Aqueous electronic protective coating, coating and method for its production
By using a quick-drying, self-healing waterborne acrylic electronic protective coating, which combines moisture-responsive components and irreversible chemical reactions, the problems of slow drying speed and micro-cracks in waterborne acrylic electronic protective materials are solved, achieving rapid drying and self-healing while meeting environmental protection requirements.
Patent Information
- Application Number
- CN202611658462.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-20
AI Technical Summary
Existing water-based acrylic electronic protection materials have a slow drying speed and are prone to microcracks due to the accumulation of internal stress. Furthermore, self-healing materials require external stimulation or contain harmful components, making it difficult to meet the multiple requirements of environmental protection, rapid drying, and self-repair.
The quick-drying, self-healing waterborne acrylic electronic protective coating contains waterborne acrylic resin, moisture-responsive components, volatile inhibitors, and quick-drying additives. It can autonomously heal microcracks in a humid environment through an irreversible chemical reaction and remains stable during liquid storage.
It achieves rapid drying with a surface drying time of ≤10 minutes and a complete drying time of ≤30 minutes. Microcracks heal themselves without external stimulation and meet low VOCs environmental protection requirements. The coating remains stable during storage.
Smart Images

Figure CN123131891A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electronic protective materials technology, specifically relating to water-based electronic protective coatings, coatings and their preparation methods. Background Technology
[0002] Traditional solvent-based electronic protection materials are limited in application due to their high volatile organic compound (VOC) content, flammability, explosiveness, and operational health risks. Water-based electronic protection materials, using water as the main dispersion medium, offer environmental advantages such as low VOCs and good construction safety, and have become an important development direction in this field.
[0003] However, existing waterborne acrylic electronic protective materials still have technical shortcomings in practical applications. First, the high latent heat of vaporization of water results in a generally slow drying speed for coatings, with surface drying times typically ranging from 15 to 30 minutes, which is insufficient to meet the high-efficiency production cycles of electronic assembly lines. To improve drying speed, some products add low-boiling-point fast-drying agents to accelerate moisture evaporation. However, during rapid film formation, the coating is prone to microcracks due to the accumulation of internal stress. These microcracks can become penetration channels for corrosive media such as moisture and salt spray during subsequent service, thereby weakening the protective effect of the electronic protective material. Second, regarding self-healing functionality, existing reported waterborne self-healing electronic protective materials mostly employ strategies such as microencapsulating repair agents or introducing reversible dynamic covalent bonds (e.g., disulfide bonds, Diels-Alder bonds). However, these solutions often have limitations such as the repair agent containing harmful components, complex synthesis processes, or the need for external stimuli (e.g., heating, ultraviolet light) to trigger repair, making it difficult to simultaneously meet the multiple requirements of environmental friendliness, rapid drying, and self-repair during service life. Especially for microcracks caused by rapid drying, there are currently no water-based electronic protection materials that can achieve irreversible chemical healing without relying on external stimuli and under environmentally friendly conditions.
[0004] Therefore, developing a water-based acrylic electronic protection material that has rapid drying capability, can self-repair microcracks induced by rapid drying, and is environmentally friendly is of great practical significance. Summary of the Invention
[0005] This invention addresses the aforementioned problems in existing technologies by proposing a water-based electronic protective coating, a coating layer, and its preparation method. The electronic protective coating of this invention is a fast-drying, self-healing water-based acrylic electronic protective coating. While achieving rapid drying (surface drying time ≤ 10 min, complete drying time ≤ 30 min), it can self-heal microcracks generated during the rapid film formation process through irreversible chemical reactions under humid environments (such as immersion in water or high humidity service conditions), and the repair process requires no external stimulation. Furthermore, the electronic protective coating of this invention should exhibit good stability during liquid storage and meet the environmental protection requirements for low VOCs.
[0006] In one aspect, the present invention provides an electronic protective coating, comprising, by weight, the following components: 40-70 parts of waterborne acrylic resin, 1-10 parts of moisture-responsive component, 0.5-5 parts of volatile inhibitor, 2-10 parts of fast-drying agent, 2-8 parts of film-forming agent, 0.1-1 part of wetting agent, 0.2-1 part of thickener, 0.1-0.5 parts of defoamer, and 7-50 parts of water.
[0007] In this invention, the total weight of the electronic protective coating is not calculated in parts of 100.
[0008] In one or more embodiments, the electronic protective coating comprises, by weight, the following components: 50-65 parts of waterborne acrylic resin, 3-7 parts of moisture-responsive component, 1-3 parts of volatile inhibitor, 3-8 parts of fast-drying agent, 3-6 parts of film-forming agent, 0.2-0.5 parts of wetting agent, 0.3-0.6 parts of thickener, 0.1-0.3 parts of defoamer, and 11-30 parts of water.
[0009] In one or more embodiments, in the electronic protective coating, the waterborne acrylic resin contains an acrylate copolymer with carboxyl or hydroxyl reactive side groups.
[0010] In one or more embodiments, the acid value of the aqueous acrylic resin is 8-30 mg KOH / g.
[0011] In one or more embodiments, the hydroxyl value of the aqueous acrylic resin is 10-50 mg KOH / g.
[0012] In one or more embodiments, the number-average molecular weight Mn of the aqueous acrylic resin is 2000-15000 g / mol.
[0013] In one or more embodiments, the weight-average molecular weight (Mw) of the aqueous acrylic resin is 8000-80000 g / mol.
[0014] In one or more embodiments, the waterborne acrylic resin comprises 30-50 wt% methyl methacrylate, 20-40 wt% butyl acrylate, 5-15 wt% hydroxyethyl methacrylate, 1-8 wt% methacrylic acid, and auxiliary monomers obtained by free radical emulsion copolymerization; preferably, the auxiliary monomers are selected from one or more of styrene, hydroxypropyl acrylate, hydroxyethyl acrylate, acrylic acid, ethyl methacrylate, isooctyl methacrylate, isooctyl acrylate, acrylamide, diacetone acrylamide, glycidyl methacrylate, vinyl tert-carbonate, and acrylonitrile, and the mass fraction of the auxiliary monomers is 1-20 wt%.
[0015] In one or more embodiments, the solid content of the waterborne acrylic resin is 40%-50%.
[0016] In one or more embodiments, the glass transition temperature of the waterborne acrylic resin is 10°C-40°C.
[0017] In one or more embodiments, the waterborne acrylic resin has a viscosity of 10-20 mPa·s at 25°C ± 0.5°C, as tested by rotational viscometer method.
[0018] In one or more embodiments, in the electronic protective coating, the moisture-responsive component is selected from one or more of a silane coupling agent, polycarbodiimide, and epoxy compound; preferably, the silane coupling agent is γ-glycidyl etheroxypropyltrimethoxysilane, preferably KH-560; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester.
[0019] In one or more embodiments, in the electronic protective coating, the volatile inhibitor is selected from one or more of volatile organic amines and volatile organic acids; preferably, the volatile organic amine is selected from triethylamine and / or dimethylethanolamine; the volatile organic acid is acetic acid.
[0020] In one or more embodiments, in the electronic protective coating, the fast-drying agent is selected from one or more alcohols and first ether alcohol solvents; preferably, the alcohol is selected from ethanol and / or isopropanol; the first ether alcohol is propylene glycol methyl ether.
[0021] In one or more embodiments, in the electronic protective coating, the film-forming aid is selected from one or more second alcohol ether solvents; preferably, the second alcohol ether is selected from dipropylene glycol butyl ether (DPnB) and / or dipropylene glycol methyl ether (DPM).
[0022] In one or more embodiments, in the electronic protective coating, the wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; preferably, the polyether-modified polysiloxane is BYK-346; and the acetylenic diol is Surfynol 104.
[0023] In one or more embodiments, in the electronic protective coating, the thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners; preferably, the polyurethane associative thickener is RM-8W and the alkali-swellable thickener is ASE-60.
[0024] In one or more embodiments, in the electronic protective coating, the defoamer is selected from one or more of silicone-based and mineral oil-based defoamers; preferably, the silicone-based defoamer is BYK-024, and the mineral oil-based defoamer is Drewplus L-475.
[0025] In one or more embodiments, the water in the electronic protective coating is preferably deionized water.
[0026] In one or more embodiments, the electronic protective coating, when sealed and stored at 25°C for 6 months, exhibits no stratification, no sedimentation, no gelation, and a viscosity change rate of 0%-10%.
[0027] In one or more embodiments, the electronic protective coating, when sealed and stored at 25°C for 6 months, exhibits no stratification, no sedimentation, no gelation, and a viscosity change rate of 0%-9%.
[0028] Another aspect of the present invention provides a method for preparing the electronic protective coating according to any embodiment of the present invention, or a method for improving the storage stability of a quick-drying self-healing electronic protective coating, the method comprising the following steps: (1) Add water-based acrylic resin to a mixing container, add water while stirring, and mix well; (2) Add the complex of volatile inhibitor and moisture-responsive component, quick-drying agent, film-forming agent and wetting agent in sequence under stirring, and stir until uniformly dispersed to obtain a dispersion; (3) Dilute the thickener with water and slowly add it dropwise to the dispersion in step (2) while stirring to adjust the viscosity; (4) Stir and add defoamer; (5) Let it stand to defoam and filter it with a filter screen.
[0029] In one or more embodiments, in step (1), the waterborne acrylic resin is 40-70 parts by weight, preferably 50-65 parts; the waterborne acrylic resin is an acrylate copolymer containing carboxyl or hydroxyl reactive side groups.
[0030] In one or more embodiments, in step (1), the stirring speed is 200-400 rpm and the stirring time is 3-10 min.
[0031] In one or more embodiments, in step (1), the amount of water added is 6-40 parts by weight, preferably 9-24 parts.
[0032] In one or more embodiments, in step (2), the complex of the volatile inhibitor and the moisture-responsive component is a complex formed by pre-mixing the volatile inhibitor and the moisture-responsive component.
