Photocurable coating, hard coating and use thereof
By introducing phenyl-epoxy modified polyhedral oligomeric silsesquioxane into the photocurable coating, an inorganic-organic nano-hybrid structure is formed, which solves the problem of balancing heat resistance and hydrophobicity in hard coating materials and improves hardness, scratch resistance and adhesion.
Patent Information
- Application Number
- CN202611493460.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing hard coating materials struggle to balance hydrophobicity and heat resistance, and the poor interfacial bonding between inorganic nanoparticles and resins results in insufficient hardness, scratch resistance, and thermal stability.
Introducing phenyl-epoxy modified polyhedral oligomeric silsesquioxane (Ph-EP-POSS) into UV-curable coatings and controlling its addition amount and grafting ratio to form an inorganic-organic nano-hybrid structure synergistically improves the hardness, scratch resistance and hydrophobicity of the hard coating.
The prepared hard coating exhibits high pencil hardness, large water contact angle and high glass transition temperature, with excellent heat resistance and hydrophobicity, and good adhesion.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application belongs to the field of optical film technology, specifically relating to a photocurable coating, a hard coating, and their applications. Background Technology
[0002] As display devices become thinner, lighter, and more powerful, the requirements for multiple properties of hard coatings for polarizers, such as high hardness and scratch resistance, weather resistance and heat resistance, and surface hydrophobicity and stain resistance, are becoming increasingly stringent.
[0003] To improve the hardness and scratch resistance of hard coatings, existing technologies often employ the introduction of inorganic nanoparticles. For example, CN111040617A adds micron-sized silica particles and modified nano-silica particles to the anti-glare hardening layer, leveraging the rigidity of silica to enhance the hardness and scratch resistance of the cured anti-glare hardening layer. CN117264260A improves the coating's hardness and scratch resistance by introducing core-shell structured silica-polymethyl methacrylate composite nanoparticles. However, the synthesis process of these composite nanoparticles is complex, and poor purification during the coating process can easily lead to increased coating haze. CN103257388A improves the coating's hardness by doping core-shell structured transition metal oxide nanoparticles. While introducing inorganic nanoparticles can improve the coating's hardness and scratch resistance, the poor interfacial bonding between inorganic nanoparticles and resins deteriorates the hard coating's thermal stability, adhesion, and wear resistance. Furthermore, inorganic nanoparticles are prone to agglomeration, increasing the haze of the hard coating and hindering its practical application.
[0004] Polyhedral oligomeric silsesquioxanes (POSS) are organic-inorganic hybrid nanomaterials with a unique three-dimensional cage structure. They possess the rigidity, dimensional stability, and thermal stability of inorganic silicon-oxygen frameworks, as well as the designability and reactivity of organic substituted functional groups. Furthermore, they can overcome the defects of poor compatibility between inorganic nanoparticles and resin matrices, making them potential modifying materials for improving the hardness, scratch resistance, adhesion, and heat resistance of hard coatings.
[0005] However, the functionalization level of the POSS structure in the prior art is relatively simple, and when the proportion of grafted reactive groups is not right, it is easy to cause an imbalance in the degree of crosslinking of the hard coating: insufficient crosslinking results in poor hardness, scratch resistance and adhesion of the hard coating; excessive crosslinking will make the hard coating brittle, resulting in a decrease in toughness. At the same time, the surface hydrophobic groups of the hard coating in the prior art are unevenly distributed, making it difficult to achieve both scratch resistance and hydrophobic and antifouling properties, and the long-term thermal stability still needs to be improved.
[0006] Therefore, how to design a modified POSS structure that combines the synergistic effects of reactive and hydrophobic groups to achieve partitioned and directional enrichment during the curing process of hard coatings, thereby improving the coating's hardness and scratch resistance while also taking into account hydrophobicity and heat resistance, is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] To address the shortcomings of existing technologies, the purpose of this application is to provide a photocurable coating, a hard coating, and their applications. By introducing a modified polyhedral oligomeric silsesquioxane (POSS) with synergistic effects of reactive and hydrophobic groups into the photocurable coating, the reactive groups crosslink and cure with the photocurable resin, thereby improving the hardness and scratch resistance of the coating. Furthermore, the hydrophobic groups are directionally segregated on the coating surface, enhancing the hydrophobic properties of the coating surface. This solves the problem that existing hard coating materials cannot simultaneously achieve both hydrophobicity and heat resistance, and improves the hardness and scratch resistance of the hard coating.
[0008] To achieve this objective, the present application adopts the following technical solution: In a first aspect, this application provides a photocurable coating, which comprises the following components by weight: 30-70 parts of photocurable resin, 1-10 parts of photoinitiator, and 0.5-5 parts of phenyl-epoxy modified polyhedral oligomeric silsesquioxane.
[0009] The "30-70 portions" can be, for example, 35 portions, 40 portions, 45 portions, 50 portions, 55 portions, 60 portions, or 65 portions, etc.
[0010] The number of portions "1-10" can be 2, 3, 4, 5, 6, 7, 8, or 9.
[0011] The "0.5-5 portions" can be, for example, 1 portion, 1.5 portions, 2 portions, 2.5 portions, 3 portions, 3.5 portions, 4 portions, or 4.5 portions, etc.
[0012] The grafting ratio of phenyl to epoxy groups in the phenyl-epoxy modified polyhedral oligomeric silsesquioxane is (1.6-3):1, for example, it can be 1.7:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1 or 2.9:1, etc.
