A coating for preventing crude oil adhesion and paraffin deposition and a preparation method thereof

The coating, which combines modified mesoporous silica with epoxy resin, solves the problems of preventing crude oil adhesion, wax deposition, and inorganic scaling, achieving a balance between durability and overall performance in water-containing crude oil environments.

CN123131900APending Publication Date: 2026-11-20CHENGDU HONRE PAINT MAKING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611449345.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously prevent crude oil adhesion, wax deposition, and inorganic scaling within the same coating system. Furthermore, traditional methods suffer from high energy consumption, environmentally unfriendly chemical additives, and insufficient durability.

Method used

A coating composed of bisphenol A type epoxy resin, hydroxyl-terminated polydimethylsiloxane, scale inhibitor-supported zwitterionic silanized mesoporous silica, and polyamide amine epoxy curing agent is formed through the modification treatment of mesoporous silica and interfacial bonding, resulting in a coating with low adhesion and scale inhibition properties.

Benefits of technology

It achieves the reduction of crude oil, asphaltene, and wax crystal adhesion under water-containing crude oil conditions, prevents inorganic scale deposition, and maintains the coating's durability and overall performance balance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application discloses a kind of anti crude oil adhesion anti wax scale coating and preparation method thereof, belong to anti wax scale coating technical field.The specific disclosure is a kind of anti crude oil adhesion anti wax scale coating, by weight parts, including the following components: bisphenol A type epoxy resin 45-70 parts, hydroxyl-terminated polydimethylsiloxane 18-38 parts, scale inhibitor loaded zwitterionic silanized mesoporous silica 4-14 parts, polyamide amine epoxy curing agent 18-30 parts, methyltrimethoxysilane 2-8 parts, methyl silicone oil 2-6 parts, dispersing agent 0.2-1.2 parts, mixed solvent 20-50 parts.The application is combined with the interface of modified mesoporous silica and epoxy network by reactive silane, while providing adhesion and structural support by epoxy network, providing flexible siloxane segment by hydroxyl-terminated polydimethylsiloxane, so that coating is balanced between crude oil adhesion, anti wax deposition, anti scale and durable adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of anti-wax scaling coatings, specifically, it relates to an anti-crude oil adhesion and anti-wax scaling coating and its preparation method. Background Technology

[0002] During extraction, transportation, storage, and heat exchange, crude oil is often situated in a complex environment involving waxy components, asphaltenes, mineralized water, and metal pipe walls. When the crude oil temperature decreases or the local wall temperature falls below the temperature required for wax precipitation, waxy components easily precipitate from the crude oil and gradually deposit on the inner surface of equipment or pipelines. As the deposit layer thickens, the flow cross-section decreases, flow resistance increases, and the frequency of equipment cleaning increases. In severe cases, it can even affect the continuous operation of the pipeline.

[0003] During crude oil production and transportation, changes in the external environment such as temperature and pressure can reduce the solubility of wax dissolved in crude oil, causing wax to precipitate and deposit on the inner wall of the pipeline. As the thickness of the wax layer increases, the effective flow area of ​​the pipeline decreases and the transportation pressure increases. However, by improving the inner surface characteristics of the pipeline, reducing the roughness of the pipe wall, or reducing the surface energy, wax deposition can be reduced to some extent.

[0004] Existing methods for preventing wax deposition or adhesion typically include heating and tracing, adding chemical wax inhibitors, using low surface energy coatings, and employing oil gels or lubricating interface coatings. Heating or tracing methods consume a lot of energy, and chemical additives may affect crude oil reprocessing and environmental compatibility. Although low surface energy coatings can reduce some oil and wax adhesion, under conditions of water-containing crude oil, mineralized water, long-term scouring, and temperature fluctuations, a simple low surface energy surface is easily affected by oil contamination, wear, or roughening.

[0005] Public information also shows that the Ca in oilfield water 2+ Mg 2+ HCO3 - CO3 2- Plasma can form inorganic scale on the inner surface of equipment; while chelating groups such as EDTA and phosphonic acid scale inhibitors can complex calcium and magnesium ions or affect scale nucleation and growth.

[0006] Furthermore, published studies on wax deposition have shown that surface materials, wettability, heat transfer, and surface temperature profile all affect wax deposition results. If the anti-wax effect is evaluated solely based on contact angle or a single surface energy index, it is difficult to rule out the coupled influence between temperature gradient, heat transfer, and actual deposition amount.

[0007] Therefore, there is still a need for a coating material that can simultaneously prevent crude oil adhesion, wax deposition, inorganic scaling, and durability stability within the same coating system. Summary of the Invention

[0008] To address the deficiencies in the aforementioned technical solutions, the present invention aims to provide an anti-crude oil adhesion and anti-wax scaling coating and its preparation method.

