A self-healing polymer coating material, lithium metal anode and preparation method

By introducing Schiff base structures and hydrogen bonds into the polymer coating, combined with a strong anchoring mechanism, the problems of microcracks and interface voids in lithium metal anodes during cycling are solved, achieving self-healing and strong adhesion, and significantly improving the cycle stability and safety of lithium metal batteries.

CN123131908APending Publication Date: 2026-11-20HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611228650.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing polymer coatings develop microcracks and interfacial voids during the cycling process of lithium metal anodes due to the volume expansion of lithium metal, leading to intensified interfacial side reactions, loss of protective function, and weak adhesion to the lithium metal interface, making them easy to peel off.

Method used

By introducing Schiff base structures and hydrogen bonds into the polyether backbone, and utilizing the exchange reaction of imine bonds in the Schiff base and the reversible "breakage-formation" of hydrogen bonds, combined with the strong coordination effect of sp² hybrid nitrogen atoms on the lithium crystal surface, a polymer coating with both self-healing and strong anchoring properties is prepared.

Benefits of technology

The self-healing polymer coating achieves rapid and robust self-healing at room temperature, maintaining structural integrity, significantly suppressing interfacial side reactions, improving the cycle stability and safety of lithium metal batteries, and extending battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123131908A_ABST
    Figure CN123131908A_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of lithium battery, and particularly relates to a self-healing polymer coating material, a lithium metal negative electrode and a preparation method. The present application is prepared by the reaction of terminal amino polyether, chain extender and polyaldehyde crosslinking agent to introduce Schiff base structure and hydrogen bond into the polyether main chain, form a polyether amine crosslinked polymer containing dynamic imine bond, and obtain a self-healing polymer coating with strong anchoring and self-healing functions after doping lithium salt. The present application utilizes the exchange reaction of imine bond in Schiff base and the reversible "breakage-formation" of hydrogen bond to realize the self-repair of cracks, and solves the problem that the existing polymer lithium metal coating produces micro-cracks due to the volume expansion of lithium metal in the cycle process, and then loses the protection function. The present application utilizes the strong coordination of Schiff base nitrogen atom to lithium (110) crystal surface to realize the close anchoring to the surface of lithium metal electrode, and significantly inhibits the occurrence of interface side reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium battery technology, specifically relating to a self-healing polymer coating material, a lithium metal anode, and a preparation method thereof. Background Technology

[0002] Lithium metal is known for its extremely high theoretical specific capacity (3860 mAh·g). -1 With its low electrochemical potential (-3.04V vs. SHE), lithium metal anodes are considered ideal anode materials for next-generation high-energy-density rechargeable batteries, showing broad application prospects in electric vehicles, advanced portable electronic devices, and large-scale energy storage systems. However, the practical application of lithium metal anodes has long been limited by their inherently high interfacial reactivity with liquid electrolytes. During battery cycling, lithium metal undergoes dramatic volume expansion and contraction, leading to continuous damage and regeneration of the electrode / electrolyte interface. This results in uncontrolled dendrite growth, accumulation of "dead lithium," excessive electrolyte consumption, and a decrease in coulombic efficiency, ultimately causing rapid capacity decay and serious safety hazards.

[0003] Constructing artificial coatings is one of the effective strategies for stabilizing lithium metal anodes. Among them, polymer-based coating materials, such as polydimethylsiloxane coatings, polyacrylonitrile-based gel coatings, and ethylene-vinyl acetate copolymer coatings, have attracted widespread attention due to their good flexibility, ease of processing, and strong structural tunability. However, existing polymer-based interface layers experience repeated volume changes in lithium metal during actual cycling, leading to the induction of microcracks within the polymer-based coating, such as... Figure 1 As shown in (A), once a crack forms, it directly exposes the fresh lithium metal surface beneath, causing the electrolyte to re-contact with the lithium metal. This induces continuous interfacial side reactions (such as electrolyte reduction and decomposition, and continuous SEI film growth), accelerating the consumption of active lithium and electrolyte, creating a vicious cycle. Furthermore, existing polymer-based artificial interface layers exhibit non-uniform lithium deposition behavior during actual cycling. Due to the non-uniform ion conduction and mechanical stress distribution of the polymer coating, lithium metal preferentially deposits in some areas while peeling off in others, resulting in interfacial voids between the polymer-based coating and the lithium metal. These interfacial voids cause localized peeling and detachment of the polymer-based coating, further damaging its isolation and protective function, causing the coating to gradually lose its protective effect on the lithium metal. These two failure modes exacerbate each other: the formation of microcracks accelerates the non-uniformity of local lithium deposition, promoting the generation of interfacial voids; while the coating peeling caused by interfacial voids further weakens the mechanical integrity of the coating, making microcracks easier to propagate. Ultimately, conventional polymer-based coating materials gradually lose their protective capabilities during long-term cycling, failing to meet the long-life requirements of high-energy-density batteries.

[0004] To address the structural failure of polymer coatings during cycling, researchers have attempted to improve the mechanical strength of polymer coatings by introducing polar groups such as carbon, cyano, and sulfonic acid groups into the polymer chain segments, or by introducing inorganic fillers such as nano-SiO2, nano-Al2O3, and nano-TiO2 to enhance the structural stability of the native interface layer. However, these enhancement strategies typically only improve mechanical strength or impart limited self-healing capabilities, failing to simultaneously achieve the dual functions of autonomous crack repair and dynamic interface anchoring. Furthermore, existing self-healing polymer coatings often rely on external thermal stimulation or added repair agents during preparation, making it difficult to achieve autonomous and efficient crack repair under battery operating conditions.