[0013] This application introduces phenyl-epoxy modified polyhedral oligomeric silsesquioxane (Ph-EP-POSS) into a photocurable coating. By grafting different proportions of epoxy groups and phenyl groups at the silicon apex of the POSS cage, an inorganic-organic nano-hybrid structure is constructed. The POSS cage-like inorganic framework structure endows the hard coating with excellent heat resistance and hardness. The epoxy groups participate in the curing and cross-linking of the photocurable resin, while the phenyl groups migrate and accumulate to the surface of the hard coating. The two interact in a directional manner, complementing each other, overcoming the problem that it is difficult to balance heat resistance and hydrophobicity due to the single or disordered distribution of grafted groups in ordinary POSS structures.
[0014] This application controls the amount of Ph-EP-POSS added to be 0.5-5 parts by weight. If the amount of Ph-EP-POSS added is too small, the nano-reinforcing effect and cross-linking density will be insufficient, and Ph-EP-POSS will not be able to effectively migrate to the coating surface to form a silicon-rich protective layer, resulting in poor hardness, scratch resistance, adhesion, thermal stability and hydrophobicity of the hard coating. If the amount of Ph-EP-POSS added is too large, local agglomeration will occur, resulting in white spots on the hard coating. Excessive cross-linking will cause the hard coating to become brittle and reduce its adhesion and wear resistance.
[0015] This application controls the grafting ratio of phenyl to epoxy groups in Ph-EP-POSS to be (1.6-3):1. Within this grafting ratio range, it ensures that the epoxy groups fully participate in the cross-linking and curing of the photocurable resin, improving the hardness, scratch resistance, adhesion, and thermal stability of the hard coating. If the epoxy group grafting density is too high, it will cause problems such as excessive cross-linking, coating embrittlement, and decreased transparency and adhesion. If the epoxy group grafting density is insufficient, it will cause problems such as low degree of cross-linking, poor hardness, scratch resistance, and thermal stability.
[0016] In some embodiments, the phenyl-epoxy modified polyhedral oligomeric silsesquioxane is prepared by a method comprising the following steps: (S1) A first reaction is carried out by mixing phenylalkoxysilane, a first catalyst, a first solvent and water to obtain oligomeric phenylsilsesquioxane; (S2) The oligophenyl silsesquioxane, the second catalyst, and the second solvent are mixed and subjected to a second reaction. Then, an epoxy silane coupling agent is added to carry out a third reaction to obtain the phenyl-epoxy modified polyhedral oligosilsesquioxane.
[0017] The method for preparing phenyl-epoxy modified polyhedral oligomeric silsesquioxanes in this application is a stepwise hydrolysis-condensation method. First, phenylalkoxysilane is hydrolyzed and condensed to obtain incompletely condensed oligomeric phenylsilsesquioxanes, forming a non-closed octahedral POSS cage structure. The POSS structure contains phenyl groups and reactive silanol groups (Si-OH). Then, an epoxy silane coupling agent is introduced to perform hydrolysis-condensation ring closure. The stepwise hydrolysis-condensation method can alleviate the uneven distribution of modified functional groups and poor molecular structure uniformity in the POSS structure.
[0018] In some embodiments, step (S1) includes the following raw materials in parts by mass: 0.5-1.5 parts of phenylalkoxysilane, 2-6 parts of the first catalyst, 30-40 parts of the first solvent, and 0.06-0.22 parts of water.
[0019] The "0.5-1.5 portions" can be, for example, 0.6 portions, 0.7 portions, 0.8 portions, 0.9 portions, 1 portion, 1.1 portions, 1.2 portions, 1.3 portions, or 1.4 portions, etc.
[0020] The "2-6 portions" can be, for example, 2.5 portions, 3 portions, 3.5 portions, 4 portions, 4.5 portions, 5 portions, or 5.5 portions, etc.
[0021] The "30-40 portions" can be, for example, 31 portions, 32 portions, 33 portions, 34 portions, 35 portions, 36 portions, 37 portions, 38 portions, or 39 portions, etc.
[0022] The "0.06-0.22 portions" can be, for example, 0.08 portions, 0.1 portions, 0.12 portions, 0.14 portions, 0.16 portions, 0.18 portions, or 0.2 portions, etc.
[0023] In some embodiments, the phenylalkoxysilane includes any one or a combination of at least two of phenyltriethoxysilane, phenyltrimethoxysilane, phenylmethyldimethoxysilane, and phenylmethyldiethoxysilane.
[0024] In some embodiments, the first catalyst includes any one or a combination of at least two of the following: fluoride ion catalysts, organic amine catalysts, inorganic weak base catalysts, quaternary ammonium base catalysts, and acid catalysts.
[0025] In some embodiments, the fluoride ion catalyst includes any one or a combination of at least two of tetrabutylammonium fluoride, tetramethylammonium fluoride, and tetraethylammonium fluoride.
[0026] In some embodiments, the organic amine catalyst includes any one or a combination of at least two of triethylamine, tripropylamine, tributylamine, and diisopropylamine.
[0027] In some embodiments, the inorganic weak base catalyst includes any one or a combination of at least two of ammonia, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium acetate, and potassium acetate.
[0028] In some embodiments, the quaternary ammonium base catalyst includes any one or a combination of at least two of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide.
[0029] In some embodiments, the acid catalyst includes any one or a combination of at least two of formic acid, acetic acid, and phosphoric acid.
[0030] In some embodiments, the first solvent includes any one or a combination of at least two of the following: alcohol solvents, ether solvents, halogenated hydrocarbon solvents, ketone solvents, ester solvents, aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, and cycloalkane solvents.
[0031] In some embodiments, the alcohol solvent includes any one or a combination of at least two of methanol, ethanol, isopropanol, n-propanol, n-butanol, and isobutanol.
[0032] In some embodiments, the ether solvent includes any one or a combination of at least two of tetrahydrofuran, 1,4-dioxane, diethyl ether, and methyl tert-butyl ether.