[0033] In one or more embodiments, in step (2), the method for preparing the complex of volatile inhibitor and moisture-responsive component is as follows: by weight, the moisture-responsive component and the volatile inhibitor are added to a sealed container at a weight ratio of 1:(0.3-0.8), and stirred at 300-500 rpm for 10-20 min at room temperature until the system is a transparent and homogeneous liquid, thereby obtaining the complex of volatile inhibitor and moisture-responsive component.
[0034] In one or more embodiments, in step (2), the volatile inhibitor is 0.5-5 parts by weight, preferably 1-3 parts; the volatile inhibitor is selected from one or more of volatile organic amines and volatile organic acids, preferably, the volatile organic amine is selected from triethylamine and / or dimethylethanolamine, and the volatile organic acid is acetic acid.
[0035] In one or more embodiments, in step (2), the moisture-responsive component is 1-10 parts by weight, preferably 3-7 parts; the moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide and epoxy compounds; preferably, the silane coupling agent is γ-glycidoxypropyltrimethoxysilane, preferably KH-560; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether and neopentanoic acid glycidyl ester.
[0036] In one or more embodiments, in step (2), the stirring time is 5-15 min until the dispersion is uniform, and the stirring speed is 200-400 rpm.
[0037] In one or more embodiments, in step (2), the quick-drying agent is 2-10 parts by weight, preferably 3-8 parts; the quick-drying agent is selected from one or more of alcohols and first ether alcohol solvents; preferably, the alcohol is selected from ethanol and / or isopropanol, and the first ether alcohol is propylene glycol methyl ether.
[0038] In one or more embodiments, in step (2), the film-forming aid is 2-8 parts by weight, preferably 3-6 parts; the film-forming aid is selected from one or more of the second alcohol ether solvents; preferably, the second alcohol ether is dipropylene glycol butyl ether (DPnB) and / or dipropylene glycol methyl ether (DPM).
[0039] In one or more embodiments, in step (2), the wetting agent is 0.1-1 parts by weight, preferably 0.2-0.5 parts; the wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; preferably, the polyether-modified polysiloxane is BYK-346 and the acetylenic diol is Surfynol 104.
[0040] In one or more embodiments, in step (3), the weight ratio of water to thickener is 9:1.
[0041] In one or more embodiments, in step (3), the thickener is 0.2-1 parts by weight, preferably 0.3-0.6 parts; the thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners; preferably, the polyurethane associative thickener is RM-8W and the alkali-swellable thickener is ASE-60.
[0042] In one or more embodiments, in step (3), the water used to dilute the thickener is 1.8-9 parts by weight, preferably 2.7-5.4 parts.
[0043] In one or more embodiments, in step (3), the stirring speed is 500-800 rpm and the stirring time is 10-15 min.
[0044] In one or more embodiments, in step (3), the viscosity is adjusted so that when tested at 25°C and using an ISO-3 flow cup, the time for the entire cup of liquid to flow out is 30-60 s.
[0045] In one or more embodiments, in step (4), the defoamer is 0.1-0.5 parts by weight, preferably 0.1-0.3 parts; the defoamer is selected from one or more of silicone and mineral oil defoamers; preferably, the silicone defoamer is BYK-024 and the mineral oil defoamer is Drewplus L-475.
[0046] In one or more embodiments, in step (4), the stirring speed is 200-400 rpm and the stirring time is 5-10 min.
[0047] In one or more embodiments, in step (5), the filter screen is preferably 200 mesh, and the filtered material is preferably sealed and packaged.
[0048] In another aspect, the present invention provides an electronic protective coating comprising, by weight, the following components: 50-65 parts of waterborne acrylic resin, 3-7 parts of moisture-responsive component, 3-6 parts of film-forming aid, 0.2-0.5 parts of wetting agent, 0.3-0.6 parts of thickener, and 0.1-0.3 parts of defoamer.
[0049] In one or more embodiments, in the electronic protective coating, the moisture-responsive component is selected from one or more of a silane coupling agent, polycarbodiimide, and epoxy compound; preferably, the silane coupling agent is γ-glycidoxypropyltrimethoxysilane, preferably KH-560; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester.
[0050] In one or more embodiments, in the electronic protective coating, the film-forming aid is selected from one or more second alcohol ether solvents; preferably, the second alcohol ether is selected from dipropylene glycol butyl ether (DPnB) and / or dipropylene glycol methyl ether (DPM).
[0051] In one or more embodiments, in the electronic protective coating, the wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; preferably, the polyether-modified polysiloxane is BYK-346; and the acetylenic diol is Surfynol 104.
[0052] In one or more embodiments, in the electronic protective coating, the thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners; preferably, the polyurethane associative thickener is RM-8W and the alkali-swellable thickener is ASE-60.
[0053] In one or more embodiments, in the electronic protective coating, the defoamer is selected from one or more of silicone-based and mineral oil-based defoamers; preferably, the silicone-based defoamer is BYK-024 and the mineral oil-based defoamer is Drewplus L-475.
[0054] In one or more embodiments, the dry film thickness of the electronic protective coating is 30-100 μm, preferably 45 μm.
[0055] In one or more embodiments, the surface drying time of the electronic protective coating is 2-10 min.
[0056] In one or more embodiments, the drying time of the electronic protective coating is 20-30 minutes.
[0057] In one or more embodiments, moisture healing of the electronic protective coating means that after the electronic protective coating is fully immersed in water for 24 hours, the immersed coating remains in a healed state and the microcracks are irreversible.
[0058] In one or more embodiments, the VOCs content of the electronic protective coating is ≤ 50 g / L.
[0059] In one or more embodiments, the water absorption rate of the electronic protective coating after immersion in water for 24 hours is ≤ 0.7%.
[0060] In one or more embodiments, the breakdown strength of the electronic protective coating after immersion in water for 24 hours is ≥ 89 kV / mm.
[0061] In one or more embodiments, the electronic protective coating exhibits salt spray resistance for ≥ 500 h without bubbling after immersion in water for 24 h.
[0062] In another aspect, the present invention provides a method for preparing the electronic protective coating according to any embodiment of the present invention, wherein the method applies the electronic protective coating according to any embodiment of the present invention or the electronic protective coating prepared by the method using one of conventional spraying, dipping, brushing or selective coating, and dries to form the electronic protective coating; preferably, a spraying method is used, in which the electronic protective coating according to any embodiment of the present invention or the electronic protective coating prepared by the method is applied to a clean tinplate or PCB board surface, and the dry film thickness is controlled to be 30-100 μm, preferably 45 μm.
[0063] An electronic product includes a substrate and an electronic protective coating as described in any embodiment of the present invention, or an electronic protective coating obtained by the preparation method described in any embodiment of the present invention, located on the surface of the substrate.
[0064] In another aspect, the present invention provides the following applications: (1) The application of the electronic protective coating described in any embodiment of the present invention or the electronic protective coating obtained by the preparation method described in any embodiment of the present invention in improving drying speed and / or improving microcrack healing rate and / or storage stability; (2) Application of volatile inhibitors and / or moisture-responsive components in improving the healing rate and / or adhesion and / or salt spray resistance and / or breakdown strength and / or water absorption of electronic protective coatings; (3) Application of volatile inhibitors and / or moisture-responsive components in improving the drying speed and / or storage stability of electronic protective coatings. Attached Figure Description
[0065] Figure 1 The following images illustrate Embodiment 1 of the present invention: a) a photograph of the electronic protective coating after surface drying; b) a photograph of the coating after immersion in water for 24 hours; c) a photograph of the coating after immersion in water for 24 hours and drying; d) a photograph of the coating after drying without immersion in water; e) a photograph of the coating after being placed at 25°C and 60% humidity for 7 days; f) a photograph of the coating after being placed at 25°C and 60% humidity for 15 days. Photo magnification: 10x.
[0066] Figure 2The following images show Comparative Example 2 of the present invention: a) a photograph of the electronic protective coating after it has dried to the touch, and b) a photograph of the coating after it has been immersed in water for 24 hours. Photo magnification: 10x.
[0067] Figure 3 The following images show Comparative Example 4 of the present invention: a) a photograph of the electronic protective coating after it has dried to the touch, and b) a photograph of the coating after it has been immersed in water for 24 hours. Photo magnification: 10x.
[0068] Figure 4 The following images are shown: Comparative Example 5 of the present invention: a) a photograph of the electronic protective coating after it has dried to the touch; b) a photograph of the coating after it has been immersed in water for 24 hours; c) a photograph of the coating after it has been placed at a temperature of 25°C and a humidity of 60% for 15 days. Photo magnification: 10x. Detailed Implementation
[0069] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used herein are explained and defined in general terms below. Unless otherwise specified, all technical and scientific terms used herein have the common meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.
[0070] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.
[0071] In this document, the terms “contains,” “includes,” “containing,” and similar terms encompass the meanings of “basically composed of” and “composed of.” For example, when this document discloses “A contains B and C,” “A is basically composed of B and C” and “A is composed of B and C” should be considered as having been disclosed in this document.
[0072] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values (including integers and fractions) within those ranges.
[0073] Unless otherwise specified, percentages refer to mass percentages and proportions refer to mass ratios in this article.
[0074] In this article, the sum of the percentages of all components in the composition is 100%.
[0075] In this document, when describing embodiments or examples, it should be understood that it is not intended to limit the invention to those embodiments or examples. Rather, all alternatives, modifications, and equivalents of the methods and materials described herein are covered within the scope of this invention.
[0076] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.
[0077] This invention provides a quick-drying waterborne acrylic electronic protective coating and its preparation method. This electronic protective coating exhibits rapid drying performance and can achieve self-healing of microcracks through irreversible chemical reactions, with the repair process requiring no external stimulation. Furthermore, the electronic protective coating should possess good stability during liquid storage and meet low VOCs environmental protection requirements.