[0005] Furthermore, the interfacial adsorption between most polymer coatings and lithium metal is weak, relying mainly on van der Waals forces or weak hydrogen bonds to maintain interfacial bonding. Under continuous interfacial stress (caused by changes in the volume of lithium metal), the coating is prone to peeling off from the lithium metal, failing to form a strong dynamic anchor. Summary of the Invention

[0006] In view of the above-mentioned defects or improvement needs of the prior art, the present invention provides a self-healing polymer coating material, a preparation method thereof, and a lithium metal anode.

[0007] This invention involves reacting terminal amino polyethers, chain extenders, and multi-aldehyde crosslinking agents to introduce Schiff base structures and hydrogen bonds into the polyether backbone. After lithium salt doping, a self-healing polymer coating with strong anchoring and self-healing functions is obtained. The self-healing polymer coating of this invention contains Schiff base structures generated by the reaction of terminal amino groups and aldehyde groups, as well as abundant hydrogen bonds. Utilizing the exchange reaction of imine bonds in the Schiff base and the reversible "breakage-formation" of hydrogen bonds, autonomous crack repair is achieved, solving the problem of existing polymer lithium metal coatings developing microcracks during cycling due to lithium metal volume expansion, thus losing their protective function. The self-healing polymer coating of this invention achieves rapid and robust self-healing at room temperature, without external thermal stimulation or additional repair agents. It can dynamically maintain structural integrity under normal battery operating conditions, continuously isolating the electrolyte from fresh lithium metal and significantly suppressing interfacial side reactions.

[0008] This invention utilizes the strong coordination effect of sp² hybrid nitrogen atoms in Schiff bases on the lithium (110) crystal plane to endow the self-healing polymer coating with strong adsorption energy between the coating and lithium metal, thus solving the problem of weak adhesion and easy peeling off of existing polymer coatings at the lithium metal interface.

[0009] This invention alleviates the cracking and detachment of the SEI layer (solid electrolyte interface film) of lithium metal anodes through a dual mechanism of tightly anchoring lithium metal and self-repairing cracks, significantly improving the cycle stability of lithium metal batteries. The lithium metal anode of this invention possesses both intrinsic self-healing capability and strong interface anchoring function, enabling it to autonomously maintain structural integrity and interface contact continuity during battery cycling, thereby achieving long-term effective protection for the lithium metal anode.

[0010] To achieve the above objectives, the technical solution of the present invention is as follows.

[0011] The first aspect of this invention provides a method for preparing a self-healing polymer coating material, comprising the following steps: reacting an amino-terminated polyether, a chain extender, and a multi-aldehyde crosslinking agent in an organic solvent under an inert atmosphere to form a polyetheramine crosslinked polymer containing dynamic imine bonds, thereby obtaining a reaction solution; dissolving a lithium salt in the reaction solution and coating it into a film to obtain a self-healing polymer coating material; wherein the amino-terminated polyether is one or more of amino-terminated polyoxypropylene ether, trimethylolpropane tri[poly(propylene glycol), amino-terminated] ether, and O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer; and the multi-aldehyde crosslinking agent is one or more of pyromellitic methylformaldehyde and terephthalaldehyde.

[0012] This invention is based on the design of dynamic chemical bonds and molecular anchoring mechanisms. It involves reacting terminal amino polyethers, chain extenders, and multi-aldehyde crosslinking agents to introduce Schiff base structures and hydrogen bonds into the polyether backbone, resulting in a self-healing polymer coating with both self-repairing and strong adsorption functions. The self-healing polymer coating of this invention utilizes the reversible imine bond exchange reaction and the reversible "breakage-formation" of hydrogen bonds in the Schiff base structure to endow the polymer with rapid and robust self-healing capabilities, enabling it to autonomously repair cracks during cycling. Simultaneously, this invention utilizes the strong adsorption energy of sp² hybridized nitrogen atoms in the Schiff base for the lithium (110) crystal facet, achieving tight anchoring of the self-healing polymer coating to the lithium metal electrode surface. Through the synergistic effect of dynamic crack repair and molecular anchoring, the problems of interface layer breakage, detachment, and repeated SEI regeneration are effectively suppressed, significantly improving the cycling stability and safety of the lithium metal anode.

[0013] Preferably, the mass ratio of the terminal amino polyether, the polyaldehyde crosslinking agent, and the chain extender is 100:2 to 5:2 to 5. More preferably, the mass ratio of the terminal amino polyether, the polyaldehyde crosslinking agent, and the chain extender is 100:5:2.

[0014] In this invention, the mass ratio of terminal amino polyether, multi-aldehyde crosslinking agent, and chain extender is 100:2 to 5:2 to 5. For example, 100:5:2. Since the tight adhesion between the self-healing polymer coating and the metal electrode originates from the Schiff base structure generated by the reaction of the terminal amino group and the aldehyde group, and the hydrogen bonds formed between the Schiff base structure and the chain extender, the self-healing performance of the self-healing polymer coating and the adhesion between the self-healing polymer coating and the metal electrode can be controlled by adjusting the amounts of terminal amino polyether, multi-aldehyde crosslinking agent, and chain extender, thereby improving the overall performance.

[0015] Preferably, the chain extender is one or more of hexamethylene diisocyanate, adipic acid, and N,N'-thiocarbonyl diimidazole.

[0016] Preferably, the lithium salt is one or more selected from lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalateborate), and lithium difluorooxalateborate. In this invention, the doping of lithium salt helps to improve the polymer's ionic conductivity.

[0017] Preferably, the method for preparing a self-healing polymer coating material includes the following steps: Under an inert atmosphere, terminal amino polyethers, chain extenders, and multi-aldehyde crosslinking agents are mixed in an organic solvent and reacted to form a polyetheramine crosslinked polymer containing dynamic imine bonds, yielding a reaction solution. A lithium salt is dissolved in the reaction solution to obtain a polymer solution. The polymer solution is then coated to form a film, resulting in a self-healing polymer coating material. The polymer solution is coated onto a substrate surface and dried to form a film, which is then peeled off to obtain the self-healing polymer coating material. The substrate is selected from glass, copper, or lithium metal substrates.

