 40 to 70 parts of UV curable resin matrix, 15 to 35 parts of reactive diluent, 2 to 8 parts of photoinitiator, 1 to 5 parts of additives, and 5 to 30 parts of chemically modified mica powder prepared by the method in the first aspect. All solid powder components must be accurately weighed before use. Liquid components are measured by the reduction method or by measuring cylinder to ensure measurement accuracy. Step 2: Perform high-speed dispersion treatment on the mixed system. Put all the raw material components weighed in Step 1 into the dispersion tank of the high-speed disperser, set the dispersion speed to 800 to 2000 rpm, and continue dispersion for 20 to 60 minutes. Under the action of high-speed shear force, the secondary aggregated particles of modified mica powder are fully opened and uniformly dispersed in the continuous phase of the resin system to form a homogeneous and stable dispersion slurry. During the dispersion process, the system temperature is controlled not to exceed 40°C by circulating cooling water to prevent the resin system from undergoing thermal polymerization. Step 3: Perform vacuum degassing on the dispersed slurry. Transfer the homogeneous slurry to the processing chamber of the vacuum degassing equipment, start the vacuum pump to reduce the pressure inside the chamber to a vacuum state of -0.08 to -0.1 MPa, and maintain this negative pressure condition for 10 to 30 minutes. This allows the micro-bubbles inside the slurry to expand rapidly and escape under the vacuum suction, completely eliminating the bubbles introduced during the mixing and dispersion process, and obtaining a modified UV conformal coating product that is free of bubble defects and can be used directly.
[0012] The composition of the UV-curable resin matrix has been optimized, preferably using a mixture of epoxy acrylate and polyurethane acrylate as the main resin. The mass ratio of the two is set in the range of 2 to 4:1. Epoxy acrylate provides high hardness and excellent chemical corrosion resistance, while polyurethane acrylate imparts good flexibility and adhesion to the coating. The synergistic effect of the two resins can take into account multiple mechanical properties of the coating. The total amount of resin matrix is 40 to 70 parts. This amount range ensures that the coating has sufficient crosslinking density to achieve excellent protective performance, while maintaining an appropriate application viscosity for easy coating operation.
[0013] The selection of the reactive diluent needs to consider both the system viscosity and curing performance requirements. Suitable reactive diluents include one or more combinations of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, and isobornyl acrylate. Tripropylene glycol diacrylate has low volatility and good dilution effect, effectively reducing system viscosity; 1,6-hexanediol diacrylate has fast curing speed and high film hardness; isobornyl acrylate has excellent odor control and low irritation properties. The total amount of reactive diluent used is 15 to 35 parts. Too little diluent will result in high system viscosity, affecting leveling performance; too much diluent will reduce the crosslinking density of the coating, affecting hardness and resistance to media.
[0014] The selection of the photoinitiator needs to match the spectral absorption characteristics of the reactive diluent and the resin system. Suitable photoinitiators include one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide. 2-hydroxy-2-methyl-1-phenyl-1-propanone is a hydrogen-abstracting photoinitiator with good deep curing ability and yellowing control performance; 1-hydroxycyclohexylphenyl ketone is an α-cleavage photoinitiator with high initiation efficiency and good storage stability; 2,4,6-trimethylbenzoyl-diphenylphosphine oxide is a phosphorus-oxygen photoinitiator with excellent photobleaching effect and low odor. The total amount of photoinitiator used is 2 to 8 parts, which ensures sufficient free radical concentration to achieve rapid and complete curing under UV irradiation.
[0015] The amount of chemically modified mica powder added has a significant impact on the electrical insulation performance of the final coating. The amount of modified mica powder added is set to be in the range of 5 to 30 parts, preferably 15 to 25 parts. When the amount of mica powder added is 20 parts, the electrical performance of the composite insulation material reaches the optimal state. At this time, the breakdown field strength of the coating can reach 22.89 kV / mm, and the volume resistivity can reach 4.73 x 10^15 ohm meters. If the amount of mica powder added is too low, the maze effect will be insufficient, and the insulation enhancement effect will not be obvious. If the amount of mica powder added is too high, the resin matrix will not encapsulate the filler sufficiently, and conductive channels will easily form between the filler particles, which is not conducive to improving the insulation performance.
[0016] This invention utilizes the bifunctional structure of silane coupling agent molecules to construct molecular bridges for interface modification. One end of the silane coupling agent molecule is a hydrolyzable alkoxy group, which hydrolyzes in an acidic aqueous solution to generate silanol groups. These silanol groups can undergo dehydration condensation reactions with the silanol and aluminum hydroxyl groups on the surface of mica powder to form Si-O-Si or Si-O-Al covalent chemical bonds with excellent thermal stability. The other end of the silane coupling agent molecule is an organic functional group such as amino or methacryloyloxy. These organic functional groups have good thermodynamic compatibility with UV-curable resin systems and can participate in the curing and cross-linking reaction of the resin. Through this molecular bridging effect, the surface properties of the modified mica powder change from hydrophilic to hydrophobic, and the interfacial bonding force between it and the organic resin matrix is upgraded from physical adsorption to chemical bonding.