[0009] To achieve the above objectives, the present invention provides an anti-crude oil adhesion and anti-wax scaling coating, wherein the coating is formed by curing a paint comprising the following raw materials; by weight, the paint comprises: 45-70 parts of bisphenol A type epoxy resin, 18-38 parts of hydroxyl-terminated polydimethylsiloxane, 4-14 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 18-30 parts of polyamide amine epoxy curing agent, 2-8 parts of methyltrimethoxysilane, 2-6 parts of methyl silicone oil, 0.2-1.2 parts of dispersant, and 20-50 parts of mixed solvent.

[0010] The bisphenol A type epoxy resin has an epoxy value of 0.44-0.54 mol / 100g; The viscosity of the hydroxyl-terminated polydimethylsiloxane at 25°C is 1500-5000 mPa·s; The viscosity of the methyl silicone oil at 25°C is 50-300 mPa·s; The dispersant is any one of DISPERBYK-163, EFKA-4046, and BYK-2155.

[0011] The mixed solvent is a mixture of two or three of butyl acetate, xylene, and ethanol.

[0012] The scale inhibitor-loaded zwitterionic silanized mesoporous silica is a modified powder obtained by loading mesoporous silica with a scale inhibitor and then silanizing it with zwitterionic silane and reactive silane. Its preparation method includes the following steps: Step 1: After sieving the mesoporous silica, vacuum dry it at 70-90℃ for 4-8 hours, cool it, and then place it in a desiccator for later use. Step 2: Dissolve or disperse the scale inhibitor in a water / ethanol mixture, wherein the volume ratio of water to ethanol in the water / ethanol mixture is 5:5-8:2, and adjust the pH to 7.5-9.0; add the dried mesoporous silica in batches under stirring conditions, ultrasonically disperse for 10-30 min, and stir at 25-45℃ for 6-12 h, while maintaining the pH of the system at 7.5-9.0 during stirring, so that the scale inhibitor can enter the mesoporous silica channels or be adsorbed on the pore walls; Step 3: Remove some of the solvent from the dispersion system obtained in Step 2 under reduced pressure at 35-45℃ to form a flowable slurry, and then let it stand for aging for 6-18 hours; centrifuge or filter the aged slurry, wash it quickly with ethanol / water washing solution until there are no obvious suspended crystals in the washing solution, and dry it under low temperature vacuum to obtain scale inhibitor-supported mesoporous silica. Step 4: Add zwitterionic silane and reactive silane to an ethanol / water mixture, adjust the pH to 4.5-5.5, and pre-hydrolyze for 20-40 min to obtain silane hydrolysate; Step 5: Add the scale inhibitor-loaded mesoporous silica to the silane hydrolysate, first ultrasonically disperse for 10-20 min, then react at 55-75℃ for 4-8 h. After the reaction, centrifuge or filter, wash with ethanol, wash with water, vacuum dry, and grind and sieve to obtain scale inhibitor-loaded zwitterionic silanized mesoporous silica.

[0013] The mesoporous silica has a particle size of 80-300 nm, a pore size of 3-12 nm, and a specific surface area of ​​300-900 m². 2 / g.

[0014] The scale inhibitor is one or a combination of two or more of EDTA, PBTCA, ATMP, and HEDP.

[0015] The scale inhibitor is a combination of EDTA and PBTCA.

[0016] Furthermore, in step 4, the mass ratio of zwitterionic silane to reactive silane is 1:1 to 3:1.

[0017] Furthermore, the zwitterionic silane is a trialkoxysilane containing a sulfonate betaine group; Furthermore, the reactive silane is 3-glycidoxypropyltrimethoxysilane.

[0018] A method for preparing an anti-crude oil adhesion and anti-wax scaling coating is as follows: Bisphenol A type epoxy resin, scale inhibitor-loaded zwitterionic silanized mesoporous silica, dispersant and part of the mixed solvent are added to a dispersion device, dispersed and ground to a fineness of less than 40 μm to obtain an epoxy dispersion; then, hydroxyl-terminated polydimethylsiloxane, methyl silicone oil, methyltrimethoxysilane and the remaining mixed solvent are added to the epoxy dispersion, stirred evenly, and then a polyamide amine epoxy curing agent is added to degas the coating to obtain an anti-crude oil adhesion and anti-wax scaling coating.

[0019] Finally, the anti-crude oil adhesion and anti-wax scaling coating is applied to the surface of the metal substrate that has been degreased, derusted and roughened. After leveling and curing, the anti-crude oil adhesion and anti-wax scaling coating is obtained.