[0018] Preferably, the mass ratio of the amino-terminated polyether to the lithium salt is 1:1.

[0019] Preferably, the organic solvent is one or more of acetone, toluene, xylene, hexane, N,N-dimethylacetamide, and N,N-dimethylformamide.

[0020] A second aspect of the present invention provides a self-healing polymer coating material, which is prepared by the method for preparing the self-healing polymer coating material described in the first aspect.

[0021] The self-healing polymer coating material of the present invention is obtained by reacting terminal amino polyether, chain extender and multi-aldehyde crosslinking agent to obtain polyetheramine crosslinked polymer containing dynamic imine bonds; then lithium salt is doped into the polyetheramine crosslinked polymer containing dynamic imine bonds.

[0022] A third aspect of the present invention provides a lithium metal anode, which is formed by a lithium metal electrode and a self-healing polymer coating modified on the surface of the lithium metal electrode, wherein the self-healing polymer coating is the self-healing polymer coating material described in the second aspect.

[0023] Preferably, the thickness of the self-healing polymer coating is 10 μm to 30 μm; and the thickness of the lithium metal electrode is 50 μm to 400 μm.

[0024] A fourth aspect of this invention provides a method for preparing a lithium metal anode, comprising the following steps: Under an inert atmosphere, terminal amino polyether, chain extender and polyaldehyde crosslinking agent are reacted in an organic solvent to obtain a reaction solution; lithium salt is dissolved in the reaction solution to obtain a polymer solution; the polymer solution is coated onto the surface of a lithium metal electrode to form a film, thereby obtaining a self-healing polymer coating modified lithium metal anode.

[0025] A further preferred method for preparing a lithium metal anode includes: mixing an amino-terminated polyether, a chain extender, and a polyaldehyde crosslinking agent in an organic solvent under an inert atmosphere and reacting them to obtain a reaction solution; dissolving a lithium salt in the reaction solution to obtain a polymer solution; coating the polymer solution onto the surface of a lithium metal electrode; and removing the organic solvent to obtain a self-healing polymer coating modified lithium metal anode.

[0026] Preferably, the inert atmosphere is argon atmosphere, and the H2O content is <0.01 ppm and the O2 content is <0.01 ppm.

[0027] The self-healing polymer coating modified lithium metal anode of the present invention can stably cycle for more than 1600 hours in a symmetric battery, and under high load LiNi 0.6 Co 0.2 Mn 0.2 The O2 (NCM622) cathode soft-pack battery retains 81.25% of its capacity after 500 cycles, making it suitable for high-energy-density, long-life lithium metal batteries.

[0028] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention involves reacting terminal amino polyethers, chain extenders, and multi-aldehyde crosslinking agents to introduce Schiff base structures and hydrogen bonds into the polyether backbone. After doping with lithium salts, a self-healing polymer coating with both strong anchoring and self-healing functions is obtained. The self-healing polymer coating of this invention contains Schiff base structures generated by the reaction of terminal amino groups and aldehyde groups, as well as abundant hydrogen bonds. Utilizing the exchange reaction of imine bonds in the Schiff base and the reversible "breakage-formation" of hydrogen bonds, autonomous crack repair is achieved, solving the problem of existing polymer lithium metal coatings developing microcracks during cycling due to lithium metal volume expansion, thus losing their protective function. The self-healing polymer coating of this invention achieves rapid and robust self-healing at room temperature, without external thermal stimulation or additional repair agents. It can dynamically maintain structural integrity under normal battery operating conditions, continuously isolating the electrolyte from fresh lithium metal and significantly suppressing interfacial side reactions.

[0029] 2. This invention utilizes the strong coordination of sp² hybridized nitrogen atoms in Schiff bases with the lithium (110) crystal plane to impart strong adsorption energy between the self-healing polymer coating and lithium metal, solving the problems of weak adhesion and easy peeling off of existing polymer coatings at the lithium metal interface. Experiments show that the peel strength between the self-healing polymer coating and the metal substrate of this invention is significantly improved, and it can withstand the interfacial stress caused by repeated volume changes of lithium metal, effectively eliminating the formation of interfacial voids and ensuring that the self-healing polymer coating remains tightly adhered to the lithium metal surface during long-term cycling.

[0030] 3. This invention, through the synergistic effect of self-healing and strong anchoring, avoids the repeated breakage and regeneration of the artificial SEI, maintains stable interfacial relaxation behavior, and significantly improves the cycle stability of the lithium metal anode. Electrochemical tests show that the lithium metal symmetric battery protected by the strong anchoring and self-healing polymer coating achieves stable cycle stability at a current density of 1 mA·cm⁻¹. -2 and a capacity of 1mAh·cm -2 Under certain conditions, it can cycle stably for more than 1600 hours with the polarization voltage always below 0.1V; while the polarization voltage of an unprotected bare lithium symmetric cell increases significantly after about 200 hours.

[0031] 4. By adjusting the ratio of end-group polyether, multi-aldehyde crosslinking agent and chain extender, this invention can regulate the mechanical properties of the self-healing polymer coating and its adhesion to lithium metal, thereby obtaining a lithium metal anode with better performance.

[0032] 5. The preparation process of this invention is simple and suitable for large-scale production. Existing technologies have relatively complex production processes, typically involving multi-step polymerization and low yields. The method of this invention is simple, low-cost, and does not require additional steps in electrode production. It effectively mitigates side reaction problems in lithium metal anodes during cycling simply through surface coating modification. Furthermore, it is compatible with existing lithium metal anode manufacturing processes and is feasible for large-scale production.