[0017] The beneficial effects of this invention are as follows: 1. The method for preparing chemically modified mica powder and UV conformal coating provided by this invention fundamentally solves the technical problem that traditional physical mixing methods cannot establish effective chemical bonds by introducing silane coupling agent molecular bridges between inorganic mica powder and organic resin matrix. One end of the silane coupling agent molecule forms Si-O-Si or Si-O-Al covalent bonds with the surface of mica powder, while the organic functional groups at the other end produce compatibility and reactivity with the resin matrix. After modification, the interfacial bonding strength between mica powder and resin is improved by orders of magnitude, and there is no longer a weak interfacial layer between the filler and the matrix. The 24-hour sedimentation volume test shows that the dispersion stability is improved by more than 134%, effectively suppressing the agglomeration and sedimentation of fillers during storage and curing.
[0018] 2. The method for preparing chemically modified mica powder and UV conformal coating provided by this invention allows the modified mica powder to be uniformly and stably dispersed in the UV conformal coating system. The lamellar mica powder can be oriented and arranged in the cured coating to form a maze effect. This physical barrier structure effectively extends the electrical breakdown path length and increases the energy threshold required for insulation failure. At the same time, the uniformly dispersed mica powder lamellars can effectively block ion migration channels and inhibit the formation and propagation of leakage current. Experimental data show that the UV conformal coating with 20 parts of modified mica powder has a breakdown field strength of 22.89 kV / mm and a volume resistivity of 4.73 x 10^15 ohmmeters, and the electrical insulation performance is significantly improved.
[0019] 3. The method for preparing chemically modified mica powder and UV conformal coating provided by the present invention provides that the silane coupling agent layer coated on the surface of the modified mica powder can effectively block the migration of metal ions in the mica powder to the resin matrix, reduce the ion migration rate and hygroscopicity of the coating, and at the same time, the chemical bonding between the organic modified layer and the resin matrix reduces the formation of interfacial micropores and defects, improves the density and uniformity of the coating structure, and these structural improvements further enhance the coating's barrier ability against corrosive media such as moisture and salt spray, and improve the overall protective performance of the conformal coating.
[0020] 4. The chemically modified mica powder and UV conformal coating preparation method provided by this invention, using a silane coupling agent modification technology route, has the advantages of simple process, convenient operation, and controllable cost. The optimal modification effect can be achieved by using only 1% to 1.5% of the mica powder mass as the coupling agent. The post-processing can be carried out using conventional washing, filtering, drying, and pulverizing equipment to achieve large-scale production. The entire technical solution has good process compatibility with existing UV conformal coating production lines, and can achieve technical upgrades without large-scale modification of production equipment and processes, thus having broad engineering application prospects. Attached Figure Description
[0021] The invention will now be further described with reference to the accompanying drawings.
[0022] Figure 1 This is a flowchart of a method for preparing chemically modified mica powder according to the present invention; Figure 2 This is a flowchart of a method for preparing a modified UV conformal coating according to the present invention. Detailed Implementation
[0023] To make the technical means, creative features, objectives and effects of this invention easier to understand, the invention will be further described below in conjunction with specific embodiments.
[0024] Example 1: Firstly, such as Figure 1 As shown, the present invention provides a method for preparing chemically modified mica powder, comprising the following steps: Step 1, mica powder pretreatment. This step aims to remove the physically adsorbed moisture on the surface of the mica powder and activate its surface hydroxyl groups, creating favorable conditions for the subsequent silane coupling agent grafting reaction. The specific operation process is as follows: Micron-sized mica powder with a particle size range of 300 to 800 mesh is selected as the basic raw material, preferably muscovite powder or sericite powder; muscovite powder belongs to layered silicate minerals, and its chemical composition is mainly potassium aluminum silicate. Its crystal structure has silicon-oxygen tetrahedral plates and aluminum-oxygen octahedral plates stacked alternately to form a typical 2:1 layered structure; sericite powder is a fine-particle variant of muscovite, with a finer particle size and a higher aspect ratio; The lamellar morphology of the two mica powders plays an important role in forming the labyrinth effect in the coating; the selected mica powder raw material is placed in the support tray of the vacuum drying oven to ensure that the powder spread thickness is uniform in order to guarantee the drying effect; Start the vacuum pump to reduce the pressure inside the drying chamber to a vacuum state of 10 to 100 Pa, and then start the heating system to raise the temperature inside the chamber to the target value of 70 to 90°C; continue drying under this temperature and vacuum conditions for 1 to 3 hours to allow the water molecules physically adsorbed on the surface of the mica powder to fully desorb and escape. After drying, the powder is naturally cooled to below 40°C under vacuum before being removed to prevent the high-temperature powder from absorbing moisture from the air. The core purpose of the drying process is to completely remove the free water molecules adsorbed on the surface of the mica powder, so that the active sites of silanol groups (Si-OH) and aluminum hydroxyl groups (Al-OH) on the surface of the powder can be fully exposed and activated. These hydroxyl groups are the active anchoring sites for the subsequent chemical grafting reaction of silane coupling agents, and their number and activity directly affect the modification grafting efficiency.