[0078] The inhibition-activation and healing mechanism of the electronic protective coating of this invention is as follows: When the electronic protective coating is stored in liquid form, volatile inhibitor molecules form reversible physical or chemical interactions (such as ion pair formation or hydrogen bonding) with the active functional groups of the moisture-responsive component, thereby inhibiting the reaction of the moisture-responsive component with the side groups of the waterborne acrylic resin or with water. This inhibition effect is stably maintained at room temperature, ensuring that the liquid electronic protective coating has storage stability for at least 6 months. When the electronic protective coating is sprayed to form a film, the fast-drying additives and moisture evaporate rapidly, and the volatile inhibitors also escape, forming microcracks on the coating surface. The active sites of the moisture-responsive component are exposed, causing an irreversible chemical reaction between the moisture-responsive component and the side groups of the waterborne acrylic resin. Under humid conditions, the microcracks in the coating can self-heal. This activation process can be completed at room temperature without additional heating.
[0079] When the coating is exposed to moisture (such as immersion in water or high humidity environments) during service, the moisture-responsive components undergo irreversible chemical reactions with the side groups of the waterborne acrylic resin. For example, the silane coupling agent hydrolyzes under moisture to generate silanol, which then condenses with the carboxyl or hydroxyl groups of the waterborne acrylic resin to form Si-OC covalent bonds; polycarbodiimide reacts with the carboxyl groups of the waterborne acrylic resin to form N-acylurea bonds. These irreversible chemical reactions can occur at room temperature and under neutral to weakly alkaline conditions, thereby permanently connecting the polymer networks on both sides of the microcrack through newly formed covalent bonds, achieving crack healing. This healing process does not require external heating or ultraviolet light irradiation. The healed coating will not re-crackle when placed in the same moisture environment, therefore, crack healing is irreversible.
[0080] Electronic protective coatings
[0081] The electronic protective coating of the present invention comprises, by weight, the following components: 40-70 parts of waterborne acrylic resin, 1-10 parts of moisture-responsive component, 0.5-5 parts of volatile inhibitor, 2-10 parts of fast-drying agent, 2-8 parts of film-forming agent, 0.1-1 part of wetting agent, 0.2-1 part of thickener, 0.1-0.5 parts of defoamer, and 7-50 parts of water.
[0082] In some preferred embodiments, the electronic protective coating of the present invention comprises the following components: 50-65 parts of waterborne acrylic resin, 3-7 parts of moisture-responsive component, 1-3 parts of volatile inhibitor, 3-8 parts of fast-drying agent, 3-6 parts of film-forming agent, 0.2-0.5 parts of wetting agent, 0.3-0.6 parts of thickener, 0.1-0.3 parts of defoamer, and 11-30 parts of water.
[0083] In this invention, the total weight of the electronic protective coating is not calculated in parts of 100.
[0084] In this invention, the waterborne acrylic resin is an acrylate copolymer containing reactive side groups such as carboxyl groups (-COOH) or hydroxyl groups (-OH). The waterborne acrylic resin itself does not contain restricted substances such as APEO (alkylphenol polyoxyethylene ether), and the volatile organic compound (VOCs) content is <2 g / L.
[0085] In this invention, the acid value of the waterborne acrylic resin is 8-30 mg KOH / g, such as 8 mg KOH / g, 10 mg KOH / g, 15 mg KOH / g, 20 mg KOH / g, 25 mg KOH / g, 28 mg KOH / g, and 30 mg KOH / g.
[0086] In this invention, the hydroxyl value of the waterborne acrylic resin is 10-50 mg KOH / g, such as 10 mg KOH / g, 15 mg KOH / g, 20 mg KOH / g, 25 mg KOH / g, 30 mg KOH / g, 35 mg KOH / g, 40 mg KOH / g, 45 mg KOH / g, and 50 mg KOH / g.
[0087] In this invention, the number average molecular weight Mn of the waterborne acrylic resin is 2000-15000 g / mol, such as 2000 g / mol, 5000 g / mol, 8000 g / mol, 10000 g / mol, 12000 g / mol, 15000 g / mol, or any range of two of the above values.
[0088] In this invention, the weight-average molecular weight (Mw) of the waterborne acrylic resin is 8000-80000 g / mol, such as 8000 g / mol, 10000 g / mol, 12000 g / mol, 15000 g / mol, 18000 g / mol, 20000 g / mol, 30000 g / mol, 40000 g / mol, 50000 g / mol, 60000 g / mol, 70000 g / mol, 80000 g / mol, or any range of two of the above values.
[0089] In this invention, the waterborne acrylic resin comprises 30-50 wt% methyl methacrylate, 20-40 wt% butyl acrylate, 5-15 wt% hydroxyethyl methacrylate, 1-8 wt% methacrylic acid, and auxiliary monomers, obtained by free radical emulsion copolymerization; preferably, the auxiliary monomers are selected from one or more of styrene, hydroxypropyl acrylate, hydroxyethyl acrylate, acrylic acid, ethyl methacrylate, isooctyl methacrylate, isooctyl acrylate, acrylamide, diacetone acrylamide, glycidyl methacrylate, ethylene tert-carbonate, and acrylonitrile, and the mass fraction of the auxiliary monomers is 1-20 wt%.
[0090] In this invention, the solid content of the waterborne acrylic resin is 40%-50%, such as 40%, 45%, or 50%.
[0091] In this invention, the glass transition temperature of the waterborne acrylic resin is 10℃-40℃, for example, 10℃, 20℃, 30℃, 40℃, or 50℃.
[0092] In this invention, the waterborne acrylic resin, as tested by rotational viscometer method, has a viscosity of 10-20 mPa·s at 25℃ ± 0.5℃, such as 10 mPa·s, 12 mPa·s, 15 mPa·s, 18 mPa·s, and 20 mPa·s.
[0093] As an example, the present invention may use commercially available waterborne acrylic resin emulsions, including but not limited to Dow Chemical's Primal AS-300, BASF's Joncryl 8000, and Wanhua Chemical's Acrylic 2603.
[0094] In this invention, the waterborne acrylic resin is 40-70 parts by weight, preferably 50-65 parts, for example 50 parts, 55 parts, 58 parts, 60 parts, 63 parts, and 65 parts.
[0095] In this invention, the moisture-responsive component refers to a compound that can be activated in the presence of water molecule moisture and undergo an irreversible chemical reaction with the side groups of the waterborne acrylic resin. The moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide, and epoxy compounds; as an example, the silane coupling agent is preferably γ-glycidyl etheroxypropyltrimethoxysilane (such as commercially available KH-560). As an example, the epoxy compound is preferably one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester. Among them, neopentanoic acid glycidyl ester is also known as (… S 2-Neopentanoic acid ethylene oxide-2-methyl ester. In the waterborne electronic protective coating system of the present invention, the activity of the moisture-responsive component is reversibly and temporarily blocked by a volatile inhibitor, thereby ensuring liquid storage stability.
[0096] In this invention, the weight of the moisture-responsive component is 1-10 parts, preferably 3-7 parts, for example 3 parts, 4 parts, 5 parts, 6 parts, or 7 parts.
[0097] In this invention, a volatile inhibitor refers to a substance capable of forming a reversible complex with the active site of a moisture-responsive component, thereby inhibiting its reactivity. This substance has a high vapor pressure at room temperature (boiling point typically ≤ 100°C), and the formation of the reversible complex includes, but is not limited to, ion pairs and hydrogen bonds. The volatile inhibitor is selected from one or more volatile organic amines and volatile organic acids; as an example, the volatile organic amine is preferably selected from triethylamine and / or dimethylethanolamine, and the volatile organic acid can be acetic acid. In the waterborne electronic protective coating system of this invention, the volatile inhibitor reversibly inhibits the pre-reaction of the moisture-responsive component with the waterborne acrylic resin or water during liquid storage; after the electronic protective coating is sprayed, the inhibitor evaporates along with the fast-drying agent and moisture, and the moisture-responsive component regains its activity.
[0098] In this invention, the volatile inhibitor is 0.5-5 parts by weight, preferably 1-3 parts, for example 1 part, 1.5 parts, 2 parts, 2.5 parts, or 3 parts.
[0099] In this invention, the fast-drying agent refers to a water-soluble organic solvent with a boiling point ≤ 100℃. The fast-drying agent is selected from one or more alcohols and first ether alcohols; as an example, alcohols are preferably selected from ethanol and / or isopropanol, and the first ether alcohol can be propylene glycol methyl ether. The function of the fast-drying agent is to accelerate the evaporation of moisture in the coating while promoting the volatilization of inhibitors.
[0100] In this invention, the quick-drying agent is 2-10 parts by weight, preferably 3-8 parts, for example 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, or 8 parts.
[0101] In this invention, the film-forming aid refers to an environmentally friendly solvent with a boiling point of 150℃-250℃, and is selected from one or more second alcohol ether solvents; as an example, the second alcohol ether is preferably selected from one or both of dipropylene glycol butyl ether (DPnB) and dipropylene glycol methyl ether (DPM). The function of the film-forming aid is to lower the minimum film-forming temperature of the waterborne acrylic resin, ensuring the formation of a continuous and dense coating at room temperature.
[0102] In this invention, the film-forming aid is 2-8 parts by weight, preferably 3-6 parts, for example 3 parts, 4 parts, 5 parts, or 6 parts.
[0103] In this invention, the wetting agent refers to a surfactant capable of reducing the surface tension of the coating and improving its wetting performance on the substrate. The wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; as an example, the polyether-modified polysiloxane is preferably BYK-346, and the acetylenic diol is preferably Surfynol 104. The wetting agent of this invention does not contain alkylphenol polyoxyethylene ether (APEO).
[0104] In this invention, the wetting agent is 0.1-1 parts by weight, preferably 0.2-0.5 parts, for example 0.2 parts, 0.3 parts, 0.4 parts, or 0.5 parts.
[0105] In this invention, the thickener refers to a polymer used to adjust the viscosity of the coating and improve its rheological properties during application. The thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners. As an example, the polyurethane associative thickener is preferably RM-8W, and the alkali-swellable thickener is preferably ASE-60.
