A weatherable high adhesion coating for tobacco packaging and method of making the same
By using components such as acrylic resin, polyurethane acrylate prepolymer and modified montmorillonite in the coating of cigarette inner liner paper, a high-adhesion and weather-resistant coating is prepared, which solves the problems of moisture absorption and insufficient adhesion of cigarette inner liner paper in high temperature and high humidity environments, and improves the moisture-proof and weather-resistant performance and appearance integrity of cigarette packaging.
Patent Information
- Application Number
- CN202611627853.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-20
AI Technical Summary
The existing coating of cigarette inner lining paper is prone to moisture and mildew in high temperature and high humidity environments, and its adhesion is insufficient, which affects the sealing and appearance integrity of cigarette packaging.
The functional additives are prepared by using components such as acrylic resin, polyurethane acrylate prepolymer, modified montmorillonite, and functional additives through hydrosilylation and imidization reactions. Combined with the hydrogen bonding between modified montmorillonite and paper-based cellulose, a coating with high adhesion and weather resistance is formed.
It significantly improves the moisture resistance, weather resistance, and adhesion of the coating, avoids delamination and peeling problems, and maintains the airtightness and appearance integrity of cigarette packaging.
Smart Images

Figure CN123131920A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of coating technology, specifically relating to a weather-resistant, high-adhesion coating for tobacco packaging and its preparation method. Background Technology
[0002] Cigarette inner lining paper is the packaging paper used as the inner layer of cigarette packs, whether soft or hard. As an important component of the cigarette packaging material system, its main functions are to wrap the cigarettes, block light, and assist in anti-counterfeiting measures. Cigarettes are quite sensitive to their storage environment; the ideal storage temperature is typically 22-27℃, and the relative humidity is 50-60%. However, retailers and ordinary consumers often lack dedicated storage facilities. Therefore, during the hot and humid rainy season and the spring dampness, cigarettes are highly susceptible to moisture and mold, which can affect their quality and safety. To reduce the adverse effects of environmental factors on cigarette quality, the surface coating of the cigarette inner lining paper must have good moisture-proof and weather-resistant properties to maintain a stable barrier effect under different temperature and humidity conditions. Simultaneously, the coating should also have high adhesion to prevent defects such as delamination and peeling during production, folding, and long-term storage. Insufficient coating adhesion not only affects the appearance and functional integrity of the inner lining paper but may also lead to a decrease in packaging airtightness, making the cigarettes more susceptible to external moisture damage.
[0003] Therefore, developing a weather-resistant, high-adhesion coating for tobacco packaging is of significant practical importance and application value. This type of coating should meet basic requirements such as moisture resistance and weather resistance while also ensuring a strong bond with the substrate, thereby improving the overall performance of the cigarette liner paper and providing more reliable packaging protection for cigarettes. Summary of the Invention
[0004] The first objective of this invention is to provide a weather-resistant, high-adhesion coating for tobacco packaging.
[0005] A second objective of this invention is to provide a method for preparing a weather-resistant, high-adhesion coating for tobacco packaging.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention relates to a weather-resistant, high-adhesion coating for tobacco packaging. By weight, the weather-resistant, high-adhesion coating comprises the following raw material components: 35-45 parts acrylic resin, 20-35 parts polyurethane acrylate prepolymer, 3-7 parts modified montmorillonite, 3-5 parts functional additives, 2-5 parts photoinitiator, 8-20 parts ethanol, 0.2-0.4 parts defoamer, 0.1-0.3 parts leveling agent, and 20-30 parts deionized water. The chemical structural formula of the functional additive is as follows: .
[0007] Preferably, the preparation process of the functional additive is as follows: (1) Dissolve Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane in anhydrous toluene, add a catalyst, heat the reactants to 70-75°C under nitrogen protection, stir and react for 24-28 h to obtain intermediate 1; (2) Add intermediate 1 and allylamine hydrochloride to pyridine and stir under reflux for 24-28 hours to obtain functional additive.
[0008] Preferably, in step (1), the ratio of 1,1,3,3,5,5,7,7-octamethyltetrasiloxane, Nadic anhydride, and anhydrous toluene is 10 mmol: 20-22 mmol: 50-60 mL; the catalyst is a Karstedt catalyst; and the amount of catalyst is 0.05-0.1 wt% of the total mass of Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane.
