A high reflectivity, high emissivity radiative cooling composite coating and a preparation method thereof

By combining barium sulfate and hexagonal boron nitride with a resin system, a multi-scale inorganic particle dispersion structure is formed, which solves the problems of increased coating viscosity and construction performance, and realizes a radiation cooling coating with high reflectivity and high emissivity, achieving a significant cooling effect.

CN123131884APending Publication Date: 2026-11-20UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611471372.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

When the content of inorganic fillers is increased, existing radiation cooling coatings tend to increase the viscosity of the system, which increases the risk of agglomeration and sedimentation, and it is difficult to simultaneously meet the requirements of high reflectivity, high emissivity and construction performance.

Method used

Barium sulfate and hexagonal boron nitride are used as functional fillers. Together with hydroxyl acrylic anticorrosive paint and aliphatic polyurethane curing agent, they form a two-component film-forming system. Through a specific feeding sequence and dispersion method, a multi-scale inorganic particle dispersion structure is formed, which enhances the ability to reflect sunlight and emit mid-infrared radiation. It is suitable for spraying, brushing or scraping.

Benefits of technology

A radiation cooling coating with high reflectivity and high emissivity is achieved, which can effectively reduce the surface temperature of metal substrates, providing an average temperature difference of 5.6℃ and a maximum instantaneous temperature difference of 9.3℃ for cooling effect, while meeting construction requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131884A_ABST
    Figure CN123131884A_ABST
Patent Text Reader

Abstract

This invention discloses a high-reflectivity, high-emissivity radiative cooling composite coating and its preparation method, belonging to the fields of functional coatings and passive radiative cooling technology. The invention uses a total mass of 100 parts of hydroxyl acrylic anti-corrosion paint (component A), aliphatic polyurethane curing agent (component B), barium sulfate, and hexagonal boron nitride, with each component comprising 32 parts, 8 parts, 50 parts, and 10 parts respectively, plus 20 parts of rosin. In preparation, the two fillers are first dispersed in component A and a portion of the rosin, then the remaining rosin is added to adjust the viscosity. Finally, component B is added and degassed. The resulting coating is sprayed, brushed, or scraped onto the surface of a metal substrate and cured at room temperature. The resulting coating has a solar-weighted reflectance of 91.2% in the 250–2500 nm wavelength band and an average emissivity of 96.07% in the 2.5–20 μm wavelength band, making it suitable for passive cooling of outdoor metal components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional coatings and passive radiation cooling technology, specifically relating to a radiation cooling composite coating with high reflectivity and high emissivity and its preparation method. Background Technology

[0002] Outdoor metal sheets, equipment housings, roofs, storage tanks, and pipes are exposed to solar radiation for extended periods. Increased surface temperatures raise the heat load on these devices and can accelerate the aging of coatings and substrates. Passive radiative cooling materials, by reducing the absorption of solar radiation while utilizing mid-infrared radiation near atmospheric windows to dissipate heat, can suppress surface temperature rise without consuming additional electrical energy.

[0003] The spectral and application properties of radiation-cooled coatings are influenced by the resin system, filler type, filler particle size, filler content, and dispersion process. Increasing the inorganic filler content generally enhances light scattering, but it also increases the system viscosity and the risk of agglomeration, sedimentation, and film defects. Therefore, a composite system with a well-defined composition, simple preparation steps, and the ability to form a continuous coating on metal surfaces by spraying, brushing, or scraping is needed to balance solar reflection, mid-infrared emission, and practical application performance. Summary of the Invention

[0004] This invention aims to provide a high-reflectivity, high-emissivity radiation-cooling composite coating and its preparation method. The coating utilizes barium sulfate and hexagonal boron nitride as functional fillers, and is combined with a two-component film-forming system consisting of component A of a hydroxyl acrylic anti-corrosion paint and component B of an aliphatic polyurethane curing agent. This results in a coating with high solar reflectivity and mid-infrared emissivity, while meeting the requirements for spraying, brushing, or scraping application on metal substrates, making it particularly suitable for passive cooling of outdoor metal substrates.

[0005] The present invention relates to a radiation-cooling composite coating with high reflectivity and high emissivity, the raw material components of which include hydroxyl acrylic anti-corrosion paint component A, aliphatic polyurethane curing agent component B, barium sulfate, hexagonal boron nitride and rosin diluent.