[0106] In this invention, the thickener is 0.2-1 parts by weight, preferably 0.3-0.6 parts, for example 0.3 parts, 0.4 parts, 0.5 parts, or 0.6 parts.
[0107] In this invention, defoamer refers to an additive used to suppress and eliminate foam generated during the preparation and application of coatings. The defoamer is selected from one or more of silicone-based and mineral oil-based defoamers. As an example, the silicone-based defoamer is preferably BYK-024, and the mineral oil-based defoamer is preferably Drewplus L-475.
[0108] In this invention, the defoamer is used in 0.1-0.5 parts by weight, preferably 0.1-0.3 parts, for example 0.1 parts, 0.2 parts, or 0.3 parts.
[0109] In this invention, water is used as the solvent for the electronic protective coating, preferably deionized water.
[0110] In this invention, the water is in the form of 7-50 parts by weight, preferably 11-30 parts, for example 11 parts, 11.8 parts, 12 parts, 13 parts, 14 parts, 15 parts, 18 parts, 20 parts, 22 parts, 25 parts, 28 parts, or 30 parts.
[0111] In this invention, the electronic protective coating is sealed and stored in an environment of 25°C for 6 months without stratification, precipitation, or gelation, and the viscosity change rate is 0%-10%, preferably 0%-9%, such as 0%, 1%, 2%, 3%, 6%, 8%, and 9%.
[0112] Electronic protective coating
[0113] In this invention, the electronic protective coating comprises the following components: 50-65 parts of waterborne acrylic resin, 3-7 parts of moisture-responsive component, 3-6 parts of film-forming aid, 0.2-0.5 parts of wetting agent, 0.3-0.6 parts of thickener, and 0.1-0.3 parts of defoamer. The electronic protective coating of this invention is prepared using the electronic protective coating described in any embodiment herein.
[0114] In this invention, the moisture-responsive component of the electronic protective coating undergoes an irreversible chemical reaction with the waterborne acrylic resin under conditions of immersion in water or high humidity. The moisture-responsive component is selected from one or more of a silane coupling agent, polycarbodiimide, and epoxy compound; as an example, the silane coupling agent is preferably γ-glycidyl etheroxypropyltrimethoxysilane (such as commercially available KH-560); the epoxy compound is preferably one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and glycidyl neopentanoate. Glycidyl neopentanoate is also known as (… S 2-Neopentanoic acid ethylene oxide-2-methyl ester. As an example, silane coupling agents hydrolyze under humid conditions to generate silanols, which then condense with the carboxyl or hydroxyl groups of the waterborne acrylic resin to form Si-OC covalent bonds; polycarbodiimide reacts with the carboxyl groups of the waterborne acrylic resin to form N-acylurea bonds. Epoxy compounds then form β-hydroxy ester or β-hydroxy ether structures with the carboxyl or hydroxyl groups of the waterborne acrylic resin. All of these reactions involve covalent bonds, which, once formed, stabilize the chemical components in the coating, achieving crack healing. After healing, the coating will not crack again when placed in the same humid environment.
[0115] In this invention, the dry film thickness of the electronic protective coating is 30-100 μm, preferably 45 μm.
[0116] In this invention, the method of applying the electronic protective coating is not particularly limited, and those skilled in the art can select a suitable coating method according to the actual working conditions. Preferably, the coating method is selected from one of spraying, dipping, brushing, or selective coating.
[0117] In some preferred embodiments, the electronic protective coating is prepared by spraying, applying the coating to a clean tinplate or PCB board surface, and controlling the dry film thickness to 45 μm (achieved by adjusting the number of spray passes or the wet film thickness). The coating is then allowed to dry naturally at room temperature (25℃±2℃, relative humidity 50%±10%).
[0118] In this invention, the surface drying time of the electronic protective coating can be 2-10 min, and the actual drying time can be 20-30 min; the surface drying time can be 2 min, 5 min, 6 min, 7 min, 8 min, or 10 min; and the actual drying time can be 20 min, 25 min, 26 min, 27 min, 28 min, or 30 min.
[0119] In this invention, the moisture healing of the electronic protective coating means that after the electronic protective coating is completely immersed in water for 24 hours, the immersed coating remains in a healed state, and the microcracks are irreversible.
[0120] In this invention, the VOCs content of the electronic protective coating is ≤ 50 g / L, for example 20 g / L, 30 g / L, 32 g / L, 33 g / L, 35 g / L, 40 g / L, or 50 g / L.
[0121] In this invention, the water absorption rate of the electronic protective coating after immersion in water for 24 hours is ≤ 0.7%, for example 0.2%, 0.3%, 0.4%, 0.5%, 0.56%, 0.58%, 0.6%, 0.65%, and 0.7%.
[0122] In this invention, the breakdown strength of the electronic protective coating after immersion in water for 24 hours is ≥ 89 kV / mm, for example 89 kV / mm, 89.1 kV / mm, 90 kV / mm, 90.4 kV / mm, 92.3 kV / mm, 95 kV / mm, 96.2 kV / mm, 100 kV / mm.
[0123] In this invention, the electronic protective coating, after being immersed in water for 24 hours, exhibits salt spray resistance for ≥ 500 hours without blistering.
[0124] Methods for preparing electronic protective coatings, or methods for improving the storage stability of quick-drying self-healing electronic protective coatings.
[0125] In this invention, the preparation method of the electronic protective coating includes the following steps: (1) Add water-based acrylic resin to a mixing container, add water while stirring, and mix well; (2) Add the complex of volatile inhibitor and moisture-responsive component, quick-drying agent, film-forming agent and wetting agent in sequence under stirring, and stir until each component is evenly dispersed to obtain a dispersion; (3) Dilute the thickener with water beforehand, and slowly add it dropwise to the dispersion in step (2) while stirring to adjust the viscosity; (4) Stir and add defoamer; (5) Let it stand to defoam and filter it with a filter screen.
[0126] In this invention, in step (1), the waterborne acrylic resin is 40-70 parts by weight, preferably 50-65 parts, for example 50 parts, 55 parts, 58 parts, 60 parts, 63 parts, or 65 parts. The waterborne acrylic resin is an acrylate copolymer containing reactive side groups such as carboxyl groups (-COOH) or hydroxyl groups (-OH).
[0127] In this invention, in step (1), the stirring speed is 200-400 rpm, for example 200 rpm, 300 rpm, 400 rpm; the stirring time is 3-10 min, for example 3 min, 5 min, 8 min, 10 min.
[0128] In this invention, in step (1), the weight of water added is 60%-80% of the total water volume, for example, 60%, 70%, or 80%. In step (1), the weight of water is 6-40 parts, preferably 9-24 parts, for example, 9 parts, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts, 22 parts, 23.5 parts, or 24 parts.
[0129] In this invention, in step (2), the complex of volatile inhibitor and moisture-responsive component is formed by pre-mixing the volatile inhibitor and moisture-responsive component to form a complex.
[0130] In this invention, the preparation method of the complex of volatile inhibitor and moisture-responsive component is as follows: Moisture-responsive component and volatile inhibitor are added to a sealed container in a weight ratio of 1:(0.3-0.8). The mixture is stirred at 300-500 rpm for 10-20 min at room temperature until the system becomes a transparent and homogeneous liquid, thus obtaining the complex of volatile inhibitor and moisture-responsive component. The complex of volatile inhibitor and moisture-responsive component should be stored under sealed conditions and used in coating formulation within 12 h after preparation to prevent the inhibitor from volatilizing and causing activity recovery. The weight ratio of moisture-responsive component to volatile inhibitor can be 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, or 1:0.8.
[0131] In this invention, in step (2), the volatile inhibitor is 0.5-5 parts by weight, preferably 1-3 parts, for example 1 part, 2 parts, or 3 parts. The volatile inhibitor is selected from one or more of volatile organic amines and volatile organic acids. Preferably, the volatile organic amine is selected from triethylamine and / or dimethylethanolamine, and the volatile organic acid can be acetic acid.
[0132] In this invention, in step (2), the weight percentage of the moisture-responsive component is 1-10 parts, preferably 3-7 parts, for example 3 parts, 4 parts, 5 parts, 6 parts, or 7 parts. The moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide, and epoxy compounds; preferably, the silane coupling agent can be γ-glycidyl etheroxypropyltrimethoxysilane (such as commercially available KH-560); the epoxy compound can be one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester.
[0133] In this invention, in step (2), after adding the complex of volatile inhibitor and moisture-responsive component, quick-drying agent, film-forming agent and wetting agent, the stirring time is 5-15 min until the components are evenly dispersed. The stirring time can be 5 min, 10 min or 15 min; the stirring speed is 200-400 rpm, for example 200 rpm, 300 rpm or 400 rpm.
[0134] In this invention, in step (2), the weight of the quick-drying agent is 2-10 parts, preferably 3-8 parts, for example 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, or 8 parts. The quick-drying agent is selected from one or more alcohols and first ether alcohol solvents; preferably, the alcohol is selected from ethanol and / or isopropanol, and the first ether alcohol can be propylene glycol methyl ether.
[0135] In this invention, in step (2), the film-forming aid is 2-8 parts by weight, preferably 3-6 parts, for example 3 parts, 4 parts, 5 parts, or 6 parts. The film-forming aid is selected from one or more of the second alcohol ether solvents; preferably, the second alcohol ether can be dipropylene glycol butyl ether (DPnB) or dipropylene glycol methyl ether (DPM).
[0136] In this invention, in step (2), the wetting agent is 0.1-1 parts by weight, preferably 0.2-0.5 parts, for example 0.2 parts, 0.3 parts, 0.4 parts, or 0.5 parts. The wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; preferably, the polyether-modified polysiloxane can be BYK-346, and the acetylenic diol can be Surfynol 104. The wetting agent of this invention does not contain alkylphenol polyoxyethylene ether (APEO).
[0137] In this invention, in step (3), the weight ratio of water to thickener is 9:1.