[0009] Preferably, in step (2), the ratio of intermediate 1, allylamine hydrochloride and pyridine is 25 mmol: 52-54 mmol: 55-65 mL.
[0010] Preferably, the preparation process of the modified montmorillonite is as follows: (a) Dissolve cyanuric chloride in ethanol, add an ethanol solution containing diethanolamine and triethylamine, stir at room temperature for 30-45 min, then heat to 50-55℃ and continue the reaction for 5-8 h to obtain intermediate 2; (b) Aminated montmorillonite was ultrasonically dispersed in acetonitrile, intermediate 2 and triethylamine were added, and the mixture was reacted at 60-65℃ for 5-8 hours. After filtration, the mixture was washed with ethanol and deionized water and dried under vacuum to obtain modified montmorillonite.
[0011] Preferably, in step (a), the ratio of cyanuric chloride, diethanolamine, and triethylamine is 0.1 mol: 0.21-0.22 mol: 21-22 g; when cyanuric chloride is dissolved in ethanol, the ratio of cyanuric chloride to ethanol is 0.1 mol: 50-55 mL; and in the ethanol solution containing diethanolamine and triethylamine, the ratio of diethanolamine to ethanol is 0.21-0.22 mol: 50-55 mL. In step (b), the ratio of amino-modified montmorillonite, intermediate 2, triethylamine and acetonitrile is 1g:0.7-1.2g:0.6-1.2g:30-50mL.
[0012] Preferably, in step (b), the preparation method of aminated montmorillonite is as follows: 3-aminopropyltriethoxysilane is added to an 85% ethanol aqueous solution, the pH is adjusted to 3-5 with acetic acid, and the mixture is stirred and hydrolyzed for 4-6 hours. Then, montmorillonite is added, and the mixture is reacted under reflux conditions for 7-9 hours. After filtration, the mixture is washed with ethanol and dried under vacuum to obtain aminated montmorillonite.
[0013] Preferably, the concentration of 3-aminopropyltriethoxysilane in the aqueous ethanol solution is 15-30 g / L; the mass ratio of montmorillonite to 3-aminopropyltriethoxysilane is 1:(0.4-0.7).
[0014] Preferably, the acrylic resin includes hard acrylic resin and soft acrylic resin, with a mass ratio of hard acrylic resin to soft acrylic resin of 1:1; the polyurethane acrylate prepolymer is a difunctional polyurethane acrylate; the photoinitiator is TPO; the defoamer is BYK-051 or BYK-052; and the leveling agent is BYK-333 or BYK-323.
[0015] This invention relates to a method for preparing a weather-resistant, high-adhesion coating for tobacco packaging, comprising the following steps: S1. First, mix 1 / 4-2 / 5 of the deionized water and acrylic resin, stir at 60-65℃ for 8-15 minutes, then add polyurethane acrylate prepolymer and functional additives and stir for 10-15 minutes to obtain a mixture; then mix ethanol and the remaining deionized water, add it to the mixture and continue stirring for 10-15 minutes; finally, add photoinitiator, modified montmorillonite, defoamer and leveling agent and stir for 20-40 minutes to obtain a weather-resistant high-adhesion coating for tobacco packaging; S2. After coating the tobacco packaging with the weather-resistant high-adhesion coating obtained in step S1 on the tobacco inner lining base paper, the coating is cured by irradiation under ultraviolet light for 5-8 minutes to obtain a weather-resistant high-adhesion coating for tobacco packaging.
[0016] Compared with the prior art, the main advantages of the present invention are as follows: 1. This invention first prepares intermediate 1 by hydrosilylation reaction of nadic anhydride with 1,1,3,3,5,5,7,7-octamethyltetrasiloxane; then, intermediate 1 is subjected to imidization reaction with allylamine hydrochloride to obtain the functional additive. This functional additive molecule has allyl carbon-carbon double bonds at both ends, which, under the action of a photoinitiator, can undergo free radical copolymerization crosslinking with the carbon-carbon double bonds in acrylic resins and polyurethane acrylate prepolymers. The functional additive's integration into the crosslinking network can, on the one hand, increase the crosslinking density and compactness of the cured coating; on the other hand, the introduction of flexible siloxane segments and alicyclic norbornene structures into the functional additive molecule's backbone can effectively improve the coating's hydrophobic properties. The synergistic effect of these two factors significantly improves the coating's moisture resistance and weather resistance.