[0033] In some embodiments, the halogenated hydrocarbon solvent includes any one or a combination of at least two of dichloromethane, trichloromethane, and 1,2-dichloroethane.
[0034] In some embodiments, the ketone solvent includes any one or a combination of at least two of acetone, butanone, methyl isobutyl ketone, and cyclohexanone.
[0035] In some embodiments, the ester solvent includes any one or a combination of at least two of methyl acetate, ethyl acetate, n-butyl acetate, and isopropyl acetate.
[0036] In some embodiments, the aromatic solvent includes toluene and / or xylene.
[0037] In some embodiments, the aliphatic hydrocarbon solvent includes n-hexane and / or n-heptane.
[0038] In some embodiments, the cycloalkane solvent includes cyclohexane and / or methylcyclohexane.
[0039] In some embodiments, the temperature of the first reaction is 20-30°C, for example, it can be 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C or 29°C.
[0040] In some implementations, the time for the first reaction is 72-120 hours, for example, 76 hours, 80 hours, 84 hours, 88 hours, 92 hours, 96 hours, 100 hours, 104 hours, 108 hours, 112 hours, or 116 hours.
[0041] In some embodiments, step (S2) includes the following raw materials by mass: 4-6 parts of oligomeric phenyl silsesquioxane, 0.05-0.1 parts of the second catalyst, 30-100 parts of the second solvent, and 1-3 parts of epoxy silane coupling agent.
[0042] The "4-6 portions" can be, for example, 4.2 portions, 4.4 portions, 4.6 portions, 4.8 portions, 5 portions, 5.2 portions, 5.4 portions, 5.6 portions, or 5.8 portions, etc.
[0043] The "0.05-0.1 parts" can be, for example, 0.06 parts, 0.07 parts, 0.08 parts, or 0.09 parts.
[0044] The "30-100 portions" can be, for example, 40 portions, 50 portions, 60 portions, 70 portions, 80 portions, or 90 portions.
[0045] Among them, "1-3 portions" can be, for example, 1.2 portions, 1.4 portions, 1.6 portions, 1.8 portions, 2 portions, 2.2 portions, 2.4 portions, 2.6 portions, or 2.8 portions, etc.
[0046] In some embodiments, the second catalyst includes any one or a combination of at least two of the following: acid catalysts, organic amine catalysts, inorganic weak base catalysts, and quaternary ammonium base catalysts.
[0047] In some embodiments, the acid catalyst includes any one or a combination of at least two of formic acid, acetic acid, and phosphoric acid.
[0048] In some embodiments, the organic amine catalyst includes any one or a combination of at least two of triethylamine, tripropylamine, tributylamine, and diisopropylamine.
[0049] In some embodiments, the inorganic weak base catalyst includes any one or a combination of at least two of ammonia, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium acetate, and potassium acetate.
[0050] In some embodiments, the quaternary ammonium base catalyst includes any one or a combination of at least two of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide.
[0051] In some embodiments, the second solvent includes any one or a combination of at least two of the following: ether solvents, aromatic solvents, halogenated hydrocarbon solvents, and ester solvents.
[0052] In some embodiments, the ether solvent includes any one or a combination of at least two of tetrahydrofuran, 1,4-dioxane, diethyl ether, and methyl tert-butyl ether.
[0053] In some embodiments, the aromatic solvent includes toluene and / or xylene.
[0054] In some embodiments, the halogenated hydrocarbon solvent includes any one or a combination of at least two of dichloromethane, trichloromethane, and 1,2-dichloroethane.
[0055] In some embodiments, the ester solvent includes any one or a combination of at least two of methyl acetate, ethyl acetate, n-butyl acetate, and isopropyl acetate.
[0056] In some embodiments, the temperature of the second reaction is 20-30°C, for example, it can be 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C or 29°C.
[0057] In some embodiments, the second reaction time is 12-60 hours, for example, it can be 16 hours, 18 hours, 20 hours, 24 hours, 28 hours, 32 hours, 36 hours, 40 hours, 44 hours, 48 hours, 52 hours or 56 hours.
[0058] In some embodiments, the epoxy silane coupling agent includes any one or a combination of at least two of 3-glycidyl etheroxypropyltrimethoxysilane, 3-glycidyl etheroxypropyltriethoxysilane, and 3-(2,3-epoxypropoxy)propylmethyldimethoxysilane.
[0059] In some embodiments, the temperature of the third reaction is 20-30°C, for example, it can be 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C or 29°C.
[0060] In some embodiments, the time for the third reaction is 12-60 hours, for example, 16 hours, 18 hours, 20 hours, 24 hours, 28 hours, 32 hours, 36 hours, 40 hours, 44 hours, 48 hours, 52 hours, or 56 hours.
[0061] In some embodiments, the third reaction is further followed by a post-processing step, which includes: adding calcium chloride to the product obtained from the third reaction to remove impurities, followed by solid-liquid separation and collection of the liquid phase; the liquid phase is then subjected to solvent removal and recrystallization to obtain the phenyl-epoxy modified polyhedral oligomeric silsesquioxane.
[0062] In some embodiments, the solid-liquid separation method includes filtration.
[0063] In some embodiments, the reagent used for recrystallization includes methanol.
[0064] In some embodiments, the photocurable resin comprises a reactive acrylate polymer and a multifunctional acrylate monomer.
[0065] In this application, the photocurable resin includes a reactive acrylate polymer and a multifunctional acrylate monomer. The molecule contains carbon-carbon double bonds and undergoes free radical polymerization under the action of a photoinitiator and irradiation to form a three-dimensional cross-linked network. The multifunctional acrylate monomer contains multiple carbon-carbon double bonds and also undergoes free radical polymerization under the action of a photoinitiator and irradiation to play a cross-linking role. The cross-linking density is increased, which improves the hardness and scratch resistance of the coating.