[0138] In this invention, in step (3), the thickener is 0.2-1 parts by weight, preferably 0.3-0.6 parts, for example 0.3 parts, 0.4 parts, 0.5 parts, or 0.6 parts. The thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners; preferably, the polyurethane associative thickener can be RM-8W, and the alkali-swellable thickener can be ASE-60.
[0139] In this invention, in step (3), the water used to dilute the thickener is 1.8-9 parts by weight, preferably 2.7-5.4 parts, for example 3 parts, 4 parts, 4.5 parts, 5 parts, or 5.4 parts.
[0140] In this invention, in step (3), when adding the diluted thickener, the stirring speed is 500-800 rpm to make the thickener disperse quickly and evenly. The stirring speed can be 500 rpm, 600 rpm, 700 rpm, or 800 rpm. After adding the thickener, continue stirring for 10-15 minutes to make the thickener fully dispersed. The stirring time can be 10 minutes, 13 minutes, or 15 minutes.
[0141] In this invention, in step (3), the viscosity is adjusted to be 30-60 s when tested at 25°C and using an ISO-3 flow cup.
[0142] In this invention, in step (4), the defoamer is used in an amount of 0.1-0.5 parts by weight, preferably 0.1-0.3 parts, for example 0.1 parts, 0.2 parts, or 0.3 parts. The defoamer is selected from one or more of silicone-based and mineral oil-based defoamers; preferably, the silicone-based defoamer can be BYK-024, and the mineral oil-based defoamer can be Drewplus L-475.
[0143] In this invention, in step (4), the defoamer is added by stirring at a speed of 200-400 rpm, for example 200 rpm, 300 rpm, or 400 rpm; and the stirring time is 5-10 min, for example 5 min, 8 min, or 10 min.
[0144] In this invention, in step (5), the filter screen is preferably 200 mesh, and the filtered material is preferably sealed and packaged.
[0145] In this invention, prolonged exposure of the container should be avoided during the preparation process to prevent excessive volatilization of the inhibitor, which could lead to premature activation. The finished product should be sealed and stored in a cool, dry place.
[0146] The present invention also provides an electronic product comprising a substrate and an electronic protective coating as described in any embodiment of the present invention located on the surface of the substrate.
[0147] The present invention also provides the application of the electronic protective coating described in any embodiment of the present invention or the electronic protective coating obtained by the preparation method described in any embodiment of the present invention in improving drying speed and / or improving microcrack healing rate and / or storage stability.
[0148] The present invention also provides the use of the volatile inhibitors and / or moisture-responsive components of the present invention in improving the healing rate and / or adhesion and / or salt spray resistance and / or breakdown strength and / or water absorption of electronic protective coatings.
[0149] The present invention also provides the use of the volatile inhibitors and / or moisture-responsive components of the present invention in improving the drying speed and / or storage stability of electronic protective coatings.
[0150] The present invention has the following beneficial effects: 1. Fast drying speed: The coating components contain fast-drying additives, and the surface drying time of the coating can be controlled within 10 minutes and the actual drying time within 30 minutes. The drying speed is better than that of conventional water-based acrylic electronic protective coatings (usually surface drying time is 15~30 minutes). 2. Moisture-triggered irreversible self-healing: Microcracks in the coating caused by rapid drying can achieve a healing rate of over 90% within 12 hours under water immersion conditions, and the healing process requires no external stimulation (heating, ultraviolet light, etc.). The healing reaction is an irreversible chemical cross-linking, resulting in a permanent repair effect. 3. Good storage stability: The volatile inhibitor has the activity of reversibly inhibiting the reaction between moisture-responsive components and resin or water. The liquid electronic protective coating can remain stable for more than 6 months under normal sealed storage conditions without significant thickening or gelling. 4. Basic protection capability after quick drying: Before the coating is fully healed, its adhesion, salt spray resistance and insulation resistance can still reach about 60% of the performance after full healing, thus ensuring the basic protection needs during the transition from production to service. 5. High thickness tolerance: The electronic protective coating of this invention can achieve rapid drying (surface drying time ≤ 10 min), good moisture healing and excellent protective performance in the coating thickness range of 30-100 μm. It is not sensitive to the fluctuation of the construction thickness and is easy to apply on a large scale. 6. Excellent environmental performance: The electronic protective coating of this invention uses water as the dispersion medium, has a VOCs content of ≤ 50 g / L, and does not contain restricted substances such as benzene compounds, formaldehyde, halogenated hydrocarbons, isocyanates and heavy metals, which meets the requirements of current mainstream environmental protection regulations. 7. Low water absorption: The water absorption of the coating decreases significantly after healing (≤ 0.7%), indicating that the microcracks are closed and the coating density is restored, which is beneficial to long-term moisture-proof performance; 8. Comprehensive protective performance meets the standards: the adhesion of the healed coating is grade 0, the salt spray resistance is ≥ 500 h without blistering, the breakdown strength is ≥ 89 kV / mm, and the water absorption rate is ≤ 0.7% after 24 h.
[0151] The present invention will be described below by way of specific embodiments. It should be understood that these embodiments are merely illustrative and not intended to limit the scope of the invention. The methods, reagents, and materials used in the embodiments and comparative examples are conventional methods, reagents, and materials in the art, unless otherwise stated. The starting material compounds in the embodiments and comparative examples are all commercially available. The test methods used herein are as follows: (1) Storage stability test of electronic protective coating The prepared electronic protective coating was sealed and stored in an environment with a temperature of 25℃±0.5℃ for 6 months. The presence of phenomena such as layering, precipitation, and gelation was observed, and the viscosity change rate of the electronic protective coating was tested.
[0152] According to GB / T 46024-2025 "Paints and Varnishes - Determination of Flow Time Using Flow Cups" (equivalent to ISO 2431:2019), using an ISO-3 flow cup, the viscosity of electronic protective coatings was determined at the initial storage and after 6 months of storage at a temperature of 25℃±0.5℃. v 0 and v 1 The viscosity change rate η is calculated according to equation (1): (1) (2) Moisture healing treatment The coating sample with microcracks was completely immersed in deionized water at 25°C for 24 hours, then removed and dried, and observed again using a magnifying glass. The required healing effect was that the original coating microcracks essentially disappeared after 24 hours of immersion.
[0153] (3) Irreversibility verification test
[0154] The water-healed coating was thoroughly dried at room temperature (48 h at 25°C and ≤30% relative humidity) to allow free water in the coating to evaporate. Microcracks were then observed under a magnifying glass to determine if they reappeared and whether the coating maintained its post-healing density. The control sample, a coating prepared with the same component formulation, underwent rapid drying without water immersion and the same drying process; therefore, its microcracks remained due to the lack of water immersion.
[0155] (4) Test of the protective performance of the coating
[0156] The protective performance of the coating was tested after quick-drying (unhealed) and after immersion in water for 24 hours to heal.
[0157] The evaluation items for the protective performance of the coating include adhesion (cross-cut test, test method reference standard GB / T 9286-2021), salt spray resistance (35℃, 5% NaCl, test method reference standard GB / T 2423.17-2024), breakdown strength (test method reference standard GB / T 1408.1-2016, unit is kV / mm) and water absorption rate (test method reference standard HG / T 3856-2006, 24 h).
[0158] The requirements for the overall protective performance of the coating are as follows: the adhesion of the coating after immersion in water for 24 hours is grade 0, the coating has a salt spray resistance of ≥ 500 hours without blistering, the breakdown strength is ≥ 89 kV / mm, and the water absorption rate is ≤ 0.7%.
[0159] (5) VOCs test
[0160] According to the method of GB / T 23986.2-2023, VOCs are determined and the coating VOCs content is required to be ≤ 50 g / L.
[0161] (6) Test methods for surface drying time and actual drying time
[0162] Referring to GB / T 1728-2020 "Determination of Drying Time of Paint Film and Putty Film", the prepared coating was naturally dried at 25℃±2℃ and relative humidity 50±10%. The surface drying time and actual drying time were tested using both the finger touch method and the filter paper method. Finger touch method (testing surface drying time): The coating was applied to a tinplate to form a film of 40±5 μm. After a period of time, the surface of the film was lightly touched with a finger. If it felt slightly sticky, but no paint or putty adhered to the finger, the surface was considered dry, and this time was recorded as the surface drying time. Filter paper method (testing actual drying time): The coating was applied to a tinplate to form a film of 40±5 μm. After a period of time (recording this time), a piece of qualitative filter paper was placed on the film, with the smooth side of the filter paper in contact with the film. A drying time tester was then gently placed on the qualitative filter paper, and a stopwatch was started simultaneously. After 30 seconds, the drying time tester was removed. Turn the test plate over so that the coating is facing down. The qualitative filter paper should fall freely. If the qualitative filter paper does not fall freely, tap it a few times on the back with the index finger of the hand holding the plate. If the qualitative filter paper falls freely and the filter paper fibers are not stuck to the paint film, the paint film is considered to be actually dry. The recorded drying time is the actual drying time.
[0163] Example 1
[0164] The component formulation for preparing the electronic protective coating in this embodiment is shown in Table 1 below: Table 1: Component formulation of the electronic protective coating in Example 1
[0165] This embodiment uses the following method to prepare electronic protective coating: (1) Add 550 g of waterborne acrylic resin to a mixing container, add 235 g of water while stirring at 300 rpm, stir for 5 min, and mix evenly; (2) First, prepare the complex of volatile inhibitor and moisture-responsive component: weigh 50 g KH-560 and 20 g triethylamine, add them to a sealed container, turn on the stirrer, turn on the stirrer at 350 rpm, stir and mix at room temperature 25℃ for 10 min, until the system is a transparent and homogeneous liquid, and the complex of volatile inhibitor and moisture-responsive component is obtained. Add the complex of volatile inhibitor and moisture-responsive component, 50 g ethanol, 40 g dipropylene glycol butyl ether, and 3 g BYK-346 to the container in step (1) in sequence under stirring. Stir at 350 rpm for 5 min until all components are evenly dispersed to obtain a dispersion. (3) Dilute 5 g of thickener with 45 g of water (the weight ratio of water to thickener is 9:1), slowly add it dropwise to the dispersion in step (2) while stirring at 600 rpm, adjust the viscosity and convert it to a flow time of 35 s (ISO-3 flow cup, test temperature 25℃), and stir for 30 min. (4) Adjust the speed to 300 rpm, add 2 g of defoamer, and stir for 5 min; (5) Let it stand to defoam and filter it with a filter screen.