[0017] 2. This invention also utilizes the nucleophilic disubstitution of chlorine atoms on the cyanuric chloride ring with diethanolamine to obtain intermediate 2. The molecule retains an active triazine ring C-Cl and introduces multiple hydroxyl-containing side chains. The residual C-Cl of intermediate 2 undergoes nucleophilic substitution with the primary amino groups on the surface of aminated montmorillonite, grafting them onto the montmorillonite sheets to obtain modified montmorillonite. The numerous hydroxyl groups on the surface of modified montmorillonite improve the dispersibility of inorganic fillers in organic resins and form hydrogen bonds with coating resins to strengthen the internal bonding of the coating. Simultaneously, they form hydrogen bonds with hydroxyl groups on the surface of paper-based cellulose, promoting the wetting and anchoring of the coating onto the paper fibers, effectively improving the adhesion of the coating to the paper substrate and preventing delamination and warping problems. Furthermore, the conjugated triazine ring grafted onto the surface of modified montmorillonite can absorb and dissipate ultraviolet energy, inhibiting the photo-oxidative degradation of the resin and paper substrate; while the exfoliated montmorillonite nanosheets can scatter and reflect ultraviolet light and construct a labyrinthine barrier structure, synergistically enhancing the anti-aging ability of the coating. Attached Figure Description
[0018] Figure 1 The infrared spectra of the modified montmorillonite and aminated montmorillonite obtained in Example 1 of this invention are shown. Detailed Implementation
[0019] The technical solution of the present invention will be further described below with reference to specific embodiments. However, those skilled in the art should understand that the following embodiments are only for illustrating the present invention and should not be regarded as limiting the present invention. Specific conditions not specified in the embodiments are performed according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the reagents or instruments used are all conventional products obtained through commercial channels.
[0020] In this embodiment of the invention, the acrylic resin includes hard acrylic resin and soft acrylic resin in a mass ratio of 1:1, wherein the Tg of the hard acrylic resin is 120-130℃ and the Tg of the soft acrylic resin is 20-25℃; the polyurethane acrylate prepolymer is an aliphatic polyurethane acrylate with a functionality of 2.
[0021] Example 1 This embodiment provides a weather-resistant, high-adhesion coating for tobacco packaging, comprising, by weight: 40 parts acrylic resin, 30 parts polyurethane acrylate prepolymer, 5 parts modified montmorillonite, 4 parts functional additives, 3 parts photoinitiator (TPO), 15 parts ethanol, 0.3 parts defoamer (BYK-051), 0.2 parts leveling agent (BYK-323), and 25 parts deionized water.
[0022] The preparation process of the functional additives is as follows: (1) Dissolve Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane in anhydrous toluene, and add a catalyst (platinum(0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, Karstedt catalyst). The ratio of 1,1,3,3,5,5,7,7-octamethyltetrasiloxane, Nadic anhydride and anhydrous toluene is 10 mmol: 21 mmol: 55 mL. The amount of catalyst is 0.08 wt% of the total mass of Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane. Under nitrogen protection, the reactants were heated to 75°C and stirred for 26 hours. Insoluble matter was removed by filtration, and the filtrate was concentrated by rotary evaporation. The residue was redissolved in dichloromethane, and n-hexane was added to precipitate the product. The product was washed with n-hexane and dried under vacuum to give intermediate 1 (yield 81.9%). 1 HNMR: (C 26 H 42 O9Si4, 400MHz, DMSO- d6 ) δ: 0.11 (s, 12H), 0.19 (s, 12H), 1.0-1.5 (m, 6H), 1.85-2.15 (m, 8H), 2.86 (m, 4H). MS (ESI) m / z=610.23 [M].