[0033] 6. The self-healing polymer coating of this invention also exhibits significant beneficial effects in practical pouch batteries. In pouch batteries assembled with a high-load NCM622 cathode, the battery protected by the self-healing polymer coating maintained a capacity retention of up to 81.25% after 500 cycles at 1C, while the bare lithium pouch battery's capacity decreased to below 80% after only 25 cycles. The self-healing polymer coating extended battery life by nearly 20 times. Simultaneously, in-situ ultrasonic transmission imaging showed that the electrode area of ​​the bare lithium pouch battery was filled with bubbles after 30 cycles (corresponding to severe interfacial side reactions), while the pouch battery protected by the self-healing polymer coating maintained good interfacial contact throughout the entire cycle, with no significant gas generation. This fully demonstrates the excellent protective effect of the lithium metal anode modified with the self-healing polymer coating of this invention in practical applications. Attached Figure Description

[0034] Figure 1 These are comparative diagrams illustrating the principles of existing polymer native interface layers and the self-healing polymer coating of this invention during battery cycling. (A) is a schematic diagram illustrating the principle of microcrack induction in existing polymer native interface layers during battery cycling; (B) is a schematic diagram illustrating the principle of the stability and integrity of the self-healing polymer coating of this invention during battery cycling.

[0035] Figure 2 The images show the self-healing polymer coating prepared in Example 1. (A) shows the self-healing polymer coating after shearing; (B) shows the self-healing polymer coating after splicing; and (C) shows the self-healing polymer coating after healing.

[0036] Figure 3 This is a comparison chart of the self-healing efficiency of the original coating and the coating after "cut-and-stitch" in Example 1.

[0037] Figure 4 The images show the adhesion test results of the self-healing polymer coating to lithium metal in Example 1. (A) is a simulated test image; (B) is an actual test image.

[0038] Figure 5 This is a comparison chart of the peel strength of BBT@Cu in Example 2 and BT@Cu in Comparative Example 1.

[0039] Figure 6 Comparison graph of cycle performance of symmetrical cells assembled with BBT@Li in Example 3, BT@Li in Comparative Example 2, and unmodified bare lithium metal anode (Li).

[0040] Figure 7 Scanning electron microscope (SEM) images of the surface and cross-section of the self-healing polymer coating of the symmetrical battery assembled with BBT@Li in Example 3 and BT@Li in Comparative Example 2 after 50 cycles are shown. Specifically, (A) is an SEM image of the surface of the self-healing polymer coating of the symmetrical battery assembled with BT@Li in Comparative Example 2 after 50 cycles; (B) is a magnified view of a portion of (A); (C) is an SEM image of the cross-section of the self-healing polymer coating of the symmetrical battery assembled with BT@Li in Comparative Example 2 after 50 cycles; (D) is an SEM image of the surface of the self-healing polymer coating of the symmetrical battery assembled with BBT@Li in Example 3 after 50 cycles; (E) is a magnified view of a portion of (D); and (F) is an SEM image of the cross-section of the self-healing polymer coating of the symmetrical battery assembled with BBT@Li in Example 3 after 50 cycles.

[0041] Figure 8 The graph shows a comparison of the cycle performance of the pouch cell assembled with BBT@Li and NCM622 cathode prepared in Example 4 and the pouch cell assembled with unmodified bare lithium metal anode (Li) and NCM622 cathode.

[0042] Figure 9 Ultrasonic images of a pouch cell assembled with BBT@Li and NCM622 cathode, and a pouch cell assembled with unmodified bare lithium metal anode (Li) and NCM622 cathode, after different numbers of cycles, prepared for Example 4. Among them, (A1) is the ultrasonic image of a pouch cell assembled with an unmodified bare lithium metal anode (Li) and an NCM622 cathode after 10 cycles; (A2) is the ultrasonic image of a pouch cell assembled with an unmodified bare lithium metal anode (Li) and an NCM622 cathode after 20 cycles; (A3) is the ultrasonic image of a pouch cell assembled with an unmodified bare lithium metal anode (Li) and an NCM622 cathode after 30 cycles; (B1) is the ultrasonic image of a pouch cell assembled with BBT@Li and an NCM622 cathode prepared in Example 4 after 10 cycles; (B2) is the ultrasonic image of a pouch cell assembled with BBT@Li and an NCM622 cathode prepared in Example 4 after 20 cycles; and (B3) is the ultrasonic image of a pouch cell assembled with BBT@Li and an NCM622 cathode prepared in Example 4 after 30 cycles. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without inventive effort are within the scope of protection of this invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0044] This invention provides a self-healing polymer coating-modified lithium metal anode, which is formed by a lithium metal electrode and a self-healing polymer coating modified on the surface of the lithium metal electrode. The raw materials for preparing the self-healing polymer coating include terminal amino polyether, chain extender, multi-aldehyde crosslinking agent, and lithium salt. In the self-healing polymer coating, the abundant Schiff base N atoms generate strong coordination with the (110) crystal plane of lithium metal, ensuring the tight anchoring of the coating to the lithium metal anode. At the same time, the exchange reaction of imine bonds in the Schiff base and the abundant hydrogen bonds in the polymer give the coating a robust self-healing ability, realizing the autonomous repair of cracks.

[0045] In embodiments of the present invention, the amino-terminated polyether is one or more of amino polyoxypropylene ethers (e.g., Shanghai Maclean Biotech Co., Ltd. P761997 T-5000, T-3000, Aladdin P108071 D400, D-2000 or D-230, with average molecular weights of 5000, 3000, 400, 2000, 230, respectively), trimethylolpropane tri[poly(propylene glycol), amino-terminated] ether (Shanghai Maclean Biotech Co., Ltd. T478164, polyetheramine T403, with an average molecular weight of 440), and O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900). The polyaldehyde crosslinking agent is one or more of trimesaldehyde and terephthalaldehyde.