[0020] The beneficial effects of this invention are: 1. This invention introduces a zwitterionic silanized mesoporous silica loaded with a scale inhibitor, enabling the coating interface to maintain its resistance to Ca2+ even after oil and water immersion and rinsing. 2+ Mg 2+The complexation or interference with scale nucleation reduces inorganic scale deposition; and the zwitterionic silane forms an interface layer containing sulfonate betaine groups on the surface of mesoporous silica. This interface layer is conducive to the formation of a hydration interface under conditions of aqueous crude oil or oil-water coexistence. Combined with the low adhesion surface provided by silicone rubber segments and methyl silicone oil, it can reduce the residence and adhesion of crude oil, asphaltene and wax crystals on the coating surface. 2. This invention establishes an interfacial bond between modified mesoporous silica and epoxy network through reactive silane. At the same time, the epoxy network provides adhesion and structural support, while the hydroxyl-terminated polydimethylsiloxane provides flexible siloxane segments, so that the coating achieves a balance between crude oil adhesion, anti-wax deposition, anti-fouling, and durable adhesion. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. The illustrative embodiments and descriptions of this invention are for explanation only and are not intended to limit the invention. Furthermore, regarding numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0022] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0023] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0024] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0025] Unless otherwise specified, the water used in the following examples and comparative examples is deionized water, the ethanol is analytical grade ethanol, and all raw materials used are commercially available general-purpose raw materials. The coating samples used carbon steel sheets as the substrate, with dimensions of 50mm × 50mm × 2mm. Before coating, the substrate surface was degreased, sanded, or sandblasted to roughen it until there were no visible oil stains or loose rust, and the surface roughness Ra of the substrate before coating was controlled to be 2.0-4.0μm.

[0026] Example 1 A coating for preventing crude oil adhesion and wax scaling, comprising, by weight: 60 parts of bisphenol A type epoxy resin, 28 parts of hydroxyl-terminated polydimethylsiloxane, 8 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 24 parts of polyamide amine epoxy curing agent, 4 parts of methyltrimethoxysilane, 4 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0027] The bisphenol A type epoxy resin is a commercially available general-purpose liquid epoxy resin with an epoxy value of 0.44-0.54 mol / 100g.

[0028] The hydroxyl-terminated polydimethylsiloxane has a viscosity of approximately 3000 mPa·s at 25°C.

[0029] The dispersant is BYK-2155.

[0030] The mesoporous silica is a white powder with a particle size of 80-300 nm, a pore size of 3-12 nm, and a specific surface area of ​​300-900 m². 2 / g.

[0031] The scale inhibitor is disodium EDTA and PBTCA in a mass ratio of 2:1.

[0032] The zwitterionic silane is a trialkoxysilane containing a sulfonate betaine group.

[0033] The reactive silane is 3-glycidoxypropyltrimethoxysilane.

[0034] The mixed solvent is composed of butyl acetate, xylene, and ethanol in a mass ratio of 2:2:1.

[0035] The method for preparing the scale inhibitor-supported zwitterionic silanized mesoporous silica is as follows: Step 1: Weigh 10.0g of mesoporous silica, first sieve it lightly with a 200-mesh sieve. If there are soft agglomerates that absorb moisture, grind them gently with an agate mortar and pestle. Then place it in a vacuum drying oven and dry it at 80℃ for 6 hours. After taking it out, immediately place it in a desiccator to cool to room temperature for later use. Step 2: Weigh 1.8g of disodium EDTA and 0.9g of PBTCA, and add them to 120mL of water / ethanol mixture, wherein the volume ratio of water to ethanol in the water / ethanol mixture is 6:4; stir at 400r / min for 20min at 25℃ to fully dissolve the disodium EDTA and uniformly disperse the PBTCA; adjust the pH of the system to 8.0-8.5 with 0.1mol / L NaOH aqueous solution to obtain a clear or slightly turbid scale inhibitor solution; The above scale inhibitor solution was transferred to a 250 mL three-necked flask equipped with a thermometer and a reflux condenser. The dried mesoporous silica was added in three batches with a 3-5 min interval between each batch, while stirring at 400 rpm. During the addition process, a uniform vortex was maintained on the liquid surface, and the powder was not poured in all at once to form a dry powder agglomerate. After addition, the mixture was dispersed using an ultrasonic probe or ultrasonic cleaner for 20 min, with the system temperature controlled not to exceed 40℃ during the ultrasonic process. Subsequently, the mixture was stirred at 500 rpm for 8 h at 35℃. The pH was checked every 2 h during stirring, and maintained at 8.0-8.5 using 0.1 mol / L NaOH aqueous solution or dilute hydrochloric acid, allowing the scale inhibitor to enter the mesoporous silica channels and adsorb onto the pore walls under weakly alkaline conditions. Step 3: After stirring, remove some of the solvent from the system under reduced pressure at 40℃ until the total volume of the system is approximately 45-55mL and still flowable, without drying into lumps; transfer the resulting slurry to a sealed glass bottle and allow it to age at 25℃ for 12 hours to further distribute the scale inhibitor evenly within the pores; after aging, centrifuge at 6000r / min for 8 minutes and discard the supernatant; wash twice quickly with a washing solution of ethanol / water volume ratio of 7:3, using 40mL of washing solution each time, gently shaking and then immediately centrifuging; the washing aims to remove free scale inhibitor from the outer surface, without prolonged immersion; no visible white crystals should appear on the surface of the solid after washing. Subsequently, vacuum dry the obtained solid at 45℃ for 10 hours to obtain scale inhibitor-loaded mesoporous silica; Step 4: Mix 95 mL of anhydrous ethanol and 5 mL of water, and add the mixture to another 250 mL three-necked flask. Adjust the pH to 4.8-5.2 with glacial acetic acid. Under stirring at 300 rpm, add 0.9 g of trialkoxysilane containing sulfonate betaine groups and 0.6 g of 3-glycidyl etheroxypropyltrimethoxysilane dropwise over a period of 5-10 min. After the addition is complete, continue stirring at room temperature for 30 min to pre-hydrolyze the silane to obtain a silane hydrolysate. Step 5: Add the scale inhibitor-loaded mesoporous silica to the silane hydrolysate in batches. After addition, disperse ultrasonically for 15 min, then heat to 65℃ and stir at 500 r / min for 6 h. During the reaction, avoid excessive ethanol evaporation that could cause a rapid increase in the solid content of the system. After the reaction, cool to room temperature and centrifuge at 6000 r / min for 8 min, discarding the supernatant. Wash the obtained solid twice with ethanol and once with deionized water to remove unreacted silane and free small molecules. Dry the washed solid under vacuum at 60℃ for 12 h, cool, grind, and pass through a 200-mesh sieve to obtain the scale inhibitor-loaded zwitterionic silanized mesoporous silica.