[0025] Step 2, preparation of silane coupling agent hydrolysate. This step aims to hydrolyze the alkoxy group in the silane coupling agent molecule into reactive silanol groups to prepare a uniform and stable silane hydrolysate solution. The specific operating procedure is as follows: First, prepare an ethanol-water mixed solvent system by adding anhydrous ethanol and deionized water to a glass reaction vessel at a mass ratio of 70 to 85:10 to 20. Anhydrous ethanol serves as the reaction medium and dispersant, while deionized water provides the water source required for silane hydrolysis. Turn on the mechanical stirrer and stir at a speed of 300 to 500 revolutions per minute to ensure the solvent is mixed evenly. Then, according to the mass ratio of silane coupling agent to solvent system of 5 to 10 to 80 to 100, accurately weigh the selected silane coupling agent and slowly add it dropwise to the ethanol-water mixture; The silane coupling agent is selected from γ-aminopropyltriethoxysilane (code KH-550, molecular formula: H2NCH2CH2CH2Si(OC2H5)3) or γ-methacryloyloxypropyltrimethoxysilane (code KH-570, molecular formula CH2=C(CH3)COOCH2CH2CH2Si(OCH3)3) or a combination of two of them; The amino functional group (-NH2) in γ-aminopropyltriethoxysilane can undergo a ring-opening reaction with the epoxy groups in epoxy acrylate resin, forming a stronger chemical interfacial bond. The methacryloyloxy functional group (C=C double bond) in γ-methacryloyloxypropyltrimethoxysilane can participate in free radical polymerization under UV light irradiation, forming a covalently cross-linked network structure with the resin matrix. The actual amount of silane coupling agent is calculated based on the mass of the mica powder to be treated, and is 0.5% to 2.5% of the mica powder mass, preferably 1.0% to 1.5%. Experiments have shown that when the concentration of the silane coupling agent is 1% to 1.5% of the mica powder mass, the dispersion effect of the modified mica powder reaches the optimal state. The 24-hour sedimentation volume test shows that the dispersion system is most stable at this time. After adding the silane coupling agent, continue stirring for 5 to 10 minutes to ensure that the system is mixed evenly. Then, glacial acetic acid was added dropwise using a dropper, while the pH value of the system was monitored in real time with a pH meter. The pH value of the system was precisely adjusted to a weakly acidic range of 4 to 5. An acidic environment is a necessary condition for the hydrolysis reaction of alkoxy groups in silane coupling agents. Under this pH condition, the alkoxy groups (-OCH3 or -OC2H5) in silane molecules can undergo hydrolysis reaction with water to generate silanol groups (Si-OH). After adjustment, continue stirring at 300 to 500 revolutions per minute for 0.5 to 1.5 hours at room temperature (20 to 25°C) to allow the hydrolysis reaction to proceed fully. After the reaction is complete, a uniform, transparent or slightly opalescent hydrolysate of the silane coupling agent is obtained, which contains a large number of silanol functional groups (Si-OH) and a small amount of unhydrolyzed alkoxy groups. The hydrolysate should be prepared and used immediately, and the storage time should not exceed 24 hours to prevent the self-condensation reaction between silanols to form siloxane oligomers.