[0023] (2) Intermediate 1 and allylamine hydrochloride were added to pyridine in a ratio of 25 mmol:53 mmol:60 mL. After stirring under reflux for 26 h, the mixture was cooled to room temperature, concentrated, extracted with dichloromethane, washed with saturated brine, dried over anhydrous sodium sulfate, and purified by silica gel column chromatography (ethyl acetate:petroleum ether volume ratio 2:1) to obtain the functional additive (yield 55.1%). The functional additive... 1 HNMR: (C 32 H 52 N₂O₇Si₄, 400MHz, DMSO- d6 ) δ: 0.12 (s, 12H), 0.19 (s, 12H), 1.0-1.5 (m, 6H), 1.82-2.19 (m, 8H), 3.1 6-3.24 (m, 4H), 3.98-4.12 (m, 4H), 5.15-5.25 (m, 4H), 5.73-5.84 (m, 2H). MS (ESI) m / z=688.24 [M].
[0024] The preparation process of modified montmorillonite is as follows: (a) Dissolve cyanuric chloride in ethanol, add an ethanol solution containing diethanolamine and triethylamine, the ratio of cyanuric chloride, diethanolamine, and triethylamine is 0.1 mol: 0.21 mol: 21 g; the ratio of cyanuric chloride to ethanol is 0.1 mol: 55 mL; in the ethanol solution containing diethanolamine and triethylamine, the ratio of diethanolamine to ethanol is 0.21 mol: 55 mL. After stirring at room temperature for 40 min, the temperature is raised to 55 °C and the reaction continues for 6 h. After cooling to room temperature, filter, wash the filtrate with saturated sodium bicarbonate aqueous solution until neutral, dry with calcium chloride, filter, and evaporate the solvent to obtain intermediate 2; intermediate 2 1 HNMR: (C 11 H 20 N5O4Cl, 400MHz, DMSO- d6 ) δ: 3.58-3.65 (t, 8H), 3.77-3.86 (t, 8H), 4.83 (s, 4H). MS (ESI) m / z=321.15 [M].
[0025] (b) Preparation of aminated montmorillonite: 3-aminopropyltriethoxysilane was added to an 85% aqueous ethanol solution, the pH was adjusted to 4 with acetic acid, and the mixture was stirred and hydrolyzed for 5 h. Then montmorillonite was added, and the mixture was reacted under reflux for 8 h. After filtration, the mixture was washed with ethanol and dried under vacuum to obtain aminated montmorillonite. The concentration of 3-aminopropyltriethoxysilane in the aqueous ethanol solution was 20 g / L. The mass ratio of montmorillonite to 3-aminopropyltriethoxysilane was 1:0.6.
[0026] Aminated montmorillonite was ultrasonically dispersed in acetonitrile, and intermediate 2 and triethylamine were added. The ratio of aminated montmorillonite, intermediate 2, triethylamine and acetonitrile was 1 g: 1.0 g: 0.9 g: 40 mL. After reacting at 65 °C for 7 h, the mixture was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified montmorillonite. Figure 1 The infrared spectra of the modified montmorillonite and the aminated montmorillonite are shown. In the figure, the aminated montmorillonite shows peak values at 2940 and 2870 cm⁻¹. -1 The characteristic vibrational peak of the methylene group appears at 1620 cm⁻¹. -1 The presence of a characteristic vibrational peak of -NH2 at 1575 and 1507 cm⁻¹ indicates the successful preparation of aminated montmorillonite; compared with aminated montmorillonite, the modified montmorillonite exhibits higher vibrational peaks at 1575 and 1507 cm⁻¹. -1 The characteristic vibrational peaks of -NH- and the C=N of the triazine ring appear at 3400 cm⁻¹. -1 The characteristic vibrational peaks of the left and right hydroxyl groups were significantly enhanced, indicating that the modification of montmorillonite was successful.