[0036] In practice, the pH is maintained at 4.8-5.2 during the pre-hydrolysis process in step 4.

[0037] A method for preparing an anti-crude oil adhesion and anti-wax scaling coating is as follows: Bisphenol A type epoxy resin, scale inhibitor-loaded zwitterionic silanized mesoporous silica, dispersant and 20 parts of mixed solvent are added to a dispersion tank, pre-dispersed at 800 r / min for 10 min, then increased to 1200 r / min for 30 min, and then milled twice with three rollers to obtain an epoxy dispersion with a fineness of less than 30 μm; Hydroxyl-terminated polydimethylsiloxane, methyl silicone oil, methyltrimethoxysilane, and the remaining mixed solvent were added to the epoxy dispersion, and the mixture was stirred at 600 rpm for 20 min. During stirring, the temperature of the liquid was controlled not to exceed 35°C to ensure a uniform mixture of the silicone rubber component and the epoxy dispersion. Subsequently, a polyamide-amine epoxy curing agent was added, and the mixture was stirred at 500 rpm for 10 min, followed by vacuum degassing for 5 min to obtain an anti-oil adhesion and anti-wax scaling coating. Finally, the coating is brushed or sprayed onto the pretreated carbon steel sheet surface, ensuring that the wet film is uniform and continuous, without any exposed substrate, sagging, or obvious bubbles. After coating, the coating is allowed to level at 25°C for 30 minutes and then cured at room temperature to obtain an anti-crude oil adhesion and anti-wax scaling coating.

[0038] Example 2 A coating for preventing crude oil adhesion and wax scaling, comprising, by weight: 62 parts bisphenol A type epoxy resin, 24 parts hydroxyl-terminated polydimethylsiloxane, 5 parts scale inhibitor-supported zwitterionic silanized mesoporous silica, 24 parts polyamide amine epoxy curing agent, 3.5 parts methyltrimethoxysilane, 3 parts methyl silicone oil, 0.8 parts EFKA-4046, and 35 parts mixed solvent. The scale inhibitor is EDTA and ATMP in a mass ratio of 2:1.

[0039] Except for the differences mentioned above, the other components, their amounts, and preparation methods in Example 2 are the same as in Example 1.

[0040] Example 3 A coating for preventing crude oil adhesion and wax scaling, comprising, by weight: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of EFKA-4046, and 35 parts of mixed solvent.

[0041] The scale inhibitor is EDTA and PBTCA in a mass ratio of 3:2.

[0042] Except for the differences mentioned above, the other components, their amounts, and preparation methods in Example 3 are the same as in Example 1.

[0043] Example 4 A coating for preventing crude oil adhesion and wax scaling, comprising, by weight: 56 parts bisphenol A type epoxy resin, 32 parts hydroxyl-terminated polydimethylsiloxane, 12 parts scale inhibitor-supported zwitterionic silanized mesoporous silica, 23 parts polyamide amine epoxy curing agent, 5 parts methyltrimethoxysilane, 5 parts methyl silicone oil, 0.8 parts EFKA-4046, and 38 parts mixed solvent. The scale inhibitor is EDTA and HEDP in a mass ratio of 2:1.