[0026] Step 3, surface modification grafting reaction. This step is the core of the entire modification process. It aims to anchor the silane coupling agent molecules to the mica powder surface through covalent bonds, thereby fundamentally changing its surface properties. The specific operation process is as follows: The mica powder dried and activated in step one and the silane hydrolysate prepared in step two are added to a glass reactor or stainless steel reaction vessel at a mass ratio of 1:2 to 5. The mass ratio of mica powder to hydrolysate determines the concentration and grafting density of silane molecules in the reaction system: if the ratio is too low, the grafting amount will be insufficient and the modification effect will be insignificant; if the ratio is too high, the silane concentration in the hydrolysate will be too low and will not be able to effectively cover the surface of the mica powder. Place the reaction vessel in a constant temperature water bath, add sufficient heat transfer medium (deionized water or glycerol-water mixture) to the water bath, start the circulating water pump and heating system, and precisely control the water bath temperature within the target range of 60 to 90°C, preferably 60 to 80°C, with a temperature control accuracy within ±2°C to ensure the stability and repeatability of the reaction conditions; once the water bath temperature reaches the set value and stabilizes, start the mechanical stirring system and continuously stir the reaction at a speed of 400 to 800 rpm for 1 to 3 hours, preferably 1.5 to 2.5 hours. During constant-temperature stirring, the silanol functional groups (Si-OH) in the silane hydrolysate undergo a dehydration condensation reaction with the exposed silanol (Si-OH) and aluminum hydroxyl (Al-OH) groups on the mica powder surface, forming stable Si-O-Si or Si-O-Al covalent chemical bonds. The chemical essence of this condensation reaction is a nucleophilic addition-elimination reaction between silanol and hydroxyl groups: under acidic catalytic conditions, the silicon atoms in the silanol are protonated and activated, and then undergo nucleophilic attack with the hydroxyl groups on the mica surface, removing one molecule of water to form a siloxane bond (Si-O-Si). Meanwhile, the organic functional group (amino or methacryloyloxy) at the other end of the silane coupling agent molecule extends outward, forming an organic coating layer on the surface of the mica powder, transforming the originally hydrophilic inorganic surface into a hydrophobic organic-inorganic hybrid surface. The stirring speed during the reaction process needs to be sufficient to maintain the mica powder particles in a suspended and dispersed state to prevent uneven reaction due to gravitational settling. After the reaction was completed, the heating system and stirrer were turned off, and the mixture was allowed to cool naturally to room temperature. Experimental data showed that under the above optimal conditions, the turbidity index of the modified product could be increased by more than 115%, the activation index by more than 134%, the contact angle by more than 190%, and the hydrophobicity and dispersibility were significantly improved.
[0027] Step four, post-processing: This step aims to separate, wash, and dry the modified product to obtain a pure chemically modified mica powder product. The specific operation process is as follows: After the reaction is complete, the mixture in the reactor is transferred to a Buchner funnel or a vacuum filtration device. A quantitative filter paper with a diameter matching the funnel is placed inside the Buchner funnel, and a vacuum pump is used to provide negative pressure suction for filtration. Under negative pressure, the liquid phase component in the mixture is drawn away through the filter paper, while the solid product (modified mica powder) is retained on the filter paper to form a filter cake. After filtration, the filter cake is peeled off the filter paper and redispersed in sufficient anhydrous ethanol. Thorough stirring and washing are performed using a glass rod or magnetic stirrer, and this washing process needs to be repeated 2 to 3 times. The purpose of washing is to utilize the good solubility of anhydrous ethanol in physically adsorbed, unreacted silane coupling agents and their oligomers to completely remove these impurities from the filter cake. Water should be avoided as a washing solution during the washing process to prevent hydrolysis or condensation side reactions of residual silanol groups. After the final washing, the filter cake is vacuum filtered again to remove most of the ethanol. The washed modified mica powder is then transferred... Transfer the mica powder to a glass petri dish or stainless steel tray and spread it into a uniform thin layer. Place the petri dish in a forced-air drying oven or vacuum drying oven and dry it continuously at a temperature of 80 to 100°C for 3 to 5 hours to remove residual ethanol solvent and trace amounts of moisture. After drying, allow the product to cool naturally to room temperature in the drying oven. The cooled modified mica powder is in a loose powder state. Grind it using a mortar and pestle or a small pulverizer to break up any possible soft agglomerates. After grinding, sieve it through a standard sieve of 80 to 200 mesh to obtain a chemically modified mica powder product with uniform particle size. The surface of this product is coated with a silane coupling agent molecular layer, which has excellent hydrophobicity and dispersion stability and can be directly used in the subsequent preparation of UV conformal coatings.