[0166] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this embodiment were tested using the methods described above.
[0167] The results showed that after the electronic protective coating of this embodiment was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 3%. The viscosity v0 at the beginning of storage was 11.6 Pa·S, and the viscosity v1 after 6 months of storage was 11.9 Pa·S.
[0168] An electronic protective coating was prepared using the electronic protective coating material of this embodiment, which had been stored for 6 months. The electronic protective material was applied to a clean tinplate surface using a spraying method, with the dry film thickness controlled at 45 μm. The coating was allowed to dry naturally at room temperature (25℃±2℃, relative humidity 50±10%). The drying time of the coating was: surface drying time 7 min, and complete drying time 25 min. Microcracks caused by rapid drying were observed on the coating surface using a magnifying glass.
[0169] After moisture healing treatment, the original microcracks healed and disappeared.
[0170] In the irreversibility verification, after the coating was left to stand in a dry environment (25°C, relative humidity ≤ 30%) for 48 h, no microcracks were observed to reappear, and the coating maintained its healed, dense state. These results indicate that the microcrack healing of the coating in this embodiment is achieved through irreversible chemical bonding.
[0171] VOCs test of coating: VOCs content is 32 g / L.
[0172] The specific test items and test results for the protective performance are shown in Table 2.
[0173] Table 2
[0174] The results in Table 2 show that after immersion in water for 24 hours, the protective performance of the coating was significantly improved compared to that of the quick-drying unhealed coating, and the overall protective performance met the standard, indicating that the density of the coating was greatly improved after immersion in water.
[0175] Example 2
[0176] The formulation and preparation method of the electronic protective coating in this embodiment are the same as those in Example 1, except that the dry film thickness prepared in this embodiment is 60 μm.
[0177] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this embodiment were tested using the methods described above.
[0178] The results showed that after the electronic protective coating of this embodiment was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 3%. The viscosity v0 at the beginning of storage was 11.6 Pa·S, and the viscosity v1 after 6 months of storage was 11.9 Pa·S.
[0179] An electronic protective coating was prepared using the electronic protective coating of this embodiment that had been stored for 6 months, with the dry film thickness controlled at 60 μm. The drying time of the coating was: surface drying time 8 min, and complete drying time 26 min. Microcracks caused by rapid drying were visible on the coating surface when observed with a magnifying glass.
[0180] After the moisture healing treatment, the original microcracks basically disappeared.
[0181] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, no microcracks were observed to reappear, and the coating maintained its healed, dense state. These results indicate that the microcrack healing of the coating in this embodiment is achieved through irreversible chemical bonding. A dry film thickness of 60 μm can achieve rapid drying and self-healing effects.
[0182] VOCs test of coating: VOCs content is 32 g / L.
[0183] The protective performance test results of the electronic protective coating prepared in Example 2 are summarized in Table 3.
[0184] Table 3
[0185] The results in Table 3 show that after immersion in water for 24 hours, the protective performance of the coating was significantly improved compared to that of the quick-drying unhealed coating, and the overall protective performance met the standard, indicating that the density of the coating was greatly improved after immersion in water.
[0186] Example 3
[0187] The preparation method of this embodiment is the same as that of the electronic protective coating in Example 1. The difference between the two is that the composition of the electronic protective coating is different. Specifically, the silane coupling agent (5 parts) in Example 1 is replaced with polycarbodiimide (Carbodilite V-02, 5 parts), while the other components and their amounts remain unchanged.
[0188] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this embodiment were tested using the methods described above.
[0189] The results showed that after the electronic protective coating of this embodiment was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 8%. The viscosity v0 at the beginning of storage was 11.3 Pa·S, and the viscosity v1 after 6 months of storage was 12.2 Pa·S.
[0190] An electronic protective coating was prepared using the electronic protective coating of this embodiment that had been stored for 6 months, with the dry film thickness controlled at 45 μm. The drying time of the coating was: surface drying time 8 min, and complete drying time 27 min. Microcracks caused by rapid drying were observed on the coating surface using a magnifying glass.
[0191] After the moisture healing treatment, the original microcracks basically disappeared.
[0192] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, no microcracks were observed to reappear, and the coating maintained its healed, dense state. These results indicate that the microcrack healing of the coating in this embodiment is achieved through irreversible chemical bonding. Using polycarbodiimide as a moisture-responsive component enables stable storage of the coating, rapid drying, and self-healing effects.
[0193] VOCs test of coating: VOCs content is 33 g / L.
[0194] The protective performance test results of the electronic protective coating prepared in Example 3 are summarized in Table 4.
[0195] Table 4
[0196] The results in Table 4 show that after immersion in water for 24 hours, the protective performance of the coating was significantly improved compared to that of the quick-drying unhealed coating, and the overall protective performance met the standard, indicating that the density of the coating was greatly improved after immersion in water.
[0197] Example 4
[0198] The preparation method of this embodiment is the same as that of the electronic protective coating in Example 1. The difference between the two is that the composition of the electronic protective coating is different. Specifically, the volatile inhibitor triethylamine (2 parts) in Example 1 is replaced with dimethylethanolamine (2 parts), while the other components and their amounts remain unchanged.
[0199] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this embodiment were tested using the methods described above.
[0200] The results showed that after the electronic protective coating of this embodiment was sealed and stored in an environment with a temperature of 25°C for 6 months, the product did not have any layering or sedimentation. The viscosity change rate was 6%. The viscosity v0 at the beginning of storage was 11.8 Pa·S, and the viscosity v1 after 6 months of storage was 12.5 Pa·S.
[0201] An electronic protective coating was prepared using the electronic protective coating of this embodiment that had been stored for 6 months, with the dry film thickness controlled at 45 μm. The drying time of the coating was: surface drying time 7 min, and complete drying time 26 min. Microcracks caused by rapid drying were observed on the coating surface using a magnifying glass.
[0202] After the moisture healing treatment, the original microcracks basically disappeared.
[0203] In the irreversibility verification, after the coating was left to stand in a dry environment (25°C, relative humidity ≤ 30%) for 48 hours, no microcracks were observed to reappear, and the coating maintained its healed, dense state. These results indicate that the microcrack healing of the coating in this embodiment is achieved through irreversible chemical bonding. Using triethylamine as a volatility inhibitor can achieve stable storage of the coating, rapid drying, and self-healing effects.
[0204] VOCs test of coating: VOCs content is 35 g / L.
[0205] The protective performance test results of the electronic protective coating prepared in Example 4 are summarized in Table 5.
[0206] Table 5
[0207] The electronic protective coating prepared in Example 4 exhibits properties comparable to those in Example 1, indicating that dimethylethanolamine also effectively inhibits the activity of moisture-responsive components and is activated by volatilization after spraying. Furthermore, after immersion in water for 24 hours to heal, the coating's protective performance is significantly improved compared to the quick-drying, unhealed coating, achieving the required overall protective performance. This demonstrates that immersion in water greatly improves the coating's density.
[0208] Example 5
[0209] The preparation method of the electronic protective coating in this embodiment is the same as that in Example 1. The difference between the two is that the formulation of the electronic protective coating components is different. Specifically, the silane coupling agent KH-560 (5 parts) in Example 1 is replaced with ethylene glycol diglycidyl ether (5 parts), and the triethylamine (2 parts) is replaced with acetic acid (2 parts). The remaining components and their amounts remain unchanged.
[0210] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this embodiment were tested using the methods described above.
[0211] The results showed that after the electronic protective coating of this embodiment was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 6%. The viscosity v0 at the beginning of storage was 11.1 Pa·S, and the viscosity v1 after 6 months of storage was 11.8 Pa·S.
[0212] An electronic protective coating was prepared using the electronic protective coating of this embodiment that had been stored for 6 months, with the dry film thickness controlled at 45 μm. The drying time of the coating was: surface drying time 9 min, and complete drying time 30 min. Microcracks caused by rapid drying were observed on the coating surface using a magnifying glass.
[0213] After the moisture healing treatment, the original microcracks basically disappeared.
[0214] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, no microcracks were observed to reappear, and the coating maintained its healed, dense state. These results indicate that the microcrack healing of the coating in this embodiment is achieved through irreversible chemical bonding. Using ethylene glycol diglycidyl ether as a moisture-responsive component enables stable storage of the coating, rapid drying, and self-healing effects.
[0215] VOCs test of coating: VOCs content is 35 g / L.
[0216] The protective performance test results of the electronic protective coating prepared in Example 5 are summarized in Table 6.
[0217] Table 6
[0218] Comparative Example 1
[0219] The preparation method of this comparative example is the same as that of the electronic protective coating in Example 1. The difference between the two is that the formulation of the electronic protective coating components is different. Specifically, the volatile inhibitor triethylamine (2 parts) in Example 1 is not added, the deionized water is adjusted to 30 parts, and the other components and their amounts remain unchanged.
[0220] The electronic protective coating prepared in this comparative example was sealed and stored. The results showed that a small amount of gel and precipitation occurred after 3 days, rendering it unusable. This indicates that without inhibitors, the moisture-responsive components undergo pre-reaction during liquid storage, leading to system instability.
[0221] Comparative Example 2
[0222] The preparation method of this comparative example is the same as that of the electronic protective coating in Example 1. The difference between the two is that the composition of the electronic protective coating is different. Specifically, the silane coupling agent in Example 1 is not added, the deionized water is adjusted to 33 parts, and the other components and their amounts remain unchanged.