[0066] In some embodiments, the photoinitiator includes any one or a combination of at least two of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexylphenyl ketone, benzyl dimethyl ketal, hydroxydimethyl acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin butyl ether.
[0067] In some embodiments, the mass ratio of the reactive acrylate polymer to the polyfunctional acrylate monomer is (1-2):1, for example, it can be 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 1.9:1, etc.
[0068] In some embodiments, the reactive acrylate-based polymer includes any one or a combination of at least two of urethane acrylate oligomers, epoxide acrylate oligomers, polyester acrylates, and polyether acrylates.
[0069] In some embodiments, the multifunctional acrylate monomers include any one or a combination of at least two of the following: dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, glycerol propoxylate triacrylate, trimethylolpropane ethoxylate triacrylate, trimethylpropyl triacrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and ethylene glycol diacrylate.
[0070] In some embodiments, the photocurable coating further includes 20-60 parts of solvent by weight, for example, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or 55 parts, etc.
[0071] In some embodiments, the solvent comprises any one or a combination of at least two of the following: lower alcohols, acetates, ketones, cellosolves, dimethylformamide, tetrahydrofuran, propylene glycol monomethyl ether, toluene, and xylene, having 1 to 6 carbon atoms (e.g., 2, 3, 4, or 5, etc.).
[0072] In some embodiments, the acetate includes any one or a combination of at least two of methyl acetate, ethyl acetate, butyl acetate, and n-butyl acetate.
[0073] In some embodiments, the ketone includes any one or a combination of at least two of ethyl methyl ketone, methyl isobutyl ketone, cyclohexanone, and diisobutyl ketone.
[0074] In some embodiments, the cellosolvent includes any one or a combination of at least two of butyl cellosolvent, phenyl cellosolvent, and tert-butyl cellosolvent.
[0075] In some embodiments, the photocurable coating further includes 0.01-5 parts by weight of additives, such as 0.05 parts, 0.1 parts, 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts or 4.5 parts, etc.
[0076] In some embodiments, the additives include any one or a combination of at least two of the following: dispersants, leveling agents, wetting agents, defoamers, antistatic agents, and balancing agents.
[0077] Secondly, this application provides a method for preparing the photocurable coating described in the first aspect, the method comprising: mixing the various components of the photocurable coating evenly to obtain the photocurable coating.
[0078] Thirdly, this application provides a hard coating material prepared by a photocurable coating as described in the first aspect.
[0079] In some embodiments, the thickness of the hard coating is 2-10 μm, for example, it can be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or 9 μm.
[0080] In some embodiments, the pencil hardness of the hard coating is ≥4H, for example, it can be 4H or 5H, etc.
[0081] In some embodiments, the water contact angle of the hard coating is ≥91°, for example, it can be 91.5°, 92°, 92.5° or 93°, etc.
[0082] In some embodiments, the glass transition temperature of the hard coating is ≥122°C, for example, it can be 123°C, 124°C, 125°C, 126°C, 127°C, 128°C or 129°C.
[0083] This application adds Ph-EP-POSS to the photocurable coating, so that the hard coating prepared by the photocurable coating has high pencil hardness, high glass transition temperature and large water contact angle. The hard coating prepared by this application has the advantages of hardness, heat resistance and hydrophobicity.
[0084] Fourthly, this application provides a method for preparing a hard coating as described in the third aspect, the method comprising: applying the photocurable coating and irradiating it for curing to obtain the hard coating.
[0085] In some embodiments, the energy source used for irradiation curing includes any one or a combination of at least two of the following: ultraviolet light source, visible light source, electron beam source, and ionizing radiation source.
[0086] In some embodiments, the irradiation dose for the irradiation curing is 50-5000 mJ / cm². 2 For example, it can be 100mJ / cm 2 200mJ / cm 2 400mJ / cm 2 600mJ / cm 2 800mJ / cm 2 1000mJ / cm 2 2000mJ / cm 2 3000mJ / cm 2 Or 4000mJ / cm 2 wait.
[0087] The above enumeration of all specific point values, including the specific point values between the listed point values, is not exhaustively listed here due to space limitations and for the sake of brevity.
[0088] Fifthly, this application provides a polarizer comprising a hard coating as described in the third aspect.
[0089] Sixthly, this application provides a display device, the display device including the polarizer as described in the fifth aspect.
[0090] In some embodiments, the display device includes a liquid crystal panel.
[0091] Compared with the prior art, this application has at least the following beneficial effects: (1) This application introduces a phenyl-epoxy-modified polyhedral oligomeric silsesquioxane (Ph-EP-POSS) inorganic-organic nano-hybrid structure into a photocurable coating, and controls the amount of Ph-EP-POSS added to be 0.5-5 parts by weight, providing the hard coating with appropriate crosslinking and nano-reinforcing effects. The POSS cage-like inorganic skeleton structure imparts excellent heat resistance to the coating, and the grafting ratio of phenyl to epoxy is controlled within the range of (1.6-3):1, ensuring that the epoxy groups fully participate in the crosslinking and curing of the photocurable resin, improving the hardness, scratch resistance and heat resistance of the coating, and imparting hydrophobicity to the coating with the help of phenyl.