[0028] Secondly, such as Figure 2 As shown, the present invention provides a method for preparing a modified UV conformal coating, comprising the following steps: Step 1, Ingredient Preparation: This step aims to accurately weigh all raw material components according to the preset mass ratio; the specific operation process is as follows: Using parts by mass as the measurement standard, prepare the following raw material components: 40 to 70 parts of UV-curable resin matrix, 15 to 35 parts of reactive diluent, 2 to 8 parts of photoinitiator, 1 to 5 parts of additives, and 5 to 30 parts (preferably 15 to 25 parts) of chemically modified mica powder prepared by the method of the first aspect. The UV-curable resin matrix preferably uses a mixture of epoxy acrylate and polyurethane acrylate as the main resin, with the mass ratio of the two set in the range of 2 to 4:1. Epoxy acrylate is an important type of UV-curable resin, which is obtained by the ring-opening esterification reaction of epoxy resin and acrylic acid. The molecule contains both epoxy groups and acrylate double bonds, combining the excellent adhesion of epoxy resin and the rapid curing characteristics of acrylate, which can provide the coating with high hardness and excellent chemical corrosion resistance. Polyurethane acrylate is a prepolymer containing double bonds obtained by reacting polyisocyanate and hydroxyl acrylate. The molecule contains urethane bond (-NHCOO-) structure, which gives the coating good flexibility, adhesion and impact resistance. The synergistic effect of the two resins can balance the hardness and flexibility of the coating and meet the multiple mechanical index requirements for the protection of printed circuit board surfaces. The reactive diluent can be selected from one or more combinations of tripropylene glycol diacrylate (TPGDA), 1,6-hexanediol diacrylate (HDDA), and isobornyl acrylate (IBOA). Tripropylene glycol diacrylate has low volatility and good dilution effect, and the long-chain ether bond structure in the molecule gives it excellent flexibility and low skin irritation. 1,6-hexanediol diacrylate is a bifunctional monomer with fast curing speed, high film hardness, and excellent scratch resistance. Isobornyl acrylate is an alicyclic monofunctional diluent with excellent odor control and low irritation properties, and the cured product has excellent gloss retention. The photoinitiator can be selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone (code-named photoinitiator 1173), 1-hydroxycyclohexylphenyl ketone (code-named photoinitiator 184), or 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (code-named TPO); 2-hydroxy-2-methyl-1-phenyl-1-propanone is a hydrogen-abstracting photoinitiator, which generates free radicals under UV light and can also abstract hydrogen donors in the system to form active centers, exhibiting good deep curing ability and yellowing control performance; 1-hydroxycyclohexylphenyl ketone is an α-cleavage type photoinitiator, with high initiation efficiency and good storage stability, and is one of the most widely used general-purpose photoinitiators; 2,4,6-trimethylbenzoyl-diphenylphosphine oxide is a phosphorus-oxygen photoinitiator, with excellent photobleaching effect and low odor characteristics, and is particularly suitable for applications with high requirements for yellowing control. Additives include leveling agents (such as modified polyether siloxane BYK-333), defoamers (such as modified polysiloxane or modified polyether defoamers), and adhesion promoters (such as γ-glycidyl etheroxypropyltrimethoxysilane). Leveling agents can reduce the surface tension difference of the system, promote the leveling and spreading of the coating, and reduce surface defects such as brush marks and orange peel. Defoamers can inhibit or eliminate bubbles generated during mixing and dispersion, preventing pinhole defects from forming after the coating is cured. Adhesion promoters can enhance the adhesion strength between the coating and the printed circuit board metal pads and substrate. All solid powder components (modified mica powder, photoinitiator, etc.) must be accurately weighed using an electronic analytical balance with an accuracy of 0.01 g before use. Liquid components should be measured using the subtraction method (differential subtraction method) or a graduated cylinder to ensure measurement accuracy. Studies have shown that when the amount of modified mica powder added is 20 parts, the electrical performance of the composite insulation material reaches its optimal state. At this time, the breakdown field strength of the coating can reach 22.89 kV / mm and the volume resistivity can reach 4.73 × 10^15 Ω·m.
[0029] Step two, high-speed dispersion: This step aims to fully disperse and depolymerize the modified mica powder in the resin system to form a homogeneous and stable dispersion slurry. The specific operation process is as follows: Add all the raw material components weighed in step one into the special dispersion tank of the high-speed disperser in the following order: liquids first, then solids. First, add all the UV-curable resin matrix and reactive diluent, and turn on the stirrer to ensure that the liquid components are fully mixed and homogeneous. Slowly add the photoinitiator and additives while stirring continuously, and continue stirring to ensure that all liquid components are completely miscible. Slowly and evenly sprinkle the chemically modified mica powder into the dispersion tank while stirring at high speed, avoiding large-scale addition that could cause powder clumping. After confirming that all materials have been added to the dispersion tank, tighten the tank lid and check the sealing performance. Set the drive motor speed of the disperser to 800 to 2000 rpm, and optimize and adjust the specific speed according to the size of the dispersion tank and the viscosity of the material. For dispersion discs with a diameter of 100 to 150 mm, a speed of 800 to 1200 rpm is suitable for low viscosity systems, while a speed of 1500 to 2000 rpm is suitable for medium to high viscosity systems; start the disperser and continue dispersing for 20 to 60 minutes at the set speed. During high-speed dispersion, the shear force and turbulence generated by the high-speed rotation of the dispersion disk can effectively break up the secondary aggregated particles of modified mica powder (formed by the aggregation of the original primary particles through van der Waals forces), so that each primary particle is fully wetted and coated by the resin system. The determination of dispersion time needs to take into account both dispersion efficiency and energy consumption: if the time is too short, the dispersion will be insufficient and some powder particles will still be agglomerated; if the time is too long, energy consumption will increase and the temperature of the resin system may rise. During the dispersion process, the system temperature is controlled to not exceed 40°C by circulating cooling water in the jacket of the dispersion tank, in order to prevent the resin system from undergoing thermal polymerization or abnormally increasing viscosity due to high temperature. When dispersion is complete, turn off the disperser, open the tank lid, and use a glass rod to dip a small amount of slurry to observe its state: the homogeneously dispersed slurry should have a uniform appearance, no obvious particle feel, and no air bubbles adhering to it.