[0006] Based on a total mass of 100 parts by weight for hydroxyl acrylic anticorrosive paint component A, aliphatic polyurethane curing agent component B, barium sulfate, and hexagonal boron nitride, the amounts of each component added are as follows: 32 parts by weight for hydroxyl acrylic anticorrosive paint component A, 8 parts by weight for aliphatic polyurethane curing agent component B, 50 parts by weight for barium sulfate, and 10 parts by weight for hexagonal boron nitride. An additional 20 parts by weight of rosin thinner are added; this component is not included in the above 100 parts by weight.

[0007] The hydroxyl acrylic anticorrosive paint component A and the aliphatic polyurethane curing agent component B are a directly purchased matching two-component system, with a mass ratio of 4:1 between the two commercial raw materials.

[0008] The median particle size D50 of barium sulfate is 9–11 μm, and the particle size distribution D97 ≤ 12 μm; the median particle size D50 of hexagonal boron nitride is 1 μm.

[0009] The method for preparing the high reflectivity and high emissivity radiation-cooling composite coating of the present invention includes the following steps:

[0010] Barium sulfate and hexagonal boron nitride are dispersed in component A of hydroxyl acrylic anticorrosive paint and part of rosin thinner; the remaining rosin thinner is added to adjust the application viscosity; after adding component B of aliphatic polyurethane curing agent, the mixture is mixed and degassed; the resulting coating is sprayed or scraped onto the surface of the treated metal substrate and cured at room temperature to form a composite coating with a thickness of 150~250 μm.

[0011] The metal substrate is a steel plate, galvanized steel plate, tin-plated steel plate, stainless steel plate, aluminum plate, or aluminum alloy plate.

[0012] The thickness of the composite coating is preferably 200 μm.

[0013] The curing time is ≥8h.

[0014] further:

[0015] The total amount of the rosin diluent added is 20 parts by mass, of which 12 parts by mass are added during the dispersion of barium sulfate and hexagonal boron nitride, and the remaining 8 parts by mass are added before the addition of component B of the aliphatic polyurethane curing agent.

[0016] After adding component B of the aliphatic polyurethane curing agent, multi-stage mixing and degassing were performed using a vacuum homogenizer.

[0017] The beneficial effects of this invention are reflected in:

[0018] The barium sulfate and hexagonal boron nitride used in this invention have different particle size scales. The two fillers are dispersed together in the resin matrix to form a multi-scale inorganic particle dispersion structure, which is beneficial for enhancing the coating's reflection of solar radiation and maintaining a high mid-infrared radiation emission capability.

[0019] This invention first disperses the filler in component A of the hydroxyl acrylic anticorrosive paint and a portion of the rosin, then adjusts the application viscosity with the remaining rosin, and finally adds component B of the aliphatic polyurethane curing agent. This order of addition avoids premature mixing of polyurethane curing agent B, which is beneficial for filler wetting, paint defoaming, and subsequent coating.

[0020] Under the formulation and testing conditions described in the examples, the resulting coating exhibited a solar-weighted reflectance of 91.2% in the 250–2500 nm wavelength range and an average emissivity of 96.07% in the 2.5–20 μm wavelength range. Outdoor temperature profiles showed that the temperature of the coated sample was lower than the ambient air temperature during the testing period, with an average temperature difference of 5.6 °C and a maximum instantaneous sub-ambient temperature difference of approximately 9.3 °C. Attached Figure Description

[0021] Figure 1 This is a flowchart illustrating the preparation process of the radiation-cooling composite coating of the present invention.

[0022] Figure 2 The reflectance spectrum of the composite coating obtained in Example 1 in the 250–2500 nm wavelength range is shown.

[0023] Figure 3 The image shows the emissivity spectrum of the composite coating obtained in Example 1 in the 2.5–20 μm band.

[0024] Figure 4 This is a schematic diagram of an outdoor cooling test device.

[0025] Figure 5 This is a schematic diagram of the enclosure and thermocouple arrangement for outdoor cooling tests.

[0026] Figure 6 This is a graph showing the temperature of the coated sample versus the ambient air temperature over time during outdoor testing. Detailed Implementation

[0027] The present invention will be further described below with reference to the accompanying drawings and embodiments. These embodiments are used to illustrate the technical solutions of the present invention and do not constitute a limitation on the scope of protection of the present invention.