[0046] The crosslinking agent is one or more of hexamethylene diisocyanate, adipic acid, N,N'-thiocarbonyl diimidazole, trimesonaldehyde, and terephthalaldehyde. The lithium salt is one or more of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and lithium bis(fluorosulfonyl)imide (LiFSI).

[0047] In embodiments of the present invention, the thickness of the self-healing polymer coating is 10 μm to 30 μm.

[0048] In this invention, the amino group (-NH2) of the terminal amino polyether undergoes a nucleophilic substitution reaction with the aldehyde group (-CHO) of the polyaldehyde crosslinking agent to generate a Schiff base structure. The Schiff base structure adopts SP...2 The strong coordination ability of hybridized N atoms with the (110) crystal plane of lithium metal ensures that the self-healing polymer coating can be stably anchored on the surface of the lithium metal anode. Simultaneously, abundant hydrogen bonds and reversible exchange reactions of Schiff bases enable the coating to self-heal rapidly and robustly. This strong anchoring and self-healing ability ensures the stability and integrity of the coating's structure during lithium metal anode cycling, reducing the formation of voids and polymer cracks between the polymer and the anode, which helps reduce side reactions between lithium metal and the electrolyte, thus improving the cycling stability of the lithium metal anode. Figure 1 As shown in (B).

[0049] This invention also provides a method for preparing a self-healing polymer coating modified lithium metal anode, comprising the following steps: S1. Mix the terminal amino polyether, chain extender and polyaldehyde crosslinking agent in an organic solvent to obtain a mixture.

[0050] S2. Stir the mixture at room temperature (25℃~30℃) for 10h~16h to allow the terminal amino polyether, chain extender, and multi-aldehyde crosslinking agent to react fully. During this period, add a certain amount of solvent every 6h to adjust the viscosity of the polymer solution. The amount of solvent added can be adjusted according to the actual reaction conditions. For example, add 1mL~10mL of solvent for every 1g of terminal amino polyether.

[0051] S3. After the reaction is complete, add the lithium salt to the reaction solution and continue stirring for 10 to 16 hours until the lithium salt is completely dissolved to obtain a homogeneous polymer solution.

[0052] S4. Coat the surface of the lithium metal electrode with the polymer solution and evaporate the organic solvent at room temperature to obtain a lithium metal anode modified with a self-healing polymer coating.

[0053] In steps S1 and S2, the solution is stirred at a speed of 200 rpm to 1500 rpm for 10 h to 16 h using a stirrer, or by using ultrasonic oscillation or high shear stirring to ensure that the solution is uniformly mixed to a clear state.

[0054] Furthermore, the mixing, stirring, coating, and drying steps described above are all carried out under an anhydrous and oxygen-free protective atmosphere, which is an inert gas, specifically an argon atmosphere. By volume fraction, the anhydrous and oxygen-free environment has an H2O content of <0.01 ppm and an O2 content of <0.01 ppm.

[0055] In step S4, the coating is performed by scraping, spraying, dipping, or spin coating.

[0056] In step S4, the organic solvent is evaporated at room temperature for 20-24 hours in an anhydrous and oxygen-free inert environment. The thickness of the lithium metal coating is 50 μm-400 μm; the thickness of the self-healing polymer coating is 10 μm-30 μm. The coating modification method of this invention is universal and can be applied to lithium metal anodes of different sizes, thicknesses, and shapes.

[0057] The self-healing polymer coating modified lithium metal anode of this invention can be used to assemble liquid batteries, semi-solid batteries, or all-solid batteries. The battery is a lithium metal battery. The electrolyte solvent is a carbonate or ether. The concentration of lithium salt (LiTFSI) in the electrolyte is 0.5 mol / L to 3 mol / L. For example, the electrolyte can be prepared by mixing ethylene carbonate (EC) and diethyl carbonate (DEC) at a volume ratio of 1:1 as a base solvent, adding lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) to the base solvent, stirring until completely dissolved, and finally adding fluoroethylene carbonate (FEC) as an additive to obtain the electrolyte. In the electrolyte, the concentration of lithium bis(trifluoromethanesulfonyl)imide is 1.0 mol / L, and the concentration of fluoroethylene carbonate is 15 wt%.

[0058] The technical solution of the present invention will be further described below through specific embodiments. Unless otherwise specified, the methods described in the following embodiments are conventional methods; the reagents and materials described are commercially available unless otherwise specified.

[0059] Example 1 A method for preparing a self-healing polymer coating material includes the following steps: Raw material selection: The amino-terminated polyether is O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900); the multi-aldehyde crosslinking agent is trimesoaldehyde; and the chain extender is N,N'-thiocarbonyldiimidazole.

[0060] Preparation of the reaction solution: Following a mass ratio of 100:5:2 for the terminal amino polyether, the multi-aldehyde crosslinking agent, and the chain extender, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer was dissolved in 2 mL of N,N-dimethylacetamide solvent under an argon atmosphere. Subsequently, 30 mg of trimesin and 12 mg of N,N'-thiocarbonyldiimidazole were added. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, approximately 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0061] Preparation of polymer solution: After the reaction is completed, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is weighed using a balance of 0.01g and added to the above reaction solution. Stirring is continued for 12h until the lithium salt (LiTFSI) is completely dissolved. Then, the resulting viscous solution is degassed in a vacuum environment for 1h to obtain the polymer solution.