[0030] Step 3, vacuum degassing. This step aims to completely eliminate air bubbles introduced during the dispersion process, obtaining a ready-to-use modified UV conformal coating product free of air bubble defects. The specific operation process is as follows: Transfer the homogeneous slurry obtained in step two to the processing chamber of the vacuum degassing equipment. Use a scraper or pouring method to transfer the slurry from the dispersion tank to the round tray or square trough of the vacuum degassing machine. Control the spreading thickness within the range of 5 to 15 mm to ensure that the bubbles can escape smoothly. Close the equipment door and lock it. Start the vacuum pump to begin vacuuming. When the pressure inside the cavity drops to a vacuum state of -0.08 to -0.1 MPa (i.e., an absolute pressure of 0.02 to 0.03 MPa), the microbubbles that were originally dissolved and encapsulated inside the slurry rapidly expand and migrate upwards under the negative pressure. The escape process of the bubbles under vacuum conditions follows the ideal gas law: P1V1=P2V2, where P1 is atmospheric pressure, V1 is the original volume of the bubble, P2 is vacuum pressure, and V2 is the volume after expansion; Since P2 is much smaller than P1, the bubble volume expands hundreds of times and rapidly rises to the surface and bursts and disappears, provided the slurry viscosity allows. Maintain this vacuum level for 10 to 30 minutes to ensure that the microbubbles inside the slurry have sufficient time to escape. After degassing, slowly release the vacuum (to prevent slurry splashing due to sudden pressure relief), open the equipment door, and remove the tray. The slurry in the tray has become a completely bubble-free transparent or translucent liquid with a smooth and clean surface. After degassing, the modified UV conformal coating is transferred to a light-shielded storage container, sealed, and stored in a cool, dry place, avoiding direct sunlight and high temperatures. The entire preparation process is now complete, and the resulting product can be directly used for surface coating protection of printed circuit boards.
[0031] For example, take 500 grams of mica powder raw material with a mesh size of 500, place it in a vacuum drying oven and dry it at 80°C for 2 hours to complete step one pretreatment; take 6.25 grams of γ-methacryloyloxypropyltrimethoxysilane (KH-570) (1.25% of the mass of mica powder), mix it with 125 grams of deionized water and 375 grams of anhydrous ethanol, add glacial acetic acid to adjust the pH to 4.5, stir and hydrolyze at room temperature for 1 hour to complete step two preparation; Take 200g of dried muscovite powder and 800g of silane hydrolysate and add them to the reactor. Stir the reaction at 600 rpm for 2 hours under a 70℃ water bath to complete the grafting reaction in step three. The reaction solution is filtered, washed three times with anhydrous ethanol, dried at 80℃ for 4 hours, ground and sieved to obtain the chemically modified muscovite powder product. Take 40 parts of epoxy acrylate, 20 parts of polyurethane acrylate, 20 parts of TPGDA diluent, 11735 parts of photoinitiator, 0.5 parts of BYK-333 leveling agent, 0.5 parts of defoamer, and 20 parts of modified mica powder and add them to a disperser. Disperse at 1500 rpm for 30 minutes to complete step two dispersion. The slurry was transferred to a vacuum degassing machine and degassed at -0.09 MPa for 20 minutes to obtain the modified UV conformal coating product. The performance of the finished product was tested, and the results are as follows: the breakdown field strength of the coating reached 22.89kV / mm, the volume resistivity reached 4.73×10^15Ω·m, the hardness reached 2H, the adhesion grade was 0, and the salt spray resistance was excellent.
[0032] Example 2: In the chemically modified mica powder preparation method of the first aspect, when γ-aminopropyltriethoxysilane (KH-550) is used as a silane coupling agent, its modification mechanism is different from that of KH-570. The amino functional group (-NH2) in the KH-550 molecule will be protonated under acidic conditions to form -NH3+, but the protonated amino group still has a certain reactivity and can undergo ring-opening addition reaction with the epoxy group in the epoxy acrylate resin under heating or catalytic conditions to form a secondary or tertiary amine structure, thereby establishing a chemical bond between the mica powder and the resin matrix. When using KH-550 for modification, the reaction temperature in step three can be appropriately increased to 75 to 85°C to promote the reaction between amino and epoxy groups. KH-550-modified mica powder has a better interfacial bonding effect when used in combination with epoxy UV resins.