[0044] Except for the differences mentioned above, the other components, their amounts, and preparation methods in Example 4 are the same as in Example 1.

[0045] Example 5 A coating for preventing crude oil adhesion and wax scaling, comprising, by weight: 55 parts bisphenol A type epoxy resin, 34 parts hydroxyl-terminated polydimethylsiloxane, 14 parts scale inhibitor-supported zwitterionic silanized mesoporous silica, 22.5 parts polyamide amine epoxy curing agent, 5.5 parts methyltrimethoxysilane, 6 parts methyl silicone oil, 0.8 parts DISPERBYK-163, and 40 parts mixed solvent. The scale inhibitor is EDTA and PBTCA in a mass ratio of 1:1.

[0046] Except for the differences mentioned above, the other components, their amounts, and preparation methods in Example 5 are the same as in Example 1.

[0047] Comparative Example 1 This comparative example provides a silicone rubber-epoxy coating containing unmodified mesoporous silica. The coating, by weight, comprises: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of unmodified mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0048] The difference between this comparative example and Example 3 is that unmodified mesoporous silica is used instead of scale inhibitor to support zwitterionic silanized mesoporous silica.

[0049] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0050] Comparative Example 2 This comparative example provides a zwitterionic silanized mesoporous silica modified coating without scale inhibitor loading. The coating comprises, by weight, 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of zwitterionic silanized mesoporous silica without scale inhibitor loading, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0051] The difference between this comparative example and Example 3 is that the mesoporous silica only undergoes zwitterionic silanization and reactive silanization, without scale inhibitor loading.

[0052] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0053] Comparative Example 3 This comparative example provides a scale inhibitor-loaded reactive silanized mesoporous silica modified coating, the coating comprising, by weight: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-loaded reactive silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0054] The difference between this comparative example and Example 3 is that no trialkoxysilane containing sulfonate betaine groups is added when preparing the modified mesoporous silica.

[0055] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0056] Comparative Example 4 This comparative example provides a silicone rubber-epoxy coating of a physically mixed scale inhibitor and mesoporous silica. The coating, by weight, comprises: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 8.2 parts of unmodified mesoporous silica, 1.8 parts of a mixed scale inhibitor of EDTA and PBTCA, 23.5 parts of a polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of a dispersant, and 35 parts of a mixed solvent.

[0057] The difference between this comparative example and Example 3 is that the scale inhibitor and mesoporous silica are added by physical mixing, without in-pore loading and bissilane modification.

[0058] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0059] Comparative Example 5 This comparative example provides a modified filler-excess silicone rubber-epoxy coating, the coating comprising, by weight: 52 parts of bisphenol A type epoxy resin, 34 parts of hydroxyl-terminated polydimethylsiloxane, 18 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 22 parts of polyamide amine epoxy curing agent, 5.5 parts of methyltrimethoxysilane, 6 parts of methyl silicone oil, 0.8 parts of dispersant, and 42 parts of mixed solvent.

[0060] This comparative example uses the above-mentioned coating formulation, wherein the amount of scale inhibitor loaded with zwitterionic silanized mesoporous silica is 18 parts, and the amount of the remaining components is determined according to the formulation listed in this comparative example.

[0061] Apart from the above, the other preparation methods in this comparative example are the same as those in Example 3.

[0062] Comparative Example 6 This comparative example provides a silicone rubber-epoxy coating with a low amount of modified filler. The coating, by weight, comprises: 62 parts of bisphenol A type epoxy resin, 28 parts of hydroxyl-terminated polydimethylsiloxane, 2 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 24 parts of polyamide amine epoxy curing agent, 4 parts of methyltrimethoxysilane, 4 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0063] This comparative example uses the above-mentioned coating formulation, wherein the amount of scale inhibitor loaded with zwitterionic silanized mesoporous silica is 2 parts, and the amount of the remaining components is determined according to the formulation listed in this comparative example.

[0064] Apart from the above, the other preparation methods in this comparative example are the same as those in Example 3.

[0065] Comparative Example 7 This comparative example provides a modified filler coating lacking reactive silane interfacial bonding. The coating, by weight, comprises: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0066] The difference between this comparative example and Example 3 is that 3-glycidoxypropyltrimethoxysilane is not added when preparing the scale inhibitor loaded with zwitterionic silanized mesoporous silica; only trialkoxysilane containing sulfonate betaine groups is used for surface treatment.