[0027] This embodiment provides a method for preparing a weather-resistant, high-adhesion coating for tobacco packaging, comprising the following steps: S1. First, mix 2 / 5 of the deionized water and acrylic resin, stir at 65°C for 15 minutes, then add polyurethane acrylate prepolymer and functional additives and stir for 15 minutes to obtain a mixture; then mix ethanol and the remaining deionized water, add to the above mixture and continue stirring for 15 minutes; finally, add photoinitiator, modified montmorillonite, defoamer and leveling agent and stir for 30 minutes to obtain a weather-resistant high-adhesion coating for tobacco packaging. S2. After coating the tobacco packaging inner liner base paper with the weather-resistant, high-adhesion coating obtained in step S1, the coating amount is 15 g / m². 2 After being irradiated with ultraviolet light for 8 minutes, the coating is cured to obtain a weather-resistant and highly adhesive coating for tobacco packaging.
[0028] Example 2 This embodiment provides a weather-resistant, high-adhesion coating for tobacco packaging, comprising, by weight: 45 parts acrylic resin, 35 parts polyurethane acrylate prepolymer, 7 parts modified montmorillonite, 5 parts functional additives, 5 parts photoinitiator (TPO), 20 parts ethanol, 0.4 parts defoamer (BYK-052), 0.3 parts leveling agent (BYK-323), and 30 parts deionized water.
[0029] The preparation process of the functional additives is as follows: (1) Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane were dissolved in anhydrous toluene, and a catalyst (platinum(O)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, Karstedt catalyst) was added. The ratio of 1,1,3,3,5,5,7,7-octamethyltetrasiloxane, nadic anhydride, and anhydrous toluene was 10 mmol: 22 mmol: 60 mL; the amount of catalyst was 0.1 wt% of the total mass of nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane. The reactants were heated to 75 °C under nitrogen protection and stirred for 24 h. The insoluble matter was removed by filtration, and the filtrate was concentrated by rotary evaporation. The residue was redissolved in dichloromethane, and n-hexane was added to precipitate the product. The product was washed with n-hexane and dried under vacuum to obtain intermediate 1 (yield 80.1%). (2) Intermediate 1 and allylamine hydrochloride were added to pyridine, with the ratio of intermediate 1, allylamine hydrochloride and pyridine being 25 mmol: 54 mmol: 65 mL. After stirring under reflux for 28 h, the mixture was cooled to room temperature, concentrated, extracted with dichloromethane, washed with saturated brine, dried over anhydrous sodium sulfate, and purified by silica gel column chromatography (ethyl acetate: petroleum ether volume ratio of 2:1) to obtain the functional additive (yield 52.3%).
[0030] The preparation process of modified montmorillonite is as follows: (a) Dissolve cyanuric chloride in ethanol, and add an ethanol solution containing diethanolamine and triethylamine. The ratio of cyanuric chloride, diethanolamine, and triethylamine is 0.1 mol: 0.22 mol: 22 g; the ratio of cyanuric chloride to ethanol is 0.1 mol: 55 mL; in the ethanol solution containing diethanolamine and triethylamine, the ratio of diethanolamine to ethanol is 0.22 mol: 55 mL. After stirring at room temperature for 45 min, the temperature is raised to 55 °C and the reaction continues for 5 h. After cooling to room temperature, the mixture is filtered. The resulting filtrate is washed with a saturated sodium bicarbonate aqueous solution until neutral, dried over calcium chloride, filtered, and the solvent is evaporated to obtain intermediate 2.
[0031] (b) Preparation of aminated montmorillonite: 3-aminopropyltriethoxysilane was added to an 85% aqueous ethanol solution, the pH was adjusted to 5 with acetic acid, and the mixture was stirred and hydrolyzed for 6 h. Then montmorillonite was added, and the mixture was reacted under reflux for 9 h. After filtration, the mixture was washed with ethanol and dried under vacuum to obtain aminated montmorillonite. The concentration of 3-aminopropyltriethoxysilane in the aqueous ethanol solution was 30 g / L. The mass ratio of montmorillonite to 3-aminopropyltriethoxysilane was 1:0.7.
[0032] Aminated montmorillonite was ultrasonically dispersed in acetonitrile, and intermediate 2 and triethylamine were added. The ratio of aminated montmorillonite, intermediate 2, triethylamine, and acetonitrile was 1 g: 1.2 g: 1.2 g: 50 mL. After reacting at 65 °C for 5 h, the mixture was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified montmorillonite.