[0062] Preparation of self-healing polymer coating material: A polymer solution was poured onto a glass plate and kept at room temperature for 24 h under argon protection. After the N,N-dimethylacetamide solvent evaporated, the glass plate was removed to obtain the self-healing polymer coating material, denoted as BBT. Here, "self-healing polymer coating material" refers to a self-healing polymer coating and does not include a lithium metal anode.

[0063] The self-healing polymer coating material prepared using the method of Example 1 was tested for self-healing performance and lithium metal adhesion performance, such as... Figure 2 and Figure 3 As shown.

[0064] The self-healing polymer coating material in Example 1, after being "shear-spliced," can lift a 200g weight without breaking. Figure 2 As shown.

[0065] The self-healing polymer coating material before "shear-splicing" is referred to as the original coating. The self-healing polymer coating material after "shear-splicing" is referred to as the coating after "shear-splicing". Figure 3 In the tests, the maximum tensile strength of the original polymer film was 28.5 MPa, while the maximum tensile strength of the coating after "shear-splicing" reached 23.6 MPa, and it did not break when stretched to 300% strain. These tests demonstrate that the self-healing polymer coating material of Example 1 possesses robust self-healing capabilities.

[0066] like Figure 4 As shown, using the self-healing polymer coating material prepared in Example 1 as the self-healing polymer coating, and lithium foil as the lithium metal anode, two pieces of the self-healing polymer coating from Example 1 were respectively attached to both sides of a lithium foil with a diameter of 12 mm and a thickness of 400 μm. A 200 g weight was suspended from the bottom of one of the self-healing polymer coatings, and the other self-healing polymer coating was lifted. When fully lifted, neither of the self-healing polymer coatings on either side detached from the lithium foil surface, demonstrating that the self-healing polymer coating of Example 1 has a strong anchoring ability and adhesion effect to the lithium metal anode.

[0067] Example 2 A method for preparing a self-healing polymer-coated copper foil includes the following steps: Raw material selection: The amino-terminated polyether is O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900); the multi-aldehyde crosslinking agent is trimesoaldehyde; and the chain extender is N,N'-thiocarbonyldiimidazole.

[0068] Preparation of the reaction solution: Following a mass ratio of 100:5:2 for the terminal amino polyether, the multi-aldehyde crosslinking agent, and the chain extender, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer was dissolved in 2 mL of N,N-dimethylacetamide solvent under an argon atmosphere. Subsequently, 30 mg of trimesaldehyde and 12 mg of N,N'-thiocarbonyldiimidazole were added. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0069] Preparation of polymer solution: After the reaction is completed, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is weighed using a balance of 0.01g and added to the above reaction solution. Stirring is continued for 12 h until the lithium salt (LiTFSI) is completely dissolved. Then, the resulting viscous solution is degassed in a vacuum environment for 1 h to obtain the polymer solution.

[0070] Preparation of copper foil modified with a self-healing polymer coating: A polymer solution was drop-coated onto the surface of a copper foil. Under argon protection, the solution was kept at room temperature for 24 hours. After the N,N-dimethylacetamide solvent evaporated, a copper foil modified with a self-healing polymer coating was obtained, denoted as BBT@Cu.

[0071] Comparative Example 1 A method for preparing a self-healing polymer-coated copper foil, differing from Example 2 in that 30 mg of pyromellitic aldehyde is not added; the specific preparation method includes the following steps: In an inert atmosphere, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900) was dissolved in 2 mL of N,N-dimethylacetamide solvent, followed by the addition of 12 mg of N,N'-thiocarbonyldiimidazole. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0072] After the reaction was complete, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was weighed using a 0.01 g balance and added to the above reaction solution. Stirring was continued for 12 h until the lithium salt (LiTFSI) was completely dissolved. The resulting viscous solution was then degassed under vacuum for 1 h to obtain a polymer solution. The polymer solution was drop-coated onto the surface of a copper foil. Under argon protection, the solution was kept at room temperature for 24 h. After the N,N-dimethylacetamide solvent evaporated, a self-healing polymer-coated copper foil was obtained, denoted as BT@Cu.

[0073] The difference between Comparative Example 1 and Example 2 is that the coating of Comparative Example 1 does not contain the Schiff base structure introduced by the reaction of aldehyde and amino groups. Therefore, the coating of Comparative Example 1 does not have a strong anchoring effect, but only a self-healing effect.

[0074] Peel strength tests were performed on the BBT@Cu prepared in Example 2 and the BT@Cu prepared in Comparative Example 1. The results are as follows: Figure 5 As shown. The magnitude of the peel force reflects the strength of the polymer coating (BT) adhering to the copper foil. From Figure 5 As can be seen, the self-healing polymer coating (BT) of Comparative Example 1 exhibits lower peel strength. This indicates that, in the absence of a strongly anchored Schiff base structure, relying solely on the thiourea structure and ether oxygen atoms is insufficient to achieve strong adhesion to the copper foil. In contrast, the BBT@Cu prepared in Example 2 exhibits a peel strength as high as 3.4 N / cm, and this significant enhancement in peel strength strongly demonstrates the crucial role of the Schiff base structure in achieving robust adhesion.

[0075] Example 3 A method for preparing a self-healing polymer coating-modified lithium metal anode includes the following steps: According to the mass ratio of terminal amino polyether, multi-aldehyde crosslinking agent and chain extender of 100:5:2, under an argon atmosphere, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900) was dissolved in 2 mL of N,N-dimethylacetamide solvent, followed by the addition of 30 mg of trimesin and 12 mg of N,N'-thiocarbonyldiimidazole. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0076] After the reaction was complete, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was weighed using a 0.01 g balance and added to the above reaction solution. Stirring was continued for 12 h until the lithium salt (LiTFSI) was completely dissolved. The resulting viscous solution was then degassed under vacuum for 1 h to obtain a polymer solution. The polymer solution was drop-coated onto the lithium metal surface. Under argon protection, the mixture was kept at room temperature for 24 h. After the N,N-dimethylacetamide solvent evaporated, a self-healing polymer-coated lithium metal anode was obtained, denoted as BBT@Li.