[0033] In the chemically modified mica powder preparation method of the first aspect, when the mica powder mesh size is set to the lower limit of 300 mesh, its specific surface area is relatively small, the modification and grafting efficiency is slightly reduced, but the powder specific gravity is moderate, the sedimentation tendency in the resin system is weak, and the storage stability is good. When the mica powder mesh size is set to the upper limit of 800 mesh, its specific surface area increases, the modification and grafting efficiency is improved, the lamellar structure is thinner and it is easier to oriented and arrange in the coating to form a maze effect, but the increase in powder specific gravity leads to an enhanced sedimentation tendency in the resin system, and it is necessary to use dispersants or thickeners to improve storage stability. Therefore, in practical applications, the appropriate mica powder mesh size needs to be selected based on the specific usage scenario and performance requirements.
[0034] In the second aspect of the modified UV conformal coating preparation method, when TPO is selected as the photoinitiator, since the spectral absorption range of TPO is concentrated in the 360 to 420 nanometer region, and the main absorption peak is located near 405 nanometers, it is necessary to use a high-pressure mercury lamp or LED curing light source with wavelengths of 365 nanometers, 385 nanometers or 405 nanometers for curing. TPO has high photoinitiation efficiency, and the dosage can be controlled between 2 and 4 parts. When used in combination with photoinitiator 1173 or 184, the ratio of the two can be set in the range of 1:1 to 2:1, which can achieve a more uniform curing depth and better yellowing control.
[0035] In the second aspect of the modified UV conformal coating preparation method, when isobornyl acrylate (IBOA) is selected as the main diluent, since IBOA is a monofunctional monomer, its dilution effect is lower than that of difunctional TPGDA or HDDA. Therefore, the amount of IBOA needs to be appropriately increased to 25 to 35 parts, and at the same time, 5 to 10 parts of difunctional diluent are used to ensure the crosslinking density and hardness of the coating. The use of IBOA can significantly reduce the odor and skin irritation of coatings, making it particularly suitable for consumer electronics products with high environmental performance requirements.
[0036] Comparative Example 1: Comparative Example 1 used unmodified muscovite powder as a filler, which was directly physically mixed with the UV-curable resin system. The specific operation was as follows: Take 20 parts of 500-mesh muscovite powder raw powder and add it directly to a resin system consisting of 40 parts epoxy acrylate, 20 parts polyurethane acrylate, 20 parts TPGDA diluent, 11735 parts photoinitiator, and 1 part additive without any chemical modification. Disperse the powder at 1500 rpm for 30 minutes and then perform vacuum degassing. Due to the large number of hydrophilic hydroxyl groups on the surface of the muscovite powder, there is a huge difference in interfacial energy between it and the hydrophobic resin system. The powder quickly agglomerates and settles in the resin, resulting in extremely poor dispersion uniformity. After dispersion, obvious stratification can be observed after standing for 10 minutes, with a large number of agglomerated mica powder particles settling at the bottom.
[0037] Comparative Example 2 Traditional stearic acid was used as a surface modifier to physically coat muscovite powder. The specific operation was as follows: 500 grams of 500-mesh muscovite powder was taken, 10 grams of stearic acid and 500 ml of anhydrous ethanol were added, and the mixture was ultrasonically dispersed for 30 minutes. Then, it was heated and refluxed for 2 hours. After that, it was filtered, washed and dried to obtain stearic acid coated muscovite powder. Twenty parts of the coated mica powder were added to the UV resin system and dispersed to prepare a three-proof paint sample. Stearic acid was physically adsorbed onto the surface of the mica powder and only van der Waals forces existed between it and the resin matrix, resulting in a weak interfacial bonding strength. During high-speed dispersion and curing, the stearic acid coating layer is prone to detachment or migration, causing the filler to re-agglomerate.
[0038] Table 1: Comparison of Embodiments of the Invention with Comparative Examples It is evident that the filler surface treatment technology of the present invention, which uses silane coupling agent (KH-570 / KH-550) to modify mica powder, is significantly superior to the comparative schemes of unmodified mica powder and stearic acid-coated mica powder in terms of various indicators such as dispersion stability, activation index, contact angle, turbidity improvement rate, breakdown field strength, volume resistivity and coating uniformity.