[0092] (2) The hard-coated pencil prepared in this application has a hardness ≥4H, a water contact angle ≥91.5°, a glass transition temperature ≥122℃, and the number of scratches appearing after 400 reciprocating rubbings of steel wool (#0000) on the hard coating under a 0.5kg load is less than 2. Furthermore, after adhesion testing using the cross-cut adhesion test, the hard coating remains completely intact and does not peel off. Therefore, the hard coating prepared in this application combines heat resistance and hydrophobicity, and exhibits good hardness and scratch resistance. Detailed Implementation
[0093] To facilitate understanding of this application, specific embodiments are provided to further illustrate the technical solutions of this application. Those skilled in the art should understand that the embodiments described are merely illustrative and should not be construed as specific limitations upon this application.
[0094] In this application, the grafting ratio of phenyl to epoxy groups in the phenyl-epoxy modified polyhedral oligomeric silsesquioxane is (1.6-3):1, and the test method for the grafting ratio is as follows: 15 mg of the phenyl-epoxy modified polyhedral oligomeric silsesquioxane to be tested was placed in an NMR tube, dissolved in 0.5 mL of deuterated chloroform, and tetramethylsilane was added as an internal standard. The NMR spectrum was measured on a 400 MHz NMR spectrometer. Phase and baseline corrections were performed on the obtained NMR spectrum. The integrated area of the phenyl proton peak (δ, 7.0-7.8 ppm, m, 5H) was recorded as A1, and the integrated area of the epoxy proton peak (δ, 2.5-3.2 ppm, m, 3H) was recorded as A2. The grafting ratio of phenyl (Ph) to epoxy (EP) was calculated using the following formula: Preparation Example 1 A phenyl-epoxy-modified polyhedral oligomeric silsesquioxane (denoted as "Ph-EP-POSS-1") is prepared by the following steps: (S1) 1 part of phenyltriethoxysilane, 4 parts of tetrabutylammonium fluoride, 35 parts of anhydrous ethanol and 0.18 parts of deionized water were subjected to hydrolysis and condensation reaction under stirring at 25°C. A white precipitate was observed at the beginning of the reaction. After 96 h of reaction, the product was filtered, the solid phase was collected and dried under vacuum to obtain oligomeric phenylsilsesquioxane. (S2) Five parts of oligophenyl silsesquioxane, 0.08 parts of formic acid, and 50 parts of tetrahydrofuran were subjected to a hydrolysis-condensation reaction at 25°C for 48 h under stirring. Then, 2.8 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added, and the hydrolysis-condensation reaction was continued at 25°C for 48 h under stirring. 0.08 parts of calcium chloride were added to the reaction system, and the mixture was stirred for 24 h to remove impurities. After filtration, the liquid phase was collected, and tetrahydrofuran was removed by rotary evaporation. The mixture was then recrystallized in icy methanol to obtain Ph-EP-POSS-1, in which the grafting ratio of phenyl to epoxy groups was 1.7:1.
[0095] Preparation Example 2 A phenyl-epoxy modified polyhedral oligomeric silsesquioxane (denoted as "Ph-EP-POSS-2") is prepared in a manner that differs from that of Preparation Example 1 only in that the amount of 3-glycidyl etheroxypropyltrimethoxysilane used in step (S2) is 1.5 parts, while the amounts of other raw materials, preparation steps, and parameters are the same as in Preparation Example 1, resulting in Ph-EP-POSS-2, wherein the grafting ratio of phenyl to epoxy groups is 2.4:1.
[0096] Preparation Example 3 A phenyl-epoxy modified polyhedral oligomeric silsesquioxane (denoted as "Ph-EP-POSS-3") was prepared in a manner that differed from that of Preparation Example 1 in that the amount of tetrabutylammonium fluoride used in step (S1) was 5.2 parts, and the reaction was carried out at 28°C for 92 h. In step (S2), the amount of 3-glycidyl etheroxypropyltrimethoxysilane used was 1 part, and the amount of formic acid used was 0.07 parts. The amounts of other raw materials, preparation steps, and parameters were the same as those in Preparation Example 1, resulting in Ph-EP-POSS-3 with a phenyl to epoxy grafting ratio of 2.9:1.
[0097] Comparative Preparation Example 1 A polyhedral oligomeric silsesquioxane (denoted as "POSS-D1") is prepared in a manner that differs from that of Preparation Example 1 only in that the amount of 3-glycidyl etheroxypropyltrimethoxysilane used in step (S2) is 0.7 parts, while the amounts of other raw materials, preparation steps, and parameters are the same as in Preparation Example 1, resulting in POSS-D1, wherein the grafting ratio of phenyl to epoxy groups is 7:1.
[0098] Comparative Preparation Example 2 A polyhedral oligomeric silsesquioxane (denoted as "POSS-D2") is prepared in a manner that differs from that of Preparation Example 1 only in that the amount of 3-glycidyl etheroxypropyltrimethoxysilane used in step (S2) is 4.7 parts. The amounts of other raw materials, preparation steps, and parameters are the same as those in Preparation Example 1, resulting in POSS-D2, wherein the grafting ratio of phenyl to epoxy groups is 1.2:1.
[0099] Comparative preparation example 3 A polyhedral oligomeric silsesquioxane (POSS-D3) is prepared in a manner that differs from that of Preparation Example 1 only in that tetrabutylammonium fluoride is replaced with triethylamine in step (S1), and step (S2) is omitted. The amounts of other raw materials, preparation steps, and parameters are the same as in Preparation Example 1, thus obtaining POSS-D3.
[0100] Comparative preparation example 4 A polyhedral oligomeric silsesquioxane (POSS-D4) is prepared in a manner that differs from that of Preparation Example 1 only in that phenyltriethoxysilane is replaced with tetraethoxysilane and tetrabutylammonium fluoride is replaced with triethylamine in step (S1), and step (S2) is omitted. The amounts of other raw materials, preparation steps, and parameters are the same as in Preparation Example 1, thus obtaining POSS-D4.