[0033] The preparation method of the weather-resistant, high-adhesion coating for tobacco packaging in this embodiment is the same as in Embodiment 1.
[0034] Example 3 This embodiment provides a weather-resistant, high-adhesion coating for tobacco packaging, comprising, by weight: 35 parts acrylic resin, 20 parts polyurethane acrylate prepolymer, 3 parts modified montmorillonite, 3 parts functional additives, 2 parts photoinitiator (TPO), 8 parts ethanol, 0.2 parts defoamer (BYK-051), 0.1 parts leveling agent (BYK-333), and 20 parts deionized water.
[0035] The preparation process of the functional additives is as follows: (1) Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane were dissolved in anhydrous toluene, and a catalyst (platinum(O)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex, Karstedt catalyst) was added. The ratio of 1,1,3,3,5,5,7,7-octamethyltetrasiloxane, nadic anhydride, and anhydrous toluene was 10 mmol: 20 mmol: 50 mL; the amount of catalyst was 0.05 wt% of the total mass of nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane. The reactants were heated to 70 °C under nitrogen protection and stirred for 28 h. The insoluble matter was removed by filtration, and the filtrate was concentrated by rotary evaporation. The residue was redissolved in dichloromethane, and n-hexane was added to precipitate the product. The product was washed with n-hexane and dried under vacuum to obtain intermediate 1 (yield 78.4%). (2) Intermediate 1 and allylamine hydrochloride were added to pyridine, with the ratio of intermediate 1, allylamine hydrochloride and pyridine being 25 mmol: 52 mmol: 55 mL. After stirring under reflux for 24 h, the mixture was cooled to room temperature, concentrated, extracted with dichloromethane, washed with saturated brine, dried over anhydrous sodium sulfate, and purified by silica gel column chromatography (ethyl acetate: petroleum ether volume ratio of 2:1) to obtain the functional additive (yield 49.5%).
[0036] The preparation process of modified montmorillonite is as follows: (a) Dissolve cyanuric chloride in ethanol, and add an ethanol solution containing diethanolamine and triethylamine. The ratio of cyanuric chloride, diethanolamine, and triethylamine is 0.1 mol: 0.21 mol: 21 g; the ratio of cyanuric chloride to ethanol is 0.1 mol: 50 mL; in the ethanol solution containing diethanolamine and triethylamine, the ratio of diethanolamine to ethanol is 0.21 mol: 50 mL. After stirring at room temperature for 30 min, the temperature is raised to 50 °C and the reaction continues for 8 h. After cooling to room temperature, the mixture is filtered. The resulting filtrate is washed with a saturated sodium bicarbonate aqueous solution until neutral, dried over calcium chloride, filtered, and the solvent is evaporated to obtain intermediate 2.
[0037] (b) Preparation of aminated montmorillonite: 3-aminopropyltriethoxysilane was added to an 85% aqueous ethanol solution, the pH was adjusted to 3 with acetic acid, and the mixture was stirred and hydrolyzed for 4 h. Then montmorillonite was added, and the mixture was reacted under reflux for 7 h. After filtration, the mixture was washed with ethanol and dried under vacuum to obtain aminated montmorillonite. The concentration of 3-aminopropyltriethoxysilane in the aqueous ethanol solution was 15 g / L. The mass ratio of montmorillonite to 3-aminopropyltriethoxysilane was 1:0.4.
[0038] Aminated montmorillonite was ultrasonically dispersed in acetonitrile, and intermediate 2 and triethylamine were added. The ratio of aminated montmorillonite, intermediate 2, triethylamine, and acetonitrile was 1 g: 0.7 g: 0.6 g: 30 mL. After reacting at 60 °C for 8 h, the mixture was filtered, washed with ethanol and deionized water, and vacuum dried to obtain modified montmorillonite.
[0039] The preparation method of the weather-resistant, high-adhesion coating for tobacco packaging in this embodiment is the same as in Embodiment 1.
[0040] Comparative Example 1 The difference between this comparative example and Example 1 is that the modified montmorillonite is replaced with montmorillonite, otherwise it is the same as Example 1.
[0041] Comparative Example 2 The difference between this comparative example and Example 1 is that the functional additive is replaced with intermediate 1, while the rest is the same as Example 1.