[0028] Raw material and parameter definitions

[0029] The hydroxy acrylic anticorrosive paint component A and the aliphatic polyurethane curing agent component B used in this embodiment were purchased from Shanghai Lishu Trading Co., Ltd. These are commercially available raw materials for industrial steel structure anticorrosive coatings. Component A uses hydroxy acrylic resin as a base and contains weather-resistant pigments, additives, and solvents; component B is an aliphatic polyurethane curing agent. The two are used in a 4:1 mass ratio with the commercial raw materials. Rosin is an organic solvent-based diluent for coatings, used for wetting and dispersing fillers and adjusting application viscosity. It volatilizes during film formation and is not used as a main crosslinking component.

[0030] D50 represents the particle size corresponding to a cumulative volume fraction of 50%; D97 represents the particle size corresponding to a cumulative volume fraction of 97%. Barium sulfate is an industrial-grade 1250-mesh powder with a D50 of 9–11 μm and a D97 ≤ 12 μm; hexagonal boron nitride has a D50 of 1 μm, a purity of 99.9%, and a density of 2.25 g / cm³. 3 .

[0031] Example 1: Preparation of Radiation-Coated Cooling Composite Coating

[0032]

[0033] Weigh out 32 parts by weight of component A of the hydroxyl acrylic anticorrosive paint, 8 parts by weight of component B of the aliphatic polyurethane curing agent, 50 parts by weight of barium sulfate, and 10 parts by weight of hexagonal boron nitride, and prepare 20 parts by weight of rosin flux. The substrate is tin-plated tinplate with a tin plating grade of E4. Before coating, the surface of the metal plate is sanded and cleaned to remove oil.

[0034] Component A of the hydroxyl acrylic anticorrosive paint was added to a mixing container. Barium sulfate and hexagonal boron nitride were added in batches, along with 12 parts by weight of rosin to fully wet and disperse the inorganic filler. The remaining 8 parts by weight of rosin were then added to adjust the brushing viscosity. Finally, component B of the aliphatic polyurethane curing agent was added. Multi-stage mixing and degassing were performed using a vacuum homogenizer to obtain the coating.

[0035] The obtained coating was applied to the surface of E4 tin-plated tinplate by brushing and cured at room temperature for more than 8 hours to obtain a radiation-cooled composite coating with a dry film thickness of approximately 200 μm after curing. The preparation process is as follows: Figure 1 As shown.

[0036] Comparative Example 1: Preparation of coatings containing only barium sulfate functional filler

[0037] This comparative example uses barium sulfate as the functional filler. 32 parts by weight of component A of the hydroxyl acrylic anticorrosive paint, 8 parts by weight of component B of the aliphatic polyurethane curing agent, and 60 parts by weight of barium sulfate were weighed out. Hexagonal boron nitride was not added, and 20 parts by weight of rosin were prepared separately. Except for the different composition of the functional filler, the order of addition of other raw materials, the mixing and dispersion method, the vacuum degassing conditions, the metal substrate treatment method, the brushing method, and the room temperature curing conditions were all the same as in Example 1.

[0038] Comparative Example 2: Preparation of coatings containing only hexagonal boron nitride functional filler

[0039] This comparative example uses boron nitride as the functional filler. 32 parts by weight of component A of the hydroxyl acrylic anticorrosive paint, 8 parts by weight of component B of the aliphatic polyurethane curing agent, and 60 parts by weight of hexagonal boron nitride were weighed out. Barium sulfate was not added, and 20 parts by weight of rosin were prepared separately. Except for the different composition of the functional filler, the order of addition of other raw materials, mixing and dispersion methods, vacuum degassing conditions, metal substrate treatment methods, brushing methods, and room temperature curing conditions were all the same as in Example 1.

[0040]

[0041] Table 2 shows the results of the formulation and actual application and curing film formation. Under the condition that the total mass of inorganic filler is 60 parts, the application and film formation of the resulting coatings obtained by using barium sulfate alone or hexagonal boron nitride alone are lower than those in Example 1. In Example 1, 50 parts by mass of barium sulfate and 10 parts by mass of hexagonal boron nitride were combined, and under the same film-forming system and diluent dosage, it could be normally brushed and formed a continuous and complete coating film.

[0042] Test Example 1: Spectral Performance

[0043] The solar reflectance performance of the coating obtained by brush application in Example 1 was tested. A UV-Vis-NIR spectrophotometer equipped with an integrating sphere was used to measure the reflectance spectrum in the 250–2500 nm band in SCI hemispherical total reflectance mode. The test included the specular reflectance component, and a barium sulfate standard white plate was used as a reference. The weighted average solar reflectance in the 250–2500 nm band was calculated based on the AM1.5G solar spectrum, resulting in a solar reflectance weighted average of 91.2%. The reflectance spectrum is shown below. Figure 2 As shown.