[0067] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0068] Comparative Example 8 This comparative example provides a silanized pH-biased silicone rubber-epoxy coating, the coating comprising, by weight: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0069] The difference between this comparative example and Example 3 is that the pH was adjusted to 8.5-9.0 when preparing the silane hydrolysate, and the treatment of zwitterionic silane and reactive silane was completed under this pH condition.

[0070] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0071] Comparative Example 9 This comparative example provides a silicone rubber-epoxy coating that omits the concentration aging loading step. The coating, by weight, comprises: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-loaded zwitterionic silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

[0072] The difference between this comparative example and Example 3 is that: when preparing scale inhibitor-loaded mesoporous silica, the scale inhibitor solution and mesoporous silica were stirred for 8 hours and then directly centrifuged, washed and dried, without undergoing 40°C vacuum concentration and 12-hour static aging treatment.

[0073] Apart from the above, the other components, their amounts, and preparation methods in this comparative example are the same as in Example 3.

[0074] Experimental Example 1 Crude oil adhesion and adhesion tests: Crude oil adhesion residue tests and adhesion tests were conducted on the coatings prepared in Examples 1-5 and Comparative Examples 1-9, respectively. The crude oil used for the crude oil adhesion residue test had a wax content of 12.5 wt% and a water content of 20 wt%, and the test temperature was 35℃. The crude oil was uniformly coated onto the coating surface, allowed to stand for 30 min, and then the sample was placed at a 45° angle and rinsed with oilfield water prepared at 35℃ at a flow rate of 200 mL / min for 60 s. After drying the free water on the surface, the crude oil residue per unit area was measured. The slip angle of crude oil was determined by dropping 20 μL of crude oil at 35℃. Adhesion was tested using the pull-off method. The post-durability adhesion was obtained after immersion in a 60℃ oil-water mixture for 7 days and rinsing for 6 hours. The test results are shown in Table 1. Table 1 Experimental Example 2 Cold finger wax prevention and CaCO3 scale prevention tests at the same temperature: Cold finger wax prevention tests were conducted on the coatings prepared in Examples 1-5 and Comparative Examples 1-9, respectively. The wax appearance temperature of the waxy crude oil used in the test was 38°C, the bulk oil phase temperature was 45°C, the surface temperature of the cold finger coating was controlled at 25.0±0.5°C, the test time was 6 hours, and the stirring rate was 200 r / min. After the test, the cold finger was removed, and the amount of wax deposited per unit area was collected and weighed.

[0075] The wax resistance rate was calculated using the following formula: Wax resistance rate = (Wax deposition amount of Comparative Example 1 - Wax deposition amount of Test Sample) / Wax deposition amount of Comparative Example 1 × 100%. In the CaCO3 scale prevention test, equal volumes of 0.05 mol / L CaCl2 solution and 0.05 mol / L NaHCO3 solution were mixed, and the pH was adjusted to 8.3. The coated sample was then immersed in the mixed solution and left to stand at 70℃ for 24 hours. After removing the sample, it was gently washed with water and dried before weighing the amount of CaCO3 deposited per unit area.

[0076] The scale inhibition rate was calculated using the following formula: Scale inhibition rate = (CaCO3 deposition amount of Comparative Example 1 - CaCO3 deposition amount of the test sample) / CaCO3 deposition amount of Comparative Example 1 × 100%; The test results are shown in Table 2: Table 2 Experimental Example 3 Durability retention test: The coatings prepared in Examples 1-5 and Comparative Examples 1-9 were immersed in a mixed medium composed of crude oil and prepared oilfield water at a mass ratio of 7:3 for 7 days at 60°C. After removal, they were rinsed with prepared oilfield water at 300 mL / min for 6 hours, dried, and the crude oil residue, cold finger anti-wax, and CaCO3 anti-scaling tests in Test Examples 1 and 2 were repeated; the test results are shown in Table 3. Table 3 As can be seen from Tables 1 to 3, Examples 1-5 all formed continuous coatings and exhibited a good overall balance in terms of crude oil residue, wax deposition, CaCO3 deposition, adhesion, and durability. The crude oil residue in Example 3 was 2.3 mg / cm³. 2 The crude oil slip angle was 10.8°, and the wax deposition was 6.9 mg / cm³. 2 The CaCO3 deposition rate was 0.20 mg / cm³. 2 The scale inhibition rate is 85.5%, and the scale inhibition rate is still 77.2% after durability, which is a superior implementation method in terms of overall performance.

[0077] The crude oil residue in Comparative Example 1 was 6.1 mg / cm³. 2 The wax deposition amount was 15.2 mg / cm³. 2 The possible reason is that although unmodified mesoporous silica can exist as a filler, its surface has a more obvious tendency to attract oleophilic stains or agglomerate, and it cannot provide a zwitterionic hydration interface or a scale inhibitor in the pores.