[0077] The BBT@Li prepared in Example 3 was assembled into a lithium symmetric battery BBT@Li||BBT@Li. The electrolyte was prepared as follows: ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed uniformly at a volume ratio of 1:1 as the base solvent. Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was added to the base solvent and stirred until completely dissolved. Finally, fluoroethylene carbonate (FEC) was added as an additive to obtain the electrolyte. In the electrolyte, the concentration of lithium bis(trifluoromethanesulfonyl)imide was 1.0 mol / L, and the concentration of fluoroethylene carbonate was 15 wt%.

[0078] Comparative Example 2 A method for preparing a self-healing polymer coating-modified lithium metal anode, differing from Example 3 in that 30 mg of pyromellitic methyl ether is not added; the specific preparation method includes the following steps: In an inert atmosphere, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900) was dissolved in 2 mL of N,N-dimethylacetamide solvent, followed by the addition of 12 mg of N,N'-thiocarbonyldiimidazole. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0079] After the reaction was complete, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was weighed using a 0.01 g balance and added to the above reaction solution. Stirring was continued for 12 h until the lithium salt (LiTFSI) was completely dissolved. The resulting viscous solution was then degassed under vacuum for 1 h to obtain a polymer solution. The polymer solution was drop-coated onto the lithium metal surface. Under argon protection, the mixture was kept at room temperature for 24 h. After the N,N-dimethylacetamide solvent evaporated, a self-healing polymer-coated lithium metal anode was obtained, denoted as BT@Li.

[0080] The BT@Li prepared in Comparative Example 2 was assembled into a lithium-ion symmetric battery BT@Li||BT@Li. The electrolyte was prepared as follows: ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed uniformly at a volume ratio of 1:1 as the base solvent. Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was added to the base solvent and stirred until completely dissolved. Finally, fluoroethylene carbonate (FEC) was added as an additive to obtain the electrolyte. In the electrolyte, the concentration of lithium bis(trifluoromethanesulfonyl)imide was 1.0 mol / L, and the concentration of fluoroethylene carbonate was 15 wt%.

[0081] The difference between Comparative Example 2 and Example 3 is that the coating of Comparative Example 2 does not contain the Schiff base structure introduced by the reaction of aldehyde and amino groups. Therefore, the coating of Comparative Example 2 does not have a strong anchoring effect, but only a self-healing effect.

[0082] Using the BBT@Li||BBT@Li symmetric battery of Example 3, the BT@Li||BT@Li symmetric battery of Comparative Example 2, and the Li||Li symmetric battery assembled from bare lithium metal (Li) without coating protection, at a current density of 1 mA / cm², 2 and a capacity of 1mAh / cm 2 Cyclic performance tests were conducted under the specified conditions, and the results are as follows: Figure 6 As shown.

[0083] from Figure 6 As can be seen, compared to the Li||Li symmetric battery, the cycle stability of both BBT@Li||BBT@Li and BT@Li||BT@Li was improved. Specifically, the BBT@Li||BBT@Li symmetric battery could cycle stably for over 1600 hours, significantly longer than the 400 hours of the Li||Li symmetric battery, and the polarization voltage remained stable at a lower level. This demonstrates that the strong anchoring and self-healing polymer coating significantly improves the cycle stability of the lithium metal anode. Meanwhile, the cycle performance of the lithium metal anode BT@Li, coated with a self-healing polymer without a Schiff base structure, was also improved (approximately 1000 hours). However, due to the lack of strong anchoring between the Schiff base N atoms and lithium metal, the improvement in cycle stability of BT@Li was limited, and its cycle stability was lower than that of the BBT@Li||BBT@Li symmetric battery. These tests demonstrate that strong anchoring and self-healing are crucial for improving the stability of the lithium metal anode.

[0084] The BBT@Li||BBT@Li symmetric cell of Example 3 and the BT@Li||BT@Li symmetric cell of Comparative Example 2 at 1 mA / cm 2 SEM images of the negative electrode surface and cross-section after 50 cycles under the specified conditions, as shown below. Figure 7 As shown. By Figure 7It can be seen that after 50 cycles, dense cracks and severe flaking appeared on the BT@Li surface. However, after 50 cycles, the strongly anchored, self-healing polymer of BBT@Li in Example 3 remained stably bonded to the lithium metal surface. The difference between Comparative Example 2's BT@Li and Example 3's BBT@Li is that Comparative Example 2's BT@Li lacks a Schiff base structure. Figure 7 The comparison illustrates the important role of Schiff base structure in lithium metal anchoring.

[0085] Example 4 A method for preparing a self-healing polymer coating-modified lithium metal anode includes the following steps: According to the mass ratio of terminal amino polyether, multi-aldehyde crosslinking agent and chain extender of 100:5:2, under an inert atmosphere, 0.6 g of O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer (Aladdin O344954, with an average molecular weight of 1900) was dissolved in 2 mL of N,N-dimethylacetamide solvent, followed by the addition of 30 mg of trimesin and 12 mg of N,N'-thiocarbonyldiimidazole. The mixture was stirred thoroughly at room temperature for 12 h to form a homogeneous reaction solution. During this period, 1 mL of N,N-dimethylacetamide solvent was added every 6 h to adjust the viscosity of the reaction solution.