[0044] The hemispherical reflectance spectrum in the 2.5–20 μm band was measured using a Fourier transform infrared spectrometer equipped with a gold integrating sphere accessory, with a gold-plated high-reflectance standard mirror as a reference. Since the coating can be considered opaque in this band, the hemispherical emissivity was calculated from the hemispherical reflectance according to Kirchhoff's thermal radiation law. The results are as follows: Figure 3 As shown, the average emissivity in the 2.5–20 μm band is 96.07%.

[0045] Test Example 2: Outdoor Cooling Performance

[0046] Outdoor testing equipment such as Figure 4 and Figure 5 As shown. The coated metal plate obtained by brush coating in Example 1 was placed at the top opening of a polystyrene foam insulation box, with the coated surface facing the sky. A thermocouple was inserted through the side of the box and in contact with the back of the sample, while the ambient air temperature was recorded. Temperature data was continuously collected during the test, and the results were obtained. Figure 6 The curve shown.

[0047] Depend on Figure 6 As can be seen, during the testing period from 10:00 to 15:00, the temperature of the coated sample was generally lower than the ambient air temperature during the same period; the average temperature difference between the sample and the ambient air was 5.6 ℃, and the maximum instantaneous temperature difference was approximately 9.3 ℃. This value represents the maximum instantaneous sub-ambient temperature difference in a single outdoor test, and does not represent the average temperature difference over the entire period. The actual temperature drop will be affected by factors such as solar irradiance, ambient temperature and humidity, wind speed, sample installation method, and sensor location. Example Description

[0048] The above embodiments illustrate the raw material composition, preparation process, and test results of the present invention. Equivalent substitutions or conventional adjustments made by those skilled in the art without departing from the essence of the present invention should be subject to the scope of protection defined in the claims.

Claims

1. A radiation-cooling composite coating with high reflectivity and high emissivity, characterized in that: The raw material components of the radiation cooling composite coating include hydroxyl acrylic anti-corrosion paint component A, aliphatic polyurethane curing agent component B, barium sulfate, hexagonal boron nitride, and rosin diluent.

2. The high reflectivity and high emissivity radiation-cooling composite coating according to claim 1, characterized in that: Based on a total mass of 100 parts by mass of hydroxy acrylic anticorrosive paint component A, aliphatic polyurethane curing agent component B, barium sulfate, and hexagonal boron nitride, the addition amounts of each component are as follows: 32 parts by mass of hydroxy acrylic anticorrosive paint component A, 8 parts by mass of aliphatic polyurethane curing agent component B, 50 parts by mass of barium sulfate, and 10 parts by mass of hexagonal boron nitride.

3. The high reflectivity and high emissivity radiation-cooling composite coating according to claim 2, characterized in that: The amount of the rosin diluent added is 20 parts by weight.

4. The high reflectivity and high emissivity radiation-cooling composite coating according to claim 2, characterized in that: The median particle size D50 of barium sulfate is 9–11 μm, and the particle size distribution D97 ≤ 12 μm.

5. The high reflectivity and high emissivity radiation-cooling composite coating according to claim 2, characterized in that: The median particle size D50 of hexagonal boron nitride is 1 μm.

6. The high reflectivity and high emissivity radiation-cooling composite coating according to claim 1 or 2, characterized in that: The radiation-cooled composite coating has a solar-weighted reflectance of 91.2% in the 250–2500 nm wavelength band and an average emissivity of 96.07% in the 2.5–20 μm wavelength band.

7. The method for preparing the radiation-cooled composite coating according to any one of claims 1-6, characterized in that... Includes the following steps: Barium sulfate and hexagonal boron nitride were added to component A of the hydroxy acrylic anticorrosive paint and a portion of the rosin thinner and dispersed. The remaining rosin thinner was added to adjust the application viscosity. After adding component B of the aliphatic polyurethane curing agent, the mixture was mixed and degassed. The resulting coating was applied to the surface of a metal substrate and cured at room temperature to form a radiation-cooled composite coating.

8. The preparation method according to claim 7, characterized in that: The metal substrate is a steel plate, galvanized steel plate, tin-plated steel plate, stainless steel plate, aluminum plate, or aluminum alloy plate.

9. The preparation method according to claim 7, characterized in that: The thickness of the radiation-cooled composite coating is 150~250 μm.

10. The preparation method according to claim 7, characterized in that: The curing time is ≥8h.