[0101] Comparative preparation example 5 A polyhedral oligomeric silsesquioxane (POSS-D5) is prepared in a manner that differs from that of Preparation Example 1 only in that step (S2) is omitted. All other preparation methods are the same as in Example 1, resulting in POSS-D5.
[0102] The raw materials used in all embodiments and comparative examples of this application are as follows: The urethane acrylate oligomer, brand name UA-306T, was purchased from Kyoeisha Chemical. Leveling agent (polyether siloxane copolymer), brand name T270, purchased from Tego Inc.
[0103] Example 1 This embodiment provides a photocurable coating comprising, by weight, the following components: 51 parts photocurable resin (the mass ratio of urethane acrylate oligomer to pentaerythritol triacrylate is 1.16:1), 1.5 parts photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts Ph-EP-POSS-1 (from Preparation Example 1), 0.05 parts leveling agent T270 (polyether siloxane copolymer, manufactured by Tego Inc.), 23 parts ethyl methyl ketone, and 24 parts methyl isobutyl ketone.
[0104] A hard coating is prepared using the photocurable coating provided in this embodiment. The specific method includes: (1) Mix the components evenly according to the above formula to obtain a light-curing coating; (2) The photocurable coating is applied to the surface of the PMMA optical film substrate and UV-cured under nitrogen purging (365nm, 300mJ / cm). 2 The hard coating is obtained by means of a process, wherein the thickness of the hard coating is 5 μm.
[0105] Example 2 This embodiment provides a photocurable coating, which comprises the following components by weight: 51 parts of photocurable resin (the mass ratio of urethane acrylate oligomer and pentaerythritol triacrylate is 1.16:1), 1.5 parts of photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of Ph-EP-POSS-2 (from Preparation Example 2), 0.05 parts of leveling agent T270 (polyether siloxane copolymer, manufactured by Tego Inc.), 23 parts of ethyl methyl ketone, and 24 parts of methyl isobutyl ketone.
[0106] A hard coating is prepared using the photocurable coating provided in this embodiment. The specific method includes: (1) Mix the components evenly according to the above formula to obtain a light-curing coating; (2) The photocurable coating is applied to the surface of the PMMA optical film substrate and UV-cured under nitrogen purging (365nm, 300mJ / cm). 2 The hard coating is obtained by means of a process, wherein the thickness of the hard coating is 5 μm.
[0107] Example 3 This embodiment provides a photocurable coating, which comprises the following components by weight: 51 parts of photocurable resin (the mass ratio of urethane acrylate oligomer and pentaerythritol triacrylate is 1.16:1), 1.5 parts of photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of Ph-EP-POSS-3 (from Preparation Example 3), 0.05 parts of leveling agent T270 (polyether siloxane copolymer, manufactured by Tego Inc.), 23 parts of ethyl methyl ketone, and 24 parts of methyl isobutyl ketone.
[0108] A hard coating is prepared using the photocurable coating provided in this embodiment. The specific method includes: (1) Mix the components evenly according to the above formula to obtain a light-curing coating; (2) The photocurable coating is applied to the surface of the PMMA optical film substrate and UV-cured under nitrogen purging (365nm, 300mJ / cm). 2 The hard coating is obtained by means of a process, wherein the thickness of the hard coating is 5 μm.
[0109] Example 4 This embodiment provides a photocurable coating, which comprises the following components by weight: 51 parts of photocurable resin (the mass ratio of urethane acrylate oligomer and pentaerythritol triacrylate is 1.16:1), 1.5 parts of photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 4 parts of Ph-EP-POSS-1 (from Preparation Example 1), 0.05 parts of leveling agent T270 (polyether siloxane copolymer, manufactured by Tego Inc.), 23 parts of ethyl methyl ketone, and 24 parts of methyl isobutyl ketone.
[0110] A hard coating is prepared using the photocurable coating provided in this embodiment. The specific method includes: (1) Mix the components evenly according to the above formula to obtain a light-curing coating; (2) The photocurable coating is applied to the surface of the PMMA optical film substrate and UV-cured under nitrogen purging (365nm, 300mJ / cm). 2 The hard coating is obtained by means of a process, wherein the thickness of the hard coating is 5 μm.
[0111] Example 5 This embodiment provides a photocurable coating, which comprises the following components by weight: 51 parts of photocurable resin (the mass ratio of urethane acrylate oligomer and pentaerythritol triacrylate is 1.85:1), 1.5 parts of photoinitiator diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 2 parts of Ph-EP-POSS-1 (from Preparation Example 1), 0.05 parts of leveling agent T270 (manufactured by Tego Inc.), 23 parts of ethyl methyl ketone, and 24 parts of methyl isobutyl ketone.
[0112] A hard coating is prepared using the photocurable coating provided in this embodiment. The specific method includes: (1) Mix the components evenly according to the above formula to obtain a light-curing coating; (2) The photocurable coating is applied to the surface of the PMMA optical film substrate and UV-cured under nitrogen purging (365nm, 300mJ / cm). 2 The hard coating is obtained by means of a process, wherein the thickness of the hard coating is 5 μm.
[0113] Comparative Example 1 This comparative example provides a photocurable coating, which differs from Example 1 only in that Ph-EP-POSS-1 is replaced with an equal mass of POSS-D1 (from Comparative Preparation Example 1); all other components and amounts are the same as in Example 1.
[0114] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0115] Comparative Example 2 This comparative example provides a photocurable coating, which differs from Example 1 only in that Ph-EP-POSS-1 is replaced with an equal mass of POSS-D2 (from Comparative Preparation Example 2); all other components and amounts are the same as in Example 1.
[0116] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0117] Comparative Example 3 This comparative example provides a photocurable coating that differs from Example 1 only in that Ph-EP-POSS-1 is replaced with an equal mass of POSS-D3 (from Comparative Preparation Example 3); all other components and amounts are the same as in Example 1.