[0078] Comparative Example 2, without scale inhibitor loading, had a crude oil residue of 2.9 mg / cm³. 2 The wax deposition amount was 8.1 mg / cm³. 2 It is relatively similar to Example 3; however, its CaCO3 deposition amount is 1.46 mg / cm³. 2 The scale inhibition rate was only -5.8%, and decreased to -1.1% after durability testing. This result indicates that the zwitterionic and silicone rubber interface can improve low adhesion and anti-wax performance, but without the complexing or scale-inhibiting effects of scale inhibitors such as EDTA and PBTCA, it is difficult to effectively inhibit CaCO3 deposition.

[0079] Comparative Example 3 retained the scale inhibitor loading and reactive silanization, thus maintaining a scale inhibition rate of 72.5%, which decreased to 57.0% after durability testing; however, its crude oil residue increased to 5.5 mg / cm³. 2 The crude oil slip angle increased to 28.3°, and the wax deposition increased to 9.0 mg / cm³. 2 The possible reason is that, without zwitterionic silanes containing sulfonate betaine groups, the hydration interface under aqueous crude oil conditions is insufficient, making it easier for asphaltenes and wax crystals to remain and nucleate on the surface.

[0080] Comparative Example 4 directly incorporated scale inhibitors and mesoporous silica into the coating. The initial scale inhibition rate of Comparative Example 4 was 60.1%, indicating that the free scale inhibitor still provided some scale inhibition effect in the initial stage of testing; however, its scale inhibition rate dropped to 32.2% after durability testing, and the adhesion was only 4.2 MPa. The possible reason is that physically mixed scale inhibitors are prone to migration or precipitation during film formation, immersion, and rinsing, and may disrupt the continuity of the coating. Therefore, while the initial data is acceptable, the durability is severely inadequate.

[0081] In Comparative Example 5, after increasing the amount of zwitterionic silanized mesoporous silica loaded with scale inhibitor to 18 parts, the crude oil residue was 5.0 mg / cm³. 2 The wax deposition amount was 13.5 mg / cm³. 2 The scale inhibition rate was 64.5%, but the initial adhesion and post-durability adhesion decreased to 4.3 MPa and 3.3 MPa, respectively. These performance changes may be related to the amount of modified filler and its compatibility with the epoxy resin, siloxane components, and curing agent; higher filler content may increase dispersion difficulty and affect the coating surface condition and interfacial bonding.

[0082] In Comparative Example 6, after reducing the amount of zwitterionic silanized mesoporous silica loaded with scale inhibitor to 2 parts, the crude oil residue increased to 4.8 mg / cm³. 2 The wax deposition level increased to 12.6 mg / cm³. 2 The scale inhibition rate decreased to 34.8%, and after durability testing, the scale inhibition rate was 34.5%. The above performance changes may be related to the amount of modified filler in the formulation and the composition of the resin system. The lower filler content may reduce the corresponding functional sites.

[0083] Comparative Example 7, without the addition of 3-glycidoxypropyltrimethoxysilane, had an initial crude oil residue of 2.7 mg / cm³. 2 The scale inhibition rate was 77.5%, indicating that the zwitterionic interface and scale inhibitor loading still played a role in the initial stage; however, its initial adhesion was only 4.8 MPa, which decreased to 3.2 MPa after durability testing, and the crude oil residue increased to 5.8 mg / cm³ after durability testing. 2 After durability testing, the scale inhibition rate dropped to 42.4%. This may be because the lack of reactive silanes resulted in insufficient interfacial bonding between the modified filler and the epoxy / silicone rubber network, making it more prone to filler migration, interfacial defects, or loss of functional sites after immersion and rinsing.

[0084] Compared to Comparative Example 8, Example 3 controlled the pH of the silane pre-hydrolysis stage at 4.8-5.2, while Comparative Example 8, after silane treatment at pH 8.5-9.0, had a crude oil residue of 4.7 mg / cm³. 2 The wax deposition amount was 12.9 mg / cm³. 2The initial adhesion was 4.9 MPa, the scale inhibition rate was 55.1%, and the scale inhibition rate after durability was 28.2%. The possible reason is that the rapid or uneven hydrolysis and condensation of silane can lead to interparticle bridging and local agglomeration, which weakens the uniformity of the zwitterionic interface and reduces the effective binding of reactive silane to the resin network, ultimately resulting in a simultaneous decrease in anti-adhesion, anti-waxing and durability.

[0085] Compared to Comparative Example 9, Example 3 underwent reduced pressure concentration and static aging during the scale inhibitor loading stage. Comparative Example 9, by omitting this step, had an initial crude oil residue of 3.1 mg / cm³. 2 The wax deposition amount was 8.2 mg / cm³. 2 The results are still similar to those of Example 3; however, the scale inhibition rate is only 47.8%, and after durability testing, the scale inhibition rate further decreases to 24.1%. The possible reason is that when centrifuged, washed, and dried directly after stirring, the scale inhibitor remains more on the outer surface of the particles or in the dispersion, with insufficient distribution in the pores and adsorption on the pore walls. Subsequent washing, soaking, and rinsing can more easily cause the loss of effective components.