[0223] The storage stability, surface drying time, actual drying time, and healing effect of the electronic protective coating prepared in this comparative example were tested using the methods described above.
[0224] The results showed that after the electronic protective coating of this comparative example was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 3%. The viscosity v0 at the beginning of storage was 11.5 Pa·S, and the viscosity v1 after 6 months of storage was 11.8 Pa·S.
[0225] An electronic protective coating was prepared using the electronic protective coating of this comparative example that had been stored for 6 months, with the dry film thickness controlled at 45 μm. The drying time of the coating was: surface drying time 7 min, and complete drying time 25 min. Microcracks caused by rapid drying were observed on the coating surface using a magnifying glass.
[0226] After moisture healing treatment, the microcracks showed no significant change or signs of healing, indicating that the coating cannot achieve self-repair of microcracks without moisture-responsive components. Furthermore, irreversibility verification experiments and protective performance tests could not be conducted.
[0227] VOCs test of coating: VOCs content is 30 g / L.
[0228] Comparative Example 3
[0229] The preparation method of this comparative example is the same as that of the electronic protective coating in Example 1. The difference between the two is that the composition of the electronic protective coating is different. Specifically, the fast-drying agent ethanol in Example 1 is not added, the amount of deionized water is adjusted to 33 parts, and the other components and their amounts remain unchanged.
[0230] The storage stability, surface drying time, and actual drying time of the electronic protective coating prepared in this embodiment were tested using the method described above.
[0231] The results showed that after the electronic protective coating of this comparative example was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 4%. The viscosity v0 at the beginning of storage was 11.7 Pa·S, and the viscosity v1 after 6 months of storage was 12.2 Pa·S.
[0232] VOCs test of coating: VOCs content is 20 g / L.
[0233] Observation of the surface of the electronic protective coating prepared in Comparative Example 3 revealed no obvious microcracks. This is because the slow drying process eliminates internal stress in the coating. However, the excessively slow drying speed (surface drying time 22 min, actual drying time 2 h) cannot meet the requirements for efficient production. Moisture healing effect and irreversibility verification tests were not conducted. The above results indicate that fast-drying agents are key to achieving rapid drying, but rapid drying can lead to microcrack problems, which need to be addressed in conjunction with the moisture healing mechanism of this invention.
[0234] Comparative Example 4
[0235] The comparative example has the same component formulation and preparation method as the electronic protective coating in Example 1. The difference is that the dry film thickness in this comparative example is controlled to be 10 μm.
[0236] The storage stability, surface drying time, actual drying time, healing effect, and protective performance of the electronic protective coating prepared in this comparative example were tested using the methods described above.
[0237] The results showed that after the electronic protective coating of this comparative example was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 3%. The viscosity v0 at the beginning of storage was 11.6 Pa·S, and the viscosity v1 after 6 months of storage was 11.9 Pa·S.
[0238] An electronic protective coating was prepared using the electronic protective coating of this comparative example that had been stored for 6 months, with the dry film thickness controlled at 10 μm. The drying time of the coating was: surface dry time 2 min, and complete dry time 9 min. Due to the thin coating and rapid drying, fewer microcracks appeared on the surface of the coating after quick drying.
[0239] After moisture healing treatment, the original microcracks did not completely disappear, and the healing effect was lower than that in Example 1.
[0240] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, no microcracks were observed to reappear, and the coating remained in the healed state.
[0241] VOCs test of coating: VOCs content is 32 g / L.
[0242] The protective performance test results of the electronic protective coating prepared in Comparative Example 4 are summarized in Table 7.
[0243] Table 7
[0244] The electronic protective coating prepared in Comparative Example 4 showed fewer microcracks after quick-drying compared to that in Example 1. This is because the coating in Comparative Example 4 was thinner, resulting in lower internal stress. However, blistering appeared after only 48 hours of initial salt spray resistance after quick-drying; the healing rate also decreased significantly after 24 hours of immersion in water, with no blistering observed after only 72 hours of healing, a breakdown strength of 56.4 kV / mm, and a water absorption rate of 1.2%. This indicates that when the coating thickness is too thin, the total amount of repair material is insufficient, and the protective performance is substandard.
[0245] Comparative Example 5
[0246] The comparative example has the same component formulation and preparation method as the electronic protective coating in Example 1. The difference is that the dry film thickness in this comparative example is controlled to be 150 μm.
[0247] The storage stability, surface drying time, actual drying time, and healing effect of the electronic protective coating prepared in this comparative example were tested using the methods described above.
[0248] The results showed that after the electronic protective coating of this comparative example was sealed and stored in an environment at 25°C for 6 months, the product did not show any stratification or sedimentation, and the viscosity change rate was 3%. The viscosity v0 at the beginning of storage was 11.6 Pa·S, and the viscosity v1 after 6 months of storage was 11.9 Pa·S.
[0249] An electronic protective coating was prepared using the electronic protective coating of this comparative example that had been stored for 6 months, with the dry film thickness controlled at 150 μm. The drying time of the coating was: surface dry time 15 min, and complete dry time 50 min. Due to the thicker coating, the drying was slow, and the density of microcracks on the coating surface after drying was significantly increased compared to Example 1.
[0250] After the moisture healing treatment, the degree of healing of the original microcracks decreased compared with Example 1, and a small number of cracks appeared at the edge of the coating.
[0251] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, the coating maintained the state after the moisture healing treatment.
[0252] VOCs test of coating: VOCs content is 32 g / L.
[0253] The above results indicate that the dry film thickness of the coating prepared in this comparative example is too thick, thus extending the surface drying time of the coating to 15 min, significantly increasing the microcrack density, and reducing the degree of healing after immersion in water for 24 h. This suggests that excessive thickness increases internal stress and reduces repair efficiency.
[0254] Comparative Example 6
[0255] The comparative example has the same component formulation as the electronic protective coating in Example 1. The difference is that in step (2) of preparing the electronic protective coating in this comparative example, the volatile inhibitor, moisture-responsive component, fast-drying agent, film-forming agent, and wetting agent are added sequentially under stirring until all components are evenly dispersed to obtain a dispersion. That is, step (2) does not require the volatile inhibitor and moisture-responsive component to be pre-mixed to form a complex.
[0256] The storage stability, surface drying time, actual drying time, and healing effect of the electronic protective coating prepared in this comparative example were tested using the methods described above.
[0257] The results showed that after the electronic protective coating of this comparative example was sealed and stored in an environment at 25°C for 6 months, the product showed almost no stratification or sedimentation, and the viscosity change rate was 10%. The viscosity v0 at the beginning of storage was 11.6 Pa·S, and the viscosity v1 after 6 months of storage was 12.8 Pa·S.
[0258] An electronic protective coating was prepared using the electronic protective coating of this comparative example that had been stored for 6 months, with the dry film thickness controlled at 45 μm. The drying time of the coating was: surface dry time 7 min, and complete dry time 25 min. Microcracks appeared on the surface of the coating after rapid drying.
[0259] After moisture healing treatment, the original microcracks did not completely disappear, and the healing effect was lower than that in Example 1.
[0260] In the irreversibility verification, after the coating was left to stand in a dry environment (25℃, relative humidity ≤ 30%) for 48 hours, the coating maintained the state after the moisture healing treatment.
[0261] VOCs test of coating: VOCs content is 32 g / L.
[0262] The above results show that although the electronic protective coating prepared in this comparative example has similar fast-drying effect and microcrack formation as in Example 1, its crack healing effect after immersion in water is not as good as that in Example 1. This may be because this comparative example adds volatile inhibitors and moisture-responsive components, rather than a complex of inhibitors and moisture-responsive components. Therefore, the moisture-responsive components are released prematurely, resulting in a poor inhibitory effect. Consequently, the viscosity change rate of the electronic protective coating in this comparative example after storage at 25℃±0.5℃ for 6 months is 10%, which is much higher than the viscosity change rate of 3% in Example 1.
[0263] Based on the analysis of the above embodiments and comparative examples, the inventiveness of this invention compared to the prior art is reflected in the following three aspects: First, this invention proposes for the first time a time-series control mechanism of "pre-compounding of inhibitors and moisture-responsive components—evaporation activation after spraying—moisture-triggered irreversible healing." Comparative Example 1 uses a coating system without volatile inhibitors, and its coating performance proves that volatile inhibitors are indispensable; Comparative Example 6 proves that pre-mixing volatile inhibitors and moisture-responsive components has a better inhibitory effect than adding them separately; Examples 1 and 4 prove that different types of volatile inhibitors can achieve this function.
[0264] Second, this invention applies moisture-responsive components to the targeted healing of microcracks in coatings of quick-drying waterborne acrylic systems. The experimental results of Comparative Example 2 show that the coating has no healing ability without moisture-responsive components; Examples 1 and 3 show that this invention can achieve irreversible chemical healing using different types of moisture-responsive components, and the dried microcracks do not reappear after healing, which is different from the reversible physical swelling healing mechanism.
[0265] Third, this invention successfully resolves the contradiction between "quick drying" and "self-healing" in water-based acrylic coatings. Comparative Example 3 demonstrates that while there are no microcracks without the quick-drying agent, the drying efficiency is low; Example 1 demonstrates that although microcracks are generated after adding the quick-drying agent, they can be repaired through a moisture healing mechanism. Meanwhile, the results of Comparative Examples 4 and 5 show that the formation of microcracks and the coating healing effect are both poor in excessively thin or thick coatings, proving that the optimal thickness range for achieving the best synergistic effect of this invention is 30–100 μm. The results of Comparative Example 6 show that the composite of volatile inhibitors and moisture-responsive components used in this invention has better effects than directly using volatile inhibitors and moisture-responsive components. This invention optimizes the coating effect and preparation process compared to existing technologies.