[0086] After the reaction was complete, 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was weighed using a 0.01 g balance and added to the above reaction solution. Stirring was continued for 12 h until the lithium salt (LiTFSI) was completely dissolved. The resulting viscous solution was then degassed under vacuum for 1 h to obtain a polymer solution. The polymer solution was drop-coated onto the lithium metal surface. Under argon protection, the mixture was kept at room temperature for 24 h. After the N,N-dimethylacetamide solvent evaporated, a self-healing polymer-coated lithium metal anode was obtained, denoted as BBT@Li.

[0087] The BBT@Li anode from Example 4 was combined with an active material loading of 10 mg / cm³. 2 NCM622 cathode (LiNi) 0.6 Co 0.2 Mn 0.2 The electrolyte was prepared by assembling lithium metal pouch cells (BBT@Li||NCM622) using O2. Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed uniformly at a volume ratio of 1:1 as the base solvent. Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was added to the base solvent and stirred until completely dissolved. Finally, fluoroethylene carbonate (FEC) was added as an additive to obtain the electrolyte. The concentration of lithium bis(trifluoromethanesulfonyl)imide in the electrolyte was 1.0 mol / L, and the concentration of fluoroethylene carbonate was 15 wt%.

[0088] Using bare lithium metal (Li) as the negative electrode, with an active material loading of 10 mg / cm³ 2 The NCM622 cathode was used to assemble a lithium metal pouch cell, Li||NCM622 pouch cell, as a control.

[0089] Figure 8 In the original test, the Li||NCM622 pouch cell exhibited rapid capacity decay at a 1C discharge rate. However, the BBT@Li||NCM622 pouch cell retained a capacity of 81.25% after 500 cycles at a 1C discharge rate. This cycle test result demonstrates that, compared to the Li||NCM622 pouch cell, the BBT@Li assembled in Example 4 significantly improves cycle stability.

[0090] Figure 9 In the ultrasonic tests, the Li||NCM622 pouch cell showed significant gas generation (blue area) near the tab after only 10 cycles, and the gas volume gradually increased with continued cycling. By the 30th cycle, the entire electrode area was filled with gas, indicating a severe side reaction between the electrolyte and lithium metal. In contrast, the BBT@Li||NCM pouch cell of Example 4 maintained excellent interfacial contact stability throughout the entire cycling process, demonstrating that the BBT self-healing polymer coating provides effective protection for the lithium metal.

[0091] In summary, the BBT polymer coating designed in this embodiment of the invention, which combines strong anchoring and self-healing, can form a dense polymer separator film in situ on the lithium metal anode surface, stably anchoring it to the lithium metal surface. Furthermore, it maintains its structural integrity through rapid and robust self-healing, thereby suppressing side reactions between lithium metal and the electrolyte and significantly improving the cycle stability of the lithium metal anode. The overall preparation process is simple, highly reproducible, and suitable for large-scale industrial production. Batteries using this lithium metal anode coating exhibit high cycle stability and are applicable to various battery systems.

[0092] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a self-healing polymer coating material, characterized in that, Includes the following steps: Under an inert atmosphere, terminal amino polyether, chain extender and polyaldehyde crosslinking agent are reacted in an organic solvent to form a polyetheramine crosslinked polymer containing dynamic imine bonds, resulting in a reaction solution; lithium salt is dissolved in the reaction solution and coated into a film to obtain a self-healing polymer coating material; The amino-terminated polyether is one or more of the following: amino-terminated polyoxypropylene ether, trimethylolpropane tri[poly(propylene glycol), amino-terminated] ether, and O,O'-bis(2-aminopropyl)polypropylene glycol-polyethylene glycol-polypropylene glycol block copolymer. The multi-aldehyde crosslinking agent is one or more of pyromellitic benzoaldehyde and terephthalaldehyde.

2. The method for preparing the self-healing polymer coating material according to claim 1, characterized in that, The mass ratio of terminal amino polyether, polyaldehyde crosslinking agent and chain extender is 100:2-5:2-5.

3. The method for preparing the self-healing polymer coating material according to claim 2, characterized in that, The mass ratio of terminal amino polyether, polyaldehyde crosslinking agent and chain extender is 100:5:

2.

4. The method for preparing the self-healing polymer coating material according to claim 1, characterized in that, The chain extender is one or more of hexamethylene diisocyanate, adipic acid and N,N'-thiocarbonyldiimidazole; The lithium salt is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(oxalateborate), and lithium difluorooxalateborate.

5. The method for preparing the self-healing polymer coating material according to claim 1, characterized in that, The mass ratio of amino-terminated polyether to lithium salt is 1:1; The organic solvent is one or more of acetone, toluene, xylene, hexane, N,N-dimethylacetamide, and N,N-dimethylformamide.

6. A self-healing polymer coating material, characterized in that, The self-healing polymer coating material is prepared using the preparation method described in any one of claims 1 to 5.

7. A lithium metal anode, comprising a lithium metal electrode and a self-healing polymer coating modified on the surface of the lithium metal electrode, characterized in that, The self-healing polymer coating is the self-healing polymer coating material as described in claim 6.

8. The lithium metal anode according to claim 7, characterized in that, The thickness of the self-healing polymer coating is 10 μm to 30 μm; the thickness of the lithium metal electrode is 50 μm to 400 μm.

9. A method for preparing a lithium metal anode according to claim 7, characterized in that, Includes the following steps: Under an inert atmosphere, terminal amino polyether, chain extender and polyaldehyde crosslinking agent are reacted in an organic solvent to obtain a reaction solution; lithium salt is dissolved in the reaction solution to obtain a polymer solution; the polymer solution is coated onto the surface of a lithium metal electrode to form a film, thereby obtaining a self-healing polymer coating modified lithium metal anode.

10. The method for preparing a lithium metal anode according to claim 9, characterized in that, The inert atmosphere is argon, with H2O content <0.01 ppm and O2 content <0.01 ppm.