[0042] Test case According to relevant standards, the weather-resistant and high-adhesion coatings for tobacco packaging obtained in Examples 1-3 and Comparative Examples 1-2 were prepared into test samples for performance determination, as follows: 1. The adhesion of each group of test samples was tested in accordance with GB / T 9286-2021 "Paints and Varnishes Cross-cut Test". The grade range was 0 to 5, with grade 0 representing no peeling.
[0043] 2. The wear resistance of each group of test samples was tested according to ASTM D4060-19, with a grinding wheel of CS-17 and a load of 1000g.
[0044] 3. Continuous radiation tests were conducted on each group of test samples using a xenon lamp aging test chamber. The blackboard temperature was set to 65℃, the relative humidity to 50%, and the irradiation intensity to 0.51W per square meter at a wavelength of 340nm. After 72 hours of continuous illumination, the color difference (ΔE) of the samples before and after aging was measured. A smaller color difference value indicates better lightfastness.
[0045] 4. The water vapor transmission rate of each group of test samples was tested in accordance with GB / T26253-2010 "Determination of water vapor transmission rate of plastic films and sheets".
[0046] 5. The weather-resistant, high-adhesion coatings for tobacco packaging obtained in Examples 1-3 and Comparative Examples 1-2 were applied to cigarette packaging of the same batch of tobacco, and cigarette samples were prepared on the same day, with an initial moisture content of 12.9%. The cigarette samples were placed in a constant temperature and humidity environment (22°C, 80% relative humidity) and a dry environment (22°C, 30% relative humidity) for 30 days to equilibrate. After unpacking and placing in the same environment for 48 hours, the moisture content of the cigarettes was tested according to GB / T22838.8-2009 "Determination of Physical Properties of Cigarettes and Filter Rods - Part 8: Moisture Content". The results are shown in Table 1.
[0047] Table 1 As shown in Table 1, the weather-resistant and high-adhesion coatings for tobacco packaging obtained in Examples 1-3 of this invention exhibit better moisture resistance, weather resistance, and adhesion compared to Comparative Examples 1-2. Furthermore, when the obtained coatings are used in cigarette packaging, the fluctuation range of the moisture content of the cigarettes after unpacking is smaller under different humidity conditions. The reason for this is that the functional additive molecules of this invention have allyl carbon-carbon double bonds at both ends. Under the action of a photoinitiator, they can undergo free radical copolymerization and crosslinking with the carbon-carbon double bonds in acrylic resin and polyurethane acrylate prepolymer, increasing the crosslinking density of the cured coating. Simultaneously, the introduction of flexible siloxane segments and alicyclic norbornene structures into the molecular skeleton effectively improves the hydrophobic properties of the coating and enhances its moisture resistance and weather resistance. The numerous hydroxyl groups on the surface of the modified montmorillonite of this invention not only improve the dispersibility of inorganic fillers in organic resins but also form hydrogen bonds with coating resins to strengthen the internal bonding of the coating. Simultaneously, they form hydrogen bonds with the hydroxyl groups on the surface of paper-based cellulose, promoting the wetting and anchoring of the coating onto the paper fibers, effectively improving the adhesion of the coating to the paper substrate and preventing delamination and curling problems.
[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. Based on the present invention, some modifications or substitutions can be made, but these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of protection claimed by the present invention.
Claims
1. A weather-resistant, high-adhesion coating for tobacco packaging, characterized in that, By weight, the weather-resistant, high-adhesion coating comprises the following raw material components: 35-45 parts acrylic resin, 20-35 parts polyurethane acrylate prepolymer, 3-7 parts modified montmorillonite, 3-5 parts functional additives, 2-5 parts photoinitiator, 8-20 parts ethanol, 0.2-0.4 parts defoamer, 0.1-0.3 parts leveling agent, and 20-30 parts deionized water; The chemical structural formula of the functional additive is as follows: .
2. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 1, characterized in that, The preparation process of the functional additive is as follows: (1) Dissolve Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane in anhydrous toluene, add a catalyst, heat the reactants to 70-75°C under nitrogen protection, stir and react for 24-28 h to obtain intermediate 1; (2) Add intermediate 1 and allylamine hydrochloride to pyridine and stir under reflux for 24-28 hours to obtain functional additive.
3. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 2, characterized in that, In step (1), the ratio of 1,1,3,3,5,5,7,7-octamethyltetrasiloxane, Nadic anhydride, and anhydrous toluene is 10 mmol: 20-22 mmol: 50-60 mL; the catalyst is Karstedt catalyst; the amount of catalyst is 0.05-0.1 wt% of the total mass of Nadic anhydride and 1,1,3,3,5,5,7,7-octamethyltetrasiloxane.
4. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 2, characterized in that, In step (2), the ratio of intermediate 1, allylamine hydrochloride and pyridine is 25 mmol: 52-54 mmol: 55-65 mL.
5. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 1, characterized in that, The preparation process of the modified montmorillonite is as follows: (a) Dissolve cyanuric chloride in ethanol, add an ethanol solution containing diethanolamine and triethylamine, stir at room temperature for 30-45 min, then heat to 50-55℃ and continue the reaction for 5-8 h to obtain intermediate 2; (b) Aminated montmorillonite was ultrasonically dispersed in acetonitrile, intermediate 2 and triethylamine were added, and the mixture was reacted at 60-65℃ for 5-8 hours. After filtration, the mixture was washed with ethanol and deionized water and dried under vacuum to obtain modified montmorillonite.
6. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 5, characterized in that, In step (a), the ratio of cyanuric chloride, diethanolamine, and triethylamine is 0.1 mol: 0.21-0.22 mol: 21-22 g; when cyanuric chloride is dissolved in ethanol, the ratio of cyanuric chloride to ethanol is 0.1 mol: 50-55 mL; in the ethanol solution containing diethanolamine and triethylamine, the ratio of diethanolamine to ethanol is 0.21-0.22 mol: 50-55 mL. In step (b), the ratio of amino-modified montmorillonite, intermediate 2, triethylamine and acetonitrile is 1g:0.7-1.2g:0.6-1.2g:30-50mL.
7. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 5, characterized in that, In step (b), the preparation method of aminated montmorillonite is as follows: 3-aminopropyltriethoxysilane is added to an 85% ethanol aqueous solution, the pH is adjusted to 3-5 with acetic acid, and the mixture is stirred and hydrolyzed for 4-6 hours. Then, montmorillonite is added, and the mixture is reacted under reflux conditions for 7-9 hours. After filtration, the mixture is washed with ethanol and dried under vacuum to obtain aminated montmorillonite.
8. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 7, characterized in that, The concentration of 3-aminopropyltriethoxysilane in an aqueous ethanol solution is 15-30 g / L; the mass ratio of montmorillonite to 3-aminopropyltriethoxysilane is 1:(0.4-0.7).
9. The weather-resistant, high-adhesion coating for tobacco packaging according to claim 1, characterized in that, The acrylic resin includes hard acrylic resin and soft acrylic resin, with a mass ratio of 1:1; the polyurethane acrylate prepolymer is a difunctional polyurethane acrylate; the photoinitiator is TPO; the defoamer is BYK-051 or BYK-052; and the leveling agent is BYK-333 or BYK-323.
10. The method for preparing a weather-resistant, high-adhesion coating for tobacco packaging according to any one of claims 1-9, characterized in that, Includes the following steps: S1. First, mix 1 / 4-2 / 5 of the deionized water and acrylic resin, stir at 60-65℃ for 8-15 minutes, then add polyurethane acrylate prepolymer and functional additives and stir for 10-15 minutes to obtain a mixture; then mix ethanol and the remaining deionized water, add it to the mixture and continue stirring for 10-15 minutes; finally, add photoinitiator, modified montmorillonite, defoamer and leveling agent and stir for 20-40 minutes to obtain a weather-resistant high-adhesion coating for tobacco packaging; S2. After coating the tobacco packaging with the weather-resistant high-adhesion coating obtained in step S1 on the tobacco inner lining base paper, the coating is cured by irradiation under ultraviolet light for 5-8 minutes to obtain a weather-resistant high-adhesion coating for tobacco packaging.