[0118] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0119] Comparative Example 4 This comparative example provides a photocurable coating that differs from Example 1 only in that Ph-EP-POSS-1 is replaced with an equal mass of POSS-D4 (from Comparative Preparation Example 4); all other components and amounts are the same as in Example 1.
[0120] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0121] Comparative Example 5 This comparative example provides a photocurable coating that differs from Example 1 only in that Ph-EP-POSS-1 is replaced with an equal mass of POSS-D5 (from Comparative Preparation Example 5); all other components and amounts are the same as in Example 1.
[0122] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0123] Comparative Example 6 This comparative example provides a photocurable coating, which differs from Example 1 only in that the amount of Ph-EP-POSS-1 (from Preparation Example 1) added is 0.1 parts; the other components and amounts are the same as in Example 1.
[0124] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0125] Comparative Example 7 This comparative example provides a photocurable coating, which differs from Example 1 only in that the amount of Ph-EP-POSS-1 (from Preparation Example 1) added is 10 parts; the other components and amounts are the same as in Example 1.
[0126] A hard coating is prepared using the photocurable coating provided in this comparative example, and the process parameters for preparing the hard coating are the same as those in Example 1.
[0127] Performance testing: (1) Pencil hardness The hardness of the hard coating was evaluated using Mitsubishi UNI Hi-UNI series pencils. The pencil hardness tester was applied to the hard coating three times under a 500g load, and the highest hardness was measured assuming no scratches were observed.
[0128] (2) Scratch resistance On a friction tester, steel wool (#0000) was rubbed back and forth on the hard coating 400 times under a load of 0.5 kg, and the resulting scratches were counted. The scratch resistance of the hard coating was evaluated using the following markings: O represents 2 or fewer scratches, Δ represents 2 to 5 scratches, and x represents 5 or more scratches.
[0129] (3) Water contact angle Using a contact angle meter Dmo-502 manufactured by Kyowa, water droplets were dropped onto the surface of the hard coating for measurement. The smaller the contact angle, the more hydrophilic the hard coating, and the larger the contact angle, the more hydrophobic the hard coating.
[0130] (4) Adhesion Use a cross-cut tape cutter to gently score a grid on the coating. Then, use 3M 600 tape to press and smooth it onto the scored areas. After 5 minutes, peel off the tape and use a magnifying glass to observe the coating within the grid. If the coating falls off, it is considered NG (not good); if the coating is completely preserved, it is considered OK.
[0131] (5) Glass transition temperature The glass transition temperature (Tg) of the hard coating was determined using a differential scanning calorimeter (DSC-Q200, TA). The determination conditions were as follows: sample size: 5 mg, temperature range: room temperature to 400 °C, heating rate: 10 °C / min.
[0132] The specific test results of the hard coatings prepared in Examples 1-5 and Comparative Examples 1-7 are shown in Table 1.
[0133] Table 1 As shown in Table 1, the hard-coated pencils prepared in Examples 1-5 have a hardness ≥4H. After 400 cycles of reciprocating rubbing with steel wool (#0000) under a 0.5kg load, the number of scratches is less than 2, the water contact angle can reach ≥91.5°, and the adhesion test by cross-cut adhesion test shows good adhesion, with a Tg of ≥122℃. Therefore, this application demonstrates that by introducing Ph-EP-POSS into the UV-curable coating and controlling the Ph to EP grafting ratio at (1.6-3):1, and the amount of Ph-EP-POSS added at 0.5-5 parts, the prepared hard coating possesses high hardness, high scratch resistance, hydrophobicity, and heat resistance.
[0134] As can be seen from Example 1 and Comparative Example 1, when the grafting ratio of phenyl to epoxy group is too large, the number of epoxy groups grafted is insufficient, resulting in a lower degree of crosslinking of the hard coating, a lower Tg, and a decrease in the hardness, scratch resistance, and thermal stability of the hard coating.
[0135] As can be seen from Example 1 and Comparative Example 2, when the grafting ratio of phenyl to epoxy group is too small, the number of phenyl grafts is insufficient, the amount of phenyl enrichment on the surface of the hard coating is small, resulting in poor hydrophobicity of the hard coating.
[0136] As can be seen from Example 1 and Comparative Example 3, introducing only a single phenyl-modified silsesquioxane into the photocurable coating results in a decrease in the hardness grade of the hard-coated pencil, poor scratch resistance and adhesion, reduced Tg, and poor thermal stability due to the lack of crosslinkable epoxy reactive groups.
[0137] As can be seen from Example 1 and Comparative Example 4, when only POSS without phenyl and epoxy group modification is introduced into the UV-curable coating, the water contact angle of the prepared hard coating is 70.3°, which shows hydrophilicity. The Tg is only 55°, which shows poor thermal stability. It also shows poor pencil hardness, scratch resistance and adhesion.
[0138] As can be seen from Example 1 and Comparative Example 5, Comparative Example 5 omits step (S2) and only prepares oligophenyl silsesquioxane. The product is only partially condensed into random oligomers. POSS also contains a large number of silanol groups (Si-OH). The hard coating surface prepared by this comparative example has poor hydrophobicity, and the pencil hardness grade can only reach H. The scratch resistance, adhesion and thermal stability are also poor.
[0139] As can be seen from Example 1 and Comparative Example 6, when the amount of Ph-EP-POSS added is too small, the nano-reinforcing effect and cross-linking density are insufficient, and Ph-EP-POSS cannot effectively migrate to the surface of the hard coating to form a silicon-rich protective layer, resulting in poor hardness, scratch resistance, adhesion, thermal stability and hydrophobicity of the hard coating.