[0086] In summary, the results in Tables 1 to 3 corroborate each other, demonstrating that the present invention does not rely on a single low surface energy component to function, but rather achieves anti-crude oil adhesion, anti-wax scaling, and durability maintenance through the synergistic effects of mesoporous loading, zwitterionic interfaces, and reactive silane grafting.

[0087] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A coating for preventing crude oil adhesion and wax scaling, said coating being formed by curing a paint comprising the following raw materials; characterized in that, The coating composition, by weight, is as follows: 45-70 parts of bisphenol A type epoxy resin, 18-38 parts of hydroxyl-terminated polydimethylsiloxane, 4-14 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 18-30 parts of polyamide amine epoxy curing agent, 2-8 parts of methyltrimethoxysilane, 2-6 parts of methyl silicone oil, 0.2-1.2 parts of dispersant, and 20-50 parts of mixed solvent.

2. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The anti-crude oil adhesion and anti-wax scaling coating comprises, by weight: 58 parts of bisphenol A type epoxy resin, 30 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of scale inhibitor-supported zwitterionic silanized mesoporous silica, 23.5 parts of polyamide amine epoxy curing agent, 4.5 parts of methyltrimethoxysilane, 5 parts of methyl silicone oil, 0.8 parts of dispersant, and 35 parts of mixed solvent.

3. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The epoxy value of the bisphenol A type epoxy resin is 0.44-0.54 mol / 100g.

4. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The viscosity of the hydroxyl-terminated polydimethylsiloxane at 25°C is 1500-5000 mPa·s.

5. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The viscosity of the methyl silicone oil at 25°C is 50-300 mPa·s.

6. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The mixed solvent is a mixture of two or three of butyl acetate, xylene, and ethanol.

7. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The scale inhibitor is one or a combination of two or more of EDTA, PBTCA, ATMP, and HEDP.

8. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, The method for preparing the scale inhibitor-supported zwitterionic silanized mesoporous silica includes the following steps: Step 1: After sieving the mesoporous silica, vacuum dry it at 70-90℃ for 4-8 hours, cool it, and then place it in a desiccator for later use. Step 2: Dissolve or disperse the scale inhibitor in a water / ethanol mixture and adjust the pH to 7.5-9.0; add the dried mesoporous silica in batches under stirring, ultrasonically disperse for 10-30 min, and then stir at 25-45℃ for 6-12 h. Step 3: Remove some of the solvent from the dispersion system obtained in Step 2 under reduced pressure at 35-45℃ to form a flowable slurry, and then let it stand for aging for 6-18 hours; centrifuge or filter the aged slurry, wash it quickly with ethanol / water washing solution until there are no obvious suspended crystals in the washing solution, and dry it under low temperature vacuum to obtain scale inhibitor-supported mesoporous silica. Step 4: Add zwitterionic silane and reactive silane to an ethanol / water mixture, adjust the pH to 4.5-5.5, and pre-hydrolyze for 20-40 min to obtain silane hydrolysate; Step 5: Add the scale inhibitor-loaded mesoporous silica to the silane hydrolysate, first ultrasonically disperse for 10-20 min, then react at 55-75℃ for 4-8 h; after the reaction is completed, centrifuge or filter, wash with ethanol, wash with water, vacuum dry and grind and sieve to obtain scale inhibitor-loaded zwitterionic silanized mesoporous silica.

9. The anti-crude oil adhesion and anti-wax scaling coating according to claim 1, characterized in that, In step 4, the mass ratio of zwitterionic silane to reactive silane is 1:1 to 3:

1.

10. A method for preparing an anti-crude oil adhesion and anti-wax scaling coating as described in any one of claims 1 to 9, characterized in that, The preparation method includes the following steps: adding bisphenol A type epoxy resin, scale inhibitor-loaded zwitterionic silanized mesoporous silica, dispersant and part of the mixed solvent into a dispersion device, dispersing and grinding to a fineness of less than 40 μm to obtain an epoxy dispersion; then adding hydroxyl-terminated polydimethylsiloxane, methyl silicone oil, methyltrimethoxysilane and the remaining mixed solvent to the epoxy dispersion, stirring evenly, and then adding a polyamide amine epoxy curing agent to degas and obtain an anti-oil adhesion and anti-wax scaling coating; finally coating the anti-oil adhesion and anti-wax scaling coating onto the surface of a metal substrate that has been degreased, derusted and roughened, leveling and curing to obtain an anti-oil adhesion and anti-wax scaling coating.