[0266] In summary, this invention achieves simultaneous storage stability (no precipitation for 6 months), rapid drying (surface drying time ≤ 10 minutes), moisture healing (heals after 24 hours of immersion in water, irreversible microcracks), and excellent protective performance (breakdown strength ≥ 89 kV / mm, water absorption ≤ 0.7%, salt spray resistance ≥ 500 hours without blistering) within a thickness range of 30–100 μm through a synergistic combination of a volatile inhibitor, a moisture-responsive component, and a fast-drying agent, along with an optimized process of pre-compounding the inhibitor and moisture-responsive component.
Claims
1. An electronic protective coating, characterized in that, By weight, electronic protective coatings contain the following components: 40-70 parts waterborne acrylic resin, 1-10 parts moisture-responsive component, 0.5-5 parts volatile inhibitor, 2-10 parts quick-drying agent, 2-8 parts film-forming agent, 0.1-1 part wetting agent, 0.2-1 part thickener, 0.1-0.5 parts defoamer, and 7-50 parts water.
2. The electronic protective coating according to claim 1, characterized in that, By weight, it contains the following components: 50-65 parts waterborne acrylic resin, 3-7 parts moisture-responsive component, 1-3 parts volatile inhibitor, 3-8 parts quick-drying agent, 3-6 parts film-forming agent, 0.2-0.5 parts wetting agent, 0.3-0.6 parts thickener, 0.1-0.3 parts defoamer, and 11-30 parts water.
3. The electronic protective coating according to claim 1 or 2, characterized in that, The electronic protective coating has one or more of the following characteristics: The aqueous acrylic resin is an acrylate copolymer containing carboxyl groups and / or hydroxyl side groups; The acid value of the aqueous acrylic resin is 8-30 mg KOH / g, and / or the hydroxyl value is 10-50 mg KOH / g; The number-average molecular weight Mn of the waterborne acrylic resin is 2000-15000 g / mol, and / or the weight-average molecular weight Mw is 8000-80000 g / mol. The moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide, and epoxy compounds; the silane coupling agent is γ-glycidyl etheroxypropyltrimethoxysilane; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester. The volatile inhibitor is selected from one or more of volatile organic amines and volatile organic acids; the volatile organic amine is selected from triethylamine and / or dimethylethanolamine; the volatile organic acid is acetic acid; The fast-drying agent is selected from one or more of alcohols and first ether alcohol solvents; the alcohol is selected from ethanol and / or isopropanol; the first ether alcohol is propylene glycol methyl ether; The film-forming aid is selected from one or more of the second alcohol ether solvents; the second alcohol ether is selected from dipropylene glycol butyl ether and / or dipropylene glycol methyl ether; The wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; the polyether-modified polysiloxane is BYK-346; the acetylenic diol is Surfynol 104. The thickener is selected from one or more of polyurethane associative and alkali-swellable thickeners; the polyurethane associative thickener is RM-8W, and the alkali-swellable thickener is ASE-60; The defoamer is selected from one or more of silicone-based and mineral oil-based defoamers; the silicone-based defoamer is BYK-024, and the mineral oil-based defoamer is Drewplus L-475; The water is deionized water; The electronic protective coating, when sealed and stored at 25°C for 6 months, showed no stratification, no sedimentation, no gelation, and a viscosity change rate of 0%-10%.
4. A method for preparing the electronic protective coating as described in any one of claims 1-3, characterized in that, The method includes the following steps: (1) Add water-based acrylic resin to a mixing container, add water while stirring, and mix well; (2) Add the complex of volatile inhibitor and moisture-responsive component, quick-drying agent, film-forming agent and wetting agent in sequence under stirring, and stir until uniformly dispersed to obtain a dispersion; (3) Dilute the thickener with water and slowly add it dropwise to the dispersion in step (2) while stirring to adjust the viscosity; (4) Stir and add defoamer; (5) Let it stand to defoam and filter it with a filter screen.
5. The method as described in claim 4, characterized in that, The method includes one or more of the following features: In step (1), the waterborne acrylic resin is 40-70 parts by weight; the waterborne acrylic resin is an acrylate copolymer containing carboxyl or hydroxyl reactive side groups. In step (1), the stirring speed is 200-400 rpm and the stirring time is 3-10 min; In step (1), the weight of water added is 6-40 parts; In step (2), the complex of volatile inhibitor and moisture-responsive component is a complex formed by pre-mixing volatile inhibitor and moisture-responsive component; In step (2), the preparation method of the complex of volatile inhibitor and moisture-responsive component is as follows: by weight, the moisture-responsive component and the volatile inhibitor are added to a sealed container at a mass ratio of 1:(0.3-0.8), and stirred at 300-500 rpm for 10-20 min at room temperature until the system is a transparent and homogeneous liquid, thus obtaining the complex of volatile inhibitor and moisture-responsive component; In step (2), the volatile inhibitor is 0.5-5 parts by weight; the volatile inhibitor is selected from one or more of volatile organic amines and volatile organic acids, the volatile organic amine is selected from triethylamine and / or dimethylethanolamine, and the volatile organic acid is acetic acid; In step (2), the moisture-responsive component is 1-10 parts by weight; the moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide and epoxy compounds; the silane coupling agent is γ-glycidyl etheroxypropyltrimethoxysilane; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether and neopentanoic acid glycidyl ester; In step (2), the stirring time is 5-15 min until the mixture is evenly dispersed, and the stirring speed is 200-400 rpm; In step (2), the weight of the quick-drying agent is 2-10 parts; In step (2), the fast-drying agent is selected from one or more of alcohols and first ether alcohol solvents; the alcohols are selected from ethanol and / or isopropanol, and the first ether alcohol is propylene glycol methyl ether; In step (2), the film-forming aid is 2-8 parts by weight; In step (2), the film-forming aid is selected from one or more of the second alcohol ether solvents; the second alcohol ether is dipropylene glycol butyl ether and / or dipropylene glycol methyl ether; In step (2), the wetting agent is 0.1-1 parts by weight; In step (2), the wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; the polyether-modified polysiloxane is BYK-346, and the acetylenic diol is Surfynol 104; In step (3), the weight ratio of water to thickener is 9:1; In step (3), the thickener is 0.2-1 parts by weight; In step (3), the thickener is selected from one or more of polyurethane associative and alkali-swellable thickeners; the polyurethane associative thickener is RM-8W, and the alkali-swellable thickener is ASE-60; In step (3), the water used to dilute the thickener is 1.8-9 parts by weight; In step (3), the stirring speed is 500-800 rpm, and the stirring time is 10-15 min; In step (3), adjust the viscosity to be such that when tested at 25°C and using an ISO-3 flow cup, the time for the entire cup of liquid to flow out is 30-60 s. In step (4), the defoamer is 0.1-0.5 parts by weight; the defoamer is selected from one or more of silicone and mineral oil defoamers; the silicone defoamer is BYK-024 and the mineral oil defoamer is Drewplus L-475. In step (4), the stirring speed is 200-400 rpm and the stirring time is 5-10 min; In step (5), the filter screen is 200 mesh, and the filtered material is sealed and packaged.
6. An electronic protective coating, characterized in that, By weight, the electronic protective coating contains the following components: 50-65 parts of water-based acrylic resin, 3-7 parts of moisture-responsive component, 3-6 parts of film-forming aid, 0.2-0.5 parts of wetting agent, 0.3-0.6 parts of thickener, and 0.1-0.3 parts of defoamer.
7. The electronic protective coating according to claim 6, characterized in that, The electronic protective coating has one or more of the following characteristics: The moisture-responsive component is selected from one or more of silane coupling agents, polycarbodiimide, and epoxy compounds; the silane coupling agent is γ-glycidyl etheroxypropyltrimethoxysilane; the epoxy compound is selected from one or more of ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, propylene glycol diglycidyl ether, and neopentanoic acid glycidyl ester. The film-forming aid is selected from one or more of the second alcohol ether solvents; the second alcohol ether is selected from dipropylene glycol butyl ether (DPnB) and / or dipropylene glycol methyl ether (DPM). The wetting agent is selected from one or more of polyether-modified polysiloxanes and acetylenic diols; the polyether-modified polysiloxane is BYK-346; the acetylenic diol is Surfynol 104. The thickener is selected from one or more of polyurethane associative (HEUR) and alkali-swellable (ASE / HASE) thickeners; the polyurethane associative thickener is RM-8W, and the alkali-swellable thickener is ASE-60. The defoamer is selected from one or more of silicone-based and mineral oil-based defoamers; the silicone-based defoamer is BYK-024, and the mineral oil-based defoamer is Drewplus L-475; The dry film thickness of the electronic protective coating is 30-100 μm; The surface drying time of the electronic protective coating is 2-10 min; The drying time of the electronic protective coating is 20-30 minutes; The moisture healing of the electronic protective coating means that after the electronic protective coating is completely immersed in water for 24 hours, the immersed coating remains in a healed state, and the microcracks are irreversible. The VOCs content of the electronic protective coating is ≤ 50 g / L; The water absorption rate of the electronic protective coating after immersion in water for 24 hours is ≤ 0.7%; The breakdown strength of the electronic protective coating after immersion in water for 24 hours is ≥ 89 kV / mm; The electronic protective coating, after immersion in water for 24 hours, exhibits salt spray resistance ≥ 500 hours without blistering; The electronic protective coating is prepared using any one of the electronic protective coatings according to claims 1-3.
8. A method for preparing the electronic protective coating as described in claim 6 or 7, characterized in that, The method involves applying the electronic protective coating as described in any one of claims 1-3 or the electronic protective coating prepared by the method described in claim 4 or 5 using one of the conventional methods of spraying, dipping, brushing, or selective coating, and then drying it to form the electronic protective coating.
9. The method as described in claim 8, characterized in that, The method includes: applying the electronic protective coating of any one of claims 1-3 or the electronic protective coating prepared by the method of claim 4 or 5 to the surface of a clean tinplate or PCB board using a spraying method, and controlling the dry film thickness to be 30-100 μm.
10. An electronic product, characterized in that, It includes a substrate and an electronic protective coating as described in claim 6 or 7 located on the surface of the substrate, or an electronic protective coating obtained by the preparation method described in claim 8 or 9.