[0140] As can be seen from Example 1 and Comparative Example 7, when the amount of Ph-EP-POSS added is too large, local agglomeration will occur, resulting in white spots on the hard coating. Excessive cross-linking will cause the hard coating to become brittle, and the adhesion and wear resistance will decrease.
[0141] This application illustrates its technical solution through the above embodiments, but it is not limited to the above process steps, meaning that this application does not necessarily rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of the raw materials used, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this application.
Claims
1. A photocurable coating, characterized in that, The photocurable coating comprises the following components by weight: 30-70 parts of photocurable resin, 1-10 parts of photoinitiator, and 0.5-5 parts of phenyl-epoxy modified polyhedral oligomeric silsesquioxane. The grafting ratio of phenyl to epoxy groups in the phenyl-epoxy modified polyhedral oligomeric silsesquioxane is (1.6-3):
1.
2. The photocurable coating according to claim 1, characterized in that, The phenyl-epoxy modified polyhedral oligomeric silsesquioxane was prepared by the following method, which includes the following steps: (S1) A first reaction is carried out by mixing phenylalkoxysilane, a first catalyst, a first solvent and water to obtain oligomeric phenylsilsesquioxane; (S2) The oligophenyl silsesquioxane, the second catalyst, and the second solvent are mixed and subjected to a second reaction. Then, an epoxy silane coupling agent is added to carry out a third reaction to obtain the phenyl-epoxy modified polyhedral oligosilsesquioxane.
3. The photocurable coating according to claim 2, characterized in that, Step (S1) includes the following raw materials by mass: 0.5-1.5 parts of phenylalkoxysilane, 2-6 parts of the first catalyst, 30-40 parts of the first solvent, and 0.06-0.22 parts of water; And / or, the phenylalkoxysilane includes any one or a combination of at least two of phenyltriethoxysilane, phenyltrimethoxysilane, phenylmethyldimethoxysilane, and phenylmethyldiethoxysilane; And / or, the first catalyst includes any one or a combination of at least two of the following: fluoride ion catalysts, organic amine catalysts, inorganic weak base catalysts, quaternary ammonium base catalysts, and acid catalysts; And / or, the first solvent includes any one or a combination of at least two of the following: alcohol solvents, ether solvents, haloalkanes solvents, ketone solvents, ester solvents, aromatic solvents, aliphatic hydrocarbon solvents, and cycloalkanes solvents; And / or, the temperature of the first reaction is 20-30°C; And / or, the duration of the first reaction is 72-120 h; And / or, step (S2) includes the following raw materials in parts by mass: 4-6 parts of oligomeric phenyl silsesquioxane, 0.05-0.1 parts of the second catalyst, 30-100 parts of the second solvent, and 1-3 parts of epoxy silane coupling agent; And / or, the second catalyst includes any one or a combination of at least two of the following: acid catalysts, organic amine catalysts, inorganic weak base catalysts, and quaternary ammonium base catalysts; And / or, the second solvent includes any one or a combination of at least two of the following: ether solvents, aromatic solvents, haloalkanes solvents, and ester solvents; And / or, the temperature of the second reaction is 20-30°C; And / or, the second reaction takes 12-60 hours; And / or, the epoxy silane coupling agent comprises any one or a combination of at least two of 3-glycidyl etheroxypropyltrimethoxysilane, 3-glycidyl etheroxypropyltriethoxysilane, and 3-(2,3-epoxypropoxy)propylmethyldimethoxysilane. And / or, the temperature of the third reaction is 20-30°C; And / or, the third reaction takes 12-60 hours.
4. The photocurable coating according to any one of claims 1-3, characterized in that, The photocurable resin comprises a reactive acrylate polymer and a multifunctional acrylate monomer; And / or, the photoinitiator comprises any one or a combination of at least two of the following: diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, 1-hydroxycyclohexylphenyl ketone, benzyl dimethyl ketal, hydroxydimethyl acetophenone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin butyl ether.
5. The photocurable coating according to claim 4, characterized in that, The mass ratio of the reactive acrylate polymer to the multifunctional acrylate monomer is (1-2):1; And / or, the reactive acrylate-based polymer includes any one or a combination of at least two of urethane acrylate oligomers, epoxide acrylate oligomers, polyester acrylates, and polyether acrylates; And / or, the multifunctional acrylate monomers include any one or a combination of at least two of the following: dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, glycerol propoxylate triacrylate, trimethylolpropane ethoxylate triacrylate, trimethylpropyl triacrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and ethylene glycol diacrylate.
6. The photocurable coating according to any one of claims 1-5, characterized in that, The photocurable coating further includes 20-60 parts by weight of solvent, which includes any one or a combination of at least two of the following: lower alcohols having 1-6 carbon atoms, acetates, ketones, cellosolves, dimethylformamide, tetrahydrofuran, propylene glycol monomethyl ether, toluene, and xylene. And / or, the UV-curable coating further includes 0.01-5 parts by weight of additives, which include any one or a combination of at least two of dispersants, leveling agents, wetting agents, defoamers, antistatic agents, and leveling agents.
7. A hard coating, characterized in that, The hard coating is prepared by a photocurable coating as described in any one of claims 1-6.
8. The hard coating according to claim 7, characterized in that, The thickness of the hard coating is 2-10 μm; And / or, the pencil hardness of the hard coating is ≥4H.
9. A polarizer, characterized in that, The polarizer includes the hard coating as described in claim 7 or 8.
10. A display device, characterized in that, The display device includes the polarizer as described in claim 9.
Citation Information
Patent Citations
Nano-composite polarized lens
CN103257388A
Preparation method of scratch-resistant optical polyester film
CN117264260A