[0039] The 24-hour sedimentation volume of KH-570 modified mica powder (Example 1) was only 2.5 mL (12.8 mL in Comparative Example 1 and 7.5 mL in Comparative Example 2), the activation index reached 94.5% (only 35.6% in Comparative Example 1 and 62.3% in Comparative Example 2), the contact angle reached 128° (42° in Comparative Example 1 and 78° in Comparative Example 2), the turbidity improvement rate reached 115% (no effective improvement in the comparative examples), and the breakdown field strength reached 22.89 kV / mm (14.52 in Comparative Example 1 and 17 in Comparative Example 2). The volume resistivity of the coating was 4.73 × 10^15 Ω·m (comparative example 1 was 1.85, and comparative example 2 was 2.94), and the coating uniformity was excellent (comparative example 1 showed obvious agglomeration, and comparative example 2 showed moderate to small agglomeration). KH-550 modified mica powder also performed well, with a settling volume of 3.1 mL, an activation index of 91.2%, a contact angle of 115°, a turbidity improvement rate of 98%, a breakdown field strength of 21.35 kV / mm, and a volume resistivity of 4.21 × 10^15 Ω·m, and the coating uniformity was excellent. Both silane modification schemes were significantly better than the two comparative schemes. Among them, the KH-570 modification was superior in dispersibility and electrical insulation performance, while the KH-550 modification also significantly improved the overall performance.
[0040] Chemical grafting modification with silane coupling agents effectively enhances the interfacial bonding between mica powder and the matrix, improves dispersibility and insulation performance, and achieves a synergistic gain of highly uniform dispersion of fillers in the coating and excellent electrical properties, so that the overall performance of the insulating coating reaches the optimal level.
[0041] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing chemically modified mica powder, characterized in that, Includes the following steps: Step 1: Pre-treat mica powder raw material to activate surface hydroxyl groups: Place mica powder raw material in a vacuum drying environment to remove water molecules physically adsorbed on the surface, so that the silanol and aluminol hydroxyl groups on the surface of the mica powder are fully exposed and activated. Step 2: Preparation of silane coupling agent hydrolysis solution: Mix silane coupling agent with deionized water and anhydrous ethanol, add glacial acetic acid to adjust pH, and continue the hydrolysis reaction at room temperature; Step 3: Perform surface modification grafting reaction: Add the dried and activated mica powder and the silane hydrolysate to the reaction vessel at a mass ratio of 1:2 to 5, and stir until the silanol functional groups and the hydroxyl groups on the surface of the mica powder undergo dehydration condensation to form Si-O-Si or Si-O-Al covalent chemical bonds. Step 4: Post-processing of the modified product: The mixture after the reaction is completed is vacuum filtered to achieve solid-liquid separation. The resulting filter cake is repeatedly washed with anhydrous ethanol to remove the physically adsorbed, unreacted silane coupling agent and its oligomers. The washed mica powder is continuously dried in an oven. After drying, it is ground, pulverized and sieved to obtain a chemically modified mica powder product with a silane coupling agent coating on the surface.
2. The method for preparing chemically modified mica powder according to claim 1, characterized in that: The mica powder raw material is either muscovite powder or sericite powder; the mesh size of the mica powder ranges from 300 to 800 mesh.
3. The method for preparing chemically modified mica powder according to claim 1, characterized in that: The silane coupling agent is one or a combination of two of γ-aminopropyltriethoxysilane or γ-methacryloyloxypropyltrimethoxysilane; the amount of the silane coupling agent is 0.5% to 2.5% of the mica powder mass.
4. The method for preparing chemically modified mica powder according to claim 1, characterized in that: In the surface modification grafting reaction, the stirring time is 1.5 to 2.5 hours; The stirring speed must be sufficient to keep the mica powder particles in a suspended and dispersed state; The washing process is repeated 2 to 3 times.
5. A method for preparing a modified UV conformal coating, characterized in that, Includes the following steps: Using mass fractions as the measurement standard, UV-curable resin matrix, reactive diluent, photoinitiator, additives, and chemically modified mica powder prepared by any one of claims 1-4 are weighed according to a preset ratio as functional fillers. All raw material components are put into the dispersion tank of a high-speed disperser for continuous dispersion. Under the action of high-speed shear force, the secondary aggregated particles of modified mica powder are fully opened and uniformly dispersed in the continuous phase of the resin system to form a homogeneous and stable dispersion slurry. The homogenized slurry is transferred to the processing chamber of the vacuum degassing equipment. The vacuum pump is started to reduce the pressure inside the chamber, causing the microbubbles inside the slurry to expand and escape under the vacuum suction.
6. The method for preparing a modified UV conformal coating according to claim 5, characterized in that: The amount of chemically modified mica powder added is 5 to 30 parts; The UV-curable resin matrix uses a mixture of epoxy acrylate and polyurethane acrylate as the main resin, with a mass ratio of 2 to 4:1 between the two resins.
7. The method for preparing a modified UV conformal coating according to claim 5, characterized in that: The active diluent is one or a combination of tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, and isobornyl acrylate. The total amount of the active diluent used is 15 to 35 parts.
8. The method for preparing a modified UV conformal coating according to claim 5, characterized in that: The photoinitiator is one or a combination of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide; The total amount of the photoinitiator is 2 to 8 parts.
9. The method for preparing a modified UV conformal coating according to claim 5, characterized in that: The amount of chemically modified mica powder added is 15 to